Aqueous coating composition containing an epoxy amine system and an aromatic carboxylic acid as a curing catalyst
The use of specific amines and aromatic carboxylic acids in aqueous epoxy systems addresses the issues of intercoat adhesion and blistering stability in automotive repainting, providing rapid cure times and superior coating performance.
Patent Information
- Application Number
- JP2022559343
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2021-03-17
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-03-17
AI Technical Summary
Existing aqueous epoxy-amine systems used in automotive repainting suffer from reduced intercoat adhesion, blistering stability, and stone chip resistance, especially under wet conditions, when using conventional curing catalysts like phenol-containing tertiary amines or aromatic carboxylic acids.
Aqueous coating compositions comprising an epoxy resin, specific difunctional and/or polyfunctional amines, and an aromatic carboxylic acid as a curing catalyst, which form a resin component with a polyfunctional organic amine, enhancing adhesion and blistering stability while maintaining rapid cure times at low temperatures.
The composition achieves excellent adhesion to substrates, intercoat adhesion, and high blistering stability, along with improved stone chip resistance, ensuring a high-quality multilayer coating appearance.
Smart Images

Figure 0007580482000001 
Figure 0007580482000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous coating composition, preferably an aqueous sandable surfacer or primer surfacer, containing an aqueous epoxy resin dispersion (A), an aqueous amine-functional resin dispersion (B), and an aromatic carboxylic acid (C). The aqueous dispersion (B) contains at least one resin component (RC) comprising at least one specific difunctional and / or multifunctional monomeric amine (A1), and at least one specific multifunctional organic amine (A2). Furthermore, the present invention relates to a kit-of-parts comprising a base varnish (A) containing the aqueous epoxy resin dispersion, and a curable component containing the aqueous amine-functional resin dispersion (B) and an aromatic carboxylic acid (C). In addition, the present invention relates to a method for producing a coating on a substrate, and a coated substrate obtained from said method. The cured coating layer formed from said composition exhibits good adhesion to the substrate under wet conditions, as well as high intercoat adhesion and blister stability, without adversely affecting the excellent sandability and good stone chip properties. [Background technology]
[0002] In the area of automotive refinishing, repairing defects in the original coating can include abrading or grinding the defects away by mechanical means, or completely stripping the original coating layer from the entire vehicle. This method of abrading or grinding typically results in the exposure of bare metal. The use of a separate undercoat system is generally recommended before the application of the final topcoat material. The exposed sanded area of bare metal is first coated with a corrosion-inhibiting primer, i.e., a primer formulated with a corrosion-inhibiting pigment, which also has adhesion to both bare metal and organic coatings. The next step involves the application of what is referred to in the art as an abradable primer surfacer. Finally, a basecoat / clearcoat system or a topcoat is applied to complete the repair.
[0003] Water-based primers and primer surfacers for coating objects are becoming more and more important because environmental protection conditions are becoming more and more stringent. Their properties must be compatible with conventional systems, i.e. systems containing solvents. Among the cold-curing coating compositions, water-dilutable epoxy resin systems cured using amine containing hardeners are becoming more and more important. These two-component (2K) systems have excellent properties, such as good drying and good adhesion to most substrates and good corrosion resistance of metals.
[0004] It is known to add curing catalysts to these systems, such as tertiary amines, Lewis-type acids such as BF3, or weak proton donors such as phenols and carboxylic acids, to accelerate the cure time of these systems and therefore the efficiency of the refinishing process. One commonly used curing catalyst for epoxy-amine systems is a phenol containing a tree tertiary amine group (i.e., tris-2,4,6-dimethylaminomethylphenol), supplied under the trade name Ancamine K54. However, the use of this catalyst in water-based epoxy-amine systems can result in reduced intercoat adhesion and increased blistering of coating layers produced from the systems under humid conditions.
[0005] Further compounds known to promote the reaction between epoxy resins and amine-functional hardeners are aromatic carboxylic acids such as benzoic acid and salicylic acid. An aqueous amine-epoxy resin system containing salicylic acid is disclosed, for example, in WO2009 / 016162 A1. The system contains an epoxy resin A, and a water-soluble or water-dispersible amine-functional hardener B, which comprises a reaction product of an amine B1 having at least one primary amino group and / or at least one secondary amino group, an adduct B2 of a polyalkylene ether polyol B21 and an epoxide component B22, and an aromatic compound B3, which is preferably salicylic acid. The use of this epoxy resin system results in improved corrosion resistance. However, the coating layer obtained from this system also exhibits reduced intercoat adhesion and blister stability under wet conditions, as well as reduced stone chip resistance.
[0006] However, sufficient intercoat adhesion and high blister stability under wet conditions, as well as sufficient stone chip resistance, are very important in refinishing procedures to ensure a consistently aesthetically high quality appearance of the painted surface under conditions encountered during normal use of the repainted vehicle.
[0007] Therefore, there is a need for an aqueous coating composition, particularly for vehicle refinishing, that exhibits fast cure times at low cure temperatures, preferably at cure temperatures below 80°C. The cured coatings produced from said compositions should exhibit good adhesion to the substrate, good intercoat adhesion and high blister stability, especially under wet conditions. In addition, the cured coatings should exhibit excellent corrosion and abrasion resistance and sufficient stone chip resistance. Finally, the cured coatings should provide a high quality appearance when combined with additional coating layers, such as pigmented basecoats and / or clearcoats. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] WO2009 / 016162 A1 Summary of the Invention [Problem to be solved by the invention]
[0009] It is therefore an object of the present invention to provide an aqueous coating composition which can be cured rapidly, especially under humid conditions, at low curing temperatures, preferably at temperatures below 80° C., without adversely affecting the excellent abrasion, corrosion and stone chip resistance of said coating layer, and which results in a cured coating layer with good adhesion to the substrate, good intercoat adhesion and high blister stability. Furthermore, the application of further coating layers, such as pigmented base coat and / or clear coat layers, should result in a multi-layer coating with a high quality appearance. [Means for solving the problem]
[0010] The above objectives are achieved by the subject matter claimed in the appended claims and also by preferred embodiments of that subject matter as described hereinafter.
[0011] A first subject of the present invention is therefore an aqueous coating composition comprising a) at least one aqueous dispersion (A) of an epoxy resin (ER1), said epoxy resin (ER) having on average at least one epoxy group per molecule; b) at least one aqueous resin dispersion (B) comprising at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) in a proportion of 0.5 to 5% by weight, and a resin component (RC) having an NH equivalent of 150 to 400 g / mol; c) at least one aromatic compound (C) having at least one carboxylic acid group; Including, The resin component (RC) comprises at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups, the at least one polyfunctional organic amine (A2) being (i) at least one difunctional and / or multifunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol; (ii) at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1), and (iii) at least one compound XR, where X is a functional group that is reactive towards epoxy groups and R is an organic group that contains at least one polyoxyalkylene unit and does not contain further X groups; containing the reaction product of It is a water-based coating composition.
[0012] The above specified coating composition is hereinafter also referred to as the coating composition of the invention and is therefore the subject of the present invention. Preferred embodiments of the coating composition of the invention will become apparent from the description hereinafter and also from the dependent claims.
[0013] In light of the prior art, it was surprising and unforeseeable for a person skilled in the art that the object on which the present invention is based could be achieved by using aromatic carboxylic acids as curing catalysts in combination with specific aqueous dispersions (B) as crosslinking agents in water-based epoxy coating systems. These systems exhibit fast curing times at low temperatures, preferably below 80°C, and are therefore highly suitable for automotive refinishing. The cured coating layers obtained from said systems have excellent adhesion to the substrate as well as excellent intercoat adhesion and blister stability under wet conditions, without adversely affecting the excellent polishability and good stone chip properties. Furthermore, the aforementioned combination of curing catalysts and aqueous dispersions (B) allows to significantly improve the crosscut adhesion and blister stability under wet conditions, compared to water-based epoxy systems containing different amino-functional curing agents, or water-based epoxy systems containing aqueous dispersions (B) and the curing catalyst Ancamine K54.
[0014] A further subject of the present invention is a kit-of-parts comprising two separate components A) and B), said components A) and B) being A) at least one aqueous base varnish containing at least one aqueous dispersion (A) of an epoxy resin (ER1), said epoxy resin (ER) having on average at least one epoxy group per molecule; B) at least one aqueous curing agent component, at least one aqueous resin dispersion (B) comprising at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) in a proportion of 0.5 to 5% by weight, and a resin component (RC) having an NH equivalent of 150 to 400 g / mol, said resin component (RC) comprising at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups, said at least one polyfunctional organic amine (A2) being (i) at least one difunctional and / or multifunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol; (ii) at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1), and (iii) at least one compound XR, where X is a functional group that is reactive towards epoxy groups and R is an organic group that contains at least one polyoxyalkylene unit and does not contain further X groups; An aqueous resin dispersion (B) containing the reaction product of at least one aromatic compound (C) having at least one carboxylic acid group; Contains Aqueous hardener component and It is a kit of parts.
[0015] Another subject of the invention is a method for producing at least one coating layer on a substrate, said method comprising the steps of: (i) applying an aqueous coating composition of the invention, or a coating composition made from a kit-of-parts of the invention, to a substrate; (ii) forming a coating film from the coating composition applied in step (i); (iii) curing the coating film formed in step (ii); (iv) optionally polishing the cured coating layer obtained in step (iii); (v) optionally applying at least one further coating layer and curing said coating layer; Includes.
[0016] A final subject of the invention is the coated substrate produced by the method of the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The measurement methods to be taken in the context of the present invention to determine certain characteristic variables can be found in the Examples section. Unless otherwise specified, these measurement methods will be taken to determine the respective characteristic variables. Where reference is made in the context of the present invention to an official standard without any indication of the official validity period, the reference is implicit to the version of that standard valid on the filing date, or, in the absence of any valid version at that time, to the last valid version.
[0018] All film thicknesses reported in the context of the present invention should be understood to be dry film thicknesses. It is therefore in each case the thickness of the cured film. Thus, where a coating material is reported to be applied at a specific film thickness, it means that the coating material is applied to result in the stated film thickness after curing.
[0019] All temperatures articulated in the context of the present invention should be understood to be the temperature of the room in which the substrate or coated substrate is placed, and therefore it is not meant to imply that the substrate itself is required to have the temperature under consideration.
[0020] The term "resin or resin component" is understood to mean products that contain organic constituents, i.e. organic reaction products, oligomers and / or polymers and, where appropriate, also monomers, such as resin component (RC). Resins have a more or less wide distribution of molar masses and are generally usable as binders in coating compositions. They therefore form at least a certain proportion of the polymer network of the coating layer present after curing.
[0021] The term "binder" or "binder component" refers herein to the non-volatile fraction of the coating material, excluding pigments and fillers, in accordance with the relevant DIN EN ISO4618:2007-03. A specific binder component in this context is an epoxy resin (ER1) or a coating additive. However, for clarity, the term "binder" is used primarily in connection with components that govern film formation and does not include curing agents or crosslinkers.
