Method for manufacturing the negative electrode
The method of prelithiating expanded natural graphite negative electrodes by electrochemical charging compensates for its inherent inefficiencies, improving initial efficiency and life characteristics through reduced irreversible capacity and low lithium ion diffusion resistance.
Patent Information
- Application Number
- JP2023512765
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-26
- Filing Date
- 2021-10-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-25
AI Technical Summary
Expanded natural graphite, used as a negative electrode active material in lithium secondary batteries, exhibits lower initial efficiency and poorer life characteristics due to its wide crystal lattice spacing, leading to increased irreversible capacity and electrolyte side reactions.
A manufacturing method involving impregnation of a negative electrode structure with a prelithiation solution and electrochemical charging of 10% to 20% of its charge capacity to prelithiate the expanded natural graphite, compensating for irreversible capacity and improving lithium ion diffusion.
The method enhances the initial efficiency and life characteristics of expanded natural graphite-based negative electrodes by reducing irreversible capacity and maintaining low lithium ion diffusion resistance, resulting in superior output and long-term performance.
Smart Images

Figure 0007580847000001
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0139477, filed on October 26, 2020, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a method for producing a negative electrode. [Background technology]
[0003] Recently, with the rapid spread of electronic devices using batteries, such as mobile phones, notebook computers, and electric vehicles, the demand for secondary batteries that are small, lightweight, and have a relatively high capacity is rapidly increasing. In particular, lithium secondary batteries are lightweight and have high energy density, and are in the spotlight as a driving power source for portable devices. Therefore, research and development efforts are being actively made to improve the performance of lithium secondary batteries.
[0004] The lithium secondary battery generally includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, an electrolyte, an organic solvent, etc. The positive electrode and the negative electrode may have an active material layer including a positive electrode active material or a negative electrode active material formed on a current collector. The positive electrode generally includes LiCoO 2 , LiMn 2 O 4 As a positive electrode active material, a lithium-containing metal oxide such as a lithium-containing metal oxide such as a lithium-containing carbon-based active material or a silicon-based active material is used as a negative electrode active material.
[0005] Meanwhile, among the negative electrode active materials, natural graphite, expanded natural graphite, artificial graphite, etc. are known as carbon-based active materials. Among them, expanded natural graphite is a type of carbon-based active material in which the spacing between crystal lattice planes in natural graphite is expanded by artificially treating natural graphite with an acid or base. The expanded natural graphite has an advantage that the spacing between crystal lattice planes is wide, making it easy to insert and extract lithium ions, and thus maximizing output characteristics. However, such wide spacing between crystal lattice planes causes an increase in specific surface area and an increase in irreversible capacity, resulting in very low initial efficiency and poor life characteristics.
[0006] Therefore, in a negative electrode using expanded natural graphite, there is an urgent need to develop a method for manufacturing a negative electrode that can improve the initial efficiency and life characteristics while exhibiting the output characteristics of expanded natural graphite at an excellent level.
[0007] Korean Patent Publication No. 10-0291067 discloses a method for prelithiating a carbon electrode and a method for manufacturing a lithium secondary battery using the same. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent No. 10-0291067 Summary of the Invention [Problem to be solved by the invention]
[0009] One object of the present invention is to relate to a method for producing a negative electrode, which can exhibit the output characteristics of expanded natural graphite and improve initial efficiency and life characteristics by electrochemically charging a negative electrode structure containing expanded natural graphite with a specific charge amount to prelithiate it. [Means for solving the problem]
[0010] The present invention provides a method for producing a negative electrode, the method including the steps of producing a negative electrode structure containing expanded natural graphite, impregnating the negative electrode structure with a prelithiation solution, and prelithiating the impregnated negative electrode structure by electrochemically charging 10% to 20% of the charge capacity of the negative electrode structure. Effect of the Invention
[0011] According to the method for producing an anode of the present invention, an anode structure containing expanded natural graphite is impregnated with a prelithiation solution, and then the impregnated anode structure is electrochemically charged at a specific charge amount. The anode produced by electrochemically charging and prelithiation at the charge amount within the above range can exhibit excellent output characteristics, initial efficiency, and life characteristics. In particular, the expanded natural graphite is generally known to have a low initial efficiency and poor life characteristics compared to general natural graphite, but the expanded natural graphite-containing anode electrochemically charged at the above charge amount can improve the initial efficiency by compensating the irreversible capacity to a preferred level, and can improve the life characteristics to a significantly higher level than general natural graphite due to the low lithium ion diffusion resistance caused by the wide spacing of the crystal lattice planes of the expanded natural graphite. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0013] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless it has a clearly different meaning in the context.
