Composite powder material, manufacturing method thereof, and electrode material
By exfoliating MXene nanosheets and evenly distributing acetylene black, a composite particle material is created with enhanced ion diffusivity and electron conductivity, addressing the limitations of existing MXene-based battery materials.
Patent Information
- Application Number
- JP2023520701
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-13
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-05-13
AI Technical Summary
Existing MXene nanosheets used in secondary batteries and capacitors require improvements in ion diffusivity and electron conductivity, particularly when combined with conductive additives like acetylene black, to enhance battery characteristics.
A composite particle material is developed by exfoliating MXene nanosheets to a single layer level, reducing size, and evenly distributing acetylene black, with specific surface area and mutual dispersion optimized to create a highly conductive and dispersible material.
The composite particle material exhibits high ion diffusivity and smooth electron transfer to the current collector, resulting in improved performance as a negative electrode active material for secondary batteries.
Smart Images

Figure 0007580094000007 
Figure 0007580094000008 
Figure 0007580094000009
Abstract
Description
Technical Field
[0001] The present invention relates to a composite particle material of a novel MXene nanosheet and a microsome, a method for producing the same, and an electrode material using the composite particle material.
Background Art
[0002] Conventionally, a particle material composed of an MXene layered compound obtained by removing Al by acid treatment from MAX phase ceramics powder such as Ti3AlC2, which is a layered compound (in this specification, it may be appropriately referred to as "MXene particle material", "MXene nanosheet", "layered compound particle material", or simply "particle material") is known (Patent Documents 1 to 4). Since Na ions and Li ions can be stored / desorbed in the void layer from which the Al layer has been removed in these MXene layered compounds, they are used as negative electrode active material materials for secondary batteries (storage batteries) and capacitors, and due to their excellent conductivity, they are expected to be applied to electromagnetic shielding thin films, conductive thin films, etc.
[0003] MAX phase ceramics are layered compounds, and the general formula is M n+1 AX n and is represented as. In the formula, M is a transition metal (Ti, Sc, Cr, Zr, Nb, etc.), A is a group A element, X is C, or [C (1.0-x) N x (0 < x ≤ 1.0)], and n is from 1 to 3.
[0004] Among them, when A is Al, since the bond between M - A is weaker than the bond between M - X, the Al layer is selectively removed by acid treatment. The present inventors have proposed a method for preparing MXene nanosheets by exfoliating using a bead mill using micro-sized beads (Patent Documents 5 and 6).
Prior Art Documents
Patent Documents
[0005]
Patent Document 1
[0006] Here, when MXene nanosheets are used in secondary batteries (storage batteries) or capacitors, not only MXene nanosheets but also acetylene black is added as a conductive auxiliary agent. In order to improve battery characteristics, it is necessary to increase ion diffusivity and smoothly move electrons to the current collector. Specifically, it is required to increase the specific surface area of the MXene and acetylene black composite particle material by peeling the nanosheets to a single layer level and appropriately reducing their size, and to uniformly arrange the acetylene black between the nanosheets. As a result of intensive investigation, we have succeeded in obtaining a composite particle material of MXene nanosheets and carbon microparticles that is effective as an ideal negative electrode active material for secondary batteries (storage batteries). Note that, since it is possible to obtain new materials by compounding microparticles other than carbon microparticles with MXene nanosheets, microparticles other than carbon microparticles are also considered in this specification.
[0007] The present invention was completed in consideration of the above-mentioned situation, and the problem to be solved by this invention is to provide a novel composite particulate material of MXene nanosheets and microobjects, a method for producing the same, and an electrode material using the composite particulate material. [Means for solving the problem]
[0008] The composite particulate material of the present invention, which solves the above problems, comprises 90 to 97 parts by mass of sheet-shaped Ti3A l a (C(1. 0-x )N x MXene and 3 to 10 parts by mass of fine particles, and the mutual dispersion degree is 1.50 to 7.00 and the specific surface area is 75 m 2 / The degree of mutual dispersion will be described in the section of the embodiment.
[0009] It is preferable that the average pore diameter is 7.0 to 20.0 nm and the pore volume is 0.10 to 0.50 mL / g.
[0010] The Ti3Al a (C(1. 0-x )N x )2(0≦x≦0.03, a is greater than 0.02) MXe It is preferable that ne has an average thickness of 1.0 to 3.5 nm, an average size in the spreading direction of the sheet of 0.5 to 1.0 μm, and a primary particle diameter of the fine particles of 30 to 50 nm. a (C(1. 0-x )N x )2(0≦x≦0.03, a is greater than 0.02) MXen It is preferable that the interlayer distance of the (002) plane of Ti3Al e is 1,400 nm to 1,700 nm. a (C(1. 0-x )N x )2(0≦x≦0.03, a is greater than 0.02) MXene The half width of the (002) plane is preferably 0.90° to 1.50°, and the surface electrical resistivity is preferably 1.0 Ω / □ to 100.0 Ω / □. Ti3Al with a zeta potential of -25.0mV to -30.0mV a (C(1. 0-x )N x )2 (0≦x≦0.03, a is greater than 0.02) It is preferable that the capacitance is composed of MXene and carbon particles having a capacitance of −20.0 mV to −25.0 mV.
[0011] The negative electrode of the present invention, which solves the above-mentioned problems, has the above-mentioned composite particulate material of the present invention as a negative electrode active material.
[0012] The method for producing a composite particulate material of the present invention that solves the above problems is a (C(1. 0-x ) N x MXene to form exfoliated matter; an acid treatment step of treating raw carbon particles in a mixed acid solution of sulfuric acid and nitric acid at 70°C or higher for 10 minutes or more to obtain carbon particles; a mixing step of obtaining a mixture in which the exfoliated matter and the carbon particles are dispersed in a second dispersion medium at a mass ratio of 90:10 to 97:3 and a concentration of the exfoliated matter is 11.5 to 17.0 mg / mL; a step of intercalating a lithium chloride aqueous solution using a shaker at a rotation speed of 100 rpm to 300 rpm; and a step of making the mixture alkaline to cause coagulation to obtain the Ti3Al a (C(1. 0-x )N x )2(0≦x≦0. 03, a is greater than 0.02), and an aggregation step for obtaining a composite particle material of MXene and the carbon microparticles. In particular, the peeling step is preferably carried out until 99% or more of the MXene is separated into the peeled material by mass. Effect of the Invention
[0013] The composite particulate material and the method for producing the same of the present invention have the above-mentioned configuration, and therefore, a (C(1. 0-x )N x )2(0≦x≦0.03, a is more than 0.02) MXene and micro particles are highly It is possible to provide a composite particulate material in which Ti3Al is dispersed. a (C(1. 0-x ) N x)2 (0≦x≦0.03, a is greater than 0.02) By adopting a composite particle material with a high specific surface area, in which MXene and microparticles are highly dispersed, as the negative electrode active material, it is possible to provide a negative electrode that can demonstrate high performance when used in secondary batteries (storage batteries) and capacitors. [Brief description of the drawings]
[0014] [Figure 1] 1 is an AFM image of a peeled product obtained in the peeling step of Example 1. [Diagram 2] 2 is a SEM photograph of a peeled product obtained in the peeling step of Example 1. [Diagram 3] 1 shows XRD profiles of the MAX phase ceramics of Example 1, the MXene after being subjected to the exfoliation process, and the composite powder material. [Figure 4] 1 is a graph showing cycle characteristics of Li-ion secondary batteries using the composite powder materials of Example 1 and Comparative Example 1 as electrode active materials. [Diagram 5] 1 is a graph showing charge / discharge curves at the 1st cycle and the 100th cycle of a Li-ion secondary battery using the composite powder material of Example 1 as an electrode active material. [Figure 6] 1 is a SEM photograph of the composite powder material of Example 1. [Figure 7] 1 is a SEM photograph of the composite powder material of Example 4. [Figure 8] 1 is a SEM photograph of the composite powder material of Example 2. [Figure 9] 2 is a SEM photograph of the composite powder material of Comparative Example 1. [Figure 10] 1 is a SEM photograph of the composite powder material of Comparative Example 2. [Figure 11] 1 is a graph showing the particle concentration dependence of the specific surface area of the obtained composite powder material of the exfoliated material (MXene) in the aggregation process. [Figure 12] FIG. 1 shows the crystal structure of MAX phase ceramics presented to explain the crystal structure of MXene. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The composite particulate material of the present invention, its manufacturing method, and electrode material will be described in detail below based on the embodiments. The composite particulate material of the present embodiment has excellent electrical properties such as electrical conductivity, and has a large void layer formed by removing the Al layer, so it can be applied to secondary batteries (Li-ion secondary batteries, Na-ion secondary batteries), active material materials (especially negative electrode active material) for capacitors, electromagnetic shielding thin films, conductive thin film materials, etc. (Composite particle material) The composite particulate material of this embodiment is a particulate material that combines exfoliated MXene with particulate or tubular carbon microparticles for application to electrode materials, etc. The particulate material in which MXene is exfoliated is obtained by exfoliating MXene, which is a powdered layered compound.
