Positive electrode active material, secondary battery, battery module, battery pack and power consuming device

A tailored blend of nickel-containing cathode materials with varying particle sizes and coatings addresses structural instability in high-nickel batteries, enhancing energy density and high-temperature performance.

JP7579987B2Active Publication Date: 2024-11-08CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023552308
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-06-24
Publication Date
2024-11-08
Estimated Expiration
2042-06-24

AI Technical Summary

Technical Problem

Conventional high-nickel cathode active materials in lithium-ion batteries face issues with structural stability, leading to reduced energy density, cycle performance, and safety due to particle fracture and increased side reactions, particularly at high temperatures.

Method used

A positive electrode active material comprising a blend of three different nickel-containing compounds with varying particle sizes and nickel contents, specifically designed to enhance consolidation density and stability, including polycrystalline and pseudo-monocrystalline materials, stabilized with surface coatings.

Benefits of technology

The solution results in batteries with improved energy density, safety, and high-temperature performance, including enhanced cycle life and storage stability by minimizing particle fracture and side reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579987000003
    Figure 0007579987000003
  • Figure 0007579987000004
    Figure 0007579987000004
  • Figure 0007579987000005
    Figure 0007579987000005
Patent Text Reader

Abstract

The present application relates to a positive electrode active material having the formula: Li x1 Ni a1 Co b1 Mn c1 O 2-y1 Q y1 I and active material A, whose composition formula is Li x2 Ni a2 Co b2 Mn c2 O 2-y2 Q y2 II, and active material B, whose composition formula is Li x3 Ni a3 Co b3 Mn c3 O 2-y3 Q y3 and active material C, which is III, wherein in formulas I, II, and III, each subscript is as defined in the specification, and wherein the average particle size Dv50 of active material A is greater than the average particle size Dv50 of active material B and greater than the average particle size Dv50 of active material C. The compaction density of the positive electrode active material of the present application is high, so that the corresponding battery has high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the technical field of lithium batteries, and in particular to positive electrode active materials, secondary batteries, battery modules, battery packs and power consuming devices. [Background technology]

[0002] In recent years, as the application scope of lithium-ion batteries becomes wider and wider, lithium-ion batteries are widely used in energy storage power systems such as hydroelectric, thermal, wind and solar power stations, as well as in multiple fields such as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, etc. As lithium-ion batteries have made great strides in development, the requirements for their energy density, cycle performance and safety performance are also increasing. In addition, due to the limited options for positive electrode active materials, high nickel positive electrode active materials are considered to be the most desirable option to meet the requirements for high energy density.

[0003] However, with the increase in nickel content, its structural stability is increasingly lower. Currently, it is an effective means to improve the rate performance and cycle performance of materials by means such as coating or doping. However, all of the conventional methods may impair the performance of lithium-ion batteries to some extent, such as reducing the gram capacity of lithium-ion batteries and reducing cycle performance. Therefore, conventional coated or doped positive electrode materials still have room for improvement. Summary of the Invention

[0004] The present application has been made in view of the above problems, and an object of the present application is to provide a positive electrode active material which has a large compaction density for the corresponding electrode plate, and which provides the corresponding battery with high energy density and safety, while at the same time providing good high-temperature cycle performance and high-temperature storage performance.

[0005] In order to achieve the above object, according to a first aspect of the present application, there is provided a positive electrode active material, the positive electrode active material comprising: An active material A having the following composition formula: Li x1 Ni a1 Co b1 Mn c1 O 2-y1 Q y1 I In formula I, 0.95≦x1≦1.3, 0.7≦a1≦0.99, 0.01≦b1≦0.15, 0.01≦c1≦0.3, a1+b1+c1=1, 0≦y1≦0.1, and Q is one or more selected from S, N, F, Cl, Br, and I; An active material B having the following composition formula: Li x2 Ni a2 Co b2 Mn c2 O 2-y2 Q y2 II In formula II, 0.95≦x2≦1.3, 0.7≦a2≦0.99, 0.01≦b2≦0.15, 0.01≦c2≦0.3, a2+b2+c2=1, 0≦y2≦0.1, and Q is one or more selected from S, N, F, Cl, Br and I; An active material C having the following composition formula: Li x3 Ni a3 Co b3 Mn c3 O 2-y3 Q y3 III and an active material C, in which, in formula III, 0.95≦x3≦1.3, 0.3≦a3<0.7, 0.01≦b3≦0.15, 0.01≦c3≦0.5, a3+b3+c3=1, 0≦y3≦0.1, and Q is one or more selected from S, N, F, Cl, Br and I; Here, the average particle diameter Dv50 of the active material A is larger than the average particle diameter Dv50 of the active material B, and is also larger than the average particle diameter Dv50 of the active material C.

[0006] As a result, the positive electrode active material of the present application contains active materials A, B, and C which have different average particle sizes and nickel contents, thereby increasing the compaction density of the corresponding electrode plate, and thus the corresponding battery has high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0007] In any embodiment, active material A has an average particle size Dv50 of 7 to 15 μm, optionally 8 to 14 μm, and a Dv90 of 15 to 25 μm, optionally 18 to 22 μm; active material B has an average particle size Dv50 of 1 to 8 μm, optionally 2 to 5 μm, and a Dv90 of 3 to 10 μm, optionally 5 to 8 μm; active material C has an average particle size Dv50 is 1 to 7 μm, optionally 2 to 5 μm, and Dv90 is 5 to 10 μm, optionally 5 to 8 μm. By further limiting the average particle size of each active material, the compaction density of the positive electrode plate containing the positive electrode active material is further improved, so that the corresponding battery has high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0008] In any embodiment, the content ratio of the active material A to the active material B to the active material C is 1:0.5-8:0.1-10, optionally 1:0.8-6:0.2-8, and further optionally 1:1.5-6:3-8. This allows the specific ratio of active materials to further increase the compaction density of the positive electrode plate containing the positive electrode active material, so that the corresponding battery has high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0009] In an optional embodiment, the sum of the contents of the active material A and the active material B is equal to the content of the active material C, and each content is calculated based on the total weight of the positive electrode active materials. Thus, the specific content of each active material further increases the compaction density of the positive electrode plate including the positive electrode active materials, so that the corresponding battery has high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0010] In an optional embodiment, the specific surface area of ​​the positive electrode active material is 0.3 to 1.8 m 2 / g, and the compaction density is 3.0 to 3.6 g / cm 3 As a result, the positive electrode active material having a specific specific surface area and compaction density allows the corresponding battery to have high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0011] In any embodiment, the active material A and / or the active material B and / or the active material C includes an element M, where M is selected from one or more of Zr, Sr, B, Ti, Mg, Sn, and Al, by subjecting each of the active materials to the above treatment, the phase structure of the material surface can be stabilized, side reactions during charging and discharging can be suppressed, and the corresponding battery can be provided with high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0012] In an optional embodiment, in the chemical formulas corresponding to the active material A, the active material B, and the active material C, x1:x2:x3 is 1:(0.73-1.37):(0.73-1.37), and a1:a2:a3 is 1:(0.71-1.42):(0.31-1). By limiting the ratio of lithium to nickel in each active material, the corresponding battery is provided with high energy density and safety, and at the same time, with good high-temperature cycle performance and high-temperature storage performance.