[0022] The aqueous coating composition of the present invention: The coating composition of the present invention is an aqueous coating composition. The term "aqueous" in the context of coating compositions is known in principle. What is meant is a coating composition that contains a significant proportion of water as a solvent. It will be recognized that it is alternatively possible for the aqueous system to contain organic solvents, at least in small amounts, for example as co-solvents with emulsifier function for the stabilization of certain components, such as resins, pigments or additives. "Aqueous" in the context of the present invention should preferably be understood to mean that the composition under consideration has a proportion of water of at least 40% by weight, preferably at least 50% by weight, even more preferably at least 60% by weight, relative to the total amount of solvents (i.e. water and organic solvents) present in each case. Preferably, the proportion of water in turn is between 50% by weight and 99% by weight, in particular between 60% by weight and 98% by weight, relative to the total amount of solvents present in each case.
[0023] The above definition of "aqueous" also applies in connection with the aqueous dispersions (A) and (B) described hereinafter, i.e. said dispersions have a proportion of water of 50% to 99% by weight, in particular 60% to 98% by weight, relative to the total amount of solvent present in each case.
[0024] Aqueous dispersion (A) of epoxy resin (ER1): The first essential component of the aqueous coating composition of the present invention is an aqueous dispersion (A) of an epoxy resin (ER1). The term "aqueous dispersion" is well known to those skilled in the art and is preferably understood to mean a dispersion that contains at least 40% by weight of water relative to the total amount of solvent present in the dispersion.
[0025] It is known that epoxy resins are polycondensation resins that contain more than one epoxy group on average. They can be produced, for example, by condensing bisphenol A or bisphenol F with epichlorohydrin, and can have two epoxy groups on average. These compounds contain hydroxyl groups along the chain and epoxy groups at the end. The crosslinking ability via epoxy groups depends on the chain length, because it decreases as the chain length / molar mass increases.
[0026] Suitable epoxy resins (ER1) are selected from glycidyl ethers of dihydric alcohols or phenols, novolax, glycidyl esters of carboxylic acids, or mixtures thereof, preferably glycidyl ethers of phenols, more preferably glycidyl ethers of bisphenol A. Thus, the preferred epoxy resins (ER1) do not contain any bisphenol F, since the presence of bisphenol F in said epoxy resins (ER1) may adversely affect the polishability of the cured coating layers produced from the coating compositions of the present invention.
[0027] Preferably, the at least one epoxy resin (ER1) has a specific epoxy equivalent weight (EEW) and viscosity. According to a first embodiment, the epoxy resin (ER1) has an epoxy equivalent weight (EEW) of preferably 100 to 400 g / eq, more preferably 120 to 300 g / eq, even more preferably 150 to 250 g / eq, and very preferably 185 to 210 g / eq, determined according to ASTM D1652-11 (2019).
[0028] Furthermore, the epoxy resin (ER1) of this first embodiment preferably has a viscosity of 1,000 to 20,000 mPa, as determined in accordance with ASTM D2196-18. * s, more preferably 1,500 to 15,000 mPa * s, most preferably 2,500 to 9,500 mPa * s at 25°C.
[0029] According to an alternative embodiment, the epoxy resin (ER1) preferably has an epoxy equivalent weight (EEW) determined according to VLN305 of 250 to 700 g / eq, more preferably 300 to 600 g / eq, even more preferably 350 to 550 g / eq and very preferably 380 to 520 g / eq.
[0030] Furthermore, the epoxy resin (ER1) of this alternative embodiment preferably has a viscosity of 100 to 3,000 mPa, determined according to DIN EN ISO 3219:1994-10. * s, more preferably 150 to 2,500 mPa * s, and even more preferably 200 to 2,000 mPa * s, most preferably 250 to 1,400 mPa * s, 100s -1 The kinematic viscosity at 23°C is
[0031] The use of the aforementioned epoxy resin (ER1) results in good optical and mechanical properties as well as high adhesion of the coating layer produced from the coating composition of the present invention. Moreover, said epoxy resin (ER1) allows stable dispersion of pigments and / or fillers without irreversible thickening or solidification during dispersion.
[0032] The at least one dispersion (A) of an epoxy resin (ER1) is preferably present in a total amount of 5 to 50% by weight, more preferably 10 to 40% by weight, even more preferably 15 to 30% by weight and very preferably 18 to 25% by weight, in each case based on the total weight of the aqueous coating composition.
[0033] Suitable total amounts of epoxy resins (ER1) in the aqueous coating composition are in the range from 1 to 30% by weight, preferably from 5 to 25% by weight, more preferably from 8 to 20% by weight and very preferably from 10 to 15% by weight, based in each case on the total weight of the aqueous coating composition.
[0034] Aqueous dispersion (B): The second essential component of the aqueous coating composition of the present invention is an aqueous dispersion (B) containing a mass proportion of 0.5 to 5% of at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) and a resin component (RC) having an NH equivalent of 150 to 400 g / mol.
[0035] Difunctional and / or polyfunctional monomeric primary and / or secondary amines (A1): Di- and / or polyfunctional monomeric primary and / or secondary amines (A1) are understood to mean low molecular weight compounds, i.e. compounds having a molecular weight of less than 500 g / mol, preferably less than 250 g / mol, and having a discrete number of amino groups per molecule, which is constant for each molecule.
[0036] At least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) preferably comprises at least 65 mol-%, preferably at least 75 mol-%, more preferably at least 90 mol-%, and most preferably 100 mol-% of amines consisting of amino groups and hydrocarbon groups. Therefore, other functional groups, such as hydroxyl, carboxyl or nitrile groups, are present only in small amounts or are not present at all. The small amount of other functional groups, preferably the absence of other functional groups, leads to improved polishability of the cured coating layer obtained from the coating composition of the present invention.
[0037] The proportion of the corresponding amine (A1) is determined by the amount of amine (A1) introduced into the aqueous dispersion (B) during its preparation, based on the total amount of the dispersion (B). When commercial products are used, the proportion of said amine (A1) can be determined by commonly known analytical methods, such as gas chromatography (GC) or mass spectrometry (MS).
[0038] Examples of suitable amines (A1) are monomeric aliphatic, aromatic and araliphatic (mixed aliphatic-aromatic) amines which are known in principle to the person skilled in the art. Examples of such amines include ethylenediamine, propylene-1,2-diamine, propylene-1,3-diamine, butane-1,4-diamine, octane-1,8-diamine, 1,3-diaminopentane, hexamethylenediamine, 2-methylpentamethylenediamine, neopentanediamine, cyclohexanediamine, 2,2,4-(2,4,4-)trimethylhexamethylenediamine, 35 isophoronediamine, bis(aminomethyl)cyclohexane, bis(4-aminocyclohexyl)methane, diethylenetriamine, triethylenetetraamine, tetraethylenepentamine, dipropylenetriamine, bis(hexamethylenediamine), N,N-5 dimethylaminodipropylenetriamine, laurylpropylenediamine, 1,2- and 1,3-(m)-xylylenediamine and 1,4-bis(aminomethyl)benzene. Further amines include aminoethylethanolamine or heterocyclic polyamines such as aminoethylpiperazine and bis(aminopropyl)piperazine.
[0039] Preferred are difunctional monomeric primary and / or secondary amines. Particularly preferred are difunctional monomeric primary amines, very particularly preferred isophorone diamine and / or m-xylene diamine. Particularly preferably, the aqueous dispersion (B) contains at least two difunctional monomeric primary amines, namely isophorone diamine and m-xylene diamine.
[0040] The proportion of the at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1), preferably isophoronediamine and / or m-xylenediamine, in the aqueous dispersion (B) is from 1 to 4.5% by weight, preferably from 1.5 to 4% by weight, relative to the total weight of the aqueous dispersion (B).
[0041] Resin component (RC): The resin component (RC) comprises at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups. By demarcation from the monomeric amines (A1) already described, these are adducts or reaction products having polymeric properties and a number of amino groups per molecule that can only be described by an average.
[0042] The resin component (RC) preferably has an NH equivalent weight of 160 to 350 g / mol, preferably 170 to 250 g / mol (see Examples section for method of determination).
[0043] The at least one polyfunctional organic amine (A2) is (i) at least one difunctional and / or multifunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol; (ii) at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A3), (iii) at least one compound XR, where X is a functional group that is reactive towards epoxy groups and R is an organic group that contains at least one polyoxyalkylene unit and does not contain further X groups; The reaction product contains:
[0044] In the case where the resin component (RC) further contains, in addition to the polyfunctional organic amine (A2), at least one polyfunctional organic amine (A3) having a primary and / or secondary amino group, said polyfunctional organic amine (A3) is (i) at least one difunctional and / or multifunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol; (ii) at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1); In the present invention, the reaction product is preferably
[0045] The polyfunctional organic amine (A3) thus differs from the polyfunctional organic amine (A2), because different starting materials are used to prepare said polyfunctional organic amine. The term "reaction product" in the sense of the present invention is understood to mean the compound obtained by reacting the listed compounds with each other. This already implies that said reaction product cannot contain further constituents that are not explicitly listed in relation to said reaction product.
[0046] Particularly preferably, the resin component (RC) consists of at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups and at least one polyfunctional organic amine (A3) having primary and / or secondary amino groups.
[0047] The at least one difunctional and / or polyfunctional epoxy resin (ER2) used to prepare the polyfunctional organic amine (A2) and the polyfunctional amine (A3) has an average epoxy equivalent weight (EEW) of less than 400 g / eq. It has been found that the correspondingly low average epoxy equivalent weight and therefore higher epoxy functionality of this component also leads here to a better polishability in the surfacer layer being finally produced. More preferably, the average epoxy equivalent weight is less than 350 g / mol, preferably less than 300 g / mol, more preferably less than 250 g / mol, very preferably between 160 and 200 g / mol, determined in accordance with DIN EN ISO3001:2019-08. The average epoxy equivalent weight can be obtained by determining the epoxy equivalent weight of all epoxy compounds used and weighing their mass proportion in the total mass of epoxy compounds. In the case of commercially available products (where the epoxy compounds may already be covalently bonded), the average epoxy equivalent weight can be determined by analysis of the product, for example by gas chromatography (GC) or mass spectrometry (MS).
[0048] It is preferred that the at least one di- and / or polyfunctional epoxy resin (ER2) has an average epoxy functionality of 1 to 5, preferably an epoxy functionality of 1 to 4, more preferably an epoxy functionality of 1 to 3, and very preferably an epoxy functionality of 2, since said epoxy resins are readily commercially available.