[0016] In this specification, when multiple upper and lower limit values are set for a certain parameter, the upper and lower limit values can be arbitrarily combined unless otherwise limited. The composite particulate material of this embodiment is a composite particulate material of MXene and microparticles.
[0017] The MXene content is 90-97% based on the sum of the masses of MXene and microparticles, with the remaining 10%-2% being microparticles. The lower limit of the MXene content is 93%, 92%, or 90%, and the upper limit is 97%, 96%, or 95%.
[0018] The composite particle material has a mutual dispersion of 1.50 to 7.00. The mutual dispersion is a value that specifies the degree of dispersion between MXene and the microparticles. When carbon microparticles are used as the microparticles, the mutual dispersion was measured by Raman spectroscopy using a 532 nm laser at 400 cm for 100 randomly selected composite particle materials. -1 Peak height A and 1332 cm -1 The standard deviation calculated from the ratio (B / A) of the peak heights B of the composite particle material is taken as the mutual dispersion. The lower limit of the mutual dispersion of the composite particle material can be 1.50, 2.00, or 2.50, and the upper limit can be 7.00, 6.00, or 5.00.
[0019] The composite particle material has a specific surface area of 75m 2 The specific surface area is 1 / g or more after pretreatment in a vacuum. The specific surface area of the composite particle material is measured by the BET method using nitrogen at 00°C for 24 hours. The lower limit of the specific surface area is 75 m 2 / g, 77.5m 2 / g, 80m 2 / g should be adopted. The upper limit is 110m. 2 / g, 107.5m 2 / g, 105m 2 By adopting / g The composite particle material preferably has an average pore diameter of 7.0 to 20.0 nm and a pore volume of 0.10 to 0.50 mL / g. The average pore diameter and pore volume were measured by a BET method using nitrogen under the condition that the pretreatment was performed in a vacuum at 100° C. for 24 hours.
[0020] MXene is a layered compound consisting of three layers of titanium and two layers of carbon, or with some of the carbon replaced with nitrogen. a (C(1. 0-x )N x )2(0≦x≦0.03, a is 0.02 The MXene is a Ti3A super MXene (hereinafter referred to as "MXene"). l a (C(1.0- x )N x )2. Here, it is preferable that 0≦x≦0.03 and a is greater than 0.02. The upper limit of a is preferably 0.05. In addition to these elements, O, OH, and halogen groups can be present as surface functional groups.
[0021] MXene may be in the form of a plate, leaf, flake, or sheet, and is generally defined as a sheet. The direction in which the layers of the layered compound are stacked is defined as the "thickness" of MXene, and the direction perpendicular to the thickness is defined as the "spread direction of the sheet." The average thickness of MXene is preferably 1.0 to 3.5 nm, and more preferably 1.5 to 3.0 nm. The average thickness is calculated as the average value of the values measured for 100 randomly selected particles. The size of the sheet can be measured by dropping a nanosheet onto a hydrophilized Si wafer and using a SEM. The average size in the spreading direction of the particles is preferably 0.5 to 1.0 μm, and more preferably 0.5 to 0.75 μm. If the maximum value in the direction perpendicular to the thickness is the "long side" and the minimum value is the "short side", the average value of [(long side + short side) / 2] measured by SEM for 100 randomly selected particles is taken as the average size in the spreading direction.
[0022] The interlayer distance of the (002) plane of MXene is preferably 1.400 nm to 1.700 nm. The interlayer distance of the void layer is 0.770 nm to 0.470 nm, defined as the interlayer distance, which is the d value of the (002) plane in the XRD of the MXene nanosheet powder, minus the interlayer distance, which is the d value of the (002) plane in the XRD of the corresponding MAX phase ceramic powder. The Li ion diameter is 0.18 nm and the Na ion diameter is 0.28 nm, and the MXene nanosheet can be used as the negative electrode active material for Na ion secondary batteries as well as Li ion secondary batteries. The interlayer distance of the (002) plane of the graphite powder used as the negative electrode active material for Li ion secondary batteries is 0.33 nm, and therefore it cannot be used for Na ion secondary batteries. This is the reason why the MXene nanosheet is particularly suitable for Na ions. This is why it is expected to be used as a secondary battery. The corresponding MAX phase ceramic powder here is Ti3Al a (C(1. 0-x )N x )2, a is 1 The particle material is made up of the material.
[0023] The size of the micro-body is sufficient if it is on the order of nanometers, and being on the order of nanometers means that the length of the longest part of the length of the micro-body is 100 nm or less. The micro-body preferably has a primary particle diameter of 100 nm or less, preferably 30 to 50 nm, and more preferably 30 to 40 nm, and may be in the form of an aggregate. The shape of the micro-body is not limited, and examples thereof include spherical, sheet, tubular, hollow, and amorphous.
[0024] In particular, the microparticles are preferably conductive, and examples of conductive microparticles include carbon microparticles made of carbon materials and metal microparticles made of metal materials. As carbon microparticles, it is preferable to adopt highly conductive materials such as acetylene black, Ketjen black, carbon nanotubes, graphene, carbon fiber, graphite powder, and hard carbon powder. As the microparticles, inorganic microparticles made of other inorganic substances can be adopted in addition to carbon microparticles made of carbon materials. As inorganic microparticles, TiO2, Al2O3, SiO2, and BaTiO3 with a primary particle diameter of 100 nm or less can be adopted. (Method of manufacturing composite particulate material) The method for producing the composite particulate material of this embodiment includes an exfoliation step, a mixing step, an intercalation step, an aggregation step, and other necessary steps. Peeling process The exfoliation process is a process in which the layered MXene is exfoliated by colliding microbeads between the layers in a dispersion medium to obtain nanosheet-like exfoliated material. The obtained exfoliated material becomes an exfoliated material suspension suspended in a dispersion medium. This exfoliated material suspension can be directly subjected to the mixing process, or the dispersion medium can be removed before being subjected to the mixing process. There is no particular limitation on the method for obtaining the layered MXene material, but the following methods can be exemplified.
