Coated Paper
The coated paper with a PHBH and EVA coating layer addresses microcracking issues, ensuring excellent foldability and sealing performance for paper containers by incorporating EVA with specific mechanical properties and optionally inorganic pigments.
Patent Information
- Application Number
- JP2024075995
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-05-08
AI Technical Summary
Coated papers containing poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBH) and adhesives suffer from microcracking during folding, leading to reduced sealing performance and leakage when used in paper containers.
A coated paper design with a paper base material having a coating layer containing PHBH and ethylene vinyl acetate (EVA), where EVA has a tensile strength of 4.0 MPa or more and elongation of 300% or more, and optionally includes an inorganic pigment, enhancing the folding suitability and barrier properties.
The coated paper exhibits excellent foldability and sealing performance, suitable for paper containers, with improved resistance to liquid permeation and enhanced barrier properties.
Smart Images

Figure 0007580003000001
Abstract
Description
[Technical field]
[0001] The present invention relates to coated paper. [Background technology]
[0002] In recent years, the development of environmentally friendly packaging using biodegradable materials has been attracting attention, and it is expected that these materials will be applied to paper containers such as paper cups and paper plates, and paper containers with uneven surfaces such as blister packs. Aliphatic polyesters such as polylactic acid and polycaprolactone are known as biodegradable materials, but aliphatic polyesters have the problem that they take a long time to biodegrade at low temperatures and decompose slowly in natural environments such as the ocean. Poly(3-hydroxybutyrate) resins are microbially produced thermoplastics that are highly degradable under aerobic and anaerobic conditions, and have the remarkable ability to be decomposed by microorganisms in a short period of time even in water such as the ocean. Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter also referred to as PHBH), a copolymer of 3-hydroxybutyrate and 3-hydroxyhexanoate, has attracted attention for its biodegradability and resin properties.
[0003] Patent Document 1 describes a paper substrate with a basis weight of 150 g / m, in which PHBH and an adhesive are applied to one side of the substrate. 2 More than 600g / m 2 The following coated papers have been proposed. Here, when manufacturing the above-mentioned paper containers, the processing step involves folding the paper, but it has been found that the coated paper described in Patent Document 1 has a problem in that many microcracks occur in the coating layer containing PHBH and adhesive due to the folding process. The occurrence of cracks in the coating layer leads to a decrease in the airtightness and sealing ability of the package, and when the contents contain liquids such as water or oil, they permeate the paper, making it unsanitary. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-195716 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a coated paper having excellent folding processability. [Means for solving the problem]
[0006] The means for solving the problems of the present invention are as follows. 1. Grammage is 100g / m 2 The above paper base material, a coating layer containing PHBH and EVA; an overlayer containing PHBH on the coating layer; having The coating layer contains 10 parts by mass or more and 250 parts by mass or less of the EVA per 100 parts by mass of the PHBH, A coated paper characterized in that the EVA has a tensile strength of 4.0 MPa or more and an elongation of 300% or more. 2. The coated paper according to 1., wherein the EVA has a tensile strength of 6.0 MPa or more and an elongation of 400% or more. 3. The coated paper according to 2., wherein the EVA has a glass transition temperature of -30°C or higher and 5°C or lower. 4. The coated paper according to any one of 1. to 3., wherein the coating layer contains an inorganic pigment. 5. A paper container having the coated paper described in any one of 1. to 4. Effect of the Invention
[0007] The coated paper of the present invention has excellent folding processability and can be suitably used for paper containers. The coated paper of the present invention has excellent folding processability even when the coating layer contains an inorganic pigment, and can be imparted with functionality such as barrier properties by the inorganic pigment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The coated paper of the present invention has a basis weight of 100 g / m2 The above paper base material, a coating layer containing PHBH and EVA; On this coating layer, there is an overlayer containing PHBH, having The coating layer contains 10 parts by mass or more and 250 parts by mass or less of EVA per 100 parts by mass of PHBH, The EVA has a tensile strength of 4.0 MPa or more and an elongation of 300% or more.
[0009] In this specification, the tensile strength and elongation are values evaluated at 3.4 and 3.5, respectively, of JIS-K-6251:2017. In this specification, the expression "A to B" (A and B are numerical values or ratios) means a numerical range including A and B.
