High concentration iron-based flocculant and its manufacturing method
The method addresses inefficiencies in producing ferric sulfate by using iron oxide under controlled conditions with oxygen and a catalyst, resulting in a highly concentrated polyferric sulfate solution with reduced sulfate ions and improved sludge flocculation efficiency.
Patent Information
- Application Number
- JP2020136891
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-19
- Filing Date
- 2020-08-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-08-14
AI Technical Summary
Existing methods for producing ferric sulfate solutions using iron oxide as a raw material face challenges in achieving high total iron concentration and efficiency, leading to high sulfate ion generation and increased processing costs due to the use of large amounts of sulfuric acid and prolonged reaction times.
A method involving the use of iron oxide as a raw material, with a molar ratio of sulfate ions to total iron less than 1.5, high temperature (100°C or higher), high pressure (0.3 MPa or more), and oxygen replacement in a sealed container, optionally with a catalyst like nitric acid, to produce a highly concentrated polyferric sulfate solution efficiently.
The method enables the production of a polyferric sulfate solution with high sludge flocculation ability and reduced sulfate ion generation, achieving high total iron concentration and efficient production in a short time.
Smart Images

Figure 0007580970000002 
Figure 0007580970000003 
Figure 0007580970000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-concentration iron-based flocculant for use in wastewater treatment and a method for producing the same. [Background technology]
[0002] Sewage sludge is treated with various coagulants before being dewatered and landfilled, and polyferric sulfate is a typical inorganic coagulant used in the coagulation treatment of sewage sludge.It is widely used both in Japan and overseas due to its characteristics such as being less corrosive so it does not damage wastewater treatment facilities, and not containing chlorine so it is effective for recycling sewage sludge cake such as composting.
[0003] In manufacturing polyferric sulfate as an iron-based inorganic flocculant, ferrous sulfate (Fe(SO4) 7H2O) is generally used as the raw material for the iron-based production. However, ferrous sulfate is a by-product obtained in the titanium oxide manufacturing process, and since its supply is unstable, there has been a demand for an alternative material to ferrous sulfate as a raw material for the production of polyferric sulfate. On the other hand, iron oxides such as magnetite and wustite are by-products of the copper smelting process and also occur naturally as ores. Because they are easier to obtain than ferrous sulfate, technological development is underway to produce polyferric sulfate using iron oxide.
[0004] The following two techniques have been published as methods for producing ferric sulfate solution using an autoclave with iron oxide as an iron-based raw material. The method for producing an iron-based inorganic flocculant described in Patent Document 1 uses iron oxide (magnetite) as an iron-based raw material, adjusts the molar ratio of sulfate ions and iron ions, and then reacts them in a closed container at a temperature of 120 to 180°C to dissolve the iron oxide. An oxidizing agent is then added to obtain an iron sulfate solution. This method aims to shorten the reaction time by proceeding with the reaction under high temperature and pressure, but it has not produced a polyferric sulfate solution with a high total iron concentration.
[0005] Patent Document 2 describes introducing water, sulfuric acid, oxygen, and iron oxide (magnetite, hematite) into a pressure vessel to produce a ferric sulfate solution under high-temperature and high-pressure conditions. In this production method, since a large amount of sulfuric acid is used to dissolve iron oxide, what is produced is a ferrous sulfate solution, and it is impossible to obtain the poly ferric sulfate solution which is the object of the present invention.
[0006] According to these prior arts, it can be said that the following techniques were known to those skilled in the art. That is, dissolving iron oxide with sulfuric acid to generate divalent or trivalent iron ions, then oxidizing this using an oxidizing agent to produce a ferric sulfate solution and using this as an iron-based flocculant, and proceeding with the reaction in a sealed container under high temperature and high pressure to promote the dissolution of iron oxide in sulfuric acid. However, since iron oxide is difficult to dissolve in sulfuric acid and takes a long time to dissolve, in the prior art, even under high-temperature and high-pressure conditions, a large amount of sulfuric acid was used to dissolve iron oxide. For this reason, the reaction product was an aqueous solution of ferric sulfate.