[0025] MXene is obtained by acid-treating a raw material consisting of Ti3-layered MAX phase ceramic powder to partially dissolve the Al layer. An example of a method for producing MXene will be described later as a pretreatment process. The raw material used in the peeling process can have the same composition as the material that constitutes the particle material described above. The composition does not change much during the peeling process.
[0026] This particulate material is treated with acid to dissolve some of the Al and turn it into MXene. This MXene is then mixed into a solvent whose main component is water to form a mixture. After that, an exfoliation process is carried out in a bead mill that rotates at high speed using beads of 10 μm to 300 μm, resulting in an exfoliation suspension in which nanosheet-like MXene exfoliates are suspended.
[0027] The dispersion medium used in the peeling step is not particularly limited, but preferably contains water at 50% by mass or more, and may contain alcohols such as methanol, ethanol, isopropanol, ketones such as methyl ethyl ketone, acetone, dimethylformamide, dimethylsulfoxide, etc. It is more preferable that the dispersion medium is 100% by mass of water.
[0028] The concentration of MXene in the mixture used in the peeling step is not particularly limited, but can be about 10.0 mg / mL to 20.0 mg / mL. The liquid property of the mixture is not particularly limited, but can be about pH 6.0 to 8.0.
[0029] The specific bead mill treatment in the peeling process will be described below. Peeling can be performed using a bead mill equipped with a mechanism for classifying a mixture of small beads and a slurry-like mixture by centrifugation. The peeled material peeled off by the bead mill treatment can be separated from the mixture before peeling by centrifugation at any time, and ultimately all of the MXene can be made into the peeled material.
[0030] For example, the lower limit of the bead size can be 10 μm, 15 μm, 20 μm, 30 μm, or 40 μm, and the upper limit can be 300 μm, 200 μm, or 100 μm. If the size is 10 μm or more, it is easy to classify the beads and the slurry. If beads of 300 μm or less are used, peeling can be prioritized over reducing the size of the particulate material. These lower and upper limits can be used in any combination. If the size of the beads is within the appropriate range, the energy applied can be increased and peeling can be prioritized, so it is most preferable to use beads of 50 μm to 100 μm.
[0031] The material of the beads is not particularly limited, but ceramics such as zirconia, alumina, and silicon nitride can be used. Partially stabilized zirconia, which has high fracture toughness, is particularly preferable. On the other hand, in a commonly used bead mill that uses beads over 300 μm and classifies beads and slurry through minute gaps, reducing the size of the particulate material takes precedence over peeling. In addition, in a ball mill such as a planetary ball mill that uses beads or balls over 300 μm, reducing the size of the particulate material takes precedence over peeling. As a result, only a portion of the material can be peeled off, and only a portion of the peeled material is classified by centrifugation, which is not at a level that can be used in industry.
[0032] Furthermore, conventionally, MXene is peeled off by ultrasonic irradiation. When ultrasonic waves are irradiated to the solvent, When this happens, cavitation occurs, and the resulting crushing causes the powder particles to collide with each other, which causes the layers that make up the layered compound to peel off. However, even if water, which is prone to cavitation, is used, peeling only progresses partially. Even if water is used, peeling only progresses partially, and it cannot be said to be at a level that can be used industrially. Even with the method using a planetary ball mill, peeling is of course even more partial, and grinding takes precedence, and the temperature rises, causing surface oxidation to progress significantly, so it cannot be said to be at a level that can be used industrially. For these reasons, a method has been used in which only a portion of the powder is peeled off by irradiating it with ultrasound, and then it is collected by classification using centrifugation.
[0033] The peripheral speed in the peeling step can be 6 m / sec to 12 m / sec. A peripheral speed of 8 m / sec to 10 m / sec is more preferable. A peripheral speed of 6 m / sec or more provides good peeling efficiency, while a peripheral speed of 12 m / sec or less suppresses the application of excessive energy and suppresses the temperature rise of the resulting particulate material, thereby suppressing the progress of oxidation on the surface of the resulting particulate material and reducing electrical resistance. A slurry feed speed of 100 mL / min to 300 mL / min can be used. A slurry particle concentration of 10.0 mg / mL to 20.0 mg / mL can be used.
[0034] At concentrations below 10.0 mg / mL, the efficiency of preparing MXene nanosheets decreased. If the concentration is 0.0 mg / mL or higher, peeling will not proceed sufficiently, so this range is preferable.
[0035] The slurry temperature is preferably in the range of 35° C. or less. If the temperature is 35° C. or less, surface oxidation can be suppressed and the electrical resistance of the particulate material can be kept low.
[0036] A bead filling amount of 40% to 80% can be used. If it is 40% or more, the peeling efficiency improves, and if it is 80% or less, it becomes easy to classify the beads and slurry. Whether or not a particulate material containing a large amount of the desired sheet-like particles has been produced can be determined by observation with SEM, TEM, etc. In particular, the thickness of the particulate material can be determined by AFM analysis. The particulate material obtained in the peeling process can be classified by a method such as centrifugation if necessary and used. The optimal conditions for the peeling process vary depending on the size of the device, so these numerical values are not limited.
[0037] It is preferable that the bead mill treatment results in 98% or more of the MXene being exfoliated by mass, more preferably 99% or more, and even more preferably 100% being exfoliated. If the exfoliation step is completed under conditions in which all of the MXene is exfoliated, it becomes possible to use the resulting mixture in the mixing step without removing the unexfoliated MXene. To remove MXene other than the exfoliated MXene, it can be separated by centrifugation, filtration, or the like.
[0038] The zeta potential of the resulting exfoliated MXene is preferably -25.0 mV to -30.0 mV in water having a pH of 6 to 8.
[0039] The chemical composition of the MXene nanosheets was determined by atomic percentages of Ti, Al, C, and N, with Ti being set at 3. The amounts of Al, C, and N were calculated when the sample was weighed out and placed on a platinum dish, and nitric acid + sulfuric acid + hydrofluoric acid were added. After heating (to about 120°C) to dissolve the sample, the sample was heated at a higher temperature (300°C) to evaporate the nitric acid and hydrofluoric acid to prepare a sample solution (sulfuric acid). The sample solution was then appropriately diluted and quantitatively analyzed using ICP. Acid treatment process In the acid treatment step, the raw carbon particles are treated with a mixed acid solution of sulfuric acid and nitric acid to obtain highly hydrophilic carbon particles. Examples of the raw carbon particles include acetylene black, Ketjen black, carbon nanotubes, graphene, carbon fiber, graphite powder, hard carbon powder, etc. From the viewpoint of electrical conductivity, acetylene black, Ketjen black, and carbon nanotubes are preferred, and from the viewpoints of electrical conductivity, purity, and price, acetylene black is more preferred.
[0040] In the acid treatment step, the carbon particles are suspended in the mixed acid, and the suspension can be used as is in the mixing step, or the mixed acid can be removed as necessary by repeatedly washing with water, etc., and the carbon particles can be used as the suspension. Washing can be performed until the pH of the washing solution becomes about 6, and can also be performed until the pH becomes about 6.5, 7, or 8.
[0041] This treatment introduces functional groups such as COOH and CO groups onto the surface of the carbon particles, making them hydrophilic. After the treatment, the carbon particles become a carbon particle suspension dispersed in the mixed acid. It does not matter whether this treatment is performed before or after the acid treatment process and the peeling process.