[0010] The coated paper of the present invention may have a paper base material, a coating layer, and an over layer, and may have coating layers on both sides of the paper base material. When having coating layers on both sides, it is sufficient to have an over layer on at least one side. In addition, other layers such as an anchor layer, a water vapor barrier layer, a gas barrier layer, and an ink receiving layer may be present between the paper base material and the coating layer. The over layer is provided in contact with the coating layer.
[0011] (Paper base material) The paper base material is a sheet (hereinafter also referred to as "base paper") mainly made of pulp, and is obtained by making paper from a stock that further contains fillers, various auxiliaries, and the like.
[0012] Examples of pulp include chemical pulps such as bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), unbleached hardwood kraft pulp (LUKP), unbleached softwood pulp (NUKP), sulfite pulp, and other mechanical pulps, stone-ground pulp, thermomechanical pulp, and other wood fibers such as deinked pulp and waste paper pulp, and non-wood fibers obtained from kenaf, bamboo, hemp, and the like, and one or more of these can be used in appropriate combination. Among these, it is preferable to use chemical pulp of wood fiber or mechanical pulp of wood fiber, and it is more preferable to use chemical pulp of wood fiber, for reasons such as the fact that foreign matter is unlikely to be mixed into the paper base material, that discoloration is unlikely to occur over time when recycled as waste paper raw material, that the surface texture is good when printed due to its high whiteness, and that its value in use is particularly high when used as a packaging material. Specifically, the blending amount of wood fiber chemical pulp such as LBKP or NBKP relative to the total pulp is preferably 80 mass % or more, more preferably 90 mass % or more, even more preferably 95 mass % or more, and most preferably 100 mass %.
[0013] Examples of fillers that can be used include inorganic fillers such as talc, kaolin, calcined kaolin, clay, heavy calcium carbonate, light calcium carbonate, white carbon, zeolite, magnesium carbonate, barium carbonate, titanium dioxide, zinc oxide, silicon oxide, amorphous silica, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, barium sulfate, and calcium sulfate, and organic fillers such as urea-formalin resin, polystyrene resin, phenolic resin, and hollow microparticles. Note that fillers are not essential materials and may not be used.
[0014] Examples of various auxiliary agents include sizing agents such as rosin, alkyl ketene dimer (AKD), alkenyl succinic anhydride (ASA), polyacrylamide polymers, polyvinyl alcohol polymers, cationic starch, various modified starches, urea-formaldehyde resin, melamine-formaldehyde resin, and other dry strength agents, wet strength agents, retention agents, drainage improvers, coagulants, aluminum sulfate, bulking agents, dyes, fluorescent brighteners, pH adjusters, defoamers, UV inhibitors, anti-fading agents, pitch control agents, slime control agents, and the like, and can be selected and used as appropriate as needed.
[0015] The surface of the paper substrate may be treated with various chemicals. Examples of chemicals include oxidized starch, hydroxyethyl etherified starch, enzyme-modified starch, polyacrylamide, polyvinyl alcohol, surface sizing agents, water-resistant agents, water retention agents, thickeners, and lubricants, and these may be used alone or in combination of two or more. Furthermore, these various chemicals may be used in combination with pigments. Examples of pigments include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, and satin white, and organic pigments such as solid, hollow, and core-shell types may be used alone or in combination of two or more.
[0016] The basis weight of the paper base material used in the present invention is 100 g / m 2 The basis weight is 100g / m 2 The above paper base material has excellent strength and can be suitably used for paper containers. The basis weight of the paper base material is 120 g / m 2 More than 140g / m 2 More preferably, 160 g / m 2 More preferably, 180 g / m 2 More preferably, 200 g / m 2 The upper limit of the basis weight of the paper base material is not particularly limited, but from the viewpoint of folding processability, it is preferably 600 g / m 2 Less than 500 g / m2 Less than 400 g / m is more preferable. 2 More preferably, 350 g / m 2 More preferably, the following is 300 g / m 2 Even more preferred is the following: The density of the paper base material can be appropriately selected depending on the desired quality and ease of handling, but is usually 0.5 g / cm 3 More than 1.0g / cm 3 The following are preferred: In the present invention, the paper base material may be either a paper consisting of only a single paper layer or a multi-layer paper having two or more paper layers. When the paper base material is a multi-layer paper, the paper materials, basis weights, etc. of each paper layer may be the same or different.