[0014] In this specification, the terms "including," "comprising," or "having" are intended to indicate the presence of implemented features, numerals, steps, components, or combinations thereof, and should be understood as not precluding the presence or additional possibility of one or more other features, numerals, steps, components, or combinations thereof.
[0015] In this specification, the average particle size (D 50 The average particle size (D) can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. 50 ) can be measured, for example, by using a laser diffraction method. The laser diffraction method generally allows measurement of particle sizes from the submicron range to about several mm, and can provide results with high reproducibility and high resolution.
[0016] The present invention will be specifically described below.
[0017] <Method of manufacturing the negative electrode> The present invention relates to a method for producing a negative electrode, and more particularly to a method for producing a negative electrode for a lithium secondary battery.
[0018] The method for producing a negative electrode of the present invention includes the steps of producing a negative electrode structure containing expanded natural graphite, impregnating the negative electrode structure with a prelithiation solution, and electrochemically charging the impregnated negative electrode structure to 10% to 20% of the charge capacity of the negative electrode structure to prelithiate the negative electrode structure.
[0019] According to the method for producing an anode of the present invention, an anode structure containing expanded natural graphite is impregnated with a prelithiation solution, and then the impregnated anode structure is electrochemically charged at a specific charge amount. The anode produced by electrochemically charging and prelithiation at the charge amount within the range can exhibit excellent output characteristics, initial efficiency, and life characteristics. In particular, the expanded natural graphite is generally known to have a low initial efficiency and poor life characteristics compared to general natural graphite, but the expanded natural graphite-containing anode electrochemically charged at the above charge amount can improve initial efficiency by compensating the irreversible capacity to a preferred level, and can improve life characteristics to a significant level compared to general natural graphite due to the low lithium ion diffusion resistance caused by the wide spacing of the crystal lattice planes of the expanded natural graphite.
[0020] The method of making an anode of the present invention includes the steps of producing an anode structure that includes expanded natural graphite.
[0021] The expanded natural graphite may be included in the negative electrode structure as a negative electrode active material.
[0022] The expanded natural graphite may be obtained by chemically bonding carbon atoms with an acid or base treated with natural graphite and then thermally decomposing the resulting mixture to expand the spacing of the crystal lattice planes of the natural graphite. Generally, the expanded natural graphite has a wider spacing between the crystal lattice planes than general natural graphite, and thus has superior output characteristics compared to general natural graphite, but has a large irreversible capacity and a low initial efficiency and life characteristics due to an increase in electrolyte side reactions caused by a large specific surface area. However, as described below, expanded natural graphite that has been prelithiated by electrochemically charging at a specific charge amount can exhibit superior output characteristics, and has a high initial efficiency due to a sufficient compensation of the irreversible capacity, and has a low lithium ion diffusion resistance due to smooth lithium ion diffusion due to the wide spacing between the crystal lattice planes, and thus exhibits a life characteristics superior to that of general natural graphite.
[0023] The lattice spacing d002 of the (002) plane of the expanded natural graphite measured by XRD can be 0.3370 nm to 0.3410 nm, specifically 0.3390 nm to 0.3405 nm. By having a lattice spacing d002 in the above range, the expanded natural graphite can have excellent output characteristics because lithium ions can easily enter and exit or diffuse therein, compared to general natural graphite having a relatively small d002. In addition, according to the method for producing a negative electrode of the present invention, the irreversible capacity of the expanded natural graphite is compensated for by a prelithiation process described below, and the expanded natural graphite having a lattice spacing d002 in the above range has low diffusion resistance of lithium ions, so that it can have excellent life characteristics even during repeated charging and discharging.