[0042] The treatment temperature is preferably 70°C or higher. In particular, it is preferably 95°C or lower to prevent boiling. The treatment time is not particularly limited, but treatment for 10 minutes or more ensures hydrophilization. During treatment, stirring or ultrasonic irradiation can be performed. After treatment, the mixture may be directly subjected to a mixing step, or the acid may be neutralized or separated. If the pH value is increased to a predetermined value or higher by neutralizing or separating the acid, the carbon particles will aggregate, so neutralization can be performed to a degree that does not cause the pH to reach the predetermined value. An example of a method for separating the acid is a method for separating the solid content by a classification operation such as centrifugation.
[0043] The mixing ratio of sulfuric acid to nitric acid, by volume, can be about 4:1 to 1:1, and is particularly preferably about 3:1 to 3:2. The concentration of the mixed acid can be about 42% to 96%, and is particularly preferably about 90.0% to 95.0%.
[0044] The zeta potential of the obtained hydrophilic carbon particles is preferably -20.0 mV to -25.0 mV in water at pH 7. The zeta potential is increased because COOH and CO are adsorbed as functional groups. If the absolute value is smaller than -20.0 mV, the dispersibility in water deteriorates. The degree of mutual dispersion of the composite particle material increases. The absolute value becomes larger than -25.0mV. If the temperature drops, the electrical conductivity will decrease. ·Mixing process The mixing step is a step of obtaining a mixture in which the exfoliated material and the carbon microparticles are dispersed in a second dispersion medium containing 50 mass% or more of water at a mass ratio of 90:10 to 97:3 and a concentration of the exfoliated material of 11.5 to 17.0 mg / mL. It is more preferable that the second dispersion medium is 100 mass% water. By including other substances in the mixture, the substances can also be incorporated into the composite particle material. In particular, by including Li ions or Na ions in the mixture, the ions can be inserted into the MXene layer that constitutes the exfoliated material.
[0045] The mixture contains the exfoliated material at a concentration of 11.5-17.0 mg / mL. The second dispersion medium may be the same as the dispersion medium used in the peeling step or a solvent that can be used in other steps, or it may be different. When the exfoliated material suspension obtained in the peeling step is directly subjected to the mixing step, the second dispersion medium contains the dispersion medium used in the peeling step. The reason for limiting the MXene particle concentration in the composite slurry to 11.5-17.0 mg / mL is that the MXene particle concentration in the composite slurry is 11.5-17.0 mg / mL. This is because if it is below .5 or exceeds 17.0, the specific surface area of the composite particle material obtained in the agglomeration process described below will be small.
[0046] It is preferable to add an aqueous solution of lithium chloride to the mixture and stir it with a shaker at a rotation speed of 100 rpm to 300 rpm for 1 to 6 hours to intercalate chlorine and lithium ions. The amplitude of the shaker is preferably 40 mm or more. Lithium chloride can be completely dissolved by stirring it with a shaker at a rotation speed of 100 rpm to 300 rpm for 1 hour or more at a ratio of 5.3 g to 30 g of pure water, and it is preferable to add it to a suspension of MXene and carbon microparticles at a predetermined particle concentration. The vibration of the shaker at that time is The width is preferably 40 mm to 45 mm. For the acid-treated carbon particles, it is preferable to add a predetermined amount of carbon particles to pure water, stir with a shaker at a rotation speed of 100 rpm to 300 rpm for 1 hour or more, and add the suspension with loosened aggregates to the mixture and mix. In this case, the amplitude of the shaker is preferably 40 mm to 45 mm. ·Agglomeration process The flocculation step is a step of flocculating the composite particle material of the exfoliated material and the carbon microparticles contained in the mixture into an aggregate by increasing the pH of the mixture obtained in the mixing step. The pH is increased by adding an alkaline substance or by removing or diluting an acidic substance. The pH is preferably increased by adding an alkaline aqueous solution for a few seconds and stirring the mixture with a shaker at a rotation speed of 100 rpm to 300 rpm for one hour or less. The amplitude of the shaker is preferably 40 mm to 45 mm.
[0047] Alternatively, this can be achieved by adding a highly hydrophobic organic solvent having a small relative dielectric constant.
[0048] The obtained aggregates are dried and then pulverized or otherwise put into a required state, thereby obtaining the composite particulate material of this embodiment having a proper particle size distribution. The proper state is the state of the composite particulate material of this embodiment described above. There are no particular limitations on the method for drying the aggregates. For example, the aggregates can be separated by a classification operation such as centrifugation or filtration, and then dried. After separation of the aggregates, they can be washed one or more times as necessary. Washing can be performed with water or the like. Drying is a process for removing water adsorbed on the surface of the composite particle material and water present between the layers in the crystals. It is preferable to wash the aggregates three times with ethanol or isopropyl alcohol, and then air-dry them. Alternatively, it is preferable to spray-dry an ethanol or isopropyl alcohol suspension in nitrogen. To remove water present between the layers in the crystals, it is preferable to dry them in a vacuum at a temperature between 100°C and 200°C for 6 to 24 hours. By selecting the process conditions appropriately, it is possible to obtain a high-quality composite particle material with high water content. This inhibits surface oxidation of the body, and allows the surface electrical resistance of the obtained composite particle material to be maintained low. Other necessary processes Other necessary steps are not particularly limited, but include a pretreatment step. The pretreatment step is an example of a method for producing MXene. For example, a mixed raw material of TiC, TiN, Al, and Ti is subjected to CIP or uniaxial pressing at 1 ton / cm 2 to 3 tonnes / cm 2 The crushed pieces of the green compact, which have been subjected to pressure treatment in the range of 1400°C to 1600°C, or without pressure treatment, are heat-treated in an inert atmosphere at temperatures between 1400°C and 1600°C to produce Ti3Al(C), a high-purity Ti3-layer MAX phase ceramic. 1-x N x )2, (0≦x<1) can be exemplified. In addition, it can be produced by contacting MAX phase ceramic powder with an acidic substance at a controlled temperature of 20°C to 30°C to remove a portion of the Al element contained in the MAX phase ceramic powder.
[0049] The raw material used in the pretreatment process is Ti3Al for the Ti3 layer. a [C (1-x) N x ]2, (a=1, 0≦x<1) is a MAX phase ceramic powder. The amount of l to be removed is adjusted so that the amount of Al (corresponding to x) remaining in the MAX phase ceramic powder produced by acid treatment with an acidic substance exceeds 0.02. It is also possible to remove all of the Al, and in that case, it is preferable not to proceed with the acid treatment beyond the extent of removing the Al.
[0050] The amount of Al removed can be adjusted by changing the contact time with the acidic substance (such as an acid aqueous solution) (the longer the contact time, the greater the amount removed), the concentration of the acidic substance (the higher the concentration, the greater the amount removed), the amount of acidic substance (the greater the absolute amount of acidic substance, the greater the amount that can be removed), and the contact temperature (the higher the temperature, the greater the amount removed).
[0051] A layered compound MAX phase ceramic powder (A element is Al) is subjected to an acid treatment to remove part of the Al, resulting in a layered compound having a void layer that constitutes a particle material. An acidic substance that is a combination of hydrofluoric acid and hydrochloric acid is used as the acid for removing part of the Al layer. In order to realize the combination of hydrofluoric acid and hydrochloric acid, it is preferable to mix a salt of hydrofluoric acid (KF, LiF, etc.) with hydrochloric acid to obtain a mixture of hydrofluoric acid and hydrochloric acid.
