Method for producing positive electrode active material for non-aqueous electrolyte secondary battery
The described manufacturing process for lithium-containing transition metal oxides in non-aqueous electrolyte secondary batteries addresses resistance issues by incorporating tungsten and boron compounds through controlled heat treatments, resulting in a low-resistance active material with enhanced output performance.
Patent Information
- Application Number
- JP2021501725
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-27
- Filing Date
- 2020-01-21
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2040-01-21
AI Technical Summary
Existing methods for producing lithium-containing transition metal oxides as positive electrode active materials in non-aqueous electrolyte secondary batteries fail to sufficiently lower the resistance, limiting the output performance due to cation mixing and inadequate conductive paths for lithium ions.
A manufacturing process involving washing, dehydration, addition of tungsten and boron compounds, and controlled heat treatments at specific temperatures to create a conductive path for lithium ions, enhancing the surface interaction and reducing resistance.
The method results in a low-resistance positive electrode active material with improved output characteristics by ensuring a conductive path for lithium ions and protecting the surface of the lithium-containing transition metal oxide.
Smart Images

Figure 0007580035000002 
Figure 0007580035000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery. [Background technology]
[0002] Lithium-containing transition metal oxides are used as positive electrode active materials in lithium ion secondary batteries, which are non-aqueous electrolyte secondary batteries. For example, Patent Document 1 describes a lithium-containing transition metal oxide having the general formula Li z Ni 1-x-y Co x M y O 2 A method for increasing the output of a lithium-ion secondary battery is disclosed in which a lithium tungstate compound is attached to the surface of primary particles of a lithium-containing transition metal oxide represented by the formula: (0≦x≦0.35, 0≦y≦0.35, 0.95≦z≦1.30, M is at least one element selected from Mn, V, Mg, Mo, Nb, Ti, and Al) to reduce the resistance of the positive electrode. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-127004 A Summary of the Invention
[0004] However, the method described in Patent Document 1 cannot sufficiently reduce the resistance of the positive electrode, and there is still room for improvement.
[0005] Therefore, an object of the present disclosure is to provide a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery having improved output characteristics compared to conventional methods by reducing the resistance of a lithium-containing transition metal oxide.
[0006] A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a washing step of washing a lithium-containing transition metal oxide with water and dehydrating it to obtain a cake-like composition, a tungsten addition step of adding at least a tungsten compound or a tungsten-containing solution to the cake-like composition to obtain a tungsten additive, a first heat treatment step of heat-treating the tungsten additive at 180°C or less, and a second heat treatment step of heat-treating the tungsten additive at a temperature higher than 180°C to 330°C in an atmosphere other than a reducing atmosphere, and further includes a boron addition step of adding a boron compound or a boron-containing solution to the cake-like composition before the tungsten addition step, the tungsten additive before the first heat treatment step, or the tungsten additive before the second heat treatment step or during the second heat treatment step after the first heat treatment step.
[0007] According to one embodiment of the present disclosure, a low-resistance positive electrode active material for a nonaqueous electrolyte secondary battery is obtained. [Brief description of the drawings]
[0008] [Figure 1] 1A to 1C are diagrams illustrating a method for producing a positive electrode active material for a nonaqueous electrolyte secondary battery according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In lithium-containing transition metal oxides, if a phenomenon called cation mixing occurs in which a transition metal such as nickel enters the site for insertion and desorption of lithium ions during charging and discharging, the resistance of the positive electrode increases, and high output cannot be obtained. For example, Patent Document 1 describes z Ni 1-x-y Co x M y O 2(wherein 0≦x≦0.35, 0≦y≦0.35, 0.95≦z≦1.30, M is at least one element selected from Mn, V, Mg, Mo, Nb, Ti and Al) on the surface of the primary particles of a lithium-containing transition metal oxide, a method is disclosed in which a conductive path of lithium ions is formed at the interface with the electrolyte, thereby reducing the resistance of the positive electrode. However, as a result of intensive studies by the present inventors, it was found that the resistance of the positive electrode cannot be sufficiently reduced by simply securing the conductive path of lithium ions by adding tungsten. Therefore, the present inventors have further studied and have come up with a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery in the following embodiment.