[0013] In an optional embodiment, active material A is a polycrystalline material, and active materials B and C are pseudo-single crystalline or single crystalline materials, thereby limiting the crystal type of each active material, thereby further providing the corresponding battery with high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0014] According to a second aspect of the present application, there is further provided a secondary battery comprising the positive electrode active material according to the first aspect of the present application.

[0015] As a result, the resulting battery has high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0016] According to a third aspect of the present application, there is provided a battery module including the secondary battery according to the second aspect of the present application.

[0017] According to a fourth aspect of the present application, there is provided a battery pack including the battery module of the third aspect of the present application.

[0018] According to a fifth aspect of the present application, there is provided a power consuming device including at least one selected from the secondary battery of the second aspect of the present application, the battery module of the third aspect of the present application, or the battery pack of the fourth aspect of the present application.

[0019] The positive electrode active material of the present application contains active materials A, B, and C which have different average particle sizes and nickel contents, thereby increasing the compaction density of a positive electrode plate containing the positive electrode active material, and further providing the corresponding battery with high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a schematic diagram of a secondary battery according to an embodiment of the present application. [Diagram 2] FIG. 2 is an exploded view of the secondary battery according to the embodiment of the present application shown in FIG. [Diagram 3] FIG. 1 is a schematic diagram of a battery module according to an embodiment of the present application. [Figure 4] FIG. 1 is a schematic diagram of a battery pack according to an embodiment of the present application. [Diagram 5] FIG. 5 is an exploded view of the battery pack shown in FIG. 4 according to an embodiment of the present application. [Figure 6] 1 is a schematic diagram of a power consuming device in which a secondary battery according to an embodiment of the present application is used as a power source; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, with reference to the drawings, the present application will be described in detail with respect to the embodiments specifically disclosing the positive electrode active material and the manufacturing method thereof, the positive electrode plate, the secondary battery, the battery module, the battery pack, and the electric device. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and duplicated description of the same structure may be omitted. This is to avoid the following description from being unnecessarily long and to allow those skilled in the art to easily understand. Note that the drawings and the following description are provided to allow those skilled in the art to fully understand the present application, and do not limit the subject matter described in the claims.

[0022] The "ranges" disclosed in this application are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Such defined ranges may be inclusive or exclusive of the end values, and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also envisaged. It is noted that if 1 and 2 are listed as the minimum range values, and 3, 4, and 5 are listed as the maximum range values, the ranges 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 are all envisaged. In this application, unless otherwise specified, the numerical range "ab" represents a shorthand representation of any combination of real numbers a to b, where a and b are both real numbers. For example, the numerical range "0-5" represents a list of all real numbers between "0-5" already listed in this specification, and "0-5" is just a shorthand representation of combinations of these numbers. Also, expressing a parameter as an integer ≧2 is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0023] Unless otherwise stated, all the embodiments and optional embodiments in the present application can be combined with each other to form a new technical solution.

[0024] Unless otherwise stated, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0025] Unless otherwise stated, all steps in this application may be performed in sequence or randomly, and preferably in sequence. For example, the method includes steps (a) and (b) to mean that the method may include steps (a) and (b) performed in sequence, or steps (b) and (a) performed in sequence. For example, the method may further include step (c) as mentioned above to mean that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), may include steps (c), (a) and (b), etc.

[0026] Unless otherwise specified, the terms "comprise" and "include" referred to in this application may be open ended or closed ended. For example, the terms "comprise" and "include" may further include or include other ingredients not listed, or may include or include only the ingredients listed.

[0027] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, "A or B" is satisfied in the following cases: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) but B is true (or exists); and A and B are both true (or exist).