[0049] Suitable epoxy resins (ER2) can be saturated or unsaturated, aliphatic and mixed aliphatic-aromatic compounds, optionally containing hydroxyl groups, and are selected, for example, from glycidyl ethers of dihydric alcohols or phenols, novolaxes, diglycidyl esters of carboxylic acids, or mixtures thereof. Among the phenols, resorcinol, hydroquinone, 2,2-bis-(4-hydroxyphenyl)-propane (bisphenol A); dihydroxydiphenylmethane (bisphenol F), tetrabromobisphenol A, 4,4'-dihydroxydiphenylcyclohexane, 2,2-bis-(4-hydroxy-3-methylphenyl)-propane, 4,4'-dihydroxydiphenyl, 4,4'-dihydroxybenzophenone, 1,1-bis-(4-hydroxyphenyl)-ethane, 2,2-bis-[4- (2'-hydroxypropoxy)-phenyl]-propane, 1,1-bis-(4-hydroxyphenyl)-isobutane, 2,2-bis(4-hydroxy-3-tert-butylphenyl)-propane, bis-(2-hydroxynaphthyl)-methane, 1,5-dihydroxynaphthalene, tris-(4-hydroxyphenyl)-methane, bis-(4-hydroxyphenyl)ether, bis-(4-hydroxyphenyl)sulfone, mixtures of isomers, as well as the halogenation and hydration products of the compounds mentioned. It is also possible to use diepoxyalkanes prepared by epoxidation of diolefins.
[0050] Particularly preferred epoxy resins (ER2) are glycidyl ethers of phenols, most preferably glycidyl ethers of bisphenol A. Therefore, particularly preferred epoxy resins (ER2) do not contain any bisphenol F. It has been found that the absence of bisphenol F in the epoxy resin (ER2) results in enhanced polishability of the cured coating layer produced from the coating composition of the present invention.
[0051] The at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) used to prepare the polyfunctional organic amine (A2) and the polyfunctional amine (A3) corresponds to the amines (A1) described above in connection with the aqueous dispersion (B).
[0052] In the preparation of the polyfunctional organic amine (A2), at least one specific compound XR is used. Preference is given to using exactly one compound XR.
[0053] The X group is a group known to those skilled in the art, for example a primary or secondary amino group, a hydroxyl group, a carboxylic acid group or a thiol group. It is important that the compound XR has exactly one X group. Otherwise, adverse effects are found in the polishability of the cured coating layer obtained from the coating composition of the present invention. Preferred X groups are amino groups, among which primary amino groups are preferred. Apart from the good reactivity of amino groups with epoxy groups, primary amines have two NH equivalents and therefore have a binding site for epoxides. Thus, incorporation of the compound XR into the side chain position of the polyfunctional organic amine (A2) can occur. The presence of an amino group, preferably a primary amine group, leads to improved polishability of the cured coating layer obtained from the coating composition of the present invention.
[0054] The R group is an organic group containing polyoxyalkylene units, particularly preferably polyethylene or polypropylene units or mixed polyethylene / polypropylene units.
[0055] It is preferred that the organic R group is composed of a polyoxyalkylene unit, apart from any molecular unit obtained from synthesis.For simplicity, such an R group is also referred to as a polyoxyalkylene group.The molecular unit obtained from synthesis is, for example, the organic group of the molecule used in starting the formation of the polyoxyalkylene chain, for example, the starter alcohol by means of which the polymerization of ethylene oxide and / or propylene oxide is initiated.
[0056] Particularly preferred compounds XR are selected from primary polyoxyalkylene monoamines, which can be synthesized or obtained commercially, for example from Huntsman Corporation under the trade name "Jeffamine".
[0057] The weight average molecular weight of compound XR may vary widely, for example in the range of 800 to 2,200 g / mol (as determined by means of size exclusion chromatography coupled with light scattering).
[0058] Particularly preferably, the at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups consists of the reaction product of components (i), (ii) and (iii), so that the polyfunctional organic amine (A2) does not contain further compounds apart from the aforementioned reaction products.
[0059] Dispersion (B) preferably has a solids content of 25 to 45% by weight, based on the total weight of the dispersion and determined in accordance with DIN EN ISO 3251:2018-07.
[0060] The aqueous dispersion (B) comprising at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) and the resin component (RC) can be prepared, for example, by a two-step process which will be described in detail later in this specification.
[0061] Process (1): In the first step (1), the amino-functional resin mixture (I) is prepared by reacting the epoxy-functional resin mixture (Ia) with a component (Ib) containing at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1). The epoxy-functional resin mixture (Ia) is prepared by reacting at least one difunctional and / or polyfunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol with at least one compound XR. For this purpose, the epoxy groups of the epoxy resin (ER2) are used in a molar stoichiometric excess relative to the reactive units X of the compound XR. The number of reactive units X means the number of potential bonding sites in the compound XR for each epoxy group. For hydroxyl or secondary amino groups, for example, there is one reactive unit per X group. For primary amino groups, there are two reactive units (two NH functionalities). Preferably, the molar ratio of the epoxy groups of the epoxy resin (ER2) to the epoxy reactive units of the X groups of the component XR is 10 to 1.1, more preferably 5 to 1.5, particularly preferably 3.5 to 1.8. The amount of epoxy groups in the epoxy resin (ER2) can be obtained or appropriately adapted by determining the epoxy equivalent weight. The amount of reactive units in the X groups can be determined, for example, by determining the amine value, OH value or acid value (DIN53176:2002-11, DIN53240-3:2016-03, DIN EN ISO2114 Correction1:2006-11).
[0062] The epoxy-functional resin mixture (Ia) preferably has an epoxy equivalent mass of 500 to 1,500 g / mol, more preferably 600 to 1,200 g / mol.
[0063] Component (Ib) which is reacted with the epoxy-functional resin mixture (Ia) comprises at least one di- and / or polyfunctional monomeric primary and / or secondary amine (A1). Preferably, component (Ib) consists of at least one such amine (A1).
[0064] Examples of suitable epoxy resins (ER2), compounds XR and amines (A1) have already been described above and may apply correspondingly.
[0065] The resin mixture (I) is an amino-functional resin mixture. Therefore, a molar excess of NH equivalents of compound (Ib) relative to the epoxy-functional resin mixture (Ia) must be used. In particular, the NH equivalents of the resin mixture (I) are between 50 and 140 g / mol, preferably between 70 and 130 g / mol (see the Examples section for the method of determination). Furthermore, the resin mixture (I) comprises a proportion of 17.5% to 40% by weight, preferably between 25% and 35% by weight, of difunctional and / or polyfunctional monomeric primary and / or secondary amines (A1), i.e. component (Ib). Both criteria can be met by the skilled person by suitable selection of the molar amounts of the two components and in the knowledge that there is a quantitative conversion of epoxy groups and NH functionality under conditions and reaction regimes known per se. Preferably, the resin mixture (I) is in dispersion in water after its preparation, in this case in an aqueous dispersion.
[0066] Resin mixture (I) can be produced as such as described above and can therefore be obtained in an aqueous dispersion. It is also possible to purchase an aqueous dispersion of resin mixture (I) commercially available (for example as Beckopox VEH2849w / 80WA (Allnex)).
[0067] Process (2): The aqueous dispersion (B) is obtained in a second step (2) by reacting component (IIa) containing the amino-functional resin mixture (I) with component (IIb) containing at least one di- and / or polyfunctional organic epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol, preferably less than 350 g / mol, more preferably less than 250 g / mol. If desired, the organic solvent used during the preparation of the aqueous dispersion (B) can be removed. Since the resin component (RC) is amine-functional, a molar excess of the NH equivalents of component (IIa) relative to the epoxy groups of component (IIb) is used.
[0068] Preference is given to using the direct reaction product from step (1) as component (IIa), since the resin mixture (I) is obtained after step (1) as an aqueous dispersion and can thus be used directly in step (2), which occurs in the aqueous phase. Before carrying out step (2), solvents or additives, such as emulsifiers, can be added to the reaction product.
[0069] Component (IIa) preferably does not contain any further compounds, apart from the amino-functional resin mixture (I), which are capable of reacting with component (IIb).
[0070] Component (IIb) preferably consists of at least one, preferably exactly one, difunctional and / or polyfunctional organic epoxy resin (ER2) having an epoxy equivalent mass that meets the above requirements. Examples of suitable epoxy compounds are those already listed above as components.
[0071] The above method also allows the use of existing commercial products (such as the above Beckopox VEH2849w / 80WA), so that the aqueous dispersion (B) can be easily obtained by simple modification of the commercial product with the appropriate epoxide (because apart from this last reaction, all further reaction processes are already practiced in the manufacture of the commercial product).
[0072] However, the aqueous dispersion (B) can also be obtained by a one-step process, in which all starting materials are reacted together by adapting the amine and epoxide stoichiometry. It would also be possible to first react the epoxy resin (ER2) with the compound XR and further react the resulting product with further epoxide and monomeric amine (A1).
[0073] The resin component (RC) is preferably present in a total amount of 10 to 30% by weight, preferably 15 to 25% by weight, based in each case on the solids content of the aqueous coating composition.
[0074] Aromatic compounds (C) having at least one carboxylic acid group: The third essential component of the aqueous coating composition of the present invention is an aromatic compound (C) having at least one carboxylic acid group. An aromatic compound refers to a compound having at least one aromatic moiety in the molecule. The carboxylic acid group can be either directly bonded to the aromatic moiety or can be bonded via a linker. Preferably, the carboxylic acid group is directly bonded to the aromatic moiety.
[0075] Preferred compounds (C) further comprise at least one hydroxyl group. The presence of at least one hydroxyl group has been found to improve the acceleration of the crosslinking reaction compared to aromatic compounds that do not have any hydroxyl groups.
[0076] Particularly preferred are resorcinol, salicylic acid, p-hydroxybenzoic acid, 2,4-dihydroxybenzoic acid (beta-resorcylic acid), 2,5-dihydroxybenzoic acid (gentisic acid), 2,6-dihydroxybenzoic acid (gamma-resorcylic acid), 3,4-dihydroxybenzoic acid (protocatechuic acid), 3,5-dihydroxybenzoic acid (alpha-resorcylic acid), 3,4,5-trihydroxybenzoic acid (gallic acid), 2-hydroxy-3-naphthoic acid, 2-hydroxy-6-naphthoic acid, and their alkyl derivatives, such as 2-hydroxy-3-, -4- and -5-methyl-benzoic acid (cresotinic acid), and mixtures thereof. Particularly preferred is salicylic acid, which is used as compound (C).
[0077] The at least one aromatic compound (C) is preferably present in a total amount of 0.1 to 5% by weight, more preferably 0.2 to 3% by weight, even more preferably 0.3 to 1% by weight and very preferably 0.4 to 0.7% by weight, in each case relative to the total weight of the aqueous coating composition.