[0024] The expanded natural graphite may have a crystallite size Lc in the c-axis direction as measured by X-ray diffraction (XRD) of 10 nm to 24 nm, specifically 16 nm to 21 nm. By having a crystallite size Lc in the above range, the expanded natural graphite can have excellent output characteristics.
[0025] The BET specific surface area of the expanded natural graphite is 4m 2 / g~8m 2 / g, specifically 4.5m 2 / g~6.5m 2 / g. When the specific surface area is within the above range, the expansion natural graphite can easily absorb and release lithium ions, thereby improving output characteristics. In addition, according to the method for producing a negative electrode of the present invention, the irreversible capacity of the expanded natural graphite is compensated for by a prelithiation process described below, and the expanded natural graphite having a specific surface area within the above range has low diffusion resistance of lithium ions, so that it can have excellent life characteristics even during repeated charging and discharging.
[0026] The average particle size of the expanded natural graphite (D 50 ) may be 8 μm to 20 μm, preferably 12 μm to 18 μm, in order to structurally stabilize the negative electrode active material during charging and discharging.
[0027] The expanded natural graphite may contain oxygen (O) in an amount of 800 ppm to 3,000 ppm, specifically 1,000 ppm to 2,800 ppm, and more specifically 1,500 ppm to 2,500 ppm, based on the weight of the expanded natural graphite. The expanded natural graphite is treated with an acid or base in the manufacturing process, whereby oxygen-containing functional groups such as hydroxyl groups (-OH) are formed on the surface and / or inside of the expanded natural graphite, resulting in a higher oxygen content than general natural graphite.
[0028] The oxygen content of the expanded natural graphite can be measured by an ONH analyzer or an XPS analyzer.
[0029] The negative electrode structure may include a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer may include the expanded natural graphite.
[0030] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity. Specifically, the negative electrode current collector can include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and aluminum-cadmium alloy, and preferably copper.
[0031] The negative electrode current collector may usually have a thickness of 3 to 500 μm.
[0032] The negative electrode current collector may have a surface with fine projections and recesses to strengthen the binding force of the negative electrode active material. For example, the negative electrode current collector may be used in various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam, a nonwoven fabric, etc.
[0033] The negative electrode active material layer may contain the above-mentioned expanded natural graphite as a negative electrode active material.
[0034] In order to fully utilize the excellent output characteristics and capacity characteristics of expanded natural graphite, the expanded natural graphite can be contained in the negative electrode active material layer in an amount of 85% by weight to 99% by weight, preferably 90% by weight to 98% by weight.
[0035] The negative electrode active material layer may further contain, in addition to the expanded natural graphite, at least one additive selected from the group consisting of a binder, a conductive material, and a thickener.
[0036] The binder is used to improve the adhesive strength between the negative electrode active material layer and the negative electrode current collector to improve the performance of the battery, and may include, for example, at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber, preferably styrene-butadiene rubber.
[0037] The binder may be included in the negative electrode active material layer in an amount of 0.5 wt % to 10 wt %, preferably 1 wt % to 5 wt %, and within this range, sufficient adhesive strength of the active material can be exhibited, and the solid content of the active material can be increased to improve the capacity of the negative electrode.
[0038] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material that can be used include graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0039] In order to exhibit sufficient conductivity, the conductive material may be contained in the negative electrode active material layer in an amount of 0.5% by weight to 10% by weight, and preferably 1% by weight to 5% by weight.
[0040] The thickener is added for smooth dispersion of expanded natural graphite during preparation of a negative electrode slurry for forming a negative electrode active material layer, and may include, for example, carboxymethyl cellulose (CMC). The thickener may be included in the negative electrode active material layer in an amount of 0.1 wt % to 5 wt %.
[0041] The negative electrode active material layer may have a thickness of 10 μm to 100 μm, and preferably 20 μm to 80 μm.
[0042] The negative electrode structure may be manufactured by coating a negative electrode slurry prepared by adding the expanded natural graphite, and optionally a binder and / or a conductive material to a solvent for forming a negative electrode slurry (e.g., water) onto the negative electrode current collector, followed by rolling and drying.