[0052] In particular, aqueous solutions of these acids are used as the acidic substances. There is no particular limitation on the mixed concentration of hydrofluoric acid and hydrochloric acid formed when the fluoride salt is assumed to be completely dissociated. The lower limit of the hydrofluoric acid concentration can be about 1.7 mol / L, 2.0 mol / L, or 2.3 mol / L, and the upper limit can be about 2.5 mol / L, 2.6 mol / L, or 2.7 mol / L. The lower limit of the hydrochloric acid concentration can be about 2.0 mol / L, 3.0 mol / L, or 4.0 mol / L, and the upper limit can be about 13.0 mol / L, 14.0 mol / L, or 15.0 mol / L.
[0053] There is no particular limitation on the mixing ratio (molar ratio) of hydrofluoric acid and hydrochloric acid formed when the fluoride salt is assumed to be completely dissociated, but the lower limit of hydrofluoric acid may be 1:13, 1:12, or 1:11, and the upper limit may be about 1:5, 1:6, or 1:7. The concentrations and mixing ratios of hydrofluoric acid and hydrochloric acid shown here may be arbitrarily combined. The acid treatment temperature is preferably 20° C. to 30° C., and more preferably 20° C. to 25° C. (Electrode Material) The electrode material of the present embodiment is a material that can be suitably used in secondary batteries. In particular, since Li ions and Na ions can be inserted and removed between layers, it can be suitably used as an electrode active material. In addition, due to its electrical conductivity, it can also be used as a conductive auxiliary. It is effective for lithium secondary batteries and sodium secondary batteries. Lithium ions and sodium ions are stored and released in the void layer obtained by removing the Al layer by acid treatment.
[0054] Here, a lithium secondary battery will be taken as an example for explanation. The electrode has an active material layer containing an active material made of the composite particle material of this embodiment, and a current collector made of a metal thin plate or the like on whose surface an active material layer made of an active material is formed. A binder can be included to form the active material layer. In addition, the active material layer can contain active materials other than the composite particle material of this embodiment, conductive assistants, and the like as necessary. As the binder, carboxymethyl cellulose, polyvinylidene fluoride, styrene-butadiene rubber, polyvinylpyrrolidone, polyvinyl alcohol, and other binders that can be used can be used. As the conductive assistant, acetylene black, ketjen black, carbon nanotubes, graphene, carbon fiber, graphite powder, hard carbon powder, and the like can be used. EXAMPLES
[0055] The composite particulate material and the method for producing the same of the present invention will be described in detail below with reference to examples. Example 1 Pre-treatment process 12.3 g of TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.), 4.9 g of Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.), and 2.8 g of Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) were mixed in isopropanol (IPA) using a ball mill for 12 hours, and the IPA was removed using an evaporator to obtain a uniformly mixed dry powder.
[0056] The uniformly mixed dry powder was placed in an alumina crucible and fired in a graphite resistance furnace at 1450℃ for 2h in an Ar gas stream to obtain Ti3AlC2 as MAX phase ceramics. The obtained Ti3AlC2 was coarsely ground using a mortar and pestle, and then ball milled in IPA using 5mm zirconia balls for 24 hours. Then, it was ground in a planetary ball mill (200 rpm, 15 min, 3 times) using 0.5mm zirconia balls to obtain a suspension. The IPA was removed from the suspension using an evaporator to obtain Ti3AlC2 powder ground to approximately 3μm.
[0057] Prepare an acid solution of 300 mL of concentrated HCl with 18 g of LiF, add 10 g of Ti3AlC2 powder while cooling with ice, and stir with a magnetic stirrer for 24 hours in a controlled environment of 10 to 20°C to etch and remove Al, resulting in Ti3Al 0.02 After etching, the particles were washed with water until the pH reached about 6. Finally, the water was replaced with ethanol. By this operation, a raw suspension in which the particulate material was suspended in ethanol was obtained.
[0058] The particle concentration in the raw suspension was measured, and Ti3Al 0.02 Water was added so that the particle concentration of C2MXene became 16.9 mg / mL. Peeling process This raw material suspension was fed into a bead mill with ZrO2 beads of 50 μm diameter at a slurry feed rate of By treating at 150mL / min and 80% ZrO2 bead loading, Ti3Al 0. 02 This process was repeated three times to produce a flaked material made of C2MXene. 0.02 The particulate material consisting of C2MXene was almost entirely turned into exfoliated material, and an exfoliated material suspension containing the exfoliated material was obtained.
[0059] The obtained suspension of exfoliated material was dropped onto a Si substrate that had been piranha-treated (immersed in a mixed solution of H2SO4:H2O2 = 3 parts by volume:1 part by volume), and an AFM analysis was performed. The AFM image is shown in Figure 1. One hundred exfoliated materials (nanosheets) were randomly selected, and the average thickness measured by AFM was calculated and shown in Table 1. Furthermore, the results of SEM observation are shown in Figure 2. One hundred exfoliated materials were randomly selected, and the vertical (maximum diameter in the direction perpendicular to the thickness direction) and horizontal (directions perpendicular to the vertical and thickness directions) dimensions were measured from the SEM photograph, and the average value was defined as the size of the exfoliated material. The average size of the 100 exfoliated materials is shown in Table 1.
[0060] Powder of MAX phase ceramics Ti3AlC2 and exfoliated material (Ti3Al0.02 C2MXen The XRD profiles of the nanosheets (e) and (f) are shown in Figure 3. Table 5 shows the interlayer distances focusing on the d value of the (002) plane.
[0061] The zeta potential of the peeled off material was measured in water at pH 7.0, and the composite particulate material described below was The results are shown in Table 6 together with the specific surface area of the materials. Acid treatment process The acid treatment of acetylene black as carbon microparticles was carried out by adding 1.0 part by mass of acetylene black to 100 parts by mass of mixed acid, which was a 3:1 volumetric mixture of sulfuric acid (98% by mass) and nitric acid (68% by mass), and immersing the mixture in an environment of 85°C for 10 minutes. The mixture was then washed with water until the pH was about 6.0, and the water was then replaced with IPA. The mixture was air-dried to obtain hydrophilic acetylene black powder. FTIR analysis detected COOH and CO groups as surface functional groups. The zeta potential at pH 7.0 in water was measured to be -22.5 mV. Acetylene black was dissolved in Ti3Al 0.02 A 5% by mass amount of the C2MXene nanosheets was added to 10 mL of pure water, and the agglomerates were broken down using a shaker at 140 rpm with an amplitude of 45 mm for 24 h to prepare a hydrophilic acetylene black slurry.
[0062] Hydrophilic acetylene black slurry was dropped onto a hydrophilic treated Si wafer and observed with an SEM. One hundred primary particles were randomly observed and their longitudinal and transverse dimensions were measured, and the average primary particle diameter was found to be 33 nm. ·Mixing process 5.3 g of lithium chloride powder and acetylene black powder treated with acid in the acid treatment process were added to 220 mL of the suspension of the peeled material obtained in the peeling process. 0.02After adding 5% by mass of C2MXene, the mixture was uniformly stirred for 5 hours at 140 rpm and amplitude 45 mm on a shaker. As mentioned above, acetylene black was added in a dispersed state in 10 mL of water. After uniform stirring, an alkaline aqueous solution was added in which 5.3 g of lithium hydroxide was dissolved in 30 mL of pure water and shaken for 24 hours at 140 rpm and amplitude 45 mm to completely dissolve the solution, and the mixture was stirred for 1 hour at 140 rpm and amplitude 45 mm on a shaker. After that, the mixture was washed with water once and replaced with IPA three times, air-dried, and then the Ti3Al 0.02 A composite particle material consisting of C2MXene exfoliation material and acetylene black powder was obtained. This method, in which the exfoliation material and carbon particles are mixed together with a substance that generates chloride ions (lithium chloride in this example), is called Method A. The concentration of the exfoliation material in the mixture in the aggregation process corresponds to 13.2 mg / mL.