[0078] Further optional components of the aqueous coating composition: The aqueous coating composition of the present invention preferably comprises at least one pigment and / or filler, i.e. the aqueous coating composition of the present invention preferably results in a colored coating layer. Preferred pigments are black and / or white pigments. The coating composition thus preferably contains at least one black pigment or at least one white pigment, or at least one white pigment and one black pigment. This means that the coating composition of the present invention preferably has a black, white or gray color (in various gradations). The composition can also contain further pigments. Preferred black pigments are typical organic and inorganic, especially inorganic, black pigments that are commercially available in powder form. Particular mention should be made of pigment black (carbon black), iron oxide (Fe3O4) pigments, such as typical synthetic iron oxides (available, for example, from Lanxess under the trade name Bayferrox), mixed oxide pigments, such as manganese black or spinel black. Very particular preference is given to pigment black (carbon black) and iron oxide pigments.
[0079] Preferred white pigments are typical inorganic white pigments, such as titanium dioxide (for example the rutile pigments known under the trade name Kronos from Kronos), zinc 15 oxide, zinc sulfate or antimony trioxide. Very particular preference is given to titanium dioxide, especially in its rutile modification.
[0080] Further preferred pigments are those known to those skilled in the art as "anti-corrosion pigments". Particularly preferred in this specification is zinc phosphate. Although zinc phosphate has a white color, it is not classified as a white pigment, but as an anti-corrosion pigment due to its anti-corrosion effect.
[0081] The proportion of pigments is preferably 15 to 25% by weight, very preferably 20% by weight, based in each case on the solids content of the coating composition.
[0082] Fillers that are preferably present are all inorganic and organic fillers that are known per se and familiar to those skilled in the art, preferably inorganic fillers.Therefore, fillers include in particular those substances known to those skilled in the art that are used in granular or powder form, for example, to achieve certain physical properties of coating composition, and are insoluble in the respective medium of use.These include in particular carbonates, such as calcium carbonate or barium carbonate, sulfates, such as calcium sulfate and barium sulfate, silicates and sheet silicates, such as talc, pyrophyllite, mica, kaolin, precipitated calcium silicate, aluminum silicate, calcium / aluminum silicate, sodium / aluminum silicate, and mullite, silicas, such as quartz, cristobalite, precipitated silica, or especially fumed silica, such as available under the trade name Aerosil (Evonik), metal oxides and hydroxides, such as aluminum hydroxide and magnesium hydroxide.
[0083] The proportion of fillers is preferably 30 to 50% by weight, in particular 30 to 40% by weight, based in each case on the solids content of the coating composition.
[0084] In addition, the coating composition may also contain at least one additive. Examples of such additives are light stabilizers, antioxidants, degassing agents, emulsifiers, slip additives, polymerization inhibitors, adhesion promoters, leveling agents, film-forming aids, thickeners, sag control agents (SCAs) or corrosion inhibitors. They are used in customary and known amounts. The same applies to the possible use of organic solvents, which are used in amounts such that they do not change the aqueous properties of the coating composition.
[0085] Properties of the Waterborne Coating Composition In order to ensure rapid and complete crosslinking under curing conditions, the aqueous coating composition preferably contains a certain molar ratio of the NH groups of the resin compound (RC) to the epoxy groups of the epoxy resin (ER1). Therefore, it is preferred if the molar ratio of the NH groups of the resin compound (RC) to the epoxy groups of the epoxy resin (ER1) is 0.74:1 to 0.95:1, preferably 0.9:1.
[0086] The solids content of the 2K coating composition may vary depending on the requirements of the individual case, but is preferably in the range of 70-85% by weight, based on the total weight of the aqueous coating composition and determined in accordance with DIN EN ISO 3251:2018-07. The solids content is primarily guided by the viscosity required for the application, more particularly for the spray application, and can therefore be adapted by the skilled person on the basis of his general technical knowledge, optionally with the support from some research tests.
[0087] The coating composition can be produced using mixing methods and mixing units which are customary and known for the production of coating compositions, such as stirred tanks, stirred mills, pearl mills, extruders, kneaders, Ultraturrax, in-line dissolvers, static mixers, toothed ring dispersers, expansion nozzles and / or microfluidizers.
[0088] The coating composition of the present invention is of excellent suitability as a surfacer and / or primer surfacer.Therefore, the coating composition of the present invention is preferably a surfacer or primer surfacer.The function, configuration and field of use of surfacer and primer surfacer are in principle known to those skilled in the art and have demarcation characteristics in this respect.Surfacers are generally applied as intermediate layers (to previously cured electrodeposition) in the context of automotive OEM painting, cured separately, and then overcoated with base coat and clear coat.Primer surfacers find use in particular in the automotive repaint sector, where they are responsible for filling local damaged areas in the original paint system and obtaining the guarantee of suitable adhesion and corrosion resistance on the substrate.
[0089] The present invention includes the following kit of parts: To prevent reaction of the epoxy resin (ER1) with the components of the aqueous dispersion (B), the coating composition of the present invention is preferably formulated as a multi-component coating composition, more preferably a two-component coating composition, in which the components of the coating composition are contained in separate containers and the coating composition is prepared by mixing the contents of the containers, preferably just prior to applying the prepared coating composition to a substrate.
[0090] The present invention therefore also relates to a kit-of-parts comprising two separate components A) and B), wherein components A) and B) are A) at least one aqueous base varnish containing at least one aqueous dispersion (A) of an epoxy resin (ER1), said epoxy resin (ER) having on average at least one epoxy group per molecule; B) at least one aqueous curing agent component, at least one aqueous resin dispersion (B) comprising at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) in a proportion of 0.5 to 5% by weight, and a resin component (RC) having an NH equivalent of 150 to 400 g / mol, said resin component (RC) comprising at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups, said at least one polyfunctional organic amine (A2) being (i) at least one difunctional and / or multifunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol; (ii) at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1), and (iii) at least one compound XR, where X is a functional group that is reactive towards epoxy groups and R is an organic group that contains at least one polyoxyalkylene unit and does not contain further X groups; An aqueous resin dispersion (B) containing the reaction product of at least one aromatic compound (C) having at least one carboxylic acid group; Contains Aqueous hardener component and That is, It also relates to kit of parts.
[0091] Thus, the kit-of-parts of the invention comprises at least the two components A) and B), preferably it consists of exactly these two components A) and B. It is also possible in the present invention that further compounds, such as solvents or additives, can be present as separate components and can be used to adapt the viscosity of the coating composition obtained after mixing components A) and B).
[0092] In said inventive kit-of-parts, the base varnish (component A)) and the hardener component (component B)) defined below are prepared and stored separately from each other and are mixed with each other only immediately before application to the substrate. The processing time or pot life (i.e. the time during which the coating composition obtained by mixing components A) and B) can be processed and applied at room temperature (15-25°C, in particular 20°C)) depends on the compounds present in the base varnish and the hardener component. In the context of the present invention, the processing time of the coating composition obtained by mixing components A) and B) is preferably at least 2 minutes and up to 60 minutes, more preferably at least 5 minutes and up to 60 minutes. A particular advantage of such two-component coating compositions is that the curing can be performed at temperatures below 100°C, thus making said two-component compositions suitable for refinishing applications.
[0093] It is likewise known that the base varnish A) usually contains, apart from the epoxy resin (ER1) used as binder and solvent, all or most of the further functional components of the composition, such as pigments, fillers and additives, whereas the hardener component B) contains, apart from the solvent and any additives present, only compounds intended for crosslinking. The terms "base varnish component" and "hardener component" in the context of multi-component coating compositions are known to the skilled artisan and, within a certain range of configurations, also have characterizing and therefore demarcating properties. It is particularly preferred in the context of the present invention if the base varnish A) contains the pigments and fillers, preferably all the pigments and fillers, used in the coating composition obtained after mixing components A) and B). It is likewise preferred that the base varnish A) does not contain any other epoxy resins apart from at least one epoxy resin (ER1), i.e. in the epoxy resin (ER1), the binder component of the base varnish A) accounts for at least 90% by weight, preferably at least 95% by weight. The binder component is obtained from the solids (non-volatile components) of the dispersion minus the pigment and filler ratios. The epoxy groups can react with the NH functionality of the polyamine components present in the hardener component B) after mixing the two main components A) and B) to form a network structure and thus contribute to hardening the coating layer produced from the coating composition.
[0094] It is even more preferred if the base varnish A) is in the form of an aqueous dispersion.
[0095] It is known in principle that pigments and fillers are used in the form of dispersions in coating compositions. This means that the preparation of a coating composition includes a step in which pigments or fillers are dispersed with resins and solvents, generally water, with the introduction of high shear forces in a grinder or dissolver. Resins here have a dispersing or emulsifying effect and simply promote the stabilization of the pigments or fillers. It is of course also possible to use additional additives to further support the dispersion. It is equally possible that the production of the dispersion includes the addition of all the coating components that will be introduced into the base varnish A) so that the base varnish A) thus finally consists of the dispersion. Thus, a dispersion is a mixture that contains at least (but not necessarily exclusively) resins and pigments and / or fillers in a mutually dispersed form.
[0096] The fact that the base varnish A) preferably contains or consists of a dispersion thus means that either the dispersion is produced as described above and then completed (for example using standard stirring equipment) with the further coating components still absent to produce the base varnish A), or, in the case of the production of the dispersion, all the constituents of the base varnish A) are introduced into the dispersion process, so that the dispersion thus constitutes the base varnish A).Since the dispersion is preferably aqueous, water is preferably used in the actual dispersion process.
[0097] With regard to the preferred aqueous dispersion (A) comprising at least one epoxy resin (ER1), aqueous dispersion (B), compound (C), pigments and / or fillers, as well as further additives and compounds which may be present in components A) and / or B) of the kit-of-parts of the invention, reference is made to the description of said components in relation to the coating composition of the invention.
[0098] What has been said regarding the coating composition of the invention applies mutatis mutandis with regard to the further preferred embodiments of the kit-of-parts of the invention.
[0099] The method of the present invention: The invention further provides a method of producing a coating on a substrate, in which the coating composition of the invention is applied to the substrate, a coating film is formed, and then cured. The cured coating layer can be polished and coated with a further coating layer. In the context of the method of the invention in which the coating composition is used, it will be appreciated that the specific and preferred embodiments with respect to the coating composition described above can apply as well.
[0100] Process (i): In step (i) of the method of the present invention, the aqueous coating composition of the present invention or the coating composition produced from the kit-of-parts of the present invention is applied to a substrate. The application of the composition to the substrate in the sense of the present invention is not limited to a direct application on the metal substrate. Instead, there may be at least one further layer between the metal substrate and the layer formed by the composition. This is the case, for example, when the coating composition is used as a surfacer in an OEM paintwork. The reason is that in such a case, there will be at least one electrodeposition layer between the surfacer layer and the metal substrate. In other words, the substrate to which the composition of the present invention is applied is thus a metal substrate coated with an electrodeposition layer.
[0101] Application of the composition to the substrate can be achieved by methods known in the art, for example by spraying, knife coating, painting, pouring, immersion, impregnation, sprinkling or rolling. Preference is given to employing the spraying method.