[0028] At present, the general high nickel positive electrode active material is mainly composed of secondary particle aggregation, polycrystalline form. As the Ni content of the high nickel positive electrode active material increases, the gram capacity of the material also increases accordingly. However, the high nickel polycrystalline secondary particle material has the following problems: 1) low deposition density, low compaction density of the produced electrode plate, further reducing the specific energy of the battery; 2) the particles are very easy to be crushed, the specific surface area of ​​the material increases, and the side reactions of the battery increase, causing serious gas generation in the battery. According to the applicant's research, the positive electrode active material of the first aspect of the present application comprises active materials A, B, and C which have different average particle sizes and nickel contents, thereby increasing the compaction density of a positive electrode plate comprising the positive electrode active material, and effectively resolving the problems of performance degradation caused by particles being crushed along the grain boundaries, increasing the specific surface area, destroying the electron / ion transport pathways, and corrosion by the electrolyte during the cold pressing and cycling processes of high-nickel positive electrode active materials in the prior art, and thus the corresponding batteries have high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0029] positive electrode active material In one embodiment of the present application, the present application provides: A positive electrode active material is provided, the positive electrode active material comprising: An active material A having the following composition formula: Li x1 Ni a1 Co b1 Mn c1 O 2-y1 Q y1 I In formula I, 0.95≦x1≦1.3, 0.7≦a1≦0.99, 0.01≦b1≦0.15, 0.01≦c1≦0.3, a1+b1+c1=1, 0≦y1≦0.1, and Q is one or more selected from S, N, F, Cl, Br, and I; An active material B having the following composition formula: Li x2 Ni a2 Co b2 Mn c2 O 2-y2 Q y2 II In formula II, 0.95≦x2≦1.3, 0.7≦a2≦0.99, 0.01≦b2≦0.15, 0.01≦c2≦0.3, a2+b2+c2=1, 0≦y2≦0.1, and Q is one or more selected from S, N, F, Cl, Br and I; An active material C having the following composition formula: Li x3 Ni a3 Co b3 Mn c3 O 2-y3 Q y3 III and an active material C, in which, in formula III, 0.95≦x3≦1.3, 0.3≦a3<0.7, 0.01≦b3≦0.15, 0.01≦c3≦0.5, a3+b3+c3=1, 0≦y3≦0.1, and Q is one or more selected from S, N, F, Cl, Br, and I; Here, the average particle diameter Dv50 of the active material A is larger than the average particle diameter Dv50 of the active material B, and is also larger than the average particle diameter Dv50 of the active material C.

[0030] According to the applicant's research, the positive electrode active material of the present application comprises active materials A, B, and C having different average particle sizes and nickel contents, thereby increasing the compaction density of a positive electrode plate comprising the positive electrode active material, and at the same time effectively resolving the problems of performance degradation caused by the particles being crushed along the grain boundaries, the specific surface area being increased, the electron / ion transport pathways being destroyed, and corrosion by the electrolyte during the cold pressing and cycling processes of the high-nickel positive electrode active material according to the conventional technology, and thus the corresponding battery has high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0031] In some embodiments, active material A has an average particle size Dv50 of 7-15 μm, optionally 8-14 μm, and a Dv90 of 15-25 μm, optionally 18-22 μm; active material B has an average particle size Dv50 of 1-8 μm, optionally 2-5 μm, and a Dv90 of 3-10 μm, optionally 5-8 μm; active material C has an average particle size Dv50is 1 to 7 μm, optionally 2 to 5 μm, and Dv90 is 5 to 10 μm, optionally 5 to 8 μm. By further limiting the average particle size of each active material, the compaction density of the positive electrode active material is further improved, so that the corresponding battery has high energy density and safety, and at the same time, good high-temperature cycle performance and high-temperature storage performance.

[0032] In some embodiments, the active material A has a Dv10 of 1 to 4 μm, preferably 2 to 3 μm, and a Dv99 of 20 to 30 μm, preferably 24 to 28 μm.

[0033] The active material B has a Dv10 of 1 to 3 μm, and preferably 1 to 2 μm, and a Dv99 of 4 to 12 μm, and preferably 6 to 10 μm.

[0034] The active material C has a Dv10 of 1 to 3 μm, and preferably 1.5 to 2.5 μm, and a Dv99 of 6 to 15 μm, and preferably 7 to 13 μm.

[0035] The Dv10 is the particle size corresponding to the cumulative volume distribution percentage of the sample reaching 10%, Dv50 is the particle size corresponding to the cumulative volume distribution percentage of the sample reaching 50%, and is also called the average particle size, Dv90 is the particle size corresponding to the cumulative volume distribution percentage of the sample reaching 90%, and Dv99 is the particle size corresponding to the cumulative volume distribution percentage of the sample reaching 99%.

[0036] In one preferred embodiment, the active material A has an average particle size Dv50 of 11.5 to 12.5 μm, the active material B has an average particle size Dv50 of 3.8 to 4.2 μm, and the active material C has an average particle size Dv50 of 3.8 to 4.2 μm.

[0037] The particle size of the positive electrode active material has a meaning known in the art, which is measured by using a laser particle size analyzer to measure the volumetric particle size and its distribution of the positive electrode active material, for example, a Mastersizer 3000 type laser particle size analyzer manufactured by Malvern Instruments Ltd. in the UK.

[0038] In some embodiments, the content ratio of the active material A, the active material B, and the active material C is 1:0.5-8:0.1-10, optionally 1:0.8-6:0.2-8, further optionally 1:1.5-6:3-8, and most preferably 1:1.5-4:2.5-5. This allows the specific ratio of active materials to further increase the compaction density of the positive electrode plate containing the positive electrode active material, so that the corresponding battery has high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance. The above contents are all calculated based on the total weight of the positive electrode active materials.

[0039] In some embodiments, the sum of the contents of the active material A and the active material B is equal to the content of the active material C, and each content is calculated based on the total weight of the positive electrode active materials. In this way, the specific content of each active material can further increase the compaction density of the positive electrode plate including the positive electrode active materials, so that the corresponding battery has high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0040] In some embodiments, based on the total weight of the positive electrode active material, the content of the active material A is 2 wt% to 98 wt%, preferably 10 wt% to 90 wt%, more preferably 30 wt% to 70 wt%, and even more preferably 20 wt% to 60 wt%. Based on the total weight of the positive electrode active material, the content of the active material B is 2 wt% to 98 wt%, preferably 10 wt% to 80 wt%, more preferably 15 wt% to 60 wt%, and even more preferably 20 wt% to 40 wt%. Based on the total weight of the positive electrode active material, the content of the active material C is 2 wt% to 98 wt%, preferably 10 wt% to 80 wt%, more preferably 10 wt% to 70 wt%, and even more preferably 10 wt% to 50 wt%.

[0041] In some embodiments, the specific surface area of ​​the positive electrode active material is 0.3 to 1.8 m2 / g, optionally 0.3 to 0.8 m 2 / g, 0.6~0.8m 2 / g, 0.8~1.0m 2 / g, 1.0-1.8m 2 / g. Thus, by using a positive electrode active material having a specific specific surface area and compaction density, the corresponding battery has high energy density and safety, and at the same time, has good high-temperature cycle performance and high-temperature storage performance.