[0043] The method of making the negative electrode of the present invention includes the step of immersing the negative electrode structure in a prelithiation solution.
[0044] The impregnation of the negative electrode structure is performed in order to allow the negative electrode structure to be sufficiently wetted with a prelithiation solution so that smooth prelithiation can be performed during electrochemical charging, which will be described later.
[0045] The prelithiation solution can include a lithium salt and an organic solvent.
[0046] The organic solvent is not particularly limited as long as it serves as a medium for carrying out an electrochemical reaction and transferring ions. Specifically, the organic solvent may be an ester-based solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether-based solvent such as dibutyl ether or tetrahydrofuran; a ketone-based solvent such as cyclohexanone; an aromatic hydrocarbon-based solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvent that can be used include carbonate-based solvents such as ethyl alcohol and isopropyl alcohol; alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a C2-C20 linear, branched or cyclic hydrocarbon group that may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; and sulfolanes. Among these, carbonate-based solvents are preferred in terms of improving electrochemical stability, and more specifically, ethyl methyl carbonate (EMC), ethylene carbonate (EC), and the like are more preferred.
[0047] The lithium salt is LiPF 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlO 4 , LiAlCl 4 , LiCF3 SO 3 , LiC 4 F 9 SO 3 , LiN(C 2 F 5 SO 3 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiN(CF 3 SO 2 ) 2 , LiCl, LiI, or LiB(C 2 O 4 ) 2 and preferably LiPF 6 may include.
[0048] The concentration of the lithium salt may be 0.1M to 3M, preferably 0.5M to 1.5M, in the prelithiation solution. When the concentration is within the above range, the lithium salt can be sufficiently dissolved so that lithium ions can be smoothly inserted into the active material, which is preferable.
[0049] The prelithiation solution may further contain at least one additive selected from the group consisting of fluoroethylene carbonate (FEC), vinylene carbonate (VC), polystyrene (PS), succinonitrile, ethylene glycol bis(propionitrile) ether, and lithium bis(fluorosulfonyl)imide (LiFSI), preferably an additive containing fluoroethylene carbonate, in order to stabilize the surface of the negative electrode active material during prelithiation and to facilitate smooth prelithiation.
[0050] The additive may be contained in the prelithiation solution in an amount of 0.1 wt % to 15 wt %, preferably 0.5 wt % to 5 wt %, based on the total weight of the prelithiation solution, in order to stabilize the surface of the negative electrode active material and facilitate smooth prelithiation.
[0051] The impregnation of the negative electrode structure may be performed for 0.5 to 15 hours, preferably 1 to 5 hours, in order to ensure stable and uniform prelithiation.
[0052] The method for producing a negative electrode of the present invention includes a step of electrochemically charging the impregnated negative electrode structure to 10% to 20% of the charge capacity of the negative electrode structure to prelithiate the negative electrode structure.
[0053] By prelithiating the impregnated negative electrode structure, lithium ions in the prelithiating solution are inserted into the interior and / or surface of the expanded natural graphite, thereby compensating for the irreversible capacity of the expanded natural graphite, and a solid electrolyte interface layer (SEI layer) can be formed in advance on the expanded natural graphite.
[0054] The prelithiation is performed by electrochemically charging the impregnated negative electrode structure. As a general prelithiation method, a method in which lithium metal is directly contacted with a negative electrode to insert lithium of lithium metal as a negative electrode, a method in which lithium metal is used as a counter electrode to electrochemically charge a negative electrode structure, etc. are known, but as described later, in order to simultaneously improve the initial efficiency, output characteristics, and life characteristics of the impregnated negative electrode structure, the charge amount during electrochemical charging is important, and it is preferable to use an electrochemical charging method that can easily control the lithium charge amount.
[0055] In the prelithiation step, the impregnated negative electrode structure is electrochemically charged to 10% to 20% of the charge capacity of the negative electrode structure. By electrochemically charging the negative electrode structure at the above charge ratio, the irreversible capacity of the expanded natural graphite is sufficiently compensated for, and initial efficiency can be improved. The high output characteristics of the expanded natural graphite are smoothly exhibited, and the lithium ion diffusion resistance is low due to the wide spacing of the crystal lattice planes, making it possible to exhibit superior life characteristics compared to general natural graphite. This not only eliminates the disadvantages of expanded natural graphite, which is generally known to have lower life characteristics and initial efficiency compared to general natural graphite, but also makes it possible to exhibit significantly improved output characteristics and life characteristics compared to general natural graphite.