[0007] The ferric sulfate produced by the prior art has the chemical formula Fe2(SO4)3, and when used as a flocculant, 3 moles of sulfate ions are generated for 2 moles of iron ions. However, since sulfate ions are not involved in the flocculation of sludge, they remain in the effluent. The treatment cost of this remaining sulfate ion has become a major problem. This is because a large amount of cost is required to neutralize it. In contrast, the chemical formula of the poly ferric sulfate produced in the present invention is as follows. The fact that less sulfate ions are generated is one of the excellent characteristics of the poly ferric sulfate solution as an inorganic flocculant. Since a large amount of sewage sludge needs to be treated, the fact that the treatment cost of the remaining sulfate ions can be low is a great merit in sewage treatment. [Fe2(OH) n (SO4) 3-n / 2 m (0 < n ≦ 2, m is a natural number) Formula (1)
Prior Art Documents
Patent Documents
[0008] [Patent Document 1] Patent No. 3379204 [Patent Document 2] US Patent No. 8658124 Summary of the Invention [Problem to be solved by the invention]
[0009] The object of the present invention is to provide a method for efficiently producing, in a short time, under high-temperature and high-pressure conditions, a polyferric sulfate solution having a high total iron concentration and high sludge flocculation ability, using iron oxide as an iron-based raw material, which is more readily available and less expensive than ferrous sulfate. [Means for solving the problem]
[0010] In order to solve these problems, the method for producing polyferric sulfate of the present invention comprises the following technical means. (1) A method for producing polyferric sulfate using iron oxide as an iron-based raw material, which comprises charging iron oxide powder, adjusted so that the molar ratio of sulfate ions to total iron is less than 1.5, and a sulfuric acid solution into a sealed vessel, replacing the gas phase in the sealed vessel with oxygen, and then carrying out an oxidation reaction under high-temperature and high-pressure conditions. (2) The method for producing polyferric sulfate according to (1), characterized in that magnetite or wustite is used as the iron-based raw material. (3) The method for producing polyferric sulfate according to (1) or (2), further comprising adding a catalyst. (4) The method for producing polyferric sulfate according to (3), wherein the catalyst is nitric acid. (5) The method for producing polyferric sulfate according to any one of (1) to (4), wherein the high temperature and high pressure conditions are a pressure of 0.3 MPa or more and a temperature of 100° C. or more. (6) The method for producing polyferric sulfate according to any one of (1) to (5), characterized in that polyferric sulfate having a high concentration, that is, a total iron concentration of 14.5% or more, is produced. (7) The method for producing polyferric sulfate according to (6), wherein the production of polyferric sulfate is completed within 4 hours.
[0011] The concentration indications used in this invention are all weight percent unless it is clearly stated that they are molar concentrations. [T-Fe] is the weight concentration of total iron, [SO4 2- ] represents the weight concentration of sulfate ions. Here, the total iron concentration refers to the concentration including not only the iron dissolved in the raw material, but also the iron present in the raw material liquid as a solid (powder, etc.) without dissolving. Even iron-based powder present in the raw material liquid contributes to the reaction for producing the polyferric sulfate solution, so it is reasonable to include the iron-based components not dissolved in the raw material liquid in the iron concentration. However, even in the case of the ferric polysulfate solution produced according to the present invention, the concentration is indicated as the total iron concentration, but it goes without saying that all of the iron is dissolved. Effect of the Invention
[0012] By employing the production method of the present invention, it has become possible to efficiently produce, in a short period of time under high temperature and pressure conditions, a polyferric sulfate solution having a high total iron concentration and high sludge flocculation ability, using easily available iron oxide as the iron-based raw material. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a flow diagram of the autoclave, which is a manufacturing device. [Diagram 2] 2 shows the relationship between the concentration of the input raw materials and the concentration of the generated slurry. The circles indicate the composition of the input raw materials, and the diamonds indicate the composition of the polyferric sulfate generated in Examples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] (manufacturing process) The method for producing polyferric sulfate in the present invention is a method including the following production steps using a production apparatus whose outline is shown in FIG. 1. (1) Sulfuric acid, water, and iron oxide are placed in a sealed container. (2) The air in the sealed container is replaced with oxygen, and nitric acid is added as a catalyst if necessary. (3) Keep the temperature inside the sealed container at 100°C or higher and the pressure at 0.3 MPa or higher, and stir for 1 to 4 hours. (4) After the reaction is complete, the resulting solution is cooled and filtered to remove the insoluble residue, which has been confirmed to be mainly the iron oxide that was added as a raw material.