[0017] The method for producing (making) the paper base material is not particularly limited, and any known production (making) method or papermaking machine can be selected, such as a Fourdrinier papermaking machine, a cylinder papermaking machine, a short wire papermaking machine, or a twin-wire papermaking machine such as a gap former type or a hybrid former type (on-top former type).The pH during papermaking may be in the acidic range (acidic papermaking), pseudo-neutral range (pseudo-neutral papermaking), neutral range (neutral papermaking), or alkaline range (alkaline papermaking), and after papermaking in the acidic range, an alkaline agent may be applied to the surface of the paper layer. Furthermore, when treating the surface of a paper substrate with a chemical, the method of surface treatment is not particularly limited, and known coating devices such as a rod metering size press, a pond type size press, a gate roll coater, a spray coater, a blade coater, or a curtain coater can be used.
[0018] (Coating layer) The coating layer contains at least PHBH and EVA.
[0019] <phbh> PHBH is a copolymer of 3-hydroxybutyrate (hereinafter also referred to as 3HB) and 3-hydroxyhexanoate (hereinafter also referred to as 3HH), and is a biodegradable resin known to be produced by microorganisms. In the present invention, the PHBH used may be derived from microorganisms or petroleum resources, but it is preferable to use the PHBH derived from microorganisms in terms of reducing the environmental load.
[0020] Microorganisms that produce PHBH are not particularly limited as long as they accumulate PHBH intracellularly, but examples include bacteria of the genus Alcaligenes, such as A. lipolytica, A. eutrophus, and A. latus, as well as bacteria of the genus Pseudomonas, Bacillus, Azotobacter, Nocardia, and Aeromonas. Among them, in terms of productivity of PHBH, strains such as Aeromonas caviae, and Alcaligenes eutrophus AC32 into which genes of PHA synthase group have been introduced (Accession No. FERM BP-6038, Date of deposit on August 7, 1997, National Institute of Advanced Industrial Science and Technology, International Patent Organism Depositary, Address: Central 6, 1-1-1 Higashi, Tsukuba-shi, Ibaraki-ken, Japan) (J. Bacteriol., 179, pp. 4821-4830 (1997)) are particularly preferred. A method for obtaining PHBH from Aeromonas caviae, a microorganism of the Aeromonas genus, is disclosed, for example, in Japanese Patent Application Laid-Open No. 05-093049. These microorganisms are used by culturing them under appropriate conditions to accumulate PHBH in the cells. The carbon source and culture conditions used in the culture can be obtained according to the methods described in JP-A-05-093049, JP-A-2001-340078, etc., but are not limited thereto.
[0021] The composition ratio (mol%) of PHBH is preferably 3HB:3HH=97:3 to 75:25, more preferably 95:5 to 85:15. If the composition of 3HH is less than 3 mol%, the properties of PHBH become similar to those of 3HB homopolymer, resulting in loss of flexibility and an excessively high film-forming processing temperature, which is undesirable. If the composition of 3HH exceeds 25 mol%, the crystallization rate becomes too slow to be suitable for film-forming processing, and the degree of crystallization decreases, making the resin flexible and decreasing the bending modulus. The composition ratio of PHBH can be measured by centrifuging the aqueous dispersion and then drying the powder obtained by NMR analysis. Microbial PHBH is a random copolymer. To adjust the molar ratio of the copolymer, there are several methods, such as selecting the bacterial cells, selecting the carbon source as the raw material, blending with PHBH of different molar ratios, and blending with 3HB homopolymer.
[0022] The mass average molecular weight of PHBH is preferably 50,000 to 1,500,000. When the mass average molecular weight of PHBH is within this range, a film can be formed at a low temperature when PHBH is applied, and a film with excellent mechanical properties can be obtained when PHBH is laminated. The mass average molecular weight of PHBH is more preferably 100,000 to 500,000, and even more preferably 150,000 to 450,000. The mass average molecular weight of PHBH can be determined by gel permeation chromatography (GPC, such as "Shodex GPC-101" manufactured by Showa Denko K.K.) using polystyrene gel (such as "Shodex K-804" manufactured by Showa Denko K.K.) in a column, using chloroform as the mobile phase, and converting it into a polystyrene-equivalent molecular weight. The measurement sample is a powder obtained by centrifuging an aqueous dispersion containing PHBH and then drying it.