[0042] In some embodiments, the active material A and / or the active material B and / or the active material C comprises an element M, where M is selected from one or more of Zr, Sr, B, Ti, Mg, Sn and Al, preferably Ti or Al, by subjecting each of the active materials to the above treatment, the phase structure of the material surface can be stabilized, side reactions during charging and discharging can be suppressed, and the corresponding battery can have high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0043] In some embodiments, the active material A and / or the active material B and / or the active material C are coated with an element M, where M is as defined above. The coating can be performed using methods known to those skilled in the art, such as dry coating or liquid phase coating methods.

[0044] In some embodiments, in the chemical formulas corresponding to the active material A, the active material B, and the active material C, x1:x2:x3 is 1:(0.73-1.37):(0.73-1.37), optionally 1:(0.9-1.1):(0.9-1.1), and a1:a2:a3 is 1:(0.71-1.42):(0.31-1), optionally 1:(0.95-1.11):(0.55-0.75). By limiting the ratio of lithium to nickel in each active material, the corresponding battery is provided with high energy density and safety, and at the same time, with good high-temperature cycle performance and high-temperature storage performance.

[0045] In some embodiments, active material A is a polycrystalline material, and active materials B and C are pseudo-single crystalline or single crystalline materials, thereby limiting the crystal type of each active material, thereby further providing the corresponding battery with high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0046] In the present application, the term "pseudo single crystal" refers to primary particles having an average particle size Dv50 of more than 1 μm and a small amount of agglomeration. The term "single crystal" refers to primary particles having an average particle size Dv50 of more than 1 μm and no significant agglomeration, and has few grain boundaries. The term "polycrystalline" refers to secondary particles made of primary particles. The "primary particles" are generally in the form of single particles dispersed at the micron level, and the "secondary particles" are generally many particles (100 to 500 nanometers) aggregated to form a sphere and have a large number of grain boundaries. The single crystal positive electrode active material is a primary particle, has a small surface area, a large mechanical strength, a large compaction density, and is not easily crushed. By appropriately adjusting the ratio of the polycrystalline and single crystal nickel-containing active materials, not only can the energy density of the battery be guaranteed, but also the battery can have excellent high-temperature performance.

[0047] A second aspect of the present application further provides a secondary battery comprising the positive electrode active material of the first aspect of the present application.

[0048] As a result, the resulting battery has high energy density and safety, as well as good high-temperature cycle performance and high-temperature storage performance.

[0049] The secondary battery, battery module, battery pack and power consuming device of the present application will be described below with appropriate reference to the drawings.

[0050] In one embodiment of the present application, a secondary battery is provided.

[0051] Generally, a secondary battery includes a positive electrode plate, a negative electrode plate, an electrolyte, and a separator. During charging and discharging of the battery, active ions shuttle between the positive electrode plate and the negative electrode plate, absorbing and releasing them. The electrolyte functions to conduct ions between the positive electrode plate and the negative electrode plate. The separator is installed between the positive electrode plate and the negative electrode plate, and mainly serves to prevent short-circuiting between the positive and negative electrodes, while allowing ions to pass through.

[0052] [Positive plate] The positive electrode plate includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer including the positive electrode active material of the first aspect of the present application.

[0053] For example, the positive electrode current collector has two opposing surfaces in the thickness direction of the positive electrode current collector, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.

[0054] In some embodiments, the positive electrode current collector may be a metal foil sheet or a composite current collector. For example, an aluminum foil may be used as the metal foil sheet. The composite current collector may include a polymeric material base layer and a metal layer formed on at least one surface of the polymeric material base layer. The composite current collector may be formed by forming a metal material (such as aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys) on a polymeric material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0055] In some embodiments, the positive electrode active material may further include a positive electrode active material for batteries well known in the art. For example, the positive electrode active material may include at least one material selected from the group consisting of lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Here, examples of the lithium transition metal oxide include lithium cobalt oxide (e.g., LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM 333 (may be abbreviated as "LiNi") 0.5 Co 0.2 Mn 0.3 O2(NCM 523 (may be abbreviated as "LiNi") 0.5 Co 0.25 Mn 0.25 O2(NCM 211 (may be abbreviated as "LiNi") 0.6 Co 0.2 Mn 0.2 O2(NCM 622 (may be abbreviated as "LiNi") 0.8 Co 0.1 Mn 0.1 O2(NCM 811 Lithium nickel cobalt aluminum oxide (e.g., LiNi 0.85 Co 0.15 Al 0.05O2) and modified compounds thereof, but are not limited thereto. Examples of lithium-containing phosphates having an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (e.g., LiFePO4 (may be abbreviated as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (e.g., LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon. Based on the total weight of the positive electrode film layer, the weight ratio of the positive electrode active material in the positive electrode film layer is 80 to 100% by weight.

[0056] In some embodiments, the positive electrode membrane layer optionally further includes an adhesive. For example, the adhesive may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. Based on the total weight of the positive electrode membrane layer, the weight ratio of the adhesive in the positive electrode membrane layer is 0 to 20% by weight.

[0057] In some embodiments, the positive electrode membrane layer optionally further includes a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. Based on the total weight of the positive electrode membrane layer, the weight ratio of the conductive agent in the positive electrode membrane layer is 0 to 20% by weight.

[0058] In some embodiments, the positive plate may be manufactured by the following method: The components for manufacturing the positive plate, such as the positive active material, conductive agent, adhesive, and any other components, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a positive slurry, in which the solid content of the positive slurry is adjusted to 40 to 80 wt % and the viscosity at room temperature is adjusted to 5000 to 25000 mPa·s. The positive slurry is coated on the surface of a positive current collector, dried, and then cold pressed by a cold rolling machine to form a positive plate, and the unit areal density of the positive powder coating is 150 to 350 mg / m 2 The compaction density of the positive plate is 3.0 to 3.6 g / cm 3 and optionally 3.3 to 3.5 g / cm 3 The formula for calculating the compaction density is: Compaction density = coating surface density / (plate thickness after pressing - current collector thickness).