[0056] If the impregnated negative electrode structure is electrochemically charged at less than 10% of the charge capacity of the negative electrode structure, the compensation for the irreversible capacity of the expanded natural graphite is small, making it difficult to improve the initial efficiency, and therefore difficult to improve the long-term cycle characteristics.If the impregnated negative electrode structure is electrochemically charged at more than 20% of the charge capacity of the negative electrode structure, the insertion of excess lithium increases resistance and reduces output, and such output reduction and resistance increase accumulate, which may degrade the long-term cycle characteristics.
[0057] Preferably, the impregnated negative electrode structure can be electrochemically charged to 13% to 16% of the charging capacity of the negative electrode structure, and when electrochemically charged in this range, the effect of simultaneously improving the initial efficiency, output characteristics, and life characteristics of the negative electrode can be maximized.
[0058] The electrochemical charging may be performed using lithium metal as a counter electrode disposed in the prelithiation solution and spaced apart from the impregnated negative electrode structure. The lithium metal used in the counter electrode is disposed in the prelithiation solution so as to be spaced apart from the negative electrode structure, thereby preventing an electrode short circuit phenomenon that may occur due to direct contact between the lithium metal and the negative electrode structure during the electrochemical charging.
[0059] The electrochemical charging may be performed using an electrochemical charger / discharger. Specifically, the electrochemical charger / discharger may be WOCS3000s (manufactured by Wonatech Co., Ltd.).
[0060] The electrochemical charging is at 0.1 mA / cm 2 ~3mA / cm 2 current density of 0.3 mA / cm 2 ~2mA / cm 2 When electrochemical charging is performed within this range, stable and uniform prelithiation can be performed on the negative electrode active material.
[0061] The electrochemical charging may be carried out at 10°C to 70°C, preferably 20°C to 40°C. At this temperature, the negative electrode structure can be stably charged and discharged to form a uniform SEI layer, which is preferable in terms of preventing damage to the negative electrode structure due to electrochemical charging.
[0062] The prelithiated negative electrode structure can be used as a negative electrode for a secondary battery, more specifically, a negative electrode for a lithium secondary battery, and can smoothly exhibit the excellent output characteristics of expanded natural graphite and have high levels of initial efficiency and life characteristics.
[0063] The negative electrode produced by the production method of the present invention can be preferably applied to secondary batteries, specifically lithium secondary batteries.
[0064] The secondary battery may include a negative electrode manufactured by the above-mentioned manufacturing method, a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte. As the positive electrode, the separator, and the electrolyte, those used in general lithium secondary batteries may be used without any restrictions.
[0065] The secondary battery is useful in the fields of portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0066] In addition, the secondary battery may be applied to a battery module including the secondary battery as a unit cell, or a battery pack including the battery module.
[0067] The battery module or the battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0068] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.
[0069] Working Example Example 1: Preparation of negative electrode <Manufacture of negative electrode structure> Expanded natural graphite (average particle size (D 50 The expanded natural graphite had a (002) plane spacing d002 of 0.3402 nm in XRD measurement, a crystallite size Lc in the c-axis direction of 17.73 nm in XRD measurement, and a BET specific surface area of 5.4 m 2 / g, and the oxygen (O) content measured with an ONH analyzer (manufacturer: LECO, instrument name: ONH 836) was 2,100 ppm based on the weight of the expanded natural graphite.
[0070] The negative electrode active material, carbon black as a conductive material, SBR (styrene-butylene rubber) as a binder, and carboxymethyl cellulose as a thickener were added to water in a weight ratio of 96.0:1.0:1.3:1.1 to prepare a negative electrode slurry.