[0063] The results of XRD measurement of the obtained composite particle material are shown in Figure 3, and the results of SEM observation are shown in Figure 4. The results are shown in Figure 6. After vacuum drying at 100°C for 24 hours, the specific surface area, average pore diameter, and average pore volume were measured by the BET method using nitrogen, and the results are shown in Table 2 and Figure 11. Furthermore, the interlayer distance and half-width of the (002) plane of MXene calculated from XRD measurement of the obtained composite particle material are shown in Table 5, along with the interlayer distance and half-width of exfoliated MXene.
[0064] Furthermore, the obtained composite particle material was subjected to Raman spectroscopy analysis using a laser with a wavelength of 532 nm. The laser irradiation conditions were set to an intensity at which the exfoliated material (MXene) contained in the composite particle material was not oxidized to precipitate anatase, and the laser irradiation frequency was set at 100 cm -1 From 2000cm -1 The measurements were performed in the range of .
[0065] Ti3Al 0.02 The vibrations due to functional groups adsorbed on titanium atoms of the peeled off C2MXene are in the range of 230-470 cm -1 (Below, the peaks that appear in this range are those within 400 cm -1The peak appearing at 580 cm is taken as a representative and is called the "A peak"), and the vibration due to the functional group adsorbed on the carbon atom is at 580 cm. -1 On the other hand, for acetylene black, SP 3 mixed Carbon orbital is 1332cm -1 (hereinafter referred to as "B peak"), SP 2 Hybrid orbitals of carbon 1500~1600cm -1 appears in.
[0066] The peak intensities of these A peak and B peak were calculated. The peak intensity was calculated from the peak height, and the B / A value was calculated. Analysis was performed on 100 randomly selected composite particle materials to calculate the B / A value, and the standard deviation of these values was taken as the mutual dispersion of the composite particle material. The results are shown in Table 3. The smaller the mutual dispersion, the more uniformly the particles are dispersed.
[0067] The composite particle material obtained was treated in a vacuum at 100°C for 5 hours, and then compressed in a φ10 mm mold at 0.5 kg / cm 2 Then, the material is pressed uniaxially at a pressure of 1.0 ton / cm 2 CIP processed at pressure The surface electrical resistance of the powder was measured by a four-terminal method using copper wires with a diameter of 0.1 mm. The results are shown in Table 4. Lithium-ion battery A CR-2025 type coin cell was prepared and its battery characteristics were examined. The composite particle material of Example 1 was used as the electrode active material, acetylene black as a conductive assistant, and polyvinylidene fluoride (PVDF) as a binder were mixed in N-methylpyrrolidone (NMP) in a mass ratio of 80:10:10 using a mortar and pestle to obtain an electrode composite paste. This paste was applied to one side of Cu foil as a current collector and dried in a vacuum at 120°C for 24 hours. The electrolyte was a 1M solution of LiPF6 as an electrolyte in ethylene carbonate ( The battery was charged at 1 C for 300 cycles, and the battery characteristics were shown in Figures 4 and 5. ... was charged at 1 C for 300 cycles. The battery was charged at 1 C for 300 cycles. The battery was charged at 1 C for 300 cycles. The battery was charged at 1 C for 300 cycles. The battery was charged at 1 C for 300 cycles. The battery was charged at 1 C for 3 Example 2 The same Ti3Al as in Example 1 was used except that the amount of acid-treated acetylene black added was 10 mass% relative to the peeled material (MXene). 0.02 A composite particulate material of C2MXene and acetylene black was prepared as the composite particulate material of this example. As in Example 1, SEM observation was performed and the results are shown in FIG. 7. As in Example 1, the BET specific surface area, average pore diameter, and average pore volume were measured and the results are shown in Table 2. As in Example 1, the mutual dispersion was calculated and the results are shown in Table 3. The surface electrical resistance of the obtained composite particulate material was measured and the results are shown in Table 4. Example 3 The same Ti3Al as in Example 1 was used except that the amount of acid-treated acetylene black added was 3 mass% relative to the peeled material (MXene). 0.02 A composite particulate material of C2MXene and acetylene black was prepared as the composite particulate material of this example. The BET specific surface area, average pore diameter, and average pore volume were measured in the same manner as in Example 1, and are shown in Table 2. The mutual dispersion was calculated in the same manner as in Example 1, and is shown in Table 3. The surface electrical resistance of the obtained composite particulate material was measured in the same manner as in Example 1, and is shown in Table 4. (Example 4) As in Example 1, a suspension of exfoliated material and acid-treated acetylene black were prepared. 5% by mass of acetylene black was added to 220 mL of the suspension of exfoliated material, based on the mass of the exfoliated material, and the mixture was uniformly stirred for 5 hours on a shaker at 140 rpm and an amplitude of 45 mm. After that, an aqueous solution of lithium hydroxide dissolved in 30 mL of pure water was added, and the mixture was uniformly stirred for 1 hour on a shaker at 140 rpm and an amplitude of 45 mm. Thereafter, the composite particle material of this embodiment was prepared in the same manner as in Example 1. As in Method A, a substance that generates chloride ions together with the exfoliated material and carbon microparticles was added. The method of flocculating the materials with an alkaline aqueous solution without mixing them together is called Method B.