[0015] (Iron oxide) The iron-based raw material used in the present invention is iron oxide. Here, iron oxide is a general term for oxides of iron, and is known to have different compositions such as ferrous oxide, ferric oxide, and triiron tetroxide depending on the oxidation number. Ferrous oxide is iron(II) oxide (FeO) and is known as wüstite, ferric oxide is iron(III) oxide (Fe2O3) and is known as hematite or maghemite, and triiron tetroxide is iron(II,III) oxide and is known as magnetite. Magnetite is an iron compound that is easily available as a raw material, as it is found in large amounts in slag from the copper smelting process and in natural ores. It also has the characteristic that it is easy to obtain concentrates by magnetic separation, as it is magnetic. Wustite is a flammable black solid at room temperature and pressure, and hematite or maghemite is also a major component of rust. Both are collected as ores. In the present invention, examples are shown for magnetite and wustite, but there are no examples for hematite or maghemite. However, in the above-mentioned Patent Document 2, magnetite and hematite are dissolved in sulfuric acid under high temperature and high pressure to produce a ferric sulfate solution. For this reason, it is technically clear that the method for producing polyferric sulfate of the present invention can be generally applied to iron oxide as the iron raw material.
[0016] (molar ratio of sulfate ions to total iron) In the present invention, it is necessary to set the molar ratio of sulfate ions to total iron in the iron oxide and sulfuric acid solution charged into a sealed vessel as raw materials to less than 1.5. When a large amount of sulfuric acid is added to give priority to dissolving iron oxide, as has been done in the prior art, a polyferric sulfate solution cannot be produced. The inventors of the present invention know from experience that unless the molar ratio is set to less than 1.5, the desired polyferric sulfate solution cannot be produced.
[0017] (Reaction temperature and pressure) The temperature inside the container is preferably adjusted to 100° C. or higher. If the reaction temperature is less than 100°C Iron oxide The dissolution and oxidation reactions do not proceed sufficiently. The reaction pressure in the present invention may be set as a practical condition taking into consideration production costs, etc., and generally, a reaction pressure of 0.3 MPa or more is sufficient. When the reaction is carried out at 0.2 MPa, a relatively large amount of residue consisting of compounds of iron and sulfuric acid is generated, which is undesirable because it reduces the recovery rate of the produced polyferric sulfate solution and the total iron concentration contained in the polyferric sulfate.
[0018] (Oxidation catalyst) In the present invention, an oxidation catalyst can be placed in a closed vessel together with the reaction raw materials. In the present invention, the oxidation reaction in the reaction in the sealed vessel is promoted by oxygen displacing the gas phase, the reaction rate is improved, and polyferric sulfate with a high total iron concentration is produced. If an oxidation catalyst is present in the sealed vessel where the atmosphere is substituted with oxygen, the oxidation of the divalent iron ions dissolved in the sulfuric acid can be further promoted, and the production efficiency of polyferric sulfate can be improved, which is preferable. The oxidation catalyst may be any catalyst that has the ability to oxidize dissolved divalent iron ions, such as sodium nitrite and potassium nitrate, but it is most preferable to use nitric acid as the catalyst, since it is believed to function as an oxidizing agent in addition to its function as an oxidation catalyst.
[0019] (Dissolution and oxidation reactions) When the iron-based raw material dissolves and the oxidation reaction of the divalent iron ions starts under high temperature and high pressure conditions in a closed vessel, the oxygen in the gas phase acts as an oxidizing agent. Also, if there is an oxidation catalyst in the raw material liquid, it acts as a catalyst, and if the oxidation catalyst is nitric acid, it also acts as an oxidizing agent. When oxygen replacement and catalyst addition are used in combination, a highly concentrated polyferric sulfate solution that could not be predicted based on conventional technical knowledge can be formed due to the synergistic effect of oxygen and the catalyst under high temperature and pressure conditions.