[0023] The average particle size of PHBH is preferably 0.1 to 50 μm. PHBH with an average particle size of less than 0.1 μm is difficult to produce by microbial production, and even when obtained by chemical synthesis, a microparticulation operation is required. If the average particle size exceeds 50 μm, uneven coating may occur on the surface when a coating liquid containing PHBH is applied. The average particle size of PHBH is more preferably 0.5 to 10 μm. The average particle size of PHBH refers to the particle size corresponding to 50% accumulation of all particles measured by adjusting an aqueous suspension of PHBH to a predetermined concentration using a general-purpose particle sizer such as a Microtrack particle sizer (manufactured by Nikkiso, FRA).
[0024] <eva> EVA (ethylene vinyl acetate copolymer) is a copolymer having ethylene and vinyl acetate as monomers, and may further have other monomers as monomers. However, the EVA of the present invention is not saponified and does not have vinyl alcohol units generated by saponification of vinyl acetate. When EVA has other monomers as monomers, the content of the structural units derived from other monomers relative to the entire EVA is preferably 30% by mass or less. This content is not particularly limited as long as it does not impair the effects of the present invention, and can be, for example, 20% by mass or less, 10% by mass or less, 5% by mass or less, 3% by mass or less, 1% by mass or less, etc.
[0025] From the viewpoint of heat seal strength, the glass transition temperature of EVA is preferably −50 to 30° C. This glass transition temperature is more preferably −40° C. or higher, even more preferably −35° C. or higher, and more preferably 20° C. or lower, even more preferably 10° C. or lower. In this specification, the glass transition temperature means the midpoint glass transition temperature measured in accordance with JIS K 7121-1987. The molar ratio of ethylene to vinyl acetate in the EVA (structural units derived from ethylene:structural units derived from vinyl acetate, also expressed as ethylene:vinyl acetate, the total being 100) is preferably 1:99 to 60:40 from the viewpoint of heat seal strength, more preferably 3:97 to 50:50, and further preferably 5:95 to 45:55.
[0026] <Coating layer> The coating layer contains 10 parts by mass or more and 250 parts by mass or less of EVA per 100 parts by mass of PHBH, and the EVA has a tensile strength of 4.0 MPa or more and an elongation of 300% or more. In the coating layer, the ratio of EVA to 100 parts by mass of PHBH is preferably 13 parts by mass or more, more preferably 16 parts by mass or more, even more preferably 19 parts by mass or more, and is preferably 246 parts by mass or less, more preferably 242 parts by mass or less, and even more preferably 238 parts by mass or less, from the viewpoint of preventing cracks from occurring during folding.
[0027] In the coating layer, the tensile strength of the EVA is preferably 4.3 MPa or more, more preferably 4.6 MPa or more, even more preferably 4.9 MPa or more, even more preferably 5.2 MPa or more, even more preferably 5.5 MPa or more, and even more preferably 5.8 MPa or more, from the viewpoint of preventing cracks during folding processing. In the coating layer, the elongation of the EVA is preferably 340% or more, more preferably 380% or more, even more preferably 420% or more, even more preferably 460% or more, even more preferably 500% or more, even more preferably 540% or more, and even more preferably 560% or more, from the viewpoint of preventing cracks during folding processing.
[0028] The coating layer only needs to contain PHBH and a specific EVA in the ratio described above, and may contain other thermoplastic resins and inorganic pigments. <Other thermoplastic resins> As the other thermoplastic resin, any resin having heat sealability at the temperature at which PHBH is fused can be used without any particular limitation. However, preferred are biodegradable resins such as aliphatic polyester-based resins such as polycaprolactone, polybutylene succinate adipate, polybutylene succinate, and polylactic acid, and aliphatic aromatic polyester-based resins such as polybutylene adipate terephthalate and polybutylene azelate terephthalate.
[0029] When the coating layer contains another thermoplastic resin, the total proportion of PHBH and EVA to the total thermoplastic resin contained in the coating layer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, even more preferably 99% by mass or more, and most preferably 100% by mass.
[0030] <Inorganic pigments> As the inorganic pigment, those used for coating on paper can be used without any particular limitation, and examples thereof include kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, bentonite, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, satin white, etc., and one or more of these can be used. Among these, one or more of kaolin, heavy calcium carbonate, light calcium carbonate, mica, talc, and bentonite are preferred.