[0102] The substrate used is, for example, a metal substrate, preferably a metal substrate used in the automotive industry (vehicle manufacturing). Advantageously, unalloyed and alloyed steel and / or iron, zinc and aluminum substrates and corresponding alloys are used. Furthermore, the coating composition can also be applied to plastic substrates, as well as substrates having metal and plastic parts. Furthermore, the composition can also be applied on old coatings, for example multi-layer coatings having defect sites.
[0103] Step (ii): After the coating composition is applied to the substrate, a polymer film is formed therefrom. Said film formation is preferably carried out by drying and / or evaporation of the applied composition. Drying and evaporation in the context of the present invention means the evaporation of organic solvents and / or water, so that the coating is dry but not yet cured, more particularly not yet forming a completely crosslinked coating film.
[0104] Drying and / or evaporation of the applied coating composition is preferably carried out at 15-25° C. for 1-60 minutes.
[0105] Step (iii): In step (iii) of the method of the present invention, the coating film formed in step (ii) is cured by known methods. Curing means the conversion of the coating composition, which is applied to the substrate as a film by methods known to those skilled in the art, into a ready-to-use state, and therefore, in other words, into a state in which the substrate provided with the coating under consideration can be put to its intended use. In the context of the problems related to refinishing as well and that have been addressed in the context of the present invention, namely obtaining good sandability, precisely sandability and subsequent overcoatability, is of course a criterion for the intended use. The curing is achieved in particular by chemical reaction of the reactive functional groups of the epoxide resin (ER1) with the compounds of the aqueous dispersion (B). As a result of these crosslinking reactions and as a result of the parallel evaporation of any organic solvents and / or water present, a coating film is produced, i.e. a cured coating layer (cured coating). Although activation of the reaction is possible by means of thermal energy, in the case of the present invention, there is the above-mentioned advantage that high temperatures are not required.
[0106] Curing is effected, for example, at temperatures of 15 to 180°C, in particular 20 to 80°C, most preferably 20 to 65°C. These preferred relatively low curing temperatures result in particular from the fact that the coating compositions are preferably formulated as (2K) coating compositions, in which case specifically only low curing temperatures are required for thermal crosslinking. The duration of the curing may vary considerably in the individual cases, for example between 5 minutes and 16 hours, preferably 20 to 80 minutes. These preferred relatively short curing times result in particular from the fact that the compositions of the invention nevertheless require only relatively short curing times at relatively low temperatures in order to nevertheless have a sufficient hardness to allow the polishing of the cured coating. Curing operations which are quite particularly preferred in this respect are effected at 40 to 65°C for 20 to 80 minutes.
[0107] Preferred layer thicknesses resulting after curing in step (iii) are those customary in the vehicle industry, for example in the range of 5 to 200 micrometers, preferably 10 to 150 micrometers, more preferably 30 to 80 micrometers.
[0108] Optional step (iv): In optional step (iv) of the method of the present invention, the cured coating layer obtained after step (iii) is polished. This step is preferably carried out when a further coating layer is to be applied on top of the cured coating layer formed in step (iii). Polishing can be carried out by methods commonly known in the art, for example by using suitable sandpaper and polishing equipment.
[0109] Optional step (v): In optional step (v) of the method of the present invention, at least one further coating layer is applied and cured. Said step can be performed after step (iii) or after optional step (iv), preferably after optional step (iv). The at least one further coating layer is selected from a pigmented base coat layer and / or a clear coat layer.
[0110] The basecoat and / or clearcoat layers can be obtained by application of commercially known water-based or solvent-based basecoat and / or clearcoat compositions. If additional coating compositions are applied, a multi-coat paint system is formed.
[0111] As already indicated above, the coating composition of the present invention can be used particularly advantageously as a primer surfacer in the refinishing sector, in particular in automotive refinishing. Thus, in a particular embodiment of the present invention, the substrate is an already fully painted metal substrate, in particular painted with a multi-coat automotive paint system, in which the respective multi-layer coating has localized damage (defects). More particularly, these are automobile bodies or parts thereof, which thus have damage, such as stone chip damage. Thus, in the damaged areas, the original multi-layer coating has been at least partially peeled off by external action. The coating composition of the present invention is then used as a primer surfacer in the repair, i.e. refinishing, of these damaged areas. Generally, in refinishing operations, the application of the primer is carried out after cleaning and polishing of the damaged original coated substrate. This removes any poorly adhered and partially peeled areas of the original coating present, and / or corrosion products that have already formed and which expose the metal substrate locally, in particular. Therefore, it is a composite substrate surface with a wide range of different interfaces. One interface here is with the fully exposed metal substrate. Further interfaces and edges can be found in the areas between the cleaned and polished damaged areas and the areas surrounding these areas with intact original coating system. At all these interfaces, one and the same coating composition must ensure proper adhesion. Therefore, the composition of the present invention confers great advantages, because even in this damaged area, excellent adhesion, corrosion resistance and polishability are nevertheless obtained.
[0112] What has been said regarding the coating composition according to the invention and the kit-of-parts according to the invention applies mutatis mutandis with respect to the further preferred embodiments of the method according to the invention.
[0113] The coated substrate of the present invention: The result after step (iii) or optional step (v) of the method of the present invention is a coated substrate.
[0114] What has been said regarding the inventive coating composition, the inventive kit-of-parts and the inventive method applies mutatis mutandis with respect to the further preferred embodiments of the inventive coated substrate.
[0115] The present invention is specifically described by the following embodiments: Embodiment 1: 1. An aqueous coating composition comprising: a) at least one aqueous dispersion (A) of an epoxy resin (ER1), said epoxy resin (ER) having on average at least one epoxy group per molecule; b) at least one aqueous resin dispersion (B) comprising at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) in a proportion of 0.5 to 5% by weight, and a resin component (RC) having an NH equivalent of 150 to 400 g / mol; c) at least one aromatic compound (C) having at least one carboxylic acid group; Including, The resin component (RC) comprises at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups, the at least one polyfunctional organic amine (A2) being (i) at least one difunctional and / or multifunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol; (ii) at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1), and (iii) at least one compound XR, where X is a functional group that is reactive towards epoxy groups and R is an organic group that contains at least one polyoxyalkylene unit and does not contain further X groups; containing the reaction product of Aqueous coating compositions.
[0116] Embodiment 2: The aqueous coating composition according to embodiment 1, wherein the epoxy resin (ER1) is selected from glycidyl ethers of dihydric alcohols or phenols, novolax, glycidyl esters of carboxylic acids, or mixtures thereof, preferably glycidyl ethers of phenols, more preferably glycidyl ethers of bisphenol A.
[0117] Embodiment 3: The aqueous coating composition according to embodiment 1 or 2, wherein the epoxy resin (ER1) has an epoxy equivalent weight (EEW) of 100 to 400 g / eq, preferably 120 to 300 g / eq, more preferably 150 to 250 g / eq, and most preferably 185 to 210 g / eq, determined according to ASTM D1652-11(2019).
[0118] Embodiment 4: The epoxy resin (ER1) has a viscosity of 1,000 to 20,000 mPa, as determined in accordance with ASTM D2196-18. * s, preferably 1,500 to 15,000 mPa * s, most preferably 2,500 to 9,500 mPa * 4. The aqueous coating composition of any one of the preceding embodiments, having a viscosity at 25° C. of 100.degree.
[0119] Embodiment 5: An aqueous coating composition according to embodiment 1 or 2, wherein the epoxy resin (ER1) has an epoxy equivalent weight (EEW), determined according to VLN305, of 250 to 700 g / eq, preferably 300 to 600 g / eq, more preferably 350 to 550 g / eq, and most preferably 380 to 520 g / eq.
[0120] Embodiment 6: The epoxy resin (ER1) has a viscosity of 100 to 3,000 mPa, determined according to DIN EN ISO 3219: 1994-10. * s, preferably 150 to 2,500 mPa * s, more preferably 200 to 2,000 mPa * s, most preferably 250 to 1,400 mPa * s, 100s -16. The aqueous coating composition of any one of embodiments 1, 2 or 5, having a kinematic viscosity at 23° C.
[0121] Embodiment 7: An aqueous coating composition according to any one of embodiments 1 to 6, wherein at least one dispersion (A) of an epoxy resin (ER1) is present in a total amount of 5 to 50% by weight, preferably 10 to 40% by weight, more preferably 15 to 30% by weight and very preferably 18 to 25% by weight, in each case relative to the total weight of the aqueous coating composition.
[0122] Embodiment 8: An aqueous coating composition according to any one of embodiments 1 to 7, wherein the epoxy resin (ER1) is present in a total amount of 1 to 30% by weight, preferably 5 to 25% by weight, more preferably 8 to 20% by weight, very preferably 10 to 15% by weight, in each case relative to the total weight of the aqueous coating composition.
[0123] Embodiment 9: An aqueous coating composition according to any one of embodiments 1 to 8, wherein the at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) consists of at least 65 mol-%, preferably at least 75 mol-%, more preferably at least 90 mol-%, and very preferably 100 mol-% of amines consisting of amino groups and hydrocarbon groups.
[0124] Embodiment 10: The aqueous coating composition according to any one of embodiments 1 to 9, wherein the at least one difunctional and / or multifunctional monomeric primary and / or secondary amine (A1) is selected from difunctional monomeric primary and / or secondary amines, preferably difunctional monomeric primary amines, very preferably isophorone diamine and / or m-xylylene diamine.
[0125] Embodiment 11: An aqueous coating composition according to any one of the preceding embodiments, wherein the proportion of at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1), preferably isophoronediamine and / or m-xylenediamine, in the aqueous dispersion (B) is from 1 to 4.5% by weight, preferably from 1.5 to 4% by weight, relative to the total weight of the aqueous dispersion (B).
[0126] Embodiment 12: The aqueous coating composition according to any one of claims 1 to 11, wherein the resin component (RC) has an NH equivalent of 160 to 350 g / mol, preferably 170 to 250 g / mol.
[0127] Embodiment 13: The resin component (RC) further comprises at least one polyfunctional organic amine (A3) having primary and / or secondary amino groups, said polyfunctional organic amine (A3) being (iii) at least one difunctional and / or multifunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol; (iv) at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1); is the reaction product of 13. The aqueous coating composition according to any one of the preceding embodiments.
[0128] Embodiment 14: An aqueous coating composition according to any one of embodiments 1 to 13, wherein the resin component (RC) consists of at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups, and at least one polyfunctional organic amine (A3) having primary and / or secondary amino groups.
[0129] Embodiment 15: The aqueous coating composition according to any one of the preceding embodiments, wherein the at least one difunctional and / or multifunctional epoxy resin (ER2) has an average epoxy equivalent mass of less than 350 g / mol, preferably less than 300 g / mol, more preferably less than 250 g / mol, even more preferably less than 200 g / mol, very preferably between 160 and 200 g / mol, determined according to DIN EN ISO 3001:2019-08.