[0010] A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a washing step of washing a lithium-containing transition metal oxide with water and dehydrating it to obtain a cake-like composition, a tungsten addition step of adding at least a tungsten compound or a tungsten-containing solution to the cake-like composition to obtain a tungsten additive, a first heat treatment step of heat-treating the tungsten additive at 180°C or less, and a second heat treatment step of heat-treating the tungsten additive at a temperature higher than 180°C to 330°C in an atmosphere other than a reducing atmosphere, and further includes a boron addition step of adding a boron compound or a boron-containing solution to the cake-like composition before the addition of the tungsten compound or the tungsten-containing solution, the tungsten additive before the first heat treatment step, or the tungsten additive before the second heat treatment step or during the second heat treatment step after the first heat treatment step. By subjecting the surface of a lithium-containing transition metal oxide to heat treatment at a temperature above 180°C and up to 330°C while causing tungsten and boron to be present on the surface, the interaction between tungsten and boron can protect the surface of the lithium-containing transition metal oxide while ensuring a conductive path for lithium ions, thereby enabling further reduction in resistance.
[0011] Hereinafter, each step of the method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to this embodiment will be described in detail.
[0012] The synthesis process of the lithium-containing transition metal oxide used in this embodiment will be described. First, a transition metal composite hydroxide such as nickel-cobalt-aluminum composite hydroxide obtained by coprecipitation is heat-treated to obtain a transition metal composite oxide. Next, the transition metal composite oxide is mixed with a lithium compound such as lithium hydroxide or lithium carbonate, and the mixture is heat-treated and then pulverized to obtain lithium-containing transition metal oxide particles.
[0013] The composition of the lithium-containing transition metal oxide is represented by the general formula Li z Ni 1-x-y Co x M y O 2 (wherein 0≦x≦0.2, 0≦y≦0.1, 0.97≦z≦1.20, and M is at least one element selected from Mn, W, Mg, Mo, Nb, Ti, Si, and Al.) In this case, the proportion of nickel in the metals other than lithium (Ni, Co, M) in the lithium-containing transition metal oxide is as high as 70 mol % to 80 mol %, and thus cation mixing is likely to occur, so that the effect of this embodiment is more pronounced.
[0014] [Cleaning process] The washing step is a step of washing the lithium-containing transition metal oxide with water and dehydrating it to obtain a cake-like composition (see FIG. 1). The lithium-containing transition metal oxide may be a particulate one obtained in the synthesis step. By washing with water, it is possible to remove unreacted lithium compounds added in the synthesis step of the lithium-containing transition metal oxide and impurities other than the lithium compounds. When washing with water, for example, 300 g to 5000 g of the lithium-containing transition metal oxide can be added per 1 L of water. The washing with water can be repeated several times. Dehydration after washing with water can be performed, for example, with a filter press. By dehydration, the water content of the cake-like composition after the washing step can be reduced to 10 wt% or less. The water content of the cake-like composition is preferably 2 wt% to 10 wt%, more preferably 4 wt% to 8 wt%, from the viewpoint of making it easier for the tungsten compound or tungsten contained in the tungsten-containing solution to be added later to spread on the surface of the lithium-containing transition metal oxide. The moisture content of the cake-like composition is calculated by drying 10 g of the cake-like composition by leaving it in a vacuum at 120° C. for 2 hours, and dividing the weight change of the cake-like composition before and after drying by the weight of the cake-like composition before drying. The moisture content of the tungsten additive is calculated in the same manner.
[0015] [Tungsten addition process] The tungsten addition step is a step of obtaining a tungsten additive by adding a tungsten compound or a tungsten-containing solution to the cake-like composition (see FIG. 1). Even after the washing step, a part of the lithium compound remains in the cake-like composition, and the remaining lithium compound dissolves in the water contained in the cake-like composition on the surface of the lithium-containing transition metal oxide contained in the cake-like composition to generate an alkaline aqueous solution. When a tungsten compound is added to the cake-like composition, the tungsten compound dissolves in the alkaline aqueous solution and spreads over the entire surface of the lithium-containing transition metal oxide. Examples of tungsten compounds that are directly added to the cake-like composition include tungsten oxide (WO 3 ), lithium tungstate (Li 2 WO 4 , Li 4 WO 5 , Li 6W 2 O 9 ) and the like can be exemplified. A tungsten-containing solution can also be added to the cake-like composition. The tungsten concentration in the tungsten-containing solution is, for example, 0.05 mol / L or more, and preferably 0.1 mol / L to 1 mol / L. The tungsten-containing solution is not particularly limited as long as it contains tungsten, but is preferably a solution in which a tungsten compound that is easily soluble in an alkaline solution, such as tungsten oxide, lithium tungstate, or ammonium tungstate, is dissolved in an aqueous solution of lithium hydroxide.
