Particles, affinity particles, test reagents, and detection methods

Particles with optimized size, density, and resin-coated magnetic material enhance detection speed and sensitivity in antigen detection by increasing gravity and magnetic force, addressing the inefficiencies of existing technologies.

JP7580936B2Active Publication Date: 2024-11-12CANON KK
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2020071661
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-26
Filing Date
2020-04-13
Publication Date
2024-11-12
Estimated Expiration
2040-04-13

AI Technical Summary

Technical Problem

Existing magnetic particles used for antigen detection in medical diagnostics suffer from insufficient detection speed due to inadequate gravity and magnetic force application, leading to prolonged time in drawing particles close to the detection plate.

Method used

Developed particles with a specific range of volume average particle diameter (0.4 μm to 1.5 μm) and density (5.1 g/cm³ to 10.0 g/cm³) with a resin coating containing functional groups for ligand binding, and a high content of magnetic material (80% to 100%) to enhance gravity and magnetic force, facilitating faster particle movement.

Benefits of technology

The enhanced particles achieve faster detection speeds by ensuring sufficient gravity and magnetic force application, allowing for quicker antigen-antibody reactions and improved detection sensitivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580936000001
    Figure 0007580936000001
  • Figure 0007580936000002
    Figure 0007580936000002
  • Figure 0007580936000003
    Figure 0007580936000003
Patent Text Reader

Abstract

To provide a particle that has a high detection speed when to-be-measured substance, such as antigen or antibody, is detected from a sample.SOLUTION: In a particle containing magnetic particle containing a magnetic substance, resin is present on a surface of the magnetic particle, a volume average particle diameter of the particle is equal to or larger than 0.4 μm and equal to or smaller than 1.5 μm, density of the particle is equal to or higher than 5.1 g / cm3 and equal to or lower than 10.0 g / cm3, and the resin has a functional group capable of linking a ligand.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to particles, affinity particles, test reagents, and detection methods. [Background technology]

[0002] In recent years, magnetic particles have been used for a wide variety of purposes. In particular, in the medical field, magnetic particles are used for specimen testing to measure antigens and antibodies in blood for use in diagnosis. Specifically, in order to detect antigens (antibodies) from a specimen, there is a method that uses magnetic particles bound to antibodies (antigens) that specifically bind to the antigens (antibodies), and a plate on which antibodies (antigens) that specifically bind to the antigens (antibodies) are immobilized. When an antigen (antibody) is present in the specimen, the magnetic particles are bound to the plate on which the antibodies (antigens) are immobilized via the antigens (antibodies) through an antigen-antibody reaction. In such a method for detecting antigens (antibodies), there is a demand for a shorter time until detection (i.e., a faster detection speed).

[0003] As particles for use in specimen testing, magnetic-material-containing resin microparticles using magnetite, a magnetic material, have been proposed (see Patent Document 1). In addition, composite particles containing solid microparticles containing magnetite and a polymer compound have been proposed (see Patent Document 2). Furthermore, magnetic marker particles having magnetic particles and a polymer coated on the surface of the magnetic particles have been proposed (Patent Document 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-099844 A [Patent Document 2] JP 2009-300239 A [Patent Document 3] Patent Publication No. 2012-177691 Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors have investigated detection of an antigen from a specimen using particles corresponding to the particles described in Patent Documents 1 to 3, on which an antibody that specifically binds to the antigen is immobilized, and a plate on which an antibody that specifically binds to the antigen is immobilized. As a result, it has been found that there are cases in which the detection speed is not sufficient.

[0006] Therefore, an object of the present invention is to provide particles that have a high detection speed when detecting a measurement target substance such as an antigen or an antibody from a sample. Another object of the present invention is to provide affinity particles, test reagents, and detection methods that use the particles. [Means for solving the problem]

[0007] The present invention relates to a particle including a magnetic particle containing a magnetic material, the magnetic particle having a resin on its surface, a volume average particle size of 0.4 μm or more and 1.5 μm or less, and a density of 5.1 g / cm. 3 More than 10.0g / cm 3 The present invention relates to particles characterized in that the resin has a functional group capable of binding a ligand.

[0008] The present invention also relates to an affinity particle comprising a particle having the above-mentioned structure and a ligand that binds to the particle.

[0009] The present invention also relates to a test reagent comprising the affinity particles having the above-mentioned structure and a dispersion medium for dispersing the affinity particles.

[0010] Furthermore, the present invention relates to a detection method which uses affinity particles having the above-mentioned structure and a plate on which a ligand that binds to the affinity particles is immobilized. Effect of the Invention

[0011] According to the present invention, it is possible to provide particles that have a high detection speed when detecting a measurement target substance such as an antigen or antibody from a sample, affinity particles that use the particles, a test reagent, and a detection method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The following is a detailed description of the embodiments of the present invention. Various physical property values ​​are values ​​at 25°C unless otherwise specified. The volume average particle size and density of the particles are the volume average particle size and density taking into account the resin present on the surface of the magnetic particles. The following description will be given taking an antigen as an example of a measurement target substance to be detected from a specimen.