[0130] Embodiment 16: The aqueous coating composition according to any one of embodiments 1 to 15, wherein the at least one difunctional and / or multifunctional epoxy resin (ER2) has an average epoxy functionality of 1 to 5, preferably an epoxy functionality of 1 to 4, more preferably an epoxy functionality of 1 to 3, and most preferably an epoxy functionality of 2.
[0131] Embodiment 17: The aqueous coating composition according to any one of the preceding embodiments, wherein the at least one difunctional and / or polyfunctional epoxy resin (ER2) is selected from glycidyl ethers of dihydric alcohols or phenols, novolax, diglycidyl esters of carboxylic acids, or mixtures thereof, preferably glycidyl ethers of phenols, very preferably glycidyl ethers of bisphenol A.
[0132] Embodiment 18: The aqueous coating composition according to any one of embodiments 1 to 17, wherein X in at least one compound XR is selected from a primary or secondary amino group, a hydroxyl group, a carboxylic acid group or a thiol group, preferably a primary amino group.
[0133] Embodiment 19: The aqueous coating composition according to any one of the preceding embodiments, wherein at least one polyoxyalkylene unit in the organic group R in at least one compound XR is selected from polyethylene units, polypropylene units and mixed polyethylene / polypropylene units.
[0134] Embodiment 20: The aqueous coating composition according to any one of the preceding embodiments, wherein R in at least one compound XR consists of polyoxyalkylene units.
[0135] Embodiment 21: The aqueous coating composition according to any one of embodiments 1 to 20, wherein at least one compound XR is selected from primary polyoxyalkylene monoamines.
[0136] Embodiment 22: At least one compound XR has a mass average molecular weight M of 800 to 2,200 g / mol, determined by GPC coupled to light scattering. w 22. The aqueous coating composition of any one of the preceding embodiments, having the following structure:
[0137] Embodiment 23: The aqueous coating composition according to any one of embodiments 1 to 22, wherein the at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups consists of the reaction product of components (i), (ii) and (iii).
[0138] Embodiment 24: An aqueous coating composition according to any one of the preceding embodiments, wherein at least one dispersion (B) has a solids content of 25 to 45% by weight, based on the total weight of the dispersion and determined according to DIN EN ISO 3251:2018-07.
[0139] Embodiment 25: An aqueous coating composition according to any one of embodiments 1 to 24, wherein the resin component (RC) is present in a total amount of 10 to 30% by weight, preferably 15 to 25% by weight, based in each case on the solids content of the aqueous coating composition.
[0140] Embodiment 26: The aqueous coating composition of any one of embodiments 1 to 25, wherein the at least one aromatic compound (C) further comprises at least one hydroxy group.
[0141] Embodiment 27: The aqueous coating composition according to any one of the preceding embodiments, wherein the at least one aromatic compound (C) is selected from resorcinol, salicylic acid, p-hydroxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 3,4,5-trihydroxybenzoic acid, 2-hydroxy-3-naphthoic acid, 2-hydroxy-6-naphthoic acid, cresothinic acid, and mixtures thereof, preferably salicylic acid.
[0142] Embodiment 28: An aqueous coating composition according to any one of embodiments 1 to 27, wherein the at least one aromatic compound (C) is present in a total amount of 0.1 to 5% by weight, preferably 0.2 to 3% by weight, more preferably 0.3 to 1% by weight and very preferably 0.4 to 0.7% by weight, in each case relative to the total weight of the aqueous coating composition.
[0143] Embodiment 29: The aqueous coating composition according to any one of embodiments 1 to 28, wherein the molar ratio of the NH groups of the aqueous resin compound (RC) to the epoxy groups of the epoxy resin (ER1) is 0.74:1 to 0.95:1, preferably 0.9:1.
[0144] Embodiment 30: The aqueous coating composition of any one of embodiments 1 to 29, further comprising at least one pigment and / or filler.
[0145] Embodiment 31: The aqueous coating composition according to embodiment 30, wherein the at least one pigment is selected from (i) black pigments, such as carbon black, iron oxide pigments, manganese black and spinel black, preferably carbon black and iron oxide pigments, (ii) white pigments, such as titanium dioxide, zinc oxide, zinc sulfate and antimony trioxide, preferably titanium dioxide, and (iii) mixtures thereof.
[0146] Embodiment 32: The aqueous coating composition according to embodiment 30 or 31, wherein the at least one filler is selected from (i) carbonates, such as calcium carbonate or barium carbonate, (ii) sulfates, such as calcium sulfate and barium sulfate, (iii) silicates and layered silicates, such as talc, pyrophyllite, mica, kaolin, precipitated calcium silicate, aluminum silicate, calcium / aluminum silicate, sodium / aluminum silicate, and mullite, (iv) silicas, such as quartz, cristobalite, precipitated silica, and fumed silica, (v) metal oxides and hydroxides, such as aluminum hydroxide and magnesium hydroxide, and (vi) mixtures thereof.
[0147] Embodiment 33: An aqueous coating composition according to any one of embodiments 30 to 32, wherein at least one pigment, preferably at least one white and / or black pigment, is present in a total amount of 15 to 20% by weight, preferably 20% by weight, in each case relative to the solids content of the aqueous coating composition.
[0148] Embodiment 34: An aqueous coating composition according to any one of embodiments 30 to 33, wherein the at least one filler is present in a total amount of 30 to 50% by weight, preferably 30 to 40% by weight, based in each case on the solids content of the aqueous coating composition.
[0149] Embodiment 35: The aqueous coating composition of any one of embodiments 1 to 34, further comprising at least one additive.
[0150] Embodiment 36: The aqueous coating composition of embodiment 35, wherein the at least one additive is selected from light stabilizers, antioxidants, degassing agents, emulsifiers, slip additives, polymerization inhibitors, adhesion promoters, leveling agents, film-forming aids, thickeners, sag control agents (SCAs), corrosion inhibitors, and mixtures thereof.
[0151] Embodiment 37: An aqueous coating composition according to any one of the preceding embodiments, having a solids content of 70 to 85% by weight, based on the total weight of the aqueous coating composition and determined according to DIN EN ISO 3251:2018-07.
[0152] Embodiment 38: The aqueous coating composition of any one of embodiments 1 to 37, which is a surfacer or a primer surfacer.
[0153] Embodiment 39: A kit-of-parts comprising two separate components A) and B), said components A) and B) being A) at least one aqueous base varnish containing at least one aqueous dispersion (A) of an epoxy resin (ER1), said epoxy resin (ER) having on average at least one epoxy group per molecule; B) at least one aqueous curing agent component, at least one aqueous resin dispersion (B) comprising at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) in a proportion of 0.5 to 5% by weight, and a resin component (RC) having an NH equivalent of 150 to 400 g / mol, said resin component (RC) comprising at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups, said at least one polyfunctional organic amine (A2) being (i) at least one difunctional and / or multifunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol; (ii) at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A3), and (iii) at least one compound XR, where X is a functional group that is reactive towards epoxy groups and R is an organic group that contains at least one polyoxyalkylene unit and does not contain further X groups; An aqueous resin dispersion (B) containing the reaction product of at least one aromatic compound (C) having at least one carboxylic acid group; An aqueous hardener component containing It's a kit of parts.
[0154] Embodiment 40: A method for producing at least one coating layer on a substrate, comprising: i) applying an aqueous coating composition according to any one of embodiments 1 to 38 or a coating composition prepared from a kit-of-parts according to embodiment 39 to a substrate; ii) forming a coating film from the coating composition applied in step (i); and iii) curing the coating film formed in step (ii); iv) optionally polishing the cured coating layer obtained in step (iii); v) optionally applying at least one further coating layer and curing said coating layer; A method comprising:
[0155] Embodiment 41: The method of embodiment 40, wherein the substrate is selected from (i) metal substrates, such as unalloyed and alloyed steel and / or iron, zinc and aluminum substrates and corresponding alloys, (ii) plastic substrates, (iii) substrates comprising metal and plastic parts, and (iv) metal substrates coated with a multi-layer coating, preferably having defects.
[0156] Embodiment 42: The method according to embodiment 40 or 41, wherein the deposition in step (ii) is carried out by drying and / or evaporating the applied coating composition at 15-25° C. for 1-60 minutes.
[0157] Embodiment 43: The method according to any one of embodiments 40 to 42, wherein the curing in step (iii) is carried out at a temperature of 15 to 180°C, preferably 20 to 80°C, more preferably 20 to 65°C, for a period of 20 minutes to 16 hours, preferably 20 to 80 minutes.
[0158] Embodiment 44: The method of any one of embodiments 40 to 43, wherein the dry thickness of the resulting cured coating layer after step (iii) is from 5 to 200 μm, preferably from 10 to 150 μm, and most preferably from 30 to 80 μm.
[0159] Embodiment 45: The method of any one of embodiments 40 to 44, wherein the at least one further coating layer applied and cured in step (v) is selected from a pigmented basecoat layer and / or a clearcoat layer.
[0160] Embodiment 46: The method of any one of embodiments 40 to 45, used to repair a multi-layer paint system having at least one defect site.
[0161] Embodiment 47: A coated substrate produced by the method of any one of embodiments 40 to 46. EXAMPLES
[0162] The present invention will now be described in more detail through the use of examples, but the present invention is in no way limited to these examples. Furthermore, the terms "parts", "%" and "ratio" in the examples represent "parts by weight", "% by weight" and "ratio by weight", respectively, unless otherwise specified.
[0163] 1. Method of decision: 1.1 Solids content (solid, non-volatile fraction) Unless otherwise stated, the solids content (also referred to as the proportion of solids, solid state content, non-volatile proportion) was determined according to DIN EN ISO3251:2018-07 at 130° C., 60 min, starting mass of 1.0 g.
[0164] 1.2 Ratio of monomeric amine (A1) in aqueous dispersion (B) The proportion of the at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) in the aqueous dispersion (B) is determined by gas chromatography in accordance with DIN 51405:2004-01 as follows: Accurately weigh out 0.1 mg of approximately 100-500 mg of each aqueous dispersion (B) (depending on amine content) into a 5 mL snap bottle on an analytical balance. Accurately weigh out 0.1 mg of approximately 5% ISTD diethylene glycol dimethyl ether into the sample. Dilute the sample with 5 mL THF (if the sample does not dissolve in THF, a suitable solvent must be found by experimentation).
[0165] The samples thus prepared are analyzed on an Agilent 7890 gas chromatograph. Injection is performed by means of an autosampler. The samples are injected directly into the split injector of the gas chromatograph equipped with a flame ionization detector and separated both on a column with a polar phase (polyethylene glycol; 50 m fused silica capillary column with polyethylene glycol phase) and on a column with a non-polar phase (polydimethylsiloxane; 50 m fused silica capillary column with polydimethylsiloxane phase). Evaluation is performed by the ISTD% method.