[0016] [First heat treatment process] The first heat treatment step is a step of heat treating the tungsten additive at 180°C or less (see FIG. 1). By drying the tungsten additive, in other words, by evaporating water from the tungsten-containing solution distributed on the surface of the tungsten additive, the tungsten compound can be attached to the surface of the lithium-containing transition metal oxide. The heat treatment temperature in the first heat treatment step is not particularly limited as long as it is a temperature at which water can be evaporated from the tungsten compound at 180°C or less, but is preferably 100°C or more, more preferably 150°C or more, from the viewpoint of efficiency. The atmosphere in the first heat treatment step can be, for example, in a vacuum. The heat treatment time in the first heat treatment step is not particularly limited, but is preferably 0.5 to 10 hours in order to sufficiently evaporate water from the tungsten-containing solution and form the tungsten compound on the surface of the lithium-containing transition metal oxide.
[0017] [Second heat treatment process] The second heat treatment step is a step of heat treating the tungsten additive at 180°C to 330°C in an atmosphere other than a reducing atmosphere after the first heat treatment step, and a positive electrode active material is produced (see FIG. 1). Here, the atmosphere other than a reducing atmosphere means an atmosphere such as an air atmosphere, an oxygen atmosphere, a decarbonation atmosphere, a vacuum, or an inert gas atmosphere. The decarbonation atmosphere is an air atmosphere in which the carbon dioxide concentration in the air is removed to 50 ppm or less, preferably 20 ppm or less. By performing heat treatment at a temperature of 180°C to 330°C, which is higher than the melting point of the boron compound, in the second heat treatment step, the boron compound or boron-containing solution added in the boron addition step described later can be melted and spread over the entire surface of the lithium-containing transition metal oxide. The heat treatment time in the second heat treatment step is not particularly limited, but is preferably 0.15 hours to 6 hours in order to sufficiently melt the boron compound or the boron-containing solution.
[0018] After the second heat treatment step, a cooling step can be performed. The boron-containing compound melted in the second heat treatment can be reprecipitated by the cooling step. The cooling step is not particularly limited as long as it is a step that can lower the temperature of the tungsten additive, but for example, slow cooling can be performed to lower the temperature of the tungsten additive to 180°C within 1 hour after the second heat treatment step, or rapid cooling can be performed to lower the temperature of the tungsten additive to 100°C or less within 1 hour after the second heat treatment step.
[0019] It is preferable to further include a cooling step after the second heat treatment step in which the temperature of the tungsten additive becomes 100°C or less within 1 hour after the second heat treatment step. In other words, it is preferable to perform rapid cooling after the second heat treatment step. By shortening the cooling time, the amount of impurities adhering to the surface during cooling can be reduced.
[0020] [Boron addition process] The boron addition step is a step of adding a boron compound or a boron-containing solution to the cake-like composition (a) before the tungsten addition step in FIG. 1, the tungsten additive (b, c) before the first heat treatment step, or the tungsten additive (d, e, f) before or during the second heat treatment step.
[0021] By adding boron to the tungsten additive, the synergistic effect of tungsten and boron not only ensures the conductive path of lithium ions, but also protects the surface of the lithium-containing transition metal oxide, thereby making it possible to further reduce the resistance of the positive electrode. Here, the effect of protecting the surface of the lithium-containing transition metal oxide means that tungsten and boron adhere to and coat the surface of the lithium-containing transition metal oxide, thereby maintaining the surface structure of the lithium-containing transition metal oxide during charging and discharging.