[0013] When detecting an antigen from a specimen, if particles bound to an antibody that specifically binds to the antigen and a plate on which the antibody that specifically binds to the antigen is immobilized are used, the plate is placed below the direction of gravity, and a magnet that generates a magnetic force is placed near the plate. This makes it possible to attract particles, including magnetic particles, near the plate by the action of gravity and magnetic force. Then, by utilizing an antigen-antibody reaction, the particles attracted near the plate are bound to the plate via the antibody and antigen. Furthermore, by placing a magnet above the direction of gravity, particles that are not bound to the plate are removed. This makes it possible to confirm the presence of particles bound to the plate and detect antigens from the specimen.

[0014] When detecting target substances such as antigens and antibodies from samples using this method, it is important to improve detection sensitivity by suppressing the adsorption of proteins other than the target substances to the magnetic particles. To achieve this, a resin having functional groups capable of binding ligands is provided on the surface of the particles.

[0015] However, it was found that even when using such particles, the gravitational and magnetic forces acting on the particles are insufficient, so it takes time to attract the particles near the plate, and sufficient detection speed may not be achieved.

[0016] Therefore, the present inventors considered that it is important to increase the volume average particle size and density of the particles in order to make the gravity and magnetic force acting on the particles sufficient. By increasing the volume average particle size of the particles, the gravity and magnetic force acting on the particles can be made sufficient, and by increasing the density of the particles, the magnetic force acting on the particles can be made sufficient. As a result, the particle movement speed is increased and a sufficient detection speed can be obtained. On the other hand, if the volume average particle size and density of the particles do not satisfy a predetermined range, the gravity and magnetic force acting on the particles are not sufficient, it takes time to attract the particles near the flat plate, and a sufficient detection speed cannot be obtained.

[0017] The particles described in Patent Document 1 are formed by dispersing nm-sized magnetite particles in an oily monomer and polymerizing them by mini-emulsion polymerization. The density of the particles is 1.3 g / cm 3 It is considered that the magnetic force acting on the particles is insufficient, and it takes time to draw the particles close to the plate, which makes it difficult to obtain a sufficient detection speed.

[0018] The particles described in Patent Document 2 are produced by shearing a magnetic material dispersed in an organic solvent. The volume average particle size of particles that can be produced in this way is limited to about 0.3 μm. This means that the gravity and magnetic force acting on the particles are insufficient, and it takes time to draw the particles close to the flat plate, which is thought to result in insufficient detection speed.

[0019] The magnetic marker particles described in Patent Document 3 have a particle density of at most 4.73 g / cm 3 Therefore, it takes time to attract the magnetic particles near the plate, and it is considered that a sufficient detection speed cannot be obtained. Also, since the content of the magnetic material in the magnetic particles is less than 100 mass %, the saturation magnetization is small, and it is considered that it takes time to attract the magnetic particles.

[0020] <Particle> The particles are preferably for specimen testing. The particles include magnetic particles containing a magnetic material. In the present invention, the region of the magnetic particles in the particles is defined as a region identified by observation with a transmission electron microscope (TEM). Images are taken with the TEM at a magnification that allows about 20 particles to fit in the field of view. Here, since the TEM can take images of components with different specific gravities with contrast, it is possible to identify the region of the magnetic material in the magnetic particles. In the obtained image, the magnetic material at the outermost position and the magnetic material at the opposite pole and outermost position are connected with a straight line, and the region of the circle drawn so that the center of the line is the center of the circle is defined as the magnetic particle.

[0021] The content of the magnetic material in the magnetic particles is 80% or more and 100% or less, and preferably 90% or more and 100% or less. By increasing the content of the magnetic material in the magnetic particles, the gravity and magnetic force acting on the particles increases, and the particle movement speed becomes faster, thereby improving the detection speed. Here, the content of the magnetic material in the magnetic particles can be calculated by the following method.

[0022] The content of magnetic material in a magnetic particle is calculated by multiplying the content of magnetic material in the particle by the average particle diameter. 3 ÷(average diameter of magnetic particles) 3 " The content and average value in the formula are calculated as follows. For at least 20 particles, an image analyzer (Luzex AP, Nireco) is used to measure the particle diameter and the diameter of the magnetic particles determined as described above, and the average value of each diameter is calculated. The magnetic material content in the particles is calculated using a thermogravimetric analyzer (TGA) or X-ray photoelectron spectroscopy (XPS). When TGA is used, it is found from the weight ratio before and after pyrolysis of the organic components, and when XPS is used, it is found from the ratio of elements specific to the magnetic material.

[0023] The volume average particle diameter of the particles is 0.4 μm or more and 1.5 μm or less. If the volume average particle diameter exceeds 1.5 μm, in addition to the detection speed being insufficient, the surface area per unit mass is reduced, so that the area in the particles where the antigen-antibody reaction can occur is reduced, and the efficiency of the antigen-antibody reaction may decrease. The volume average particle diameter of the particles is preferably 0.7 μm or more and 1.2 μm or less, and more preferably 0.7 μm or more and 0.9 μm or less. The volume average particle diameter can be measured by dynamic light scattering.

[0024] The particle density is 5.1 g / cm 3 More than 10.0g / cm 3 Less than 5.1 g / cm 3 More than 6.5g / cm 3 The density can be measured by a dry automatic density meter.