[0068] The results of SEM observation of the obtained composite particulate material are shown in Figure 8. As in Example 1, the results of measurement of the BET specific surface area, average pore diameter distribution, and average pore volume are shown in Table 2 and Figure 11. As in Example 1, the results of calculation of the mutual dispersion are shown in Table 3. Furthermore, the interlayer distance and half-width of the (002) plane of MXene calculated from the XRD measurement of the obtained particulate material are shown in Table 5. Example 5 In Example 1, the concentration of the exfoliated material in the mixture in the aggregation step was 15.5 mg / mL, whereas in Example 1, the concentration of Ti3Al was 13.2 mg / mL. 0.02 A composite particulate material of C2MXene and acetylene black was prepared and used as the composite particulate material of this example. The results of measuring the BET specific surface area in the same manner as in Example 1 are shown in Figure 11. The results of calculating the mutual dispersion degree in the same manner as in Example 1 are shown in Table 3. Example 6 The same procedure as in Example 1 was repeated except that the following were used: TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.) 11.9 g, TiN powder (TN-30-10-0020, Rare Metallic Co., Ltd.) 0.38 g, Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.) 4.9 g, and Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) 2.8 g. 0.97 N 0.03 )2 was obtained. Acid treatment and peeling were performed in the same manner as in Example 1. The zeta potential in water at pH 7 was measured in the same manner as in Example 1, and is shown in Table 6. Acetylene black was treated with acid in the same manner as in Example 1 to prepare a composite particle material, and the BET specific surface area was measured in the same manner as in Example 1. The results are shown in Table 6. The surface electrical resistivity is shown in Table 4. Comparative Example 1 A suspension of exfoliated material was prepared in the same manner as in Example 1. An aqueous solution of lithium hydroxide dissolved in 40 mL of pure water was added to 220 mL of the suspension of exfoliated material, and the mixture was stirred at 140 rpm for 1 hour using a shaker to prepare a mixed suspension. As in Example 1, the concentration of exfoliated material in the mixture was set to 13.2 mg / mL. The mixture was washed with water once and replaced with IPA three times, and then air-dried. The acetylene black aggregate powder was The powder was added at 10% by mass based on the mass of the peeled material, and stirred in NMP with a mortar and pestle. The exfoliated material and acetylene black were then vacuum dried at 00°C for 24 hours to prepare a composite particulate material of this comparative example. An SEM photograph of the composite particulate material is shown in Figure 9. The BET specific surface area, average pore diameter distribution, and average pore volume were measured in the same manner as in Example 1, and the results are shown in Table 2. The mutual dispersion is shown in Table 3. The surface electrical resistance is shown in Table 4. The battery characteristics were measured in the same manner as in Example 1, and the results are shown in Figure 4. Comparative Example 2 The composite particulate material of this comparative example was prepared in the same manner as in Example 1, except that the acetylene black powder was not subjected to the acid treatment step shown in Example 1. A SEM photograph of the composite particulate material is shown in Figure 10. As in Example 1, the BET specific surface area, average pore diameter, and average pore volume were measured. The results of the measurement of the mutual dispersion are shown in Table 2. The results of the measurement of the mutual dispersion are shown in Table 3. Comparative Example 3 The composite particulate material of this comparative example was prepared in the same manner as in Example 1, except that the bead mill treatment was performed in ethanol as the exfoliation step. As in Example 1, the average thickness and average size of the exfoliated products were measured and the results are shown in Table 1. The specific surface area, average pore diameter, and average pore volume were measured and the results are shown in Table 2. The mutual dispersion is shown in Table 3. Comparative Example 4 A composite particulate material of MXene and acetylene black was prepared in the same manner as in Example 1, except that the concentration of the exfoliated material in the mixture in the aggregation step was set to 11.0 mg / mL, whereas in Example 1, the concentration was 13.2 mg / mL. This composite particulate material was used as the composite particulate material of this comparative example. The results of measuring the BET specific surface area in the same manner as in Example 1 are shown in FIG. Comparative Example 5 A composite particulate material of MXene and acetylene black was prepared in the same manner as in Example 1, except that the concentration of the exfoliated material in the mixture in the aggregation step was set to 5.0 mg / mL, whereas in Example 1, the concentration was 13.2 mg / mL. This composite particulate material was used as the composite particulate material of this comparative example. The results of measuring the BET specific surface area in the same manner as in Example 1 are shown in FIG. Comparative Example 6 A composite particulate material of MXene and acetylene black was prepared in the same manner as in Example 1, except that the concentration of the exfoliated material in the mixture in the aggregation step was set to 17.6 mg / mL, instead of 13.2 mg / mL in Example 1, to provide the composite particulate material of this comparative example. The results of measuring the BET specific surface area in the same manner as in Example 1 are shown in FIG. Comparative Example 7 A composite particulate material of MXene and acetylene black was prepared in the same manner as in Example 1, except that the concentration of the exfoliated material in the mixture in the aggregation step was set to 26.5 mg / mL, instead of 13.2 mg / mL in Example 1, to provide the composite particulate material of this comparative example. The results of measuring the BET specific surface area in the same manner as in Example 1 are shown in FIG. Comparative Example 8 The same procedure as in Example 1 was repeated except that the following were used: TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.) 11.7 g, TiN powder (TN-30-10-0020, Rare Metallic Co., Ltd.) 0.64 g, Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.) 4.9 g, and Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) 2.8 g. 0.95 N 0.05 ) 2 was obtained. Acid treatment and peeling were performed in the same manner as in Example 1. Acetylene black was acid-treated in the same manner as in Example 1 to produce a composite particle material, and the BET specific surface area was measured in the same manner as in Example 1. The zeta potential of MXene in water at pH 7 is also shown in Table 6. Comparative Example 9 The same procedure as in Example 1 was repeated except that the following were used: TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.) 11.1 g, TiN powder (TN-30-10-0020, Rare Metallic Co., Ltd.) 1.3 g, Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.) 4.9 g, and Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) 2.8 g. 0.90 N 0.10 ) 2 was obtained. Acid treatment and peeling were performed in the same manner as in Example 1. Acetylene black was acid-treated in the same manner as in Example 1 to prepare a composite particle material, and the BET specific surface area was measured in the same manner as in Example 1. The zeta potential of MXene in water at pH 7 was also measured, and is shown in Table 6. (Comparative Example 10) The same procedure as in Example 1 was repeated except that the following were used: TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.) 10.4 g, TiN powder (TN-30-10-0020, Rare Metallic Co., Ltd.) 1.9 g, Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.) 4.9 g, and Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) 2.8 g. 0.85 N 0.15 ) 2 was obtained. Acid treatment and peeling were performed in the same manner as in Example 1. Acetylene black was acid-treated in the same manner as in Example 1 to prepare a composite particle material, and the BET specific surface area was measured in the same manner as in Example 1. The zeta potential of MXene in water at pH 7 was also measured, and is shown in Table 6. (Comparative Example 11) The same procedure as in Example 1 was used to prepare Ti3Al(C) as MAX phase ceramics, except that the following were used: TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.) 9.2 g, TiN powder (TN-30-10-0020, Rare Metallic Co., Ltd.) 3.2 g, Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.) 4.9 g, and Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) 2.8 g. 0.75 N 0.25 ) 2 was obtained. Acid treatment and peeling were performed in the same manner as in Example 1. Acetylene black was acid-treated in the same manner as in Example 1 to produce a composite particle material, and the BET specific surface area was measured in the same manner as in Example 1. The zeta potential of MXene was also measured, and is shown in Table 6.
[0069] [Table 1]
[0070] [Table 2]
[0071] [Table 3]
[0072] [Table 4]
[0073] [Table 5]
[0074] [Table 6] (result) As is clear from Table 1, by using only water-free ethanol as a dispersion medium in the peeling process, the thickness of the peeled off material increases and the size of the peeled off material decreases. It was found that the thickness of the peeled off material decreases and the size of the peeled off material increases as the amount of water increases.
[0075] As is clear from Tables 2 and 3 and Figures 6 to 10, by using a composite particle material of carbon particles (acetylene black) that have been hydrophilized by acid treatment with a mixture of sulfuric acid and nitric acid and MXene exfoliated particles with a small thickness and appropriate size, a large specific surface area and a high degree of mutual dispersion can be obtained. It was found that the composite particle material was small (excellent in dispersion). Furthermore, it was found that the mutual dispersion and specific surface area changed by changing the amount of carbon particles added.
[0076] In the process of uniformly mixing MXene and carbon particles, chloride ions are intercalated. It was found that Method A, in which intercalation is performed, has smaller average pore diameter and pore volume, and a larger specific surface area, compared to Method B, in which intercalation is not performed. Furthermore, it was found in the XRD profile that Method A has a larger interlayer distance on the (002) plane of MXene than Method B (shown in Table 5). A reference diagram for measuring the interlayer distance is shown in Figure 12. The crystal structure of MXene has the crystal structure obtained by removing the A phase from the MAX phase shown in Figure 12.