[0020] The inventors of the present invention speculate that the reason why the present invention enables efficient production of highly concentrated polyferric sulfate in a short period of time, which was not achievable by conventional techniques, is as follows. However, the technical interpretation of the present invention is not restricted by this speculation in any way. In a conventional method for producing ferric sulfate, an iron oxide raw material is dissolved in a high-temperature, high-pressure sulfuric acid solution in a pressure vessel to form a solution containing divalent and trivalent iron ions, and after this solution is removed from the pressure vessel, an oxidizing agent is added to oxidize the remaining divalent iron ions to produce a polyferric sulfate solution (Patent Document 1). However, with this method, some of the divalent iron ions formed in the pressure vessel react with sulfuric acid to form iron-sulfuric acid compounds that precipitate out of the reaction solution. In the present invention, oxygen gas present in a sealed container immediately acts as an oxidant on the ferrous ions dissolved in the container, preventing the precipitation of the ferrous ions as ferric sulfate compounds and making it possible to efficiently form highly concentrated polyferric sulfate. This is a new technical finding made by the present inventors, and the present invention was made based on this finding. EXAMPLES
[0021] [Example 1] In a 1L sealed container, add 221g of magnetite, sulfuric acid, and SO4 2-The molar ratio of iron ions to iron ions was 1.3, and 2.7 g of nitric acid was added as a catalyst. The sealed container was closed, and the gas phase in the sealed container was replaced with oxygen. Using a heater and an oxygen cylinder equipped in the sealed container, the temperature of the slurry was increased to 130°C and the pressure of the gas phase in the sealed container to 1.0 MPa, and the reaction was carried out for 1 hour. During the reaction, the temperature and pressure of the gas phase in the sealed container were maintained at 130°C and 1.0 MPa. After 1 hour of reaction, the slurry was separated from the sealed container and cooled. The end point of the reaction was determined by measuring the concentration of ferrous iron contained in the cooled slurry, and the slurry was then filtered to obtain a polyferric sulfate product.
[0022] The obtained polyferric sulfate had a high total iron concentration (T-Fe) of 15.9%. 2+ ) was less than 0.01%, and all the iron ions had been oxidized to trivalent ions. The sulfate ion concentration was 36.7%, and SO4 2- The molar ratio of iron / T-Fe was 1.34. The ratio of iron distributed from the raw material to the product (iron dissolution rate) was 91.9%. The residue was magnetite. Divalent iron ion concentration (Fe 2+ ) was less than 0.01%, which indicates that the reaction to produce polyferric sulfate was completed within an hour. 2- Since the / T-Fe molar ratio was 1.34, which is smaller than 1.5, it is clear that polyferric sulfate was formed.
[0023] [Example 2] (Reactor gas phase pressure: 0.3 MPa) The reaction was carried out under the same conditions as in Example 1, except that the pressure of the gas phase in the sealed vessel was 0.3 MPa and the reaction time was 2 hours, and the resulting slurry was cooled. The end point of the reaction was determined by measuring the concentration of ferrous iron contained in the cooled slurry, and the slurry was then filtered to obtain a polyferric sulfate product.
[0024] The obtained polyferric sulfate had a high total iron concentration (T-Fe) of 14.7%. 2+ ) was less than 0.01%, and all the iron ions had been oxidized to trivalent ions. The sulfate ion concentration was 37.5%, and SO4 2- The molar ratio of iron / T-Fe was 1.48. The ratio of iron distributed from the raw material to the product (iron dissolution rate) was 84.5%. The residue was magnetite. Divalent iron ion concentration (Fe 2+ ) was less than 0.01%, which indicates that the reaction to produce polyferric sulfate was completed within 2 hours. 2- Since the / T-Fe molar ratio was 1.48, which is smaller than 1.5, it is clear that polyferric sulfate was formed.
[0025] [Example 3] (Low iron concentration raw material) In a 1L sealed container, 298g of magnetite with an iron concentration of 52.1% and sulfuric acid are mixed with SO4 2- The reaction was carried out under the same conditions as in Example 1, except that the molar ratio of iron ions to iron ions was 1.3 and the reaction time was 4 hours, and the resulting slurry was cooled. The end point of the reaction was determined by measuring the concentration of ferrous iron contained in the cooled slurry, and the slurry was then filtered to obtain a polyferric sulfate product.