[0025] (magnetic material) A magnetic body is a material that is magnetized by application of a magnetic field. The magnetic body preferably includes at least one selected from the group consisting of metals and metal oxides. Examples of metals include iron, manganese, nickel, cobalt, and chromium. Examples of metal oxides include triiron tetroxide (Fe3O4), diiron trioxide (γ-Fe2O3), and ferrite. Among them, the magnetic body is preferably at least one selected from the group consisting of iron, nickel, and magnetite. Iron and nickel have high density, while magnetite has high saturation magnetization and low residual magnetization. This increases the gravitational force and magnetic force acting on the particles, improving the detection speed. Furthermore, the magnetic body is preferably iron or nickel.

[0026] Here, magnetization refers to the phenomenon whereby a magnetic material becomes a magnet when an external magnetic field is applied to it, saturation magnetization refers to the value at which magnetization, which increases with the strength of the magnetic field, reaches saturation, and residual magnetization refers to the magnetization that remains in a magnetic material when an external magnetic field is applied to the magnetic material and then the magnetic field is removed.

[0027] When the magnetic body contains iron, the content of iron atoms in the magnetic body is preferably 80% or more and 100% or less, since the density of the magnetic body can be improved. When the magnetic body contains nickel, the content of nickel atoms in the magnetic body is preferably 80% or more and 100% or less, since the density of the magnetic body can be improved. These contents indicate the number of iron atoms or nickel atoms (mol) relative to the total number of atoms (mol) in the magnetic body.

[0028] The number of magnetic bodies in a magnetic particle is preferably 1 or more. When the number of magnetic bodies in a magnetic particle is 2 or more, the particle size of the magnetic body is preferably 50 nm or less, and preferably 5 nm or more and 30 nm or less. When the number of magnetic bodies in a magnetic particle is 1, the particle size is preferably 0.1 μm or more, and more preferably 1.2 μm or less. In particular, it is preferable that the number of magnetic bodies in a magnetic particle is 1, and the content of the magnetic body in the magnetic particle is 100%. In other words, it is preferable that the magnetic particle is a single particle. This increases the particle density and improves the detection speed.

[0029] In order to improve the detection speed of particles, it is preferable to improve the settling velocity of the particles. The equation for calculating the settling velocity of a particle is Stokes' equation (V={g(ρ p -ρ f )D 2} / 18μ) is known. V is the settling velocity (cm / s), g is the gravitational acceleration (980.7cm / s 2 ), ρ p is the particle density (g / cm 3 ), ρ f is the density of the dispersion medium (g / cm 3 ) where D is the particle size (cm) and μ is the viscosity of the dispersion medium (g / cm s). According to Stokes' law, the settling velocity V of a particle increases in proportion to the square of the particle size.

[0030] The settling velocity calculated by the Stokes' law is preferably 1.0E-05 (cm / s) or more. If the settling velocity is less than 1.0E-05, it takes a long time to detect, and the detection velocity may not be sufficient. The settling velocity is more preferably 5.0E-05 (cm / s) or more, and even more preferably 1.0E-04 (cm / s) or more.

[0031] (resin) Hereinafter, the term "(meth)acrylate" refers to "acrylate or methacrylate".

[0032] The resin has a functional group capable of binding a ligand. The functional group capable of binding a ligand is preferably at least one selected from the group consisting of a carboxyl group, an amino group, a thiol group, an epoxy group, a maleimide group, and a succinimidyl group. Among these, the functional group capable of binding a ligand is preferably a carboxyl group.

[0033] In polymerizing the resin, it is preferable to use a monomer having a carboxyl group, such as (meth)acrylic acid; a monomer having an amino group, such as (meth)acrylamide; a monomer having an epoxy group, such as glycidyl (meth)acrylate; or a monomer having a succinimidyl group, such as N-succinimidyl acrylate.

[0034] In addition to the above monomers, when polymerizing the resin, (meth)acrylates having a hydrophilic group such as glycerol (meth)acrylate, 2-hydroxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, etc.; styrenes such as styrene, p-chlorostyrene, α-methylstyrene, etc.; etc. can also be used. In order to suppress non-specific adsorption to magnetic particles, it is preferable to use (meth)acrylates having a hydrophilic group.

[0035] Functional groups capable of binding ligands can also be added after polymerization of the resin. For example, a thiol group can be introduced by adding a mercaptodiol to a resin obtained by polymerizing a monomer having a carboxyl group, such as (meth)acrylic acid. A maleimide group can also be introduced by adding N-(2-hydroxyethyl)maleimide to the resin obtained by polymerization.

[0036] The resin preferably has repeating units of the following formulae (2) and (3).

[0037] [ka]

[0038] [ka]

[0039] The resin preferably has units derived from styrene and acrylic acid, where a unit means a unit structure corresponding to one monomer.

[0040] The resin preferably has a siloxane bond. That is, when polymerizing the resin, it is preferable to use a monomer containing an organic silane such as vinyltrimethoxysilane, vinyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, or 3-acryloxypropyltrimethoxysilane.

[0041] The weight average molecular weight of the resin is preferably 10,000 or more, and more preferably 100,000 or less. Also, it is more preferably 40,000 or more and 100,000 or less, and even more preferably 60,000 or more and 80,000 or less. The weight average molecular weight can be measured by gel permeation chromatography.