[0059] [Negative plate] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer including a negative electrode active material.

[0060] For example, the negative electrode current collector has two opposing surfaces in the thickness direction of the negative electrode current collector, and the negative electrode film layer is disposed on either one or both of the two opposing surfaces of the negative electrode current collector.

[0061] In some embodiments, the negative electrode current collector may be a metal foil sheet or a composite current collector. For example, a copper foil may be used as the metal foil sheet. The composite current collector may include a polymeric base layer and a metal layer formed on at least one surface of the polymeric substrate. The composite current collector may be formed by forming a metal material (such as copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymeric substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0062] In some embodiments, the negative electrode active material may be a negative electrode active material for batteries well known in the art. For example, the negative electrode active material may include at least one of materials such as artificial graphite, natural graphite, soft carbon, hard carbon, silicone-based materials, tin-based materials, and lithium titanate. The silicone-based material may be selected from at least one of silicone alone, silicone oxide, silicone carbon composite, silicone nitrogen composite, and silicone alloy. The tin-based material may be selected from at least one of tin alone, tin oxide, and tin alloy. However, the present application is not limited to these materials, and other conventional materials that can be used as a negative electrode active material for a battery may be used. These negative electrode active materials may be used alone or in combination of two or more. Based on the total weight of the negative electrode film layer, the weight ratio of the negative electrode active material in the negative electrode film layer is 70 to 100% by weight.

[0063] In some embodiments, the negative electrode membrane layer optionally further comprises an adhesive. The adhesive may be selected from at least one of styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS). Based on the total weight of the negative electrode membrane layer, the weight ratio of the adhesive in the negative electrode membrane layer is 0 to 30 wt%.

[0064] In some embodiments, the negative electrode film layer optionally further comprises a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. Based on the total weight of the negative electrode film layer, the weight ratio of the conductive agent in the negative electrode film layer is 0 to 20% by weight.

[0065] In some embodiments, the negative electrode membrane layer optionally further includes other auxiliary agents, such as a thickener (e.g., sodium carboxymethylcellulose (CMC-Na)). Based on the total weight of the negative electrode membrane layer, the weight ratio of the other auxiliary agents in the negative electrode membrane layer is 0 to 15% by weight.

[0066] In some embodiments, the negative electrode plate may be manufactured by the following method. The above-mentioned components for manufacturing the negative electrode plate, such as the negative electrode active material, conductive agent, adhesive, and any other components, are dispersed in a solvent (e.g., deionized water) to form a negative electrode slurry, in which the solid content of the negative electrode slurry is adjusted to 30 to 70 wt % and the viscosity at room temperature is adjusted to 2000 to 10000 mPa·s. The obtained negative electrode slurry is coated on a negative electrode current collector, and after a drying process, it is cold pressed, for example, by a roll, to obtain a negative electrode plate. The unit area density of the negative electrode powder coating is 75 to 220 mg / m 2 The compaction density of the negative plate is 1.2 to 2.0 g / m 3 It is.

[0067] [Electrolyte] The electrolyte serves to conduct ions between the positive and negative plates. The present application does not specifically limit the type of electrolyte, which can be selected according to need. For example, the electrolyte may be liquid, gel, or all solid.

[0068] In some embodiments, the electrolyte employs an electrolyte solution, the electrolyte solution including an electrolyte salt and a solvent.

[0069] In some embodiments, the electrolyte salt may be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluoro(oxalato)borate (LiDFOB), lithium bis(oxalato)borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalato)phosphate (LiDFOP), and lithium tetrafluoro(oxalato)phosphate (LiTFOP). The concentration of the electrolyte salt is generally 0.5 to 5 mol / L.

[0070] In some embodiments, the solvent may be selected from one or more of fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), and ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0071] In some embodiments, the electrolyte solution optionally further includes additives. For example, the additives may include an anode film-forming additive and a cathode film-forming additive, and may further include additives that can improve some performance of the battery, such as an additive that improves the overcharge performance of the battery, an additive that improves the high temperature or low temperature performance of the battery, etc.

[0072] [Separator] In some embodiments, the secondary battery further includes a separator. The present application is not particularly limited to the type of separator, and any known separator with a porous structure having good chemical stability and mechanical stability may be selected.

[0073] In some embodiments, the material of the separator may be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single layer film or a multi-layer composite film, and there is no particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, and there is no particular limitation.

[0074] In some embodiments, the separator has a thickness of 6 to 40 μm, optionally 12 to 20 μm.

[0075] In some embodiments, the positive and negative plates and the separator may be fabricated into an electrode assembly by a winding or lamination process.

[0076] In some embodiments, the secondary battery may include an exterior body, which may be used to package the electrode assembly and the electrolyte.

[0077] In some embodiments, the exterior of the secondary battery may be a hard case, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior of the secondary battery may be a pouch, such as a bag-shaped pouch. The material of the pouch may be plastic, such as polypropylene, polybutylene terephthalate, polybutylene succinate, etc.

[0078] The present application is not particularly limited to the shape of the secondary battery, which may be cylindrical, rectangular, or any other shape. For example, FIG. 1 shows a secondary battery 5 with a rectangular structure as an example.

[0079] In some embodiments, referring to FIG. 2, the exterior body may include a case 51 and a cover plate 53. Here, the case 51 may include a bottom plate and a side plate connected on the bottom plate, and the bottom plate and the side plate surround the bottom plate to form a receiving cavity. The case 51 has an opening communicating with the receiving cavity, and the cover plate 53 can be provided to cover the opening to close the receiving cavity. The positive electrode plate, the negative electrode plate and the separator can form an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is packaged in the receiving cavity. The electrolyte permeates the electrode assembly 52. ​​The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and can be selected by those skilled in the art according to actual specific needs.

[0080] In some embodiments, the secondary batteries may be assembled into a battery module, and the number of secondary batteries included in the battery module may be one or more, with the specific number being selectable by one skilled in the art based on the application and capacity of the battery module.