[0026] The obtained polyferric sulfate had a high total iron concentration (T-Fe) of 16.3%. 2+ ) was less than 0.01%, and all the iron ions had been oxidized to trivalent ions. The sulfate ion concentration was 40.3%, and SO4 2- The molar ratio of iron / T-Fe was 1.44. The ratio of iron distributed from the raw material to the product (iron dissolution rate) was 83.6%. The residue was magnetite. Divalent iron ion concentration (Fe 2+ ) was less than 0.01%, which indicates that the reaction to produce polyferric sulfate was completed within 4 hours. 2-Since the / T-Fe molar ratio was 1.44, which is smaller than 1.5, it is clear that polyferric sulfate was formed.
[0027] [Example 4] (Wustite) In a 1L sealed container, add 210g of wustite (iron concentration: 74.2%), sulfuric acid, and SO4 2- The reaction was carried out under the same conditions as in Example 1, except that the molar ratio of iron ions to ferric ions was 1.3, and the resulting slurry was cooled. The end point of the reaction was determined by measuring the concentration of ferrous iron contained in the cooled slurry, and the slurry was then filtered to obtain a polyferric sulfate product.
[0028] The obtained polyferric sulfate had a high total iron concentration (T-Fe) of 14.6%. 2+ ) was less than 0.01%, and all the iron ions had been oxidized to trivalent ions. The sulfate ion concentration was 37.2%, and SO4 2- The molar ratio of iron / T-Fe was 1.48. The ratio of iron distributed from the raw material to the product (iron dissolution rate) was 84.1%. The residues were wustite, magnetite, and hematite. Divalent iron ion concentration (Fe 2+ ) was less than 0.01%, which indicates that the reaction to produce polyferric sulfate was completed within an hour. 2- Since the / T-Fe molar ratio was 1.48, which is smaller than 1.5, it is clear that polyferric sulfate was formed.
[0029] [Comparative Example 1] In a 1L sealed container, add 221g of magnetite, sulfuric acid, and SO4 2-The iron ions were added so that the molar ratio of iron ions to iron ions was 1.3. The gas phase in the sealed container was not replaced with oxygen, but the gas phase was kept as air, and the sealed container was closed. The temperature of the slurry was raised to 130°C using a heater equipped in the sealed container, and the reaction was carried out for 4 hours. During the reaction, the temperature in the sealed container was kept at 130°C, and the pressure was maintained by steam pressure (about 0.2 MPa). After the reaction time had elapsed for 4 hours, the slurry was separated from the sealed vessel and cooled.
[0030] The concentration of ferrous iron contained in the cooled slurry was measured, and it was confirmed that ferrous iron remained. Therefore, even though the reaction was continued for 4 hours, the reaction to produce polyferric sulfate was not completed. In order to complete the reaction, the slurry was filtered, and then 41.7 g of hydrogen peroxide was added to the filtrate to complete the oxidation of ferrous iron, thereby obtaining the product polyferric sulfate. The total iron concentration (T-Fe) of the obtained polyferric sulfate was 14.2%, and the divalent iron ion concentration (Fe 2+ ) is less than 0.01%, sulfate ion concentration is 33.3%, SO4 2- The molar ratio of Fe / T-Fe was 1.36. The percentage of iron distributed from the raw material to the product (iron dissolution rate) was 76.1%. The residue was szomolnokite (Fe(SO4)(H2O)).
[0031] [Comparative Example 2] The reaction was carried out under the same conditions as in Comparative Example 1, except that 2.7 g of nitric acid was added as a catalyst to the slurry before heating, and the resulting slurry was cooled. The concentration of ferrous iron contained in the cooled slurry was measured, and it was confirmed that ferrous iron remained. Therefore, the slurry was filtered, and then 33.5 g of hydrogen peroxide was added to the filtrate to complete the oxidation of the ferrous iron, thereby obtaining the product polyferric sulfate. The total iron concentration (T-Fe) of the obtained polyferric sulfate was 13.7%, and the divalent iron ion concentration (Fe 2+ ) is less than 0.01%, sulfate ion concentration is 34.7%, SO4 2-The molar ratio of iron / T-Fe was 1.47. The percentage of iron distributed from the raw material to the product (iron dissolution rate) was 72.4%. The residue was iron hydroxide sulfate (Fe(SO4)2H).