[0042] <Affinity particles> The affinity particle of the present invention has a particle having the above-mentioned configuration and a ligand that binds to the particle. A ligand is a compound that specifically binds to a receptor possessed by a substance to be measured. The site where the ligand binds to the substance to be measured is fixed, and the ligand has a high affinity selectively or specifically. Examples of combinations of a substance to be measured and a ligand include an antigen and an antibody, an enzyme protein and its substrate, a signal substance such as a hormone or a neurotransmitter and its receptor, and the like. The ligand is preferably either an antigen or an antibody. In addition, one type of ligand may be bound to the affinity particle, or multiple types of ligands may be bound to the affinity particle. By using affinity particles bound to multiple types of ligands, it becomes easy to detect multiple types of substances to be measured. In addition, when there are multiple recognition sites where the substance to be measured is recognized by the ligand, it is preferable to bind multiple types of ligands corresponding to the multiple recognition sites to the affinity particle.

[0043] In order to immobilize a ligand on a particle to make it an affinity particle, a conventionally known method such as chemical bonding or physical adsorption can be applied by utilizing a functional group of the particle to which the ligand can be bonded. In particular, when bonding a ligand to a particle by amide bonding, a catalyst such as 1-[3-(dimethylaminopropyl)-3-ethylcarbodiimide] can be used.

[0044] Affinity particles are preferably used in a method in which a ligand-immobilized plate is used, the particles are bound to the plate via the substance to be measured through an antigen-antibody reaction, unbound particles are removed from near the plate by magnetic force, and the particles bound to the plate are detected.

[0045] <Test Reagents> The test reagent includes affinity particles having the above-mentioned configuration and a dispersion medium for dispersing the affinity particles. The content of the affinity particles is preferably 0.001% by mass or more and 20% by mass or less, and more preferably 0.01% by mass or more and 10% by mass or less, with the total mass of the dispersion medium being 100% by mass. The test reagent may include a solvent, a blocking agent, etc. Two or more types of the solvent, the blocking agent, etc. may be combined. Examples of the solvent include buffer solutions such as phosphate buffer, glycine buffer, Good's buffer, Tris buffer, and ammonia buffer.

[0046] <Detection method> In this embodiment, a method for detecting a substance to be measured contained in a sample includes at least the following steps.

[0047] (1st step) In the first step, a specimen containing a substance to be measured and a test reagent having affinity particles and a dispersion medium for dispersing the affinity particles are added to a container having a first ligand fixed to the lower side in the direction of gravity.

[0048] (2nd process) In the second step, a magnetic field is applied so that the affinity particles bind to the first ligand via the substance to be measured.

[0049] (3rd step) In the third step, a magnetic field is applied so that affinity particles that are not bound to the first ligand via the substance to be measured are moved away from the first ligand.

[0050] In the detection method according to this embodiment, the first ligand and the second ligand may be any ligand capable of binding to the substance to be measured, and the above-mentioned ligands may be used. The first ligand and the second ligand may be the same or different.

[0051] The first ligand can be provided on a flat surface provided on the lower side of the container (housing) in the direction of gravity, or on a flat plate provided in the container. An example of the detection method includes the following steps. (1) A first step of placing a specimen and the test reagent having the above-mentioned configuration in a container having a flat plate on the lower side in the direction of gravity, the flat plate having a ligand that binds to affinity particles immobilized thereon. (2) A second step in which a magnet is placed near the plate to attract the affinity particles in the test reagent near the plate. (3) and a third step of removing affinity particles that are not bound to the plate by placing a magnet on the upper side in the direction of gravity. Furthermore, by executing a step of detecting a signal from affinity particles bound to the first ligand via the substance to be measured, the presence or absence and concentration of the substance to be measured can be measured. The presence (presence or absence and concentration) of the substance to be measured in the sample can be confirmed by the particles binding to the plate via the substance to be measured in the sample due to the antigen-antibody reaction. EXAMPLES

[0052] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples without departing from the gist of the present invention. Note that "parts" and "%" used to describe the amounts of components are based on mass unless otherwise specified.

[0053] <Example 1> In a 300 mL flask, 100 mL of 10 mM Tris buffer solution (Tokyo Chemical Industry Co., Ltd.) and 1.0 g of magnetic iron particles (NP-FE-1, EM Japan Co., Ltd.) were mixed and stirred at 25° C. for 20 minutes. The pH of the Tris buffer solution was adjusted to 9.0 with hydrochloric acid. The volume average particle size of the iron particles was 0.8 μm. 1.0 g of dopamine hydrochloride (Sigma-Aldrich Japan LLC) was added to the obtained solution and stirred overnight at 25° C. to obtain a dispersion liquid.

[0054] Thereafter, the dispersion was centrifuged, the supernatant was removed, and the dispersion was washed with ion-exchanged water three times. A phosphate buffer solution (Kishida Chemical Co., Ltd.) with a pH of 7.4 was added to the precipitate, and a dispersion solution was obtained in which the precipitate was replaced with a phosphate buffer solution. 1.0 g of N-vinylpyrrolidone-acrylic acid copolymer (Polymer Source Co., Ltd.), which is a resin, was dissolved in the obtained dispersion. Here, the weight-average molecular weight of the N-vinylpyrrolidone-acrylic acid copolymer was 60,000, and the ratio of the total molar amount of the unit structure corresponding to vinylpyrrolidone to the total molar amount of the unit structure corresponding to acrylic acid was 4:6.