[0166] Gas Chromatography Conditions: Oven program: 40°C (holding time 5 min) (3°C / min) → 100°C (10°C / min) → 230°C (holding time 5 min), Carrier gas: Hydrogen, Separation column: Agilent Innowax: Length 50 m, film thickness 0.2 μm, diameter 0.2 mm, pressure 1.0 bar HP-1, Length 50 m, film thickness 0.33 μm, diameter 0.2 mm, pressure 1.3 bar, Injector temperature: 250℃ (lower if necessary), Injector volume: 0.3μL (manual injection 0.3~0.6μL), Detector: Flame ionization detector, Detector temperature: 275℃, Divided flow: 15mL / min.
[0167] The amines (A1) are defined by their retention times on polar and non-polar columns. Unknown components should be subjected to GC / MS analysis.
[0168] The internal standard containing the detected amine is accurately weighed to 0.1 mg according to the approximate ratio in the sample on the analytical balance. The concentration of the amine in the overall calibration solution corresponds to the concentration of the amine in the sample prepared (the concentration of the amine is calculated by the GC analysis program). The calibration solution is then analyzed under the same conditions as the sample and the substance specific correction factor are identified.
[0169] The amine content of the samples is calculated by the ISTD % method with the aid of the GC analyzer program.
[0170] 1.3 Epoxy equivalent weight The epoxy equivalent mass was determined according to ASTM D1652-11 (2019) for epoxy resin (ER1) and according to DIN EN ISO3001:2019-08 for epoxy resin (ER2).
[0171] 1.4 Ratio of resin component (RC) in aqueous dispersion (B) The determination was carried out as described in point 1.1, except that each aqueous dispersion (B) was kept at 130° C. for 8 hours (instead of 60 minutes), to ensure that the amount of remaining non-volatile monomeric amine (A1) was negligible and that the mass obtained corresponded to the proportion of the resin component (RC) present in the aqueous dispersion (B).
[0172] 1.5 NH equivalent The NH equivalent weight of the resin component (RC) is determined according to the following two-step method:
[0173] Step 1: First of all, the NH equivalent of the resin mixture (I) present in the aqueous dispersion is determined. For this purpose, the different weight ratios of primary and secondary amino groups (each as % nitrogen) in the aqueous dispersion are determined using the method for aliphatic amines according to DIN EN ISO9702 (October 1998). The obtained weight ratios are then used to obtain the molar amount of NH groups in 100 g of aqueous dispersion using the following equation: n(NH) = (m(N from primary amino group) / (14g / mol)) * 2+m(N from secondary amino group) / (14g / mol) In this equation, "m" represents the mass ratio measured for primary and secondary amino groups.
[0174] Using the molar amount of NH groups and the mass of the sample (100 g), it is possible to obtain the NH equivalent of the sample (aqueous dispersion (B)), i.e. the mass of the sample in which 1 mole of NH functionality is present.
[0175] By determining the ratio of the sample resin mixture (I), the NH equivalent of the resin mixture (I) can then be calculated using the following equation: NH equivalent (resin mixture (I) = NH equivalent (sample) * Ratio (resin mixture in sample (I))
[0176] Step 2: The NH equivalent of the resin component (RC) is then calculated from the NH equivalent of the resin mixture (I) previously determined, the mass of the resin mixture (I) used in stage (B), the mass of the component (IIb) used in stage (B), and the molar amount of epoxy groups used in component (IIb) (determined by the mass of the component (IIb) used and the epoxy equivalent mass). This estimates the quantitative reaction of the epoxy groups of component (IIb) with the NH functionality of the resin mixture (I). The total mass of the resin component (RC) is obtained by adding the mass of the resin mixture (I) used and the mass of the component (IIb) used.
[0177] 1.6 Determination of abrasiveness The coated substrates prepared as described in point 3.1 below were stored at 20°C for 20 minutes, after which 09560 black control powder (from 3M) was applied to the coated surface and dry sanded using Excenter (FESTOOL LEX3), 5mm excentric stroke, and sandpaper from RODIM, Standard P400 type, until the black control powder was completely removed.
[0178] Abrasiveness was determined by sandpaper evaluation as follows: 0 → No clogging (very good abrasiveness) 1 → Minimal clogging (abrasiveness is still acceptable) 2 → Clogging, formation of small "nodules" (poor abrasiveness) 3 → Severe clogging, formation of "nodules" (spacers) (very poor abrasiveness)
[0179] The clogging of the coating material on the sandpaper is very immediately visible with the use of black control powder. No clogging means that the abraded removed material is obtained as a fine dust and therefore does not clog the sandpaper and lead to difficult to remove residues on the coating surface.
[0180] 1.7 Determination of bulging after constant climatic testing The panels produced as described in point 3.2 were stored for 10 days in a conditioning chamber under CH test conditions according to DIN EN ISO 6270-2:2005-09. Within 1 hour after removal from the conditioning chamber, the panels were then inspected for blistering according to DIN EN ISO 4628-2:2016-07.
[0181] The occurrence of blistering was assessed through a combination of two values as follows: The number of blisters was assessed by a quantitative number 1-5, with m1 representing very few blisters and m5 representing very many blisters.
[0182] The size of the blister was again rated by a size number from 1 to 5, with g1 representing a very small blister and g5 representing a very large blister.
[0183] Thus, the designation m0g0 denotes a coating system that has no blistering after condensation-water storage, whereas the designation m1g1 denotes a coating system that has very little small blistering.
[0184] 1.8 Determination of cross-cut adhesion after constant climatic testing The panels produced as described in point 3.2 were stored for 10 days in a conditioning chamber under CH test conditions according to DIN EN ISO 6270-2: 2005-09. Within 1 hour of removal from the conditioning chamber, the cross-cut adhesion was then determined according to DIN EN ISO 2409: 2013-06 (rating GT0 to GT5, GT0 = best score, GT5 = worst score).
[0185] 1.9 Determination of Stone Chip Resistance Stone chip resistance was determined according to ISO 20567-1 (Determination of stone chip resistance of coatings - part 1: multiple impact test with 2 bar pressure and 2 × 500 g grit (ISO 20567-1:2017)).
[0186] 1.10 Determining Dry Film Thickness The dry film thickness was determined according to DIN EN ISO 2808 of May 2007 using a Fischer Dualscope MP40, probe ED10.
[0187] 2. Preparation of Aqueous Dispersion (B) 2.1 Preparation of the aqueous dispersion (B1) An aqueous dispersion (B1) was prepared according to the following procedure: 683.00 g of Beckopox VEH 2849W (an aqueous dispersion of resin mixture (I) containing 27.5% by weight of monomeric amines (isophorone diamine and xylylene diamine) and 72.5% by weight of polyamines, further having an NH equivalent of 108 g / mol) and 1663.77 g of demineralized water were combined in a reaction vessel, continuously stirred and held at 95° C. for 1 hour. The mixture is then cooled to 70°C, and a mixture of 163.44g of bisphenol A diglycidyl ether based epoxy resin with an average epoxy equivalent mass of 186.5g / mol, 39.46g of polyalkylene polyether epoxide based on oxidized polypropylene with an average epoxy equivalent mass of 395g / mol, 81.96g of ethoxypropanol, 81.47g of methyl ethyl ketone and 81.72g of isobutanol is weighed out continuously with stirring over a period of 4 hours, and the mixture is kept at 70°C for another hour. The reaction product thus obtained is cooled to 45°C. The viscosity of the product is 150-250mPa at 25°C. * It is s.
[0188] In a subsequent process step, the solvents isobutanol and methyl ethyl ketone are removed from the product by distillation under reduced pressure. The resulting aqueous dispersion (B1) has a residual content of isobutanol and methyl ethyl ketone of <0.5% (gas chromatography).
[0189] The content of monomeric amine (A1) in the aqueous dispersion is 2.4% and the content of resin component (RC) is 31% by weight. The resin component further has an amine equivalent weight (NH equivalent weight) of 171 g / mol.
[0190] 2.2 Preparation of the aqueous dispersion (B2) 876.19 g of Beckopox VEH 2849W (aqueous dispersion of resin mixture (I), said resin mixture containing 27.5% by weight of monomeric amines (A1) (isophorone diamine and xylene diamine) and 72.5% by weight of polyfunctional organic amines (A2) and having an NH equivalent of 108 g / mol) and 2132.20 g of (demineralized) water were combined in a reaction vessel, continuously stirred and held at 95° C. for 1 hour. Then, a mixture of 233.41 g of bisphenol A diglycidyl ether based epoxy resin with an average epoxy equivalent weight of 186.5 g / mol, 117.30 g of ethoxypropanol, 117.30 g of methyl ethyl ketone, 117.30 g of isobutanol and 58.21 g of salicylic acid was added continuously with stirring over a period of 4 hours. The resulting dispersion is then cooled to 30° C. with stirring.
[0191] In a subsequent process step, the process solvents ethoxypropanol, methyl ethyl ketone and isobutanol are removed from the dispersion by distillation under reduced pressure.
[0192] The content of monomeric amine (A1) in the aqueous dispersion is 3% by weight (1.5% by weight of m-xylylenediamine and 1.5% by weight of isophoronediamine), and the content of resin component (RC) is 32% by weight. The resin component has an amine equivalent weight (NH equivalent weight) of 171 g / mol.
[0193] 3. Preparation of the aqueous coating composition With regard to the components and their amounts of the formulations described, the following should be borne in mind: Any reference to a commercial product is a reference to exactly that commercial product, regardless of the particular principal name chosen for the component.
[0194] The inventive aqueous coating compositions (I1) and (I2) and comparative aqueous coating compositions (C1) and (C2) were prepared by mixing the base varnish (A) with the curable component (B), adding additional water, and intimately mixing. The prepared coating compositions were applied onto a substrate and cured within 1 hour after their preparation. The components of the base varnish (A) and the curable component (B) are listed in Table 1.
[0195] [Table 1]
[0196] *The present invention 1) Water-based emulsion of liquid bisphenol A based epoxy resin, EEW=193-204g / eq (Blue Cube Germany) 2) Polymeric non-ionic dispersing additive, 50% solids content (Allnex Belgium SA) 3) Silicone-free, polymeric defoamer (Byk Chemie GmbH) 4) Hydrated magnesium silicate, D 50 =1.8μm(Elementis) 5) Rutile TiO2, inorganic coatings of zirconium and alumina, organic treatments (Huntsman) 6) Powdered iron oxide black pigment (Lanxess AG) 7) Precipitated barium sulfate, average particle size 1.7 μm (Solvay) 8) Organically modified basic zinc orthophosphate hydrate (Heubach GmbH) 9) Zinc-5-nitroisophthalate (Heubach GmbH) 10) Polyether-modified polydimethylsiloxane (BYK Chemie GmbH) 11) Contains 1.6% by weight of salicylic acid 12) The amine resin contains the reaction product of an amine having at least one primary and / or at least one secondary amino group, an adduct of a polyalkylene ether polyol, an epoxy resin and salicylic acid; NH equivalent: 138 g / mol, amount of salicylic acid relative to the solid content: 10-15% by weight (Allnex Belgium SA) 13) (Tris-2,4,6-dimethylaminoethylphenol) (Evonik Industries AG) 14) Amount of cure catalyst Salicylic Acid or Ancamine K54
[0197] 3. Production of coated substrates from coating compositions I1, I2, C1 and C2 3.1 Preparation of Coated Substrates C-I1, C-I2, C-C1 and C-C2 for Polishability Abrasivity was tested on the resulting coated substrates according to the following procedure: Cold rolled steel panels (60cm x 50cm) were used as substrates. They were pretreated / cleaned as follows: cleaned with 360-4 Glasurit metal cleaner, polished with P80, gold type from Mirka, cleaned again and polishing dust removed with 360-4 Glasurit. Ventilated for 15 minutes.