[0022] The boron compounds added directly to the cake composition or tungsten additive include boric acid (H 3 BO 3 ), Metaboric acid (HBO 2 ), tetraboric acid (H 2 B 4 O 7 ) and the like can be exemplified. The particle size of the boron compound is not particularly limited, but from the viewpoint of dispersibility, it is preferably 100 μm or less, more preferably 50 μm or less, and particularly preferably 10 μm or less. A boron-containing solution can also be added to the cake-like composition or the tungsten additive. The boron concentration in the boron-containing solution is, for example, 0.05 mol / L to 2 mol / L, and preferably 0.1 mol / L to 1 mol / L. The boron-containing solution is not particularly limited as long as it contains boron, but examples thereof include boric acid, metaboric acid, and tetraboric acid, and further includes lithium hydroxide (LiOH) and lithium carbonate (Li 2 CO 3 It is preferable to add an acid such as tungsten additive or the like to the boron-containing solution to make the pH of the solution 7 or higher. In this case, deterioration of the surface of the positive electrode active material (cake-like composition or tungsten additive) due to acid can be prevented.
[0023] The moisture content of the cake-like composition or the tungsten additive before the boron addition step is preferably 2 wt% or less. If the moisture content of the cake-like composition or the tungsten additive is higher than 2 wt%, the cake-like composition or the tungsten additive will aggregate with each other, making it difficult to disperse the boron compound.
[0024] The boron doping step is preferably carried out after the first heat treatment step (e, f). The first heat treatment evaporates the moisture contained in the tungsten compound, making the powder of the tungsten additive smoother and improving the dispersibility of the boron compound.
[0025] When the boron addition step is carried out before and during the first heat treatment step (a, b, c, d), the first heat treatment step and the second heat treatment step can be carried out continuously by setting a time below 180°C for a predetermined time and then a time above 180°C for a predetermined time.
[0026] The boron addition step is preferably a step of adding boric acid to the cake-like composition or the tungsten additive. The boric acid compound is preferred because it discharges less water than the boron-containing aqueous solution, minimizing the load on the equipment.
[0027] A non-aqueous electrolyte secondary battery to which the positive electrode active material produced by the above-mentioned production method is applied is obtained, for example, by housing an electrode assembly, which is formed by laminating or winding electrodes (positive electrode, negative electrode) and a separator, together with a non-aqueous electrolyte in a housing such as a battery can or a laminate. The positive electrode, negative electrode, separator, and non-aqueous electrolyte in this embodiment are, for example, as follows.
[0028] <Positive electrode> The positive electrode includes a positive electrode current collector such as a metal foil and a positive electrode composite layer formed on the positive electrode current collector. The positive electrode current collector may be a foil of a metal such as aluminum that is stable in the potential range of the positive electrode, or a film having the metal disposed on its surface.
[0029] The positive electrode mixture layer preferably contains a positive electrode active material, and further contains a conductive material, a binder, etc. The positive electrode can be produced, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a conductive material, a binder, etc., onto a positive electrode current collector, drying the coating, and then rolling to form a positive electrode mixture layer on both sides of the positive electrode current collector.
[0030] As the conductive material, carbon powder such as carbon black, acetylene black, ketjen black, graphite, etc. may be used alone or in combination of two or more kinds.
[0031] Examples of the binder include fluorine-based polymers, rubber-based polymers, etc. For example, examples of the fluorine-based polymers include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), or modified versions thereof, and examples of the rubber-based polymers include ethylene-propylene-isoprene copolymers, ethylene-propylene-butadiene copolymers, etc. These may be used alone or in combination of two or more kinds.
[0032] <Negative electrode> The negative electrode includes a negative electrode current collector such as a metal foil, and a negative electrode composite layer formed on the negative electrode current collector. For the negative electrode current collector, a foil of a metal such as copper that is stable in the potential range of the negative electrode, a film with the metal disposed on the surface layer, or the like can be used. The negative electrode composite layer contains a negative electrode active material, and preferably also contains a thickener, a binder, and the like. The negative electrode can be produced, for example, by applying a negative electrode composite slurry in which a negative electrode active material, a thickener, and a binder are dispersed in water at a predetermined weight ratio onto the negative electrode current collector, drying the coating, and then rolling to form a negative electrode composite layer on both sides of the negative electrode current collector.
[0033] As the negative electrode active material, a carbon material capable of absorbing and releasing lithium ions can be used, and in addition to graphite, non-graphitizable carbon, graphitizable carbon, fibrous carbon, coke, carbon black, etc. Furthermore, as a non-carbon-based material, silicon, tin, and alloys and oxides mainly containing these can be used.