[0031] From the viewpoint of the fixation of the coating layer, the inorganic pigment preferably has a volume 50% average particle size (D50, hereinafter also referred to as "average particle size") of 6.0 μm or less, measured by a laser diffraction / scattering method. Examples of measuring devices for the laser diffraction / scattering method include a particle size distribution measuring device "Partica" from Horiba, Ltd. and a particle size distribution measuring device "MASTER SIZER S" from Malvern Instruments. From the viewpoint of the fixation of the coating layer, the average particle size of the inorganic pigment is more preferably 5.0 μm or less, even more preferably 4.0 μm or less, even more preferably 3.0 μm or less, and even more preferably 2.0 μm or less. There is no particular lower limit for the average particle size of the inorganic pigment, but from the viewpoint of dispersibility, for example, it is preferably 0.1 μm or more, and more preferably 0.2 μm or more. When two or more inorganic pigments are contained, it is preferable that the average particle size of at least one of the inorganic pigments is within the above-mentioned numerical range, and the proportion of the inorganic pigments satisfying this average particle size relative to the total inorganic pigments is preferably 50 mass % or more, and more preferably 70 mass % or more.
[0032] When the coating layer contains an inorganic pigment, the solid content mass ratio of PHBH to inorganic pigment (PHBH: inorganic pigment, total 100) is preferably 90:10 to 0.01:99.99. By further blending an inorganic pigment into a coating liquid containing PHBH and EVA, the fixation of the resulting coating layer is improved. Although the mechanism is unclear, the present inventors speculate that this is because inorganic pigments have better thermal conductivity than organic PHBH and adhesives, so that the inorganic pigments quickly rise in temperature when heated, and this heat is transferred from the inorganic pigment to PHBH, so that PHBH is sufficiently heated and melted, making it easy to form a film. The solid content mass ratio of PHBH to inorganic pigment (PHBH:inorganic pigment, total 100) is more preferably 70:30 to 1:99, further preferably 60:40 to 2:98, and even further preferably 50:50 to 3:97, from the viewpoint of fixation of the coating layer.
[0033] The coating layer may contain, in addition to PHBH, EVA, other thermoplastic resins, and inorganic pigments, other water-soluble resins and water-dispersible resins, and may further contain, as necessary, various auxiliaries that are blended into coating solutions in the papermaking field, such as dispersants, viscosity improvers, water retention agents, defoamers, water resistance agents, pH adjusters, cationic resins, anionic resins, UV absorbers, metal salts, lubricants, coloring dyes, and pigments.
[0034] (Overlayer) The coated paper of the present invention has an overlayer containing PHBH on the coating layer. The over layer only needs to contain PHBH, and may contain other components that the coating layer can contain. However, the ratio of PHBH to the entire over layer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, even more preferably 99% by mass or more, and most preferably 100% by mass.
[0035] (Manufacturing method) The coating layer and the overlayer can be produced by a conventionally known coating method. For example, the coating device may be a blade coater, a bar coater, a roll coater, an air knife coater, a reverse roll coater, a curtain coater, a spray coater, a size press coater, a gate roll coater, etc. In addition, the coating system may be an aqueous coating using a solvent such as water, a solvent coating using a solvent such as an organic solvent, etc., and the aqueous coating is preferable.
[0036] The coating weight of the coating layer and overlayer is 1g / m2 in dry weight. 2 More than 50g / m 2 It is preferable that the coating amount is 1 g / m or less. 2 If the coating weight is less than 50 g / m, it may be difficult to form a uniform coating film. 2 If the amount is more than this, the drying load during coating will be large. The coating amount of the coating layer is 3g / m 2 More preferably, 5 g / m 2 More preferably, 40 g / m 2 Less than 30 g / m is more preferable. 2 The following is more preferable: The coating amounts of the coating layer and the over layer may be the same or different.
[0037] Coated paper The coated paper of the present invention has excellent folding processability and can be subjected to heat sealing process, and therefore is suitable for use in paper containers. When the coated paper of the present invention is used for a paper container, the shape of the paper container is not particularly limited and can be cubic, cylindrical, cup-shaped, etc. When the paper container is made up of multiple members such as a body member, a bottom plate member, and a lid member, the coated paper of the present invention can be used for one or more of the members that make up the paper container.