[0198] Each coating composition I1, I2, C1 and C2 was respectively applied on the substrate with a standard paint gun (e.g. SATA100 B F1.6mm RP at 2.0 bar) in a stirred, thin continuous spray operation, evaporated for 5 minutes, applied in a further complete spray operation, evaporated for 5 minutes and then cured for 35 minutes at a temperature of 60° C. The dry film thickness was in each case between 60 μm and 80 μm.
[0199] Prior to the determination of the sandability described in point 1.6, the manufactured panels were stored at 23° C. for 20 minutes (if cured at 60° C.) or for 16 hours (if cured at 23° C.).
[0200] 3.2 Preparation of coated substrates C-I1, C-I2, C-C1 and C-C2 for stone chip resistance and moisture resistance tests First, the substrates were cleaned according to their material type: metal substrates were cleaned with Glasurit Sheet Metal Cleaner 360-4, plastic parts were cleaned with Glasurit Universal Cleaner for Plastics 541-30, and old paintwork or new factory primed parts were cleaned with Glasurit KH Remover for Silicone and Tar 541-5.
[0201] The substrate is then polished depending on its material type: layered steel with P80, galvanized sheet steel with a polishing pad, aluminum with P150, plastic and old paintwork or new parts primed at the factory with a polishing pad. The polishing dust is then removed using the cleaning agent mentioned above. After dry rubbing, application of the respective aqueous primer surfacer composition I1, I2, C1 or C2 is carried out. For this purpose, the respective composition is applied in two full coats without intermediate evaporation times using a flow cup gun (SATA BF100 RP1.6 at 2.0 bar) so that resulting dry film thicknesses of 60 μm and 80 μm are obtained. After application of the second coat, the resulting primer surfacer layer is cured at 60 ° C for 40 minutes.
[0202] After the coated substrate is cooled, the primer surfacer layer is polished. For this purpose, control black (09560 Black Fa.3M) is applied to the coated surface, and the surface is polished using an eccentric polisher (LEX3 from Festool), a stroke of 5 mm, and sandpaper P400 (standard type from RODIM). The polished surface is then cleaned with Glasurit Cleaner 700-1, after which a basecoat layer is applied. For this purpose, a commercially available water-based basecoat composition (Glasurit90-1250 Deep Black, available from BASF Coatings GmbH) is applied with a paint spray gun (SATA5000 HVLP1.3, at 2.0 bar) with an evaporation time of approximately 5 minutes, so that the resulting dry film thickness is between 10 μm and 15 μm in two cover coats and one effect coat.
[0203] Subsequently, a commercial solvent-based clear coating composition (Glasurit HS Clear Coat High Gloss VOC 923-630, available from BASF Coatings GmbH) is applied using a paint spray gun (SATA5000 RP1.3 at 2.0 bar) in two coats at a dry film thickness of 50-60 μm with an intermediate evaporation time of 3 minutes. Final curing of the applied base coat and clear coat layers is carried out at 60° C. for 30 minutes.
[0204] The fabricated panels were aged at 23° C. for at least 10 days before humidity testing and stone chip resistance were performed.
[0205] 4.Results The results obtained for abrasion, blistering, cross-cut adhesion and stone chip resistance of coated panels prepared as described above are listed in Table 2.
[0206] [Table 2]
[0207] 5. Review of Results The coated panels produced using the coating compositions (I1) and (I2) of the present invention exhibited excellent abrasion and high stone chip resistance without adversely affecting the excellent blister stability and cross-cut adhesion of the multi-layer coatings produced using said coating compositions of the present invention as primer surfacers. The excellent properties achieved are due to the combination of the aqueous dispersion (B) containing a specific resin component (RC) and salicylic acid as a curing catalyst. Surprisingly, comparable results are obtained when salicylic acid is not added as a separate compound during the preparation of the coating composition (coating composition I1), but is incorporated by the aqueous dispersion (B2) (coating composition I2). As salicylic acid is known to catalyze the reaction between epoxy and amino groups, the use of salicylic acid during the preparation of the aqueous dispersion (B) allows for the efficient preparation of the aqueous dispersion (B) without the use of additional catalysts, without adversely affecting the catalysis during the curing of the coating composition.
[0208] In contrast, the use of the known curing catalyst Ancamine K54 in combination with the aqueous dispersion (B) as a crosslinker (Comparative Coating Composition C1) results in coated panels with significantly reduced blister stability and crosscut adhesion under humid conditions compared to panels coated with the inventive coating compositions (I1) or (I2) containing salicylic acid as the curing catalyst.
[0209] The use of an aqueous dispersion of curing agent without a specific resin component (RC) (Comparative Coating Composition C2) in combination with salicylic acid as a curing catalyst also results in significantly reduced blister stability, cross-cut adhesion and stone chip resistance.
[0210] Therefore, excellent abrasion and high stone chip resistance without adversely affecting the high blister stability and cross-cut adhesion of the multi-layer coating can only be obtained if the primer surfacer contains a combination of an aqueous dispersion (B) with a specific resin component (RC) and salicylic acid as curing catalyst.
Claims
1. 1. An aqueous coating composition comprising: a) at least one aqueous dispersion (A) of an epoxy resin (ER1), said epoxy resin (ER1) having on average at least one epoxy group per molecule; b) at least one aqueous resin dispersion (B) comprising at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) in a proportion of 0.5 to 5% by weight, and a resin component (RC) having an NH equivalent of 150 to 400 g / mol, c) at least one aromatic compound (C) having at least one carboxylic acid group; Including, The resin component (RC) comprises at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups, and the at least one polyfunctional organic amine (A2) is (i) at least one difunctional and / or multifunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol; (ii) at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1), and (iii) at least one compound X-R, where X is a functional group that is reactive towards epoxy groups and R is an organic group that contains at least one polyoxyalkylene unit and does not contain any further X groups; comprising the reaction product of the at least one aromatic compound (C) having at least one carboxylic acid group is selected from resorcinol, salicylic acid, p-hydroxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2-hydroxy-3-naphthoic acid, 3,4,5-trihydroxybenzoic acid, 2-hydroxy-6-naphthoic acid, cresotinic acid, and mixtures thereof; said at least one compound X-R is selected from primary polyoxyalkylene monoamines; Aqueous coating compositions.
2. 2. The aqueous coating composition according to claim 1, wherein the epoxy resin (ER1) is present in a total amount of 1 to 30% by weight, based in each case on the total weight of the aqueous coating composition.
3. 3. The aqueous coating composition according to claim 1, wherein the at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) consists of at least 65 mol-% of amines consisting of amino groups and hydrocarbon groups.
4. 4. The aqueous coating composition according to claim 1, wherein the at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) is selected from difunctional monomeric primary and / or secondary amines.
5. 5. Aqueous coating composition according to claim 1, wherein the proportion of at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) in the aqueous dispersion is from 1 to 4.5% by weight, relative to the total weight of the aqueous dispersion (B).
6. 6. The aqueous coating composition according to claim 1, wherein the resin component (RC) has an NH equivalent of 160 to 350 g / mol.
7. 7. The aqueous coating composition according to claim 1, wherein the at least one di- and / or multi-functional epoxy resin (ER2) is selected from glycidyl ethers of dihydric alcohols or phenols, novolaks, diglycidyl esters of carboxylic acids, or mixtures thereof.
8. 8. The aqueous coating composition according to claim 1, wherein the resin component (RC) is present in a total amount of 10 to 30% by weight, based in each case on the solids content of the aqueous coating composition.
9. The aqueous coating composition of claim 1, wherein the at least one aromatic compound (C) is salicylic acid.
10. 10. The aqueous coating composition according to claim 1, wherein the at least one aromatic compound (C) is present in a total amount of 0.1 to 5% by weight, based in each case on the total weight of the aqueous coating composition.
11. The aqueous coating composition of claim 1 , wherein the coating composition is a surfacer or a primer surfacer.
12. A kit-of-parts comprising two separate components A) and B), said components A) and B) being A) at least one aqueous base varnish containing at least one aqueous dispersion (A) of an epoxy resin (ER1), said epoxy resin (ER1) having on average at least one epoxy group per molecule; B) at least one aqueous curing agent component; at least one aqueous resin dispersion (B) comprising at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A1) in a proportion of 0.5 to 5% by weight, and a resin component (RC) having an NH equivalent of 150 to 400 g / mol, said resin component (RC) comprising at least one polyfunctional organic amine (A2) having primary and / or secondary amino groups, said at least one polyfunctional organic amine (A2) being (i) at least one difunctional and / or multifunctional epoxy resin (ER2) having an average epoxy equivalent mass of less than 400 g / mol; (ii) at least one difunctional and / or polyfunctional monomeric primary and / or secondary amine (A3), and (iii) at least one compound X-R, where X is a functional group that is reactive towards epoxy groups and R is an organic group that contains at least one polyoxyalkylene unit and does not contain any further X groups; An aqueous resin dispersion (B) containing a reaction product of at least one aromatic compound (C) having at least one carboxylic acid group; Contains the at least one aromatic compound (C) having at least one carboxylic acid group is selected from resorcinol, salicylic acid, p-hydroxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2-hydroxy-3-naphthoic acid, 3,4,5-trihydroxybenzoic acid, 2-hydroxy-6-naphthoic acid, cresotinic acid, and mixtures thereof; said at least one compound X-R is selected from primary polyoxyalkylene monoamines; Aqueous hardener component and Includes a kit of parts.
13. 1. A method for producing at least one coating layer on a substrate, comprising: i) applying an aqueous coating composition according to any one of claims 1 to 11 or a coating composition made from a kit-of-parts according to claim 12 to a substrate; ii) forming a coating film from the coating composition applied in step (i); and iii) curing the coating film formed in step (ii); iv) optionally polishing the cured coating layer obtained in step (iii); v) optionally applying at least one further coating layer and curing said coating layer; A method comprising:
14. 14. A coated substrate produced by the method of claim 13.
Citation Information
Patent Citations
Corrosion-resistant coating composition for steel and steel applied therewith
JP2002212495A
Water-based paints based on epoxy resins
JP2010535259A
Aqueous coating material
JP2019173008A
Water-borne paints based on epoxy resins
WO2009016162A1
Amine compound, amine composition, and epoxy resin curing agent