[0055] 0.4 g of 3-methacryloxypropyltrimethoxysilane (LS-3380, manufactured by Shin-Etsu Chemical Co., Ltd.) and 1.3 g of styrene (manufactured by Kishida Chemical Co., Ltd.) were added to the dispersion containing the resin, and the mixture was stirred for 15 minutes while blowing nitrogen at 25°C to obtain an emulsion. The obtained emulsion was heated to 70°C using an oil bath. A solution of 0.3 g of potassium peroxodisulfate (manufactured by Wako Pure Chemical Industries, Ltd. (now Fujifilm Wako Pure Chemical Co., Ltd.)) dissolved in 10 mL of phosphate buffer solution (manufactured by Kishida Chemical Co., Ltd.) with a pH of 7.4 was added to the heated emulsion. After stirring the emulsion at 70°C for 7 hours, the temperature of the emulsion was returned to 25°C. The emulsion was then centrifuged to collect particles with resin present on the surface of the magnetic particles, the supernatant was discarded, and the particles were redispersed in ion-exchanged water. This procedure of recovering the particles by centrifugation and redispersing them in ion-exchanged water was repeated three times to obtain a dispersion of Particle 1 with a particle content of 1.0%.

[0056] <Example 2> In the preparation of the particle dispersion of Example 1, the material added to the resin-containing dispersion was changed to styrene (manufactured by Kishida Chemical Co., Ltd.) alone. A dispersion of particles 2 with a particle content of 1.0% was obtained in the same procedure as in the preparation of the particle dispersion of Example 1.

[0057] <Example 3> In a 300 mL flask, 100 mL of 10 mM Tris buffer solution (Tokyo Chemical Industry Co., Ltd.) and 1.0 g of magnetic iron particles (NP-FE-1, EM Japan Co., Ltd.) were mixed and stirred at 25° C. for 20 minutes. The pH of the Tris buffer solution was adjusted to 9.0 with hydrochloric acid. The volume average particle size of the iron particles was 0.8 μm. 1.0 g of dopamine hydrochloride (Sigma-Aldrich Japan LLC) was added to the obtained solution and stirred overnight at 25° C. to obtain a dispersion liquid.

[0058] Thereafter, the dispersion was centrifuged, the supernatant was removed, and the operation of washing with ion-exchanged water was performed three times, and ion-exchanged water was added to the precipitate to obtain a dispersion in which ion-exchanged water was substituted. 1.0 g of polyvinylpyrrolidone (PVP-K30, manufactured by Kishida Chemical Co., Ltd.) and 2.0 g of 1-amino-3,6,9,12,15,18-hexaoxaheneicosane-21-acid were mixed with the obtained dispersion, and the mixture was stirred overnight at 25°C to obtain a dispersion. The dispersion was centrifuged to collect particles having resin on the surface of the magnetic particles, the supernatant was discarded, and the particles were redispersed in ion-exchanged water. This operation of collecting the particles by centrifugation and redispersing them with ion-exchanged water was performed three times to obtain a dispersion of particles 3 with a particle content of 1.0%. The weight average molecular weight of the resin was 60,000.

[0059] <Example 4> A 1-L separable flask was charged with 750 g of an aqueous solution containing 0.5% sodium dodecylbenzenesulfonate and 0.5% nonionic emulsifier (EMULGEN 150, Kao Corporation) and 30 g of iron particles (NP-FE-1, EM Japan Co., Ltd.) in that order to obtain a solution. The obtained solution was dispersed with a homogenizer and heated to 70°C.

[0060] A dispersion liquid obtained by dispersing 14 g of cyclohexyl methacrylate, 1 g of trimethylolpropane trimethacrylate, and 0.3 g of t-butylperoxy-2-ethylhexanate (Perbutyl O, manufactured by Nippon Oil & Fats) in 75 g of aqueous solution was added dropwise to the obtained solution over a period of 1 hour. Here, the aqueous solution contains 0.5% sodium dodecylbenzenesulfonate and 0.5% of a nonionic emulsifier (Emulgen 150, manufactured by Kao Corporation). This resulted in a liquid containing particles having a first layer containing a resin on the surface of the magnetic particles.

[0061] A dispersion liquid prepared by dispersing 14 g of cyclohexyl methacrylate, 1 g of trimethylolpropane trimethacrylate, and 0.3 g of t-butylperoxy-2-ethylhexanate (Perbutyl O, manufactured by Nippon Oil & Fats Corporation (now NOF Corporation)) in 75 g of aqueous solution was added dropwise to the obtained liquid over a period of 1 hour. Here, the aqueous solution contained 0.5% sodium dodecylbenzenesulfonate and 0.5% of a nonionic emulsifier (Emulgen 150, manufactured by Kao Corporation). This resulted in a liquid containing particles with two layers (first layer and second layer) containing resin present on the surface of the magnetic particles. The weight-average molecular weight of the resin contained in the two layers was 80,000.

[0062] The obtained liquid was heated to 80°C, and polymerization was continued for 2 hours to complete the reaction, obtaining a dispersion. The dispersion was centrifuged to collect magnetic particles with resin on their surfaces, the supernatant was discarded, and the particles were redispersed in ion-exchanged water. This operation of collecting the particles by centrifugation and redispersing them in ion-exchanged water was repeated three times to obtain a dispersion of particles 4 with a particle content of 1.0%.

[0063] <Example 5> In the preparation of the particle dispersion of Example 3, the type of magnetic material was changed to nickel particles. Here, the volume average particle size of the nickel particles was 0.45 μm. Otherwise, the same procedure as in the preparation of the particle dispersion of Example 3 was used to obtain a particle 5 dispersion with a particle content of 1.0%.