[0034] As the binder, PTFE or the like can be used as in the case of the positive electrode, but styrene-butadiene copolymer (SBR) or its modified form may also be used. As the thickener, carboxymethyl cellulose (CMC) or the like can be used.
[0035] <Non-aqueous electrolyte> As the non-aqueous solvent (organic solvent) of the non-aqueous electrolyte, carbonates, lactones, ethers, ketones, esters, etc. can be used, and two or more of these solvents can be mixed and used. For example, cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, mixed solvents of cyclic carbonates and chain carbonates, etc. can be used.
[0036] The electrolyte salt for the non-aqueous electrolyte is LiPF 6 , LiBF 4 , LiCF 3 SO 3 The amount of electrolyte salt dissolved in the non-aqueous solvent may be, for example, 0.5 to 2.0 mol / L.
[0037] <separator> The separator may be a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. The separator may be made of an olefin resin such as polyethylene or polypropylene, or cellulose. The separator may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. The separator may also be a multilayer separator including a polyethylene layer and a polypropylene layer, and may have a material such as an aramid resin or ceramic applied to the surface of the separator. EXAMPLES
[0038] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0039] [Production of positive electrode active material] <Example 1> Ni obtained by coprecipitation 0.91 Co 0.045 Al 0.045 (OH) 2 A nickel-cobalt-aluminum composite hydroxide represented by the formula (I) was heat-treated at 500°C to obtain an oxide. LiOH and the oxide were mixed in an Ishikawa-type mortar so that the molar ratio of Li to the entire transition metals was 1.08:1 to obtain a mixture. The mixture was placed in a calcination furnace and calcined from room temperature to 650°C at a temperature increase rate of 2.0°C / min under an oxygen flow with an oxygen concentration of 95% (flow rate of 2mL / min per 10 cm3 and 5L / min per 1 kg of the mixture), and then calcined from 650°C to 710°C at a temperature increase rate of 0.5°C / min to obtain Li with an average secondary particle size of about 11 μm. 1.05 Ni 0.91 Co 0.045 Al 0.045 O 2 The resulting particles were lithium nickel cobalt aluminum composite oxide (lithium-containing transition metal oxide) represented by the formula: The composition of the lithium-containing transition metal oxide particles was measured using an ICP emission spectrometer.
[0040] 800g of pure water was added to 1000g of the lithium nickel cobalt aluminum composite oxide particles, stirred, filtered and separated, washed with pure water and dehydrated to obtain a cake-like composition after washing. The water content of the cake-like composition was 4wt%.
[0041] Next, 0.19 wt% of WO in terms of tungsten element relative to the lithium-containing transition metal oxide was added to the cake-like composition. 3 The powder was added, and the first heat treatment step was carried out in a vacuum at a temperature of 180° C. for 3 hours, and then the mixture was cooled in a furnace to room temperature, thereby obtaining a tungsten additive having a water content of 0.08 wt %.
[0042] To the tungsten additive, boric acid was added in an amount of 0.01 wt% in terms of boron element relative to the lithium-containing transition metal oxide, and a second heat treatment step was performed for 3 hours in an air atmosphere at 250° C. After the second heat treatment step, the tungsten additive was cooled to 100° C. or less within 1 hour, thereby obtaining the positive electrode active material of Example 1.
[0043] <Example 2> A positive electrode active material was produced in the same manner as in Example 1, except that the temperature in the second heat treatment step was 185°C.
[0044] <Example 3> A positive electrode active material was produced in the same manner as in Example 1, except that the temperature in the second heat treatment step was 330°C.
[0045] <Example 4> A positive electrode active material was prepared in the same manner as in Example 1, except that the amount of boric acid added was 0.005 wt % in terms of boron element relative to the lithium-containing transition metal oxide.
[0046] <Example 5> A positive electrode active material was prepared in the same manner as in Example 1, except that the amount of boric acid added was 0.05 wt % in terms of boron element relative to the lithium-containing transition metal oxide.
[0047] <Example 6> A positive electrode active material was prepared in the same manner as in Example 1, except that the amount of boric acid added was 0.1 wt % in terms of boron element relative to the lithium-containing transition metal oxide.