[0071] The negative electrode slurry was coated on one side of a copper negative electrode current collector (thickness: 15 μm), roll pressed, and dried in a vacuum oven at 130° C. for 10 hours to form a negative electrode active material layer (thickness: 111 μm) on one side of the copper negative electrode current collector. 2 In this case, the loading amount of the negative electrode active material layer was 3.61 mAh / cm 2 It was made to be like this.
[0072] <Impregnation of negative electrode structure> The prepared negative electrode structure was immersed in a prelithiation solution for 3 hours.
[0073] The prelithiation solution was prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 30:70 in an organic solvent and dissolving LiPF as a lithium salt. 6 was added at a concentration of 1 M, and fluoroethylene carbonate (FEC) was used as an additive at 2 wt % based on the total weight of the prelithiation solution.
[0074] <Prelithiation process> A lithium metal counter electrode was immersed in the prelithiation solution at a predetermined distance from the negative electrode structure.
[0075] Next, the negative electrode structure was subjected to a prelithiation process. The prelithiation process was carried out at 25° C. Specifically, the negative electrode structure was subjected to a prelithiation process at 0.5 mA / cm 2 The negative electrode structure was electrochemically charged at a current density of 15.7% of the charge capacity of the negative electrode structure.
[0076] The negative electrode structure was washed with an ethyl methyl carbonate solvent and dried at room temperature to obtain the negative electrode of Example 1.
[0077] Example 2: Preparation of the negative electrode The negative electrode of Example 2 was produced in the same manner as in Example 1, except that the negative electrode structure was electrochemically charged to a charge amount of 17.5% of the charge capacity of the negative electrode structure.
[0078] Example 3: Preparation of negative electrode The negative electrode of Example 3 was produced in the same manner as in Example 1, except that the negative electrode structure was electrochemically charged to a charge amount of 11.4% of the charge capacity of the negative electrode structure.
[0079] Comparative Example 1: Production of negative electrode The negative electrode structure in Example 1 that was not subjected to the impregnation and prelithiation steps was used as the negative electrode of Comparative Example 1.
[0080] Comparative Example 2: Production of negative electrode The negative electrode active material is not expanded natural graphite, but ordinary natural graphite (D 50 The negative electrode of Comparative Example 2 was produced in the same manner as in Example 1, except that a 0.1% Cr-Al-N-type tantalum oxide (16 μm) was used and the impregnation and prelithiation steps of the negative electrode structure were not carried out.
[0081] The (002) plane spacing d002 in the XRD measurement of the general natural graphite was 0.3355 nm, the crystallite size Lc in the c-axis direction in the XRD measurement of the general natural graphite was 27.57 nm, and the BET specific surface area was 2.3 m 2 / g, and the oxygen (O) content measured with an ONH analyzer (manufacturer: LECO, device name: ONH 836) was 300 ppm based on the weight of the general natural graphite.
[0082] Comparative Example 3: Production of negative electrode The negative electrode of Comparative Example 3 was prepared in the same manner as in Example 1, except that the general natural graphite used in Comparative Example 2 was used as the negative electrode active material, and the negative electrode structure was electrochemically charged with a charge amount of 9.3% of the charge capacity of the negative electrode structure.
[0083] Comparative Example 4: Production of negative electrode The negative electrode of Comparative Example 4 was prepared in the same manner as in Example 1, except that the general natural graphite used in Comparative Example 2 was used as the negative electrode active material, and the negative electrode structure was electrochemically charged with a charge amount of 15.7% of the charge capacity of the negative electrode structure.
[0084] Comparative Example 5: Production of negative electrode A negative electrode of Comparative Example 5 was produced in the same manner as in Example 1, except that the negative electrode structure was electrochemically charged with a charge amount of 24.2% of the charge capacity of the negative electrode structure.
[0085] Comparative Example 6: Production of negative electrode A negative electrode of Comparative Example 6 was produced in the same manner as in Example 1, except that the negative electrode structure was electrochemically charged with a charge amount of 8.9% of the charge capacity of the negative electrode structure.
[0086] Experimental Example Experimental example 1: Evaluation of initial efficiency <Manufacturing lithium secondary batteries> As the positive electrode, lithium metal was prepared.