[0064] <Comparative Example 1> In the preparation of the particle dispersion of Example 3, the type of magnetic material was changed to magnetite particles. Here, the volume average particle size of the magnetite particles was 0.7 μm. Otherwise, the same procedure as in the preparation of the particle dispersion of Example 3 was used to obtain a dispersion of particles 6 with a particle content of 1.0%.

[0065] <Comparative Example 2> FeCl3 and FeCl2 were dissolved in water to obtain a solution. This solution was vigorously stirred while being maintained at 25°C. Ammonia water was then added to the solution to obtain a suspension of magnetite. Oleic acid was added to the obtained suspension, and the suspension was stirred at 70°C for 1 hour and at 110°C for 1 hour to obtain a slurry. This slurry was washed with a large amount of water and dried under reduced pressure to obtain powdered hydrophobic magnetite. The average particle size of the obtained hydrophobic magnetite was 11 nm, and the molecular weight distribution was 1.3. Here, the average particle size of the hydrophobic magnetite was a value calculated using a transmission electron microscope.

[0066] Next, 2 g of styrene and 3 g of hydrophobized magnetite were weighed into 4 g of chloroform to obtain mixed liquid 1. 0.01 g of sodium dodecyl sulfate was dissolved in 12 g of water to obtain mixed liquid 2. Mixed liquid 1 and mixed liquid 2 were mixed to obtain mixed liquid 3, and mixed liquid 3 was sheared for 10 minutes while being cooled in a stirring homogenizer to obtain a liquid containing magnetic particles containing a plurality of magnetic bodies.

[0067] The liquid containing the magnetic particles was subjected to a reduced pressure treatment in an evaporator, and chloroform was preferentially distilled from the dispersion medium. The obtained magnetic particles were deoxygenated by nitrogen bubbling, and then 0.01 g of a polymerization initiator was added, and styrene was polymerized at 70°C for 6 hours to obtain a dispersion liquid of particles 7 (content of particles 7: 1.0%) in which a resin was present on the surface of the magnetic particles. 2,2'-azobis(2-methylpropionamidine) dihydrochloride was used as the polymerization initiator. The weight-average molecular weight of the resin was 70,000.

[0068] <Comparative Example 3> FeCl3 and FeCl2 were dissolved in water to obtain a solution. This solution was vigorously stirred while being maintained at 25°C. Ammonia water was then added to this solution to obtain a suspension of magnetite. Oleic acid was added to the obtained suspension, and the suspension was stirred at 70°C for 1 hour and at 110°C for 1 hour to obtain a slurry. This slurry was washed with a large amount of water and dried under reduced pressure to obtain a powder of hydrophobic magnetite.

[0069] To the obtained hydrophobic magnetite, an aqueous solution in which 0.3 g of a nonionic surfactant having a polyethylene oxide chain (Emulgen 1150S-70, manufactured by Kao Corporation) was dissolved was added, and sonication was performed. As a result, a colloidal solution of magnetite particles in which the particle surface was given hydrophilicity by adsorbing the nonionic surfactant to the hydrophobic magnetite particle surface was obtained. To this colloidal solution, an aqueous solution in which 10 μL of aminoundecane, an ionic surfactant, was dissolved in 56 μL of HCl solution was added, and a colloidal solution of magnetite particles in which both the nonionic surfactant and the ionic surfactant were adsorbed to the particle surface was obtained.

[0070] To the resulting colloidal solution, 2.7 g of styrene, 0.3 g of acrylic acid, 0.025 g of a polymerization initiator, 0.08 g of divinylbenzene, and 2.5 g of diethyl ether were added, and sonication was performed to obtain an emulsion. Here, azobisisobutyronitrile was used as the polymerization initiator, and divinylbenzene was used as the crosslinking agent.

[0071] Water was added to the emulsion so that the total amount became 125 g, and sonication was performed. After that, it was heated while stirring at 350 rpm, and when the temperature of the emulsion reached 70°C, an aqueous solution in which 50 mg of a water-soluble polymerization initiator (V-50, manufactured by Wako Pure Chemical Industries, Ltd. (currently Fujifilm Wako Pure Chemical Corporation)) was dissolved in 5 mL of pure water was added. After that, a polymerization reaction was performed for 12 hours, and a dispersion of particles 10 (particle content 1.0%) in which a resin was present on the surface of the magnetic particles was obtained. The weight average molecular weight of the resin was 60,000.

[0072] [Content of magnetic material in magnetic particles] The content of magnetic material in a magnetic particle is calculated by multiplying the content of magnetic material in the particle by the average particle diameter. 3 ÷(average diameter of magnetic particles) 3 " The content and average value in the formula were calculated as follows. For at least 20 particles, the particle diameter and the magnetic particle diameter were measured using an image analyzer (Luzex AP, manufactured by Nireco), and the average value of each diameter was calculated. The content of magnetic material in the particles was calculated using X-ray photoelectron spectroscopy (XPS).

[0073] [Method for measuring volume average particle size] The volume average particle diameter of the particles was measured using an aqueous solution obtained by diluting the particle dispersion 250 times (by volume) with pure water as a measurement sample, using a particle size distribution meter (Nanotrac UPA-EX150, manufactured by Nikkiso Co., Ltd.) using the dynamic light scattering method. The measurement conditions were: SetZero: 30s, number of measurements: 3, measurement time: 180 seconds, shape: aspheric, refractive index: 1.51.