[0038] The coated paper of the present invention has a heat seal strength of 150°C at a pressure of 0.2MPa (20.0N / cm) measured in accordance with JIS Z1707:2019 7.4 "Heat seal strength test". 2 ), the heat seal strength when heat-sealed with a pressure application time of 1.0 second and then T-peeled is preferably 6.0 N / 15 mm or more, more preferably 6.5 N / 15 mm or more, even more preferably 7.0 N / 15 mm or more, and even more preferably 7.5 N / 15 mm or more. Furthermore, the heat seal strength of the coated paper of the present invention, measured in the same manner except that the pressing temperature is 160°C, is preferably 8.0 N / 15 mm or more, more preferably 8.5 N / 15 mm or more, even more preferably 9.0 N / 15 mm or more, and even more preferably 9.5 / 15 mm or more. EXAMPLES
[0039] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, parts and % are by mass, respectively, unless otherwise specified. (Evaluation method) -Flexibility (assuming bottom) The bottom part of the paper cup is produced by hand squeezing using a POM draw die and draw punch. Conditions: The sample evaluation surface was placed on the draw die side, the clearance between the draw die and the draw punch was 250 μm, and a backing paper of approximately 90 μm was placed on the non-evaluation side of the sample. Drawing was then performed to create a paper cup bottom with a bottom surface diameter of 600 mm and a skirt length of approximately 5 mm. After that, 2% brilliant blue dye solution adjusted to a surface tension of 29.6 mN / m using Tipol Eight (surfactant) was applied to the bottom bend and bottom surface, left to stand for 30 seconds, then wiped off with a JK wiper, and the penetration was evaluated according to the following criteria: If the evaluation was 5 to 3, there was no problem in practical use. 5: No penetration 4: Penetration into the coating surface and base paper layer confirmed in less than 5% of the bent area 3: Penetration into the coating surface and base paper layer confirmed in 5% to less than 30% of the bent area 2: Penetration into the coating surface and base paper layer confirmed in 30% to less than 70% of the bent area 1: Penetration into the coating surface and base paper layer confirmed in 70% or more of the bent area
[0040] ·Bending resistance (180° mountain bending) The paper was folded so that the base paper faces overlapped, and the folded part was pressed 10 times with a roller. The blue dye solution mentioned above was then applied to the folded part, and after leaving it for 30 seconds, it was wiped off with a JK wiper and the penetration was evaluated. The evaluation criteria were the same as those for the bottom.
[0041] Heat seal strength The test was conducted in accordance with JIS Z1707:2019 7.4 "Heat seal strength test". Two square test pieces with sides of 100 mm were cut out from the obtained coated paper, and the coating layers were brought into contact with each other and pressed at a pressure of 130°C, 140°C, 150°C, or 160°C and a pressure of 0.2 MPa (20.0 N / cm 2 ), heat-sealed with pressure for 1.0 second, and then left to stand for 24 hours in an environment of 23°C and 50% humidity. A measurement sample with a long side of 100 mm and a short side of 15 mm was then cut out from the heat-sealed 100 mm square test piece. The peeled long edge was then clamped between the upper and lower jigs of a vertical tensile testing machine (Tensilon, manufactured by A&D Corporation), and the peel strength, i.e., HS strength (N / 15 mm), was measured while peeling the measurement sample (T-type) from the long edge side at a speed of 200 mm / min. The peeled surface was visually observed and evaluated according to the following criteria. The measurement was carried out twice, and the peel strength was shown as the average value. If the evaluation results differed based on visual observation, both were shown. 〇: Breakage on the entire heat-sealed surface △: Partial damage to the heat-sealed surface ×: Peeling occurs between coating layers (no material breakage) -: No heat seal
[0042] (material) Paper base material: basis weight 220g / m 2 Cup base paper (product name: CUP-HD, manufactured by Nippon Paper Industries Co., Ltd.) PHBH: Kaneka Corporation, mass average molecular weight 600,000 Inorganic pigment: Shiraishi Kogyosha, kaolin, KCS, average particle size 3.6 μm, aspect ratio 10 to 15