[0048] <Example 7> The cake-like composition after the washing step contained 0.19 wt% WO in terms of tungsten element relative to the lithium-containing transition metal oxide particles. 3The powder and 0.01 wt% boric acid in terms of boron element relative to the lithium-containing transition metal oxide were simultaneously added, and a first heat treatment step was performed in a vacuum at 180° C. for 3 hours, followed by a second heat treatment step in an air atmosphere at 250° C. for 3 hours. The tungsten additive after the second heat treatment step was cooled to 100° C. or less within 1 hour to produce the positive electrode active material of Example 7.
[0049] <Example 8> WO 3 A positive electrode active material was prepared in the same manner as in Example 7, except that a tungsten-containing solution was added to the cake-like composition instead of the powder. The tungsten-containing solution was prepared by dissolving 2.4 g of WO in an aqueous solution obtained by dissolving 1 g of lithium hydroxide (LiOH) in 20 g of pure water. 3 The tungsten-containing solution was added to the cake-like composition so that the tungsten-containing solution was 0.19 wt % in terms of tungsten element relative to the lithium-containing transition metal oxide particles.
[0050] <Example 9> A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere in the second heat treatment step was an oxygen atmosphere.
[0051] <Example 10> A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere in the second heat treatment step was a decarbonation atmosphere.
[0052] <Example 11> A positive electrode active material was produced in the same manner as in Example 1, except that the tungsten additive after the second heat treatment step was cooled to 180° C. in one hour.
[0053] <Example 12> The boron-containing solution was prepared by adding 6.4 g of boric acid to an aqueous solution in which 0.24 g of lithium hydroxide (LiOH) was dissolved in 15 g of pure water and stirring the solution. A positive electrode active material was prepared in the same manner as in Example 1, except that the boron-containing solution was added in an amount equivalent to 0.01 wt% of boron element relative to the lithium-containing transition metal oxide particles instead of boric acid.
[0054] <Comparative Example 1> A positive electrode active material was produced in the same manner as in Example 1, except that boric acid was not added and the second heat treatment step was not performed.
[0055] <Comparative Example 2> WO 3 A positive electrode active material was prepared in the same manner as in Comparative Example 1, except that a tungsten-containing solution was added to the cake-like composition instead of the powder. The tungsten-containing solution was prepared by dissolving 2.4 g of WO in an aqueous solution obtained by dissolving 1 g of lithium hydroxide (LiOH) in 20 g of pure water. 3 The tungsten-containing solution was added to the cake-like composition so that the tungsten-containing solution was 0.19 wt % in terms of tungsten element relative to the lithium-containing transition metal oxide particles.
[0056] <Comparative Example 3> A positive electrode active material was prepared in the same manner as in Example 1, except that boric acid was not added.
[0057] <Comparative Example 4> A positive electrode active material was produced in the same manner as in Example 8, except that the second heat treatment step was not carried out.
[0058] <Comparative Example 5> A positive electrode active material was produced in the same manner as in Example 1, except that the temperature in the second heat treatment step was 150°C.
[0059] <Comparative Example 6> A positive electrode active material was produced in the same manner as in Example 1, except that the temperature in the second heat treatment step was 400°C.
[0060] <Comparative Example 7> A positive electrode active material was prepared in the same manner as in Example 7, except that tungsten was not added.
[0061] <Comparative Example 8> A positive electrode active material was produced by carrying out only the same cleaning step and first heat treatment as in Example 1, without carrying out the addition of tungsten, the addition of boric acid, and the second heat treatment.
[0062] <Comparative Example 9> A positive electrode active material was prepared in the same manner as in Example 1, except that tungsten was not added.
[0063] <Comparative Example 10> A positive electrode active material was prepared in the same manner as in Example 1, except that tungsten and boric acid were not added.
[0064] [Preparation of positive electrode] The positive electrode active materials prepared in Examples 1 to 11 and Comparative Examples 1 to 10, acetylene black, and polyvinylidene fluoride were mixed in a mass ratio of 85:10:5, and were kneaded using an agate mortar and pestle to form thin pellets. After that, the mixture was rolled to a predetermined thickness using a roller, and then punched into a predetermined circular shape to form a positive electrode.