[0074] [Method of measuring density] The density of the magnetic particles was measured using a dry automatic densitometer (AccuPic II 1340, manufactured by Shimadzu Corporation) at a temperature of 23°C.

[0075] The measurement device has a sample chamber connected to a helium gas inlet pipe, and an expansion chamber connected to a helium gas outlet pipe. The sample chamber and the expansion chamber are connected by a connecting pipe. The helium gas inlet pipe, the connecting pipe, and the helium gas outlet pipe are all equipped with stop valves. The sample chamber has a pressure gauge that measures the pressure inside the chamber.

[0076] Using the above-mentioned measuring device, the measurement was carried out as follows. First, the volume of the sample chamber (V CELL ), and the volume of the expansion chamber (V EXP) was measured. The samples used were those dried under reduced pressure at 40°C for 24 hours. The pressure is a gauge pressure, which is the absolute pressure minus the ambient pressure. The sample was placed in the sample chamber, and helium gas was flowed through the helium gas inlet tube of the sample chamber, the connecting tube, and the helium gas outlet tube of the expansion chamber for 2 hours to replace the inside of the measurement device with helium gas. Next, the stop valves of the connecting tube and the helium gas outlet tube were closed, and helium gas was introduced into the sample chamber from the helium gas inlet tube until the pressure reached 134 kPa, and the stop valve of the helium gas inlet tube was closed. The pressure (P1) of the sample chamber was measured 5 minutes after closing the stop valve of the helium gas inlet tube. Furthermore, the stop valve of the connecting tube was opened to transfer the helium gas to the expansion chamber, and the pressure (P2) at that time was measured.

[0077] From the following equation (4), the volume of the sample (V SAMP ) was calculated, and the obtained value and the weight of the sample (W SAMP ) to obtain the density of the sample, ρ(W SAMP / V SAMP ) was sought. V SAMP =V CELL -V EXP [(P1-P2)-1] Equation (4)

[0078] [Method for measuring weight average molecular weight] The weight average molecular weight of the resin was measured by gel permeation chromatography (GPC) as follows. The resin was dissolved in tetrahydrofuran (THF) at 25°C for 24 hours. The obtained solution was filtered through a membrane filter to obtain a sample solution. The sample solution was adjusted so that the concentration of components soluble in THF was about 0.3%. Using this sample solution, the weight average molecular weight of the resin was measured under the following conditions. Equipment: Waters2695 Separations Module, Waters RI detector: 2414detector, Waters Column: 4 KF-806M columns, Showa Denko Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Oven temperature: 40℃ Sample injection volume: 100 μL

[0079] The weight-average molecular weight of the resin was calculated using a molecular weight calibration curve prepared using standard polystyrene resins (TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500, manufactured by Tosoh Corporation).

[0080] <Preparation of affinity particles> Anti-CRP antibodies were bound to each of the magnetic particles in the Examples and Comparative Examples as follows: Here, CRP is an abbreviation for C-Reactive Protein, a protein that appears in the blood when inflammation occurs in the body or tissue is destroyed.

[0081] First, the dispersion of magnetic particles was centrifuged at 15000 rpm (20400 g) for 15 minutes to precipitate the magnetic particles. After removing the supernatant, the pellet of magnetic particles was redispersed in MES buffer, and water-soluble carbodiimide (WSC) and N-hydroxysuccinimide were added. Then, the mixture was stirred at 25°C for 30 minutes, and the magnetic particles were collected by centrifugation. The collected magnetic particles were washed with MES buffer, redispersed in MES buffer, and anti-CRP antibody was added so that the final antibody concentration was 2 mg / mL. Then, the mixture was stirred at 25°C for 60 minutes, and the magnetic particles were collected by centrifugation, and the magnetic particles were washed with HEPES buffer to obtain a dispersion of affinity particles bound to anti-CRP antibody.

[0082] The binding of the antibody to the magnetic particles was confirmed by a BCA (bicinchoninic acid) assay, which can colorimetrically quantify proteins, measuring the decrease in antibody concentration in the MES buffer to which the antibody was added.

[0083] [Confirmation of non-specific adsorption] The non-specific adsorption of affinity particles was confirmed using the affinity particle dispersion of the Example. 51 μL of serum solution diluted 50 times with phosphate saline was added to 50 μL of affinity particle dispersion, and the presence or absence of particle aggregation due to non-specific adsorption to the affinity particles was visually confirmed before and after the addition, and no significant aggregation was observed.

[0084] [Checking detection sensitivity] The detection sensitivity of the affinity particles was confirmed using the dispersion of the affinity particles of the embodiment. The plate bound to the anti-CRP antibody was set at the bottom of a 6 mL vial. An aqueous solution containing 0.01% affinity particles was placed in the vial to disperse the affinity particles. 30 μL of anti-CRP antigen was added to the vial, and a neodymium magnet was applied to the bottom of the vial for 5 minutes, after which the neodymium magnet was removed and the vial was left to stand for 1 minute. Next, a neodymium magnet was applied to the top of the vial for 1 minute, and the affinity particles in the supernatant were removed. The plate bound to the anti-CRP antibody was then taken out, and it was confirmed by a scanning electron microscope (SEM) that the affinity particles were bound to the antibody on the plate via the antigen.