[0087] A propylene polymer separator was interposed between the negative electrode prepared in Example 1 and the positive electrode prepared above, and an electrolyte was injected to prepare a coin-type lithium secondary battery. The electrolyte was prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 20:80 in an organic solvent, and then dissolving LiPF as a lithium salt. 6 was added at a concentration of 1 M, and fluoroethylene carbonate (FEC) was added as an additive at 0.5 wt % based on the total weight of the prelithiation solution.
[0088] Coin-type lithium secondary batteries were produced in the same manner as in Example 1, except that the negative electrodes produced in Examples 2 to 3 and Comparative Examples 1 to 6 were used.
[0089] <Evaluation of initial efficiency> The charge capacity and discharge capacity of the coin-type half cells of the examples and comparative examples prepared above were measured, and the initial efficiency was calculated by the following formula, and the results are shown in Table 1. The charge and discharge conditions were as follows.
[0090] Charging conditions: CCCV mode, 0.1C charging, cut-off at 5mV and 0.005C Discharge conditions: CC mode, 0.1C discharge, 1.5V cut-off
[0091] Initial efficiency = (discharge capacity at 1st cycle / charge capacity) x 100
[0092] Experimental example 2: Evaluation of output characteristics <Manufacturing lithium secondary batteries> LiCoO as a positive electrode active material 2 A positive electrode slurry was prepared by mixing Super C as a conductive material and PVdF as a binder in a weight ratio of 96:1:3. The positive electrode slurry was coated on an aluminum current collector, rolled, and dried at 130° C. to prepare a positive electrode.
[0093] A propylene polymer separator was interposed between the negative electrode prepared in Example 1 and the positive electrode prepared above, and an electrolyte was injected to prepare a coin-type lithium secondary battery. The electrolyte was an organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 20:80, and LiPF 6 was added at a concentration of 1 M, and fluoroethylene carbonate (FEC) was added as an additive at 0.5 wt % based on the total weight of the prelithiation solution.
[0094] Coin-type lithium secondary batteries were manufactured in the same manner as in Example 1, except that the negative electrodes manufactured in Examples 2 to 3 and Comparative Examples 1 to 6 were used.
[0095] <Evaluation of output characteristics> The lithium secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 6 were cycle-charged and discharged at a high current to measure the capacity retention rate after 100 cycles, and the output characteristics were evaluated.
[0096] Specifically, the lithium secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 6 were charged and discharged up to the 100th cycle under the conditions of charge (CC / CV mode, 5C charge, cut-off at 4.2V and 0.005C) and discharge (CC mode, 5C discharge, cut-off at 3.0V).
[0097] The 100 cycle capacity retention rate was evaluated by the following formula, and the results are shown in Table 1.
[0098] Capacity retention rate (%) = {(discharge capacity at 100th cycle) / (discharge capacity at first cycle)} x 100
[0099] Experimental Example 3: Evaluation of cycle capacity retention rate <Manufacturing lithium secondary batteries> The lithium secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 6 were manufactured in the same manner as the lithium secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 6 manufactured in Experimental Example 2.
[0100] <Evaluation of cycle capacity retention rate> The lithium secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 6 were evaluated for their cycle capacity retention rates.
[0101] Specifically, the lithium secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 6 were charged and discharged at 45° C. (CC / CV mode, 1C charge, cut-off at 4.2 V and 0.005 C) and discharged (CC mode, 1C discharge, cut-off at 3.0 V) up to the 400th cycle.
[0102] The capacity retention rate after 400 cycles was evaluated by the following formula, and the results are shown in Table 1.
[0103] Capacity retention rate (%) = {(discharge capacity at 400th cycle) / (discharge capacity at first cycle)} x 100
[0104] [Table 1]
[0105] Referring to Table 1, it can be seen that the secondary batteries of Examples 1 to 3, in which expanded natural graphite was prelithiated by electrochemically charging it at a preferred charge amount, have excellent initial efficiency, output characteristics, and life performance.
[0106] However, it can be seen that the secondary battery of Comparative Example 1, in which the expanded natural graphite was not prelithiated, exhibits very low levels of initial efficiency and life performance.