[0081] Fig. 3 shows an example of a battery module 4. Referring to Fig. 3, in the battery module 4, the secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the secondary batteries 5 may be fixed by fasteners.

[0082] Optionally, the battery module 4 may further include a housing having an accommodating space, and the multiple secondary batteries 5 are accommodated in the accommodating space.

[0083] In some embodiments, the battery modules may be further assembled into a battery pack, and the number of battery modules included in the battery pack may be one or more, and the specific number can be selected by one skilled in the art based on the application and capacity of the battery pack.

[0084] 4 and 5 show an example of a battery pack 1. Referring to FIG. 4 and FIG. 5, the battery pack 1 may include a battery box and a plurality of battery modules 4 installed in the battery box. The battery box includes an upper housing 2 and a lower housing 3, and the upper housing 2 is provided to cover the lower housing 3 to form a sealed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box according to any manner.

[0085] The present application further provides a power consuming device, the power consuming device including at least one of the secondary battery, the battery module, or the battery pack according to the present application. The secondary battery, the battery module, or the battery pack may be used as a power source for the power consuming device, or may be used as an energy storage unit for the power consuming device. The power consuming device may include, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), a train, a ship, a satellite, an energy storage system, etc.

[0086] The power consumption device can be a secondary battery, a battery module, or a battery pack depending on the needs of the usage.

[0087] 6 shows an example of a power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. A battery pack or a battery module can be adopted to meet the power consuming device's demand for high power and high energy density of secondary batteries.

[0088] Another example of the device may be a mobile phone, a tablet computer, a notebook computer, etc. Such devices are generally required to be lightweight and may employ a secondary battery as a power source.

[0089] Working Example In order to clarify the technical problems, technical solutions and beneficial effects that the present application aims to solve, the present application will be described in more detail below in conjunction with the embodiments and drawings. It is obvious that the described embodiments are only some of the embodiments of the present application, but not all of the embodiments. The following description of at least one exemplary embodiment is merely illustrative in nature and in no way restricts the present application and its applications. All other embodiments obtained based on the embodiments of the present application without the need for creative efforts by those skilled in the art are within the scope of protection of the present application.

[0090] If specific techniques or conditions are not specified in the examples, they will be performed according to techniques or conditions described in the literature in the art or in the product instructions. Reagents or instruments used that are not specified by manufacturer are all common products that can be purchased commercially.

[0091] 1. Manufacturing Examples Manufacture of positive electrode active material Manufacturing Example 1 (1) Preparation of a positive electrode active material precursor: In a continuous stirred tank reactor, nickel sulfate, manganese sulfate, and cobalt sulfate were added to deionized water in a molar ratio of Ni:Co:Mn=8:1:1 (based on each element) to prepare a transition metal salt solution with a total molar concentration of 2 mol / L. 4 mol / L of sodium hydroxide as a precipitant and 0.4 mol / L of ammonia water as a complexing agent were added, and the mixture was co-precipitated at pH 11.3 for 24 hours to prepare a precursor of large-particle lithium polycrystalline ternary positive electrode material A, Ni. 0.8 Co 0.1 Mn 0.1 Nickel sulfate, manganese sulfate, and cobalt sulfate were added to deionized water in a molar ratio of Ni:Co:Mn=8:1:1 to prepare a transition metal salt solution with a total molar concentration of 2 mol / L. 4 mol / L sodium hydroxide as a precipitant and 0.4 mol / L ammonia water as a complexing agent were added, and the mixture was co-precipitated at pH 11.4 for 24 hours to produce the precursor Ni of the small particle single crystal ternary positive electrode active material B. 0.8 Co0.1 Mn 0.1 Nickel sulfate, manganese sulfate, and cobalt sulfate were added to deionized water in a molar ratio of Ni:Co:Mn=55:12:33 to prepare a transition metal salt solution with a total molar concentration of 2 mol / L. 4 mol / L sodium hydroxide as a precipitant and 0.4 mol / L ammonia water as a complexing agent were added, and the mixture was co-precipitated at pH 11.4 for 24 hours to produce the precursor Ni of the small particle single crystal ternary positive electrode active material C. 0.55 Co 0.12 Mn 0.33 (OH)2 was produced.

[0092] (2) Manufacturing method of the positive electrode active material A: Precursor Ni of the positive electrode active material A 0.8 Co 0.1 Mn 0.1 The materials were mixed in a high-speed mixer with a molar ratio of 1:1.05, then sintered in a kiln at 800°C for 5 hours, cooled to room temperature, and then put into a jet mill and mechanically ground for 5 hours to obtain the positive electrode active material A, Li(Ni 0.8 Co 0.1 Mn 0.1 The positive electrode active material A and 0.3 wt% Al2O3 based on the active material A were mixed in a high-speed mixer, and then sintered in a kiln at 500°C for 5 hours to form a coating layer of the positive electrode active material A, and a surface-modified positive electrode active material A was obtained.

[0093] (3) Manufacturing method of the positive electrode active material B: Precursor Ni of the positive electrode active material B 0.8 Co 0.1 Mn 0.1 The materials were mixed in a high-speed mixer with a molar ratio of 1:1.05, then sintered in a kiln at 850°C for 5 hours, cooled to room temperature, and mechanically ground in a jet mill for 5 hours to obtain the positive electrode active material B, Li(Ni 0.8 Co 0.1 Mn 0.1The positive electrode active material B and a compound Al2O3 containing 0.2 wt% of the coating element Al were mixed in a plow roller / high-speed mixer, and then sintered in a kiln at 500°C for 5 hours to form a coating layer of the positive electrode active material B, and a surface-modified positive electrode active material B was obtained.