[0043] PVA1: Kuraray, 28-98, tensile strength 61MPa, elongation 88% PVA2: Kuraray, HR3010, highly water resistant, tensile strength 49MPa, elongation 132% Partially saponified EVA: Kuraray, RS-1713, tensile strength 54 MPa, elongation 164% EVA1: Sumika Chemtex, S-400HQ, Tg 0°C, ethylene:vinyl acetate = 20:80, tensile strength 12.7MPa, elongation 550% EVA2: Sumika Chemtex, S-305HQ, Tg 7℃, ethylene:vinyl acetate=10:90, tensile strength 18.0MPa, elongation 420% EVA3: Sumika Chemtex, S-410HQ, Tg-18℃, ethylene:vinyl acetate=30:70, tensile strength 6.2MPa, elongation 850% EVA4: Sumika Chemtex, S-408HQE, Tg-30℃, ethylene:vinyl acetate=40:60, tensile strength 5.0MPa, elongation 650% EVA5: Sumika Chemtex Co., Ltd., Sumika Flex S-355HQ, Tg 10°C, ethylene:vinyl acetate = 10:90, tensile strength 20.6MPa, elongation 420%
[0044] Coated Paper PHBH, EVA or PVA, and an inorganic pigment were mixed and stirred in the parts by mass shown in Table 1 to obtain a coating liquid with a solid content concentration of 40% by mass. The coating liquid was applied onto one side of the paper substrate by a bar blade method so as to obtain the dry mass shown in Table 1, and then dried at 105°C for 1 minute. Furthermore, an overcoating solution of an aqueous dispersion of PHBH (solid content concentration: 40% by mass) was applied onto the coated surface by a bar blade method to give the dry weight shown in Table 1, and the coated surface was dried at 160°C for 3 minutes to obtain a coated paper having a coating layer and an overlayer.
[0045] [Table 1]
[0046] The buckling resistance evaluations of Comparative Examples 1 to 3, which had coating layers in which general-purpose PVA or highly water-resistant PVA was added to PHBH, were rated as "1" or "2." In addition, the buckling resistance evaluation of Comparative Example 4, in which partially saponified EVA was added to PHBH, was also rated as "1," and no improvement was observed. However, surprisingly, improvements were observed in Examples 2 to 4 where EVA was added. From Examples 2 to 5, it was found that the ratio of EVA to PHBH 100 parts by mass is effective in the range of 20 parts by mass to 235 parts by mass, and from Examples 6 to 9, it was found that EVA with different tensile strength and elongation also has the effect of improving buckling resistance. In Example 8, the buckling resistance (assuming bottom) was evaluated as "3", and although improvement was seen, it was not sufficient. It is considered that the tensile strength and elongation of EVA have an effect. Focusing on heat sealability, comparing Examples 4, 6, 7, 8, and 9 horizontally, the evaluation result at 150°C for Example 6 was "9.0", while Examples 4 and 9 were both "9.4", and Examples 7 and 8 were "12.4" and "12.1", respectively, showing that the heat seal strength was significantly better than the others. The reason for this is unknown, but it is thought to be influenced by the glass transition temperature of EVA. Moreover, the heat seal strength at 140°C of Example 1, in which a pigment was added to the coating layer in addition to EVA, was also "7.1", which was superior to Example 2 and other examples. That is, a comparison between Example 1 and Example 2 shows that the heat seal strength can be further increased under the same heat seal conditions by further adding an inorganic pigment to the coating layer. The difference is also confirmed when comparing at low temperatures such as 140°C and 150°C. The cause is unknown, but it is thought that the inorganic pigment in the coating layer efficiently conducts heat to the overlayer, which allows the opposing overlayer to fuse quickly during heat sealing processing.< / eva> < / phbh>
Claims
1. Basis weight: 100g / m 2 The above paper base material, a coating layer containing PHBH and EVA; an over layer containing PHBH on the coating layer; having The coating layer contains 10 parts by mass or more and 250 parts by mass or less of the EVA per 100 parts by mass of the PHBH, A coated paper characterized in that the EVA has a tensile strength of 4.0 MPa or more and an elongation of 300% or more.
2. 2. The coated paper according to claim 1, wherein the EVA has a tensile strength of 6.0 MPa or more and an elongation of 400% or more.
3. 3. The coated paper according to claim 2, characterized in that the EVA has a glass transition temperature of -30°C or more and 5°C or less.
4. 2. The coated paper of claim 1, wherein the coating layer contains an inorganic pigment.
5. A paper container comprising the coated paper according to any one of claims 1 to 4.
Citation Information
Patent Citations
Multilayer film
JP2015536255A
Coated paper
JP2021195716A