[0085] <Evaluation> In the present invention, in the following evaluation criteria, 4 was defined as an acceptable level, and 3, 2, or 1 was defined as an unacceptable level. Table 1 shows the evaluation results.

[0086] (detection speed) 10 mL of an aqueous solution containing 0.01% affinity particles was placed in a vial to disperse the affinity particles. A neodymium magnet was placed on the bottom of the vial for 60 seconds, after which the neodymium magnet was removed and the sedimentation of the particles in the vial was visually observed. The easier it is for the affinity particles to sediment, the faster the detection speed for the concentration of the sedimented affinity particles. 4: The affinity particles were completely sedimented within 80 seconds, and the supernatant was clear. 3: The affinity particles were completely sedimented within 120 seconds, and the supernatant was clear. 2: The affinity particles partially settled in 120 seconds, and the affinity particles were observed in part of the supernatant. 1: The affinity particles partially settled in 120 seconds, and the affinity particles were found throughout the supernatant.

[0087] [Table 1]

Claims

1. A particle including a magnetic particle containing a magnetic material, a resin is present on the surface of the magnetic particles; The volume average particle size of the particles is 0.7 μm or more and 0.9 μm or less, The density of the particles is 5.1 g / cm 3 10.0g / cm or more 3 1. A particle comprising the resin having at least one functional group selected from the group consisting of a carboxyl group, an amino group, a thiol group, an epoxy group, a maleimide group, and a succinimidyl group.

2. The density of the particles is 5.1 g / cm 3 6.5g / cm or more 3 The particle of claim 1, wherein:

3. 3. The particle according to claim 1, wherein the resin has a weight average molecular weight of 10,000 or more.

4. The particle according to claim 1 , wherein the resin has repeating units represented by the following formulas (2) and (3): [Formula 1] [Case 2]

5. 5. The particle according to claim 1, wherein the resin has units derived from styrene and acrylic acid.

6. A particle described in any one of claims 1 to 4, wherein the resin has units derived from any one of (meth)acrylic acid, (meth)acrylamide, glycidyl (meth)acrylate, N-succinimidyl acrylate, glycerol (meth)acrylate, 2-hydroxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, styrene, p-chlorostyrene, α-methylstyrene, and vinylpyrrolidone.

7. The particle according to claim 1 , which is for use in specimen testing.

8. The number of the magnetic bodies in the magnetic particle is one, and The particle according to claim 1 , wherein the content of the magnetic material in the magnetic particle is 100%.

9. The particle according to claim 1 , wherein the magnetic material comprises at least one selected from the group consisting of metals and metal oxides.

10. The particle according to claim 1 , wherein the magnetic material comprises at least one selected from the group consisting of iron, nickel, and magnetite.

11. The magnetic material contains the iron, The particle according to claim 10 , wherein the content of iron atoms in the magnetic material is 80 mol % or more and 100 mol % or less.

12. The magnetic body contains nickel, The particle according to claim 10 , wherein the content of nickel atoms in the magnetic material is 80 mol % or more and 100 mol % or less.

13. 13. The particle according to claim 1, wherein the functional group is a carboxyl group.

14. The particle according to claim 1 , wherein the resin has a siloxane bond.

15. A particle comprising a magnetic particle containing a magnetic material, a resin is present on the surface of the magnetic particles; The volume average particle size of the particles is 0.4 μm or more and 1.5 μm or less, the particle has a density of 5.1 g / cm 3 or more and 10.0 g / cm 3 or less, the resin has at least one group selected from the group consisting of a carboxyl group, an amino group, a thiol group, an epoxy group, a maleimide group, and a succinimidyl group, The particles are characterized in that the resin has a siloxane bond.

16. 16. An affinity particle comprising the particle according to claim 1 and a ligand that binds to the particle.

17. The affinity particle according to claim 16, wherein the ligand is either an antibody or an antigen.

18. A test reagent comprising the affinity particles according to claim 16 or 17 and a dispersion medium for dispersing the affinity particles.

19. A method for detecting a target substance contained in a sample, comprising: A first step of adding a specimen containing a substance to be measured and a test reagent containing affinity particles and a dispersion medium for dispersing the affinity particles to a container having a first ligand fixed to the lower side in the direction of gravity; a second step of applying a magnetic field so that the affinity particles bind to the first ligand via the target substance; a third step of applying a magnetic field so that the affinity particles that are not bound to the first ligand via the measurement target substance are moved away from the first ligand; The affinity particle comprises a particle according to any one of claims 1 to 15 and a second ligand that binds to the particle, A detection method, characterized in that the first ligand and the second ligand are capable of binding to the substance to be measured.

20. 20. The method of claim 19, wherein the first ligand and the second ligand are the same.

21. 20. The method of claim 19, wherein the first ligand and the second ligand are different.

22. 22. The detection method according to claim 19, further comprising the step of detecting a signal from the affinity particles bound to the first ligand via the substance to be measured.

Citation Information

Patent Citations

  • Magnetic polymer article, its manufacturing and diagnostic medicine

    JP1999191510A

  • Magnetic polymer latex and its production method

    JP2004099844A

  • Production method of metal / carbon nanotube-compound sintered compact

    JP2006265686A

  • Method for preparing coated magnetic particles

    JP2007527454A

  • Composite particle, method for manufacturing the same, dispersion, magnetic biosensing device and magnetic biosensing method

    JP2009300239A