[0094] (4) Method for producing the positive electrode active material C: Precursor Ni of the positive electrode active material C 0.55 Co 0.12 Mn 0.33 The materials were mixed in a high-speed mixer with a molar ratio of 1:1.1, then sintered in a kiln at 700°C for 5 hours, cooled to room temperature, and mechanically pulverized for 5 hours using a jet mill to obtain the positive electrode active material C, Li(Ni 0.55 Co 0.12 Mn 0.33 The positive electrode active material C and a 0.2 wt% mixture of aluminum oxide Al2O3 and titanium oxide TiO2 in a mass ratio of 1:1 were mixed in a high-speed mixer, and then sintered in a kiln at 500°C for 5 hours to form a coating layer of the positive electrode active material C, thereby obtaining a surface-modified positive electrode active material C.

[0095] (5) The positive electrode active material A, the positive electrode active material B, and the positive electrode active material C were mixed uniformly in a mass ratio of 7:2:1 in a high-speed mixer to obtain the positive electrode active material of the present invention. The parameters of the positive electrode active material are summarized in Table 1.

[0096] The positive electrode active materials of Examples 2 to 19 and Comparative Examples 1 to 8 are manufactured by a method similar to that of the positive electrode active material of Example 1. However, the type, composition, particle size and crystal type of each active material were changed. The parameters of the different finished products are shown in Table 1.

[0097] Table 1. Related parameters of the positive electrode active materials of each Example and Comparative Example

[0098] [Table 1]

[0099] II. Application Examples Example 1 1) Manufacturing of positive electrodes The positive electrode active material of Preparation Example 1, conductive carbon black SP, and adhesive PVDF were dispersed and uniformly mixed in a solvent NMP in a weight ratio of 98:1:1 to obtain a positive electrode slurry. The positive electrode slurry was uniformly applied to an aluminum foil positive electrode current collector, dried, and cold pressed to obtain a positive electrode plate. The coating amount per unit area was 0.27 g / 1540.25 mm. 2 and their compacted densities are summarized in Table 1.

[0100] 2) Manufacturing of negative electrodes The negative electrode active material graphite, the thickener sodium carboxymethylcellulose, the adhesive styrene butadiene rubber, and the conductive agent acetylene black are mixed in a mass ratio of 97:1:1:1, deionized water is added, and the negative electrode slurry is obtained under the action of a vacuum stirrer. The negative electrode slurry is uniformly coated on copper foil, the copper foil is dried at room temperature, and then transferred to a drying box at 120°C for 1 hour. After that, the negative electrode plate is obtained through cold pressing and slitting, and the coating amount per unit area is 0.17g / 1540.25mm. 2 It is.

[0101] 3) Separator A polypropylene separator having a thickness of 12 μm was used.

[0102] 4) Electrolyte production The organic solvent is a mixture containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC), where the volume ratio of EC, EMC, and DEC is 20:20:60. In a glove box with an argon gas atmosphere having a water content of <10 ppm, a sufficiently dried lithium salt LiPF6 was dissolved in the organic solvent and mixed uniformly to obtain an electrolyte. Here, the concentration of the lithium salt is 1 mol / L.

[0103] 5) Battery manufacturing A positive electrode plate, a separator, and a negative electrode plate are stacked in this order, and a separator is placed between the positive and negative electrodes to perform an isolating function. The stack is then wound into a rectangular bare cell, which is then inserted into an aluminum plastic film and baked at 80°C to remove moisture. The corresponding non-aqueous electrolyte is then injected and sealed. The finished battery is then obtained through processes such as leaving, hot and cold pressing, chemical formation, clamping, and capacity selection.

[0104] The secondary batteries of Examples 2 to 19 and Comparative Examples 1 to 8 were produced using methods similar to those of the secondary battery of Example 1. However, the positive electrode active materials of the corresponding production examples were used.

[0105] 3. Battery performance test 1. High temperature cycle performance test The battery was placed in a drying box at 60°C and left to stand for 2 hours, and then a charge / discharge test was performed after maintaining the battery temperature at 60°C. It was charged at a constant current of 1C to 3.65V, then charged at a constant voltage, and when the charging current became less than 0.05C, it was turned off and rested for 5 minutes, and then discharged at a constant current of 1C to 2.8V, and rested for 5 minutes. This was considered as one charge / discharge cycle of the battery, and was repeated until the battery capacity was attenuated to 80% of its initial value, and the number of cycles was recorded.

[0106] 2. High temperature gas generation test As a test method for high-temperature gas generation in batteries, the battery was fully charged to 4.35V at 1C, then placed in a thermostatic box at 70℃ and left to stand for 30 days. The initial volume of the battery and the volume after standing for 30 days were measured using the drainage method, and the volume expansion rate of the battery was obtained. The volume expansion rate of the battery (%) = (volume after standing for 30 days / initial volume - 1) x 100%.

[0107] 3. Battery Gram Capacity Test For the battery capacity test, the lithium-ion battery is left in a constant temperature environment of 25°C for 2 hours, then charged at 2.8V to 4.35V at 1 / 3C to 4.35V, and then charged at a constant voltage of 4.35V until the current is ≦0.05mA, left to stand for 5 minutes, and then discharged at 1C to 2.8V. The capacity C 放 It was recorded.

[0108] The gram capacity = the capacity C of the battery 放 (mAh) / mass of positive electrode active material (g).

[0109] 4. High temperature storage performance test At 25°C, the battery was charged at a constant current of 0.33C to 4.35V, then charged at a constant voltage until the current was below 0.05C, and then discharged at a constant current of 0.33C to 2.8V, and then tested to obtain the initial discharge capacity of the battery. At 25°C, the battery was charged at a constant current of 0.33C to 4.35V, then charged at a constant voltage until the current was below 0.05C, and then the fully charged battery was placed in a drying box at 60°C and stored for 60 days. After 60 days of high temperature storage, the battery was taken out, allowed to cool naturally to 25°C, discharged at a constant current of 0.33C to 2.8V, then charged at a constant current of 0.33C to 4.35V, then charged at a constant voltage until the current was below 0.05C, and then discharged at a constant current of 0.33C to 2.8V, and then tested to obtain the discharge capacity of the battery after 60 days of high temperature storage.

[0110] Capacity retention rate (%) of battery after 60 days of high temperature storage = discharge capacity after 60 days of high temperature storage / initial discharge capacity × 100%.