[0077] If the interlayer distance of the gap is defined as the distance obtained by subtracting the interlayer distance of 0.945 nm of the (002) plane of the MAX phase from the interlayer distance of the (002) plane of MXene, this suggests that the interlayer distance of the gap has become larger, meaning that larger ions can be inserted and removed.
[0078] When the amount of carbon microparticles was 3% by mass or more, the specific surface area increased, and when it was less than 10% by mass, the mutual dispersion degree improved. Therefore, based on the mass of MXene and carbon microparticles, it was found that the ratio of carbon microparticles is preferably 3 to 10% by mass. In this case, the mutual dispersion degree was 1.50 when the carbon microparticles were 3% by mass and 7.00 when the carbon microparticles were 10% by mass, and it was found that the mutual dispersion degree is preferably 1.50 or more and 7.00 or less.
[0079] Specific surface area is 75m 2 / g or more, sufficient battery characteristics were observed. The highest specific surface area in the example was 110m 2 / g composite particle material. .
[0080] Specific surface area is 75m 2 / g or more and shows excellent mutual dispersion. 0.02 C2MXene and Two methods (Method A and Method B) for producing conductive carbon black composite particle materials are compared. Method A produces Ti3Al 0.02 When composite particles of C2MXene and carbon black were prepared, the average pore diameter was 7.0-15.0 nm and the average pore volume was 0.10-0.30 mL / g. 0.02 When composite particle material was produced from C2MXene and conductive carbon black, the average pore diameter was 15.0 to 20.0 nm and the average pore volume was 0.30 to 0.50 mL / g, indicating that method A had smaller average pore diameter and average pore volume than method B.
[0081] Ti3Al 0.02C2MXene, Ti3Al 0.02 (C 0.97 N 0.03 ) Zeta of 2MXene in water at pH 7.0 The electric potentials are negative and their absolute values are 28.9 and 29.3, respectively. 0.02 (C 0.95 N 0.05 )2MXene, Ti3Al 0.02 (C 0.90 N 0.10 )2MXene, Ti3Al 0.02 (C 0.85 N 0.15 )2MXene, Ti3Al 0.02 (C 0.75 N 0.25 The absolute values of the zeta potentials of 2MXene in water at pH 7.0 are 31.5, 32.1, 32.4, and 33.1, respectively. The latter means that it is difficult to aggregate. The zeta potential of acid-treated acetylene black in water at pH 7.0 is negative. It was found that the COOH and CO groups dissociate and become hydrophilic. Therefore, it is possible to mix the aqueous suspension of MXene and the aqueous suspension of acid-treated acetylene black uniformly by stirring, and it was found that adding an alkaline aqueous solution allows the formation of aggregates while maintaining the uniform dispersion state.
[0082] The surface electrical resistance of the uniformly mixed composite particle material and the conventional composite particle material was measured using pellets that were uniaxially pressed and then CIP-treated. It was found that the surface electrical resistance was small (Table 4). When used as the negative electrode active material in a secondary battery, it is possible to effectively transfer electrons to the current collector.
[0083] By exfoliating MXene nanosheets to the monolayer level and reducing their size appropriately, Furthermore, by making it into a composite particle material with hydrophilically treated acetylene black, the specific surface area was increased and the acetylene black was uniformly dispersed, resulting in the production of a composite particle material with excellent ion diffusivity and the ability to smoothly transfer electrons to the current collector, making it ideal for use as a negative electrode active material in secondary batteries (storage batteries).
Claims
1. 90 to 97 parts by weight of sheet-like Ti 3 A a (C( 1 . 0-x ) N x ) 2 (0≦x≦0.03, a is greater than 0.02) MXene and 3 to 10 parts by mass of fine particles, Specific surface area is 75m 2 / g or more.
2. The composite particulate material according to claim 1 , wherein the microparticles are carbon microparticles.
3. In Raman spectroscopy using a 532 nm laser, -1 Peak height A and 1332 cm -1 2. The composite particle material according to claim 1, wherein the interdispersity, which is the standard deviation of the ratio (B / A) of peak heights B of the composite particle material, is 1.50 to 7.
00.
4. The composite particulate material according to any one of claims 1 to 3, having an average pore diameter of 7.0 to 20.0 nm and a pore volume of 0.10 to 0.50 mL / g.
5. The Ti 3 A a (C( 1 . 0-x ) N x ) 2 (0≦x≦0.03, a is greater than 0.02) MXene has an average thickness of 1.0 to 3.5 nm and an average size in the spreading direction of the sheet of 0.5 to 1.0 μm; 5. The composite particulate material according to claim 1, wherein the microparticles have a primary particle diameter of 30 to 50 nm.
6. The Ti 3 A a (C( 1 . 0-x ) N x ) 2 (0≦x≦0.03, a is greater than 0.02) A composite particle material described in any one of claims 1 to 5, wherein in the crystal structure of MXene, the interlayer distance of the (002) plane is 1.400 nm to 1.700 nm and the half-width is 0.9 degrees to 1.50 degrees.
7. Any one of claims 1 to 6, wherein the surface electrical resistance is from 1.0 Ω / □ to 100.0 Ω / □.
2. The composite particulate material according to claim 1. (Surface Electrical Resistance) The composite particle material was treated in a vacuum at 100°C for 5 hours, and then pressed in a φ10mm mold at 0.5kg / cm 2 Then, the mold is pressed uniaxially at a pressure of 1.0 ton / cm 2 CIP-processed powder The surface electrical resistance is measured by a four-terminal method using copper wires with a diameter of 0.1 mm using a body.
8. The particles are Ti with a zeta potential of -25.0 mV to -30.0 mV. 3 A a (C( 1 . 0-x ) N x ) 2 (0≦x≦0.03, a is greater than 0.02) MXene and a composite particulate material according to any one of claims 1 to 7, having a zeta potential of -20.0 mV to -25.0 mV. The zeta potential is measured in water at pH 7.
0.
9. 9. A negative electrode comprising the composite particulate material according to claim 1 as a negative electrode active material.
10. Ti 3 A a (C( 1 . 0-x ) N x ) 2 (0≦x≦0.03, a is greater than 0.02) A peeling step of peeling MXene to form a peeled product; an acid treatment step of treating the raw carbon particles in a mixed acid solution of sulfuric acid and nitric acid at 70° C. or higher for 10 minutes or more to obtain carbon particles; a mixing step of obtaining a mixture in which the exfoliated material and the carbon microparticles are dispersed in a second dispersion medium at a mass ratio of 90:10 to 97:3 and at a concentration of 11.5 to 17.0 mg / mL; Adding an aqueous lithium chloride solution to intercalate the mixture on a shaker at 100 to 300 rpm; The mixture is made alkaline to flocculate the Ti 3 A a (C( 1 . 0-x ) N x ) 2 (0≦x≦0.03, a is more than 0.02) A composite of MXene and the carbon particles an agglomeration step to obtain a particulate material; A method for producing a composite particulate material comprising:
11. The method for producing a composite particulate material according to claim 10 , wherein the exfoliation step is carried out until 99% or more of the MXene is exfoliated by mass.
Citation Information
Patent Citations
Electrode material including layer compound
JP2016063171A
Method for manufacturing electrode material for electrochemical capacitor including layer compound
JP2017076739A
MXene particle material, slurry, secondary battery, transparent electrode, and method for manufacturing MXene particle material
JP6564552B1
MXene particulate materials, methods for producing these particulate materials, and secondary batteries
JP6564553B1
Compositions comprising free-standing two-dimensional nanocrystals
US20140162130A1