[0107] Moreover, the secondary battery of Comparative Example 2, in which the ordinary natural graphite was not prelithiated, not only exhibited extremely low output characteristics but also exhibited a decrease in life performance, compared to the Examples.
[0108] In addition, the secondary batteries of Comparative Examples 3 and 4, in which general natural graphite was prelithiated, showed a significant decrease in output characteristics and high lithium ion diffusion resistance, while the initial efficiency was improved to some extent. Such a decrease in output characteristics leads to a decrease in life characteristics due to repeated charging and discharging, and it can be confirmed that Comparative Examples 3 and 4 showed a decrease in life characteristics compared to Examples 1 to 3, in which expanded natural graphite was used.
[0109] In addition, in Comparative Example 5, in which expanded natural graphite was electrochemically charged at a very high charge amount and pre-lithiated, it was confirmed that the excessive lithium charge acted as a resistance, resulting in a significant decrease in output characteristics, and that such a decrease in output characteristics led to a decrease in life performance. Meanwhile, in Comparative Example 6, in which expanded natural graphite was pre-lithiated at a very low charge amount and electrochemically charged, it was confirmed that the irreversible capacity of the expanded natural graphite could not be sufficiently removed, resulting in a significant decrease in initial efficiency, and that such insufficient removal of the irreversible capacity led to a significant decrease in life performance.
[0110] Therefore, it can be confirmed that the expanded natural graphite produced by the production method of the present invention can exhibit excellent output characteristics, has high initial efficiency due to sufficient compensation of irreversible capacity, and has smooth lithium ion diffusion due to the wide spacing of crystal lattice planes, thereby exhibiting better life characteristics than general natural graphite.
Claims
1. Producing an anode structure comprising expanded natural graphite; impregnating the negative electrode structure with a prelithiation solution; and prelithiating the impregnated negative electrode structure by electrochemically charging the negative electrode structure to 10% to 20% of the charge capacity of the negative electrode structure; The method for producing a negative electrode, wherein the expanded natural graphite has a BET specific surface area of 4 m 2 / g to 8 m 2 / g.
2. In the prelithiation step, the impregnated negative electrode structure is 2. The method for producing a negative electrode according to claim 1, wherein 13% to 16% of the charge capacity of the structure is electrochemically charged.
3. The electrochemical charging is performed by placing the impregnated negative electrode structure in the prelithiation solution.
3. The method of claim 1, wherein the negative electrode is produced by using lithium metal as a counter electrode. method.
4. The method according to any one of claims 1 to 3, wherein the impregnation is carried out for a period of from 0.5 to 15 hours. A method for manufacturing a negative electrode.
5. The method for producing a negative electrode according to claim 1 , wherein the prelithiation solution contains a lithium salt and an organic solvent.
6. The electrochemical charging is performed at 0.1 mA / cm 2 ~3 mA / cm 2 The method for producing a negative electrode according to claim 1 , wherein the current density is 0.01 to 0.
5.
7. The method for producing a negative electrode according to any one of claims 1 to 6, wherein the lattice spacing d002 of the (002) plane of the expanded natural graphite in XRD measurement is 0.3370 nm to 0.3410 nm.
8. 8. The method for producing a negative electrode according to claim 1, wherein the expanded natural graphite has a crystallite size Lc in the c-axis direction as measured by XRD of 10 nm to 24 nm.
9. 9. The method for producing a negative electrode according to claim 1, wherein the expanded natural graphite contains oxygen (O) in an amount of 800 ppm to 3,000 ppm based on the weight of the expanded natural graphite.
10. The average particle diameter (D 50 10. The method for producing a negative electrode according to claim 1 , wherein the thickness of the first electrode is 8 μm to 20 μm.
11. the negative electrode structure includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector, The method for producing a negative electrode according to claim 1 , wherein the negative electrode active material layer contains the expanded natural graphite.
Citation Information
Patent Citations
Lithium secondary battery
JP1994275271A
Lithium secondary battery
JP1994325753A
Manufacture of nonaqueous electrolyte secondary battery
JP1995235330A
Lithium ion secondary battery and negative electrode material thereof
JP1996273666A
Expanded graphite particle, its production, lithium secondary cell, its negative pole and negative pole material
JP2000053408A