[0111] 4. Test results of each embodiment and comparative example According to the above method, the batteries of the examples and the comparative examples were manufactured, and the performance parameters were measured. The results are shown in Table 2 below.

[0112] Table 2. Performance of the batteries in the comparative examples and examples

[0113] [Table 2]

[0114] As can be seen from the above examples and comparative examples, when the proportion of polycrystalline high nickel large particles is large, the gram capacity of the battery containing the mixed positive electrode material is significantly improved, but the particles split under high temperature conditions, lithium-nickel mixing is serious, and other problems exist, which cause the deterioration of its high temperature performance, and the volume expansion rate is high due to serious side reactions such as gas generation, and the higher the nickel content, the more prominent this feature becomes. When the positive electrode active material only contains single crystal low nickel active material C (Comparative Example 3), the side reactions in the battery are few, and the high temperature cycle and high temperature storage performance are high, but the demand for high energy density cannot be met, and even if a certain proportion of single crystal high nickel active material B (Comparative Example 6) is mixed, the energy density is still low.

[0115] By reasonably adjusting and mixing A, B and C, the mixed ternary positive electrode material can effectively solve the problems of high-nickel active material such as grain fracture along the grain boundary, increase in specific surface area, destruction of electron / ion transport pathways, and corrosion by electrolyte during the cold pressing and cycling process, and reduce side reactions such as gas generation during high-temperature storage, so that the mixed positive electrode can ensure high capacity and have excellent high-temperature performance.

[0116] It should be noted that the present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is an example, and any embodiment having substantially the same configuration as the technical idea and achieving the same effect within the scope of the technical proposal of the present application is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can make to the embodiment and other forms configured by combining some of the components in the embodiment are also included in the scope of the present application, within the scope of the purpose of the present application. [Explanation of symbols]

[0117] 1 battery pack 2 Upper housing 3 Lower housing 4 Battery Module 5 secondary battery 51 cases 52 Electrode Assembly 53 Top cover assembly

Claims

1. A positive electrode active material, An active material A having the following composition formula: Li x1 Ni a1 Co b1 Mn c1 O 2-y1 Q y1 I In formula I, 0.95≦x1≦1.3, 0.7≦a1≦0.99, 0.01≦b1≦0.15, 0.01≦c1≦0.3, a1+b1+c1=1, 0≦y1≦0.1, and Q is one or more selected from S, N, F, Cl, Br and I; An active material B having the following composition formula: Li x2 Ni a2 Co b2 Mn c2 O 2-y2 Q y2 II In formula II, 0.95≦x2≦1.3, 0.7≦a2≦0.99, 0.01≦b2≦0.15, 0.01≦c2≦0.3, a2+b2+c2=1, 0≦y2≦0.1, and Q is one or more selected from S, N, F, Cl, Br and I; An active material C having the following composition formula: Li x3 Ni a3 Co b3 Mn c3 O 2-y3 Q y3 --- and the active material C, in which, in formula III, 0.95≦x3≦1.3, 0.3≦a3<0.7, 0.01≦b3≦0.15, 0.01≦c3≦0.5, a3+b3+c3=1, and 0≦y3≦0.1, and Q is one or more selected from S, N, F, Cl, Br, and I; Here, the average particle diameter Dv50 of the active material A is larger than the average particle diameter Dv50 of the active material B, and is also larger than the average particle diameter Dv50 of the active material C.

2. The active material A has an average particle diameter Dv50 of 7 to 15 μm, optionally 8 to 14 μm, and a Dv90 of 15 to 25 μm, optionally 18 to 22 μm; the active material B has an average particle diameter Dv50 of 1 to 8 μm, optionally 2 to 5 μm, and a Dv90 of 3 to 10 μm, optionally 5 to 8 μm; and the active material C has an average particle diameter Dv50 of 1 to 7 μm, optionally 2 to 5 μm, and a Dv90 of 5 to 10 μm, optionally 5 to 8 μm. The positive electrode active material according to claim 1,

3. The content ratio of the active material A, the active material B, and the active material C is 1:0.5-8:0.1-10, optionally 1:0.8-6:0.2-8, and further optionally 1:1.5-6:3-8. The positive electrode active material according to claim 1,

4. 2. The positive electrode active material according to claim 1, wherein a sum of the contents of the active material A and the active material B is equal to a content of the active material C, and the contents of each are calculated based on a total weight of the positive electrode active material.

5. The specific surface area of ​​the positive electrode active material is 0.3 to 1.8 m 2 / g, and the compaction density is 3.0 to 3.6 g / cm 3 The positive electrode active material according to claim 1 ,

6. 2. The positive electrode active material according to claim 1, wherein the active material A and / or the active material B and / or the active material C comprises an element M, where M is selected from one or more of Zr, Sr, B, Ti, Mg, Sn, and Al.

7. In the chemical formulas corresponding to the active material A, the active material B, and the active material C, x1:x2:x3 is 1:(0.73 to 1.37):(0.73 to 1.37), and a1:a2:a3 is 1:(0.71 to 1.42):(0.31 to 1). The positive electrode active material according to claim 1, characterized in that

8. 2. The positive electrode active material according to claim 1, wherein the active material A is a polycrystalline material, and the active materials B and C are pseudo-single crystal or single crystal materials.

9. A secondary battery comprising the positive electrode active material according to any one of claims 1 to 8.

10. A battery module comprising the secondary battery according to claim 9.

11. A battery pack comprising the battery module according to claim 10.

12. A power consuming device comprising at least one selected from the group consisting of the secondary battery according to claim 9, the battery module according to claim 10, and the battery pack according to claim 11.

Citation Information

Patent Citations

  • Preparation method of electrode slurry of ternary material

    CN110098403A

  • Nonaqueous secondary battery, and its using method

    JP2007258122A

  • Positive electrode for lithium ion secondary battery

    JP2019040787A

  • Secondary battery electrode including a composite layer with a double layer structure containing active materials with different particle sizes, and a method for manufacturing the same

    JP2022516395A