[0032] For Examples 1 to 4 and Comparative Examples 1 and 2, the iron raw material, reaction conditions, and properties of the produced polyferric sulfate are summarized in Table 1. In Examples 1 to 4, the reaction was completed within 1 to 4 hours, but in Comparative Examples 1 and 2, the oxidation reaction was not completed even after four hours of high temperature and high pressure, and the divalent iron remained unoxidized. Therefore, hydrogen peroxide was added to oxidize all of the divalent iron remaining in the slurry to trivalent iron. Therefore, the characteristics of the products in Comparative Examples 1 and 2 both represent the characteristics of the products after additional H2O2 is added to complete the oxidation reaction.
[0033] [Table 1]
[0034] In all of the slurries produced in Examples 1 to 4 and Comparative Examples 1 and 2, SO4 2- Since the / Fe ratio is less than 1.5, it is clear that polyferric sulfate is produced. However, the slurries in Examples 1 to 4 were subjected to the action of oxygen gas in a sealed container, and polyferric sulfate with a high total iron concentration of 14.6 to 16.3% was produced. This characteristic is an excellent characteristic that could not be obtained by conventional techniques as an inorganic flocculant, even without comparing it with the slurries in Comparative Examples 1 and 2. Moreover, it can be confirmed that polyferric sulfate is efficiently produced, as the reaction was completed within 1 hour in Examples 1 and 4, within 2 hours in Example 2 where the pressure inside the sealed container was 0.3 MPa, and within 4 hours in Example 3 where a raw material with a low iron concentration was used.
[0035] In contrast, it was clear that the production conditions of Comparative Examples 1 and 2 did not allow efficient production of polyferric sulfate in a short time, which is a feature of the present invention. That is, in Comparative Examples 1 and 2, even though the reaction for producing polyferric sulfate was continued for 4 hours under high-temperature and high-pressure conditions, divalent iron remained without being oxidized, and it was necessary to add aqueous hydrogen peroxide to oxidize all of this to trivalent iron. Furthermore, a relatively large amount of insoluble residue is generated, and polyferric sulfate is not efficiently produced. This is because much of the iron that is not incorporated into polyferric sulfate is precipitated as insoluble residue, as shown by the low iron dissolution rate in Comparative Examples 1 and 2. This also makes clear the technical significance of replacing the gas phase in the sealed container with oxygen in the present invention.
[0036] From the above results, it is clear that the method for producing polyferric sulfate of the present invention achieves the remarkable effect of efficiently producing polyferric sulfate having high sludge flocculation ability in a short period of time when the air in a sealed container is replaced with oxygen gas. [Industrial Applicability]
[0037] Regarding flocculants used in the treatment of wastewater such as sewage, since flocculants with high flocculation performance can be produced in a short period of time, they can be widely used in the field of wastewater treatment.
Claims
1. A method for producing polyferric sulfate using iron oxide as an iron-based raw material, comprising: charging iron oxide powder, the molar ratio of sulfate ions to total iron being adjusted to less than 1.5, and a sulfuric acid solution into a sealed container; replacing the gas phase in the sealed container with oxygen; and then carrying out an oxidation reaction at a pressure of 0.3 MPa or more and a temperature of 100° C. or more.
2. 2. The method for producing polyferric sulfate according to claim 1, wherein magnetite or wustite is used as the iron-based raw material.
3. The method for producing polyferric sulfate according to any one of claims 1 to 2, further comprising adding a catalyst.
4. 4. The method for producing polyferric sulfate according to claim 3, wherein the catalyst is nitric acid.
5. A method for producing polyferric sulfate described in any one of claims 1 to 4, which produces high-concentration polyferric sulfate having a total iron concentration of 14.5% or more by carrying out an oxidation reaction in the presence of a nitric acid catalyst.
6. 6. The method for producing polyferric sulfate according to claim 5, wherein the production of polyferric sulfate is completed within 4 hours.
Citation Information
Patent Citations
Method to efficiently produce iron(III) polysulfate
JP1999292545A
Method for producing iron-based inorganic flocculant
JP3379204B2
Manufacturing method of ploy ferric sulfate
KR1020020086450A
Process for making liquid ferric sulfate
US4814158A
Process for the manufacturing of ferric sulfate
US8658124B1