[0065] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 20:5:75. Lithium hexafluorophosphate (LiPF 6 ) was dissolved in water to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0066] [Preparation of test cell] The positive electrode of Example 1 and the negative electrode made of lithium metal were stacked so as to face each other with a separator interposed therebetween to prepare an electrode body. The electrode body and the non-aqueous electrolyte were then inserted into an aluminum coin-shaped exterior body and sealed by crimping with a press machine to prepare a test cell. Test cells were prepared in the same manner in the other Examples and Comparative Examples.
[0067] [Measurement of reaction resistance] The above test cell was charged at a constant current of 0.7 mA under a temperature condition of 25° C. until the cell voltage reached 4.3 V, and then charged at a constant voltage of 4.3 V until the current value reached 0.07 mA. Subsequently, a constant current discharge was performed at 0.7 mA until the cell voltage reached 2.5 V. Thereafter, again under a temperature condition of 25° C., a constant current charge was performed at 0.7 mA until the cell voltage reached 4.3 V, and then a constant voltage charge was performed at 4.3 V until the current value reached 0.07 mA. Next, the test cell was measured for AC impedance at 20 kHz to 0.01 Hz using an AC impedance measuring device, and a Cole-Cole plot was drawn from the measured data, and the reaction resistance was calculated from the size of the arc between 10 Hz and 0.1 Hz. The reaction resistance in Table 1 is expressed relatively to the reaction resistance of the test cell containing the positive electrode active material of Comparative Example 1, which is set to 100, and the reaction resistance of the other test cells.
[0068] [Table 1]
[0069] It was confirmed that in Examples 1 to 12, the reaction resistance was lower than that in Comparative Example 1. In other words, it was confirmed that according to the manufacturing method of the positive electrode active material for a nonaqueous electrolyte secondary battery which is one aspect of the present disclosure, a nonaqueous electrolyte secondary battery having a lower resistance value and improved output characteristics than the conventional one can be manufactured. In addition, it was confirmed that the reaction resistance of Example 1 in which rapid cooling was performed was smaller than that of Example 11 in which slow cooling was performed, and rapid cooling is preferable. On the other hand, the reaction resistance of Comparative Examples 3 to 10 was higher than that of Comparative Example 1. In addition, the reaction resistance of Comparative Example 2 was the same as that of Comparative Example 1.
Claims
1. a washing step of washing the lithium-containing transition metal oxide with water and dehydrating it to obtain a cake-like composition; a tungsten addition step of adding at least a tungsten compound or a tungsten-containing solution to the cake-like composition to obtain a tungsten additive; A first heat treatment step of heat treating the tungsten additive at 100° C. or more and 180° C. or less; A second heat treatment step of heat treating the tungsten additive at a temperature of more than 180° C. to 330° C. in an atmosphere other than a reducing atmosphere; and a cooling step after the second heat treatment step, in which the temperature of the tungsten additive is cooled to 100° C. or less within 1 hour after the second heat treatment step; The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery further includes a boron addition step of adding a boron compound or a boron-containing solution to the cake-like composition before a tungsten addition step, the tungsten additive before the first heat treatment step, or the tungsten additive after the first heat treatment step and before the second heat treatment step or during the second heat treatment step.
2. The composition of the lithium-containing transition metal oxide is represented by the general formula Li z Ni 1-x-y Co x M y O 2 2. The method for producing a positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, wherein: (wherein 0≦x≦0.2, 0≦y≦0.1, 0.97≦z≦1.20, and M is at least one element selected from Mn, W, Mg, Mo, Nb, Ti, Si, and Al).
3. 3. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the boron addition step is carried out after the first heat treatment step.
4. 4. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the water content of the cake-like composition after the washing step is 10 wt % or less, and the water content of the cake-like composition or the tungsten additive before the boron addition step is 2 wt % or less.
5. 5. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein in the boron addition step, the boron compound is boric acid.
Citation Information
Patent Citations
Non-aqueous electrolyte secondary battery
JP2000173584A
Method of manufacturing positive electrode active material, and positive electrode active material
JP2010040383A
Cathode active material for non-aqueous secondary battery and manufacturing method for the same
JP2015201388A
Positive electrode active material for nonaqueous electrolyte secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery arranged by use of positive electrode active material
JP2016127004A
Nonaqueous electrolyte secondary battery positive electrode active material and nonaqueous electrolyte secondary battery
WO2017018099A1