Process for recovering various metals from complex rare and precious materials by full-wet method
By using an aqueous phase system free of sodium salts, cyanides, nitrogen oxides, and sulfides, combined with ion exchange technology and distillation concentration, the problem of efficient recovery of precious metals from complex rare and precious materials is solved. This achieves high enrichment ratio and high recovery rate, avoids wastewater generation, and is suitable for the whole-process wastewater-free treatment of high-selenium and low-tellurium precious metal materials.
Patent Information
- Application Number
- CN202411128723.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-16
AI Technical Summary
Existing technologies, when processing complex and rare materials, suffer from low leaching rates of platinum, palladium, and rhodium during the chlorination process, making enrichment difficult. Filtering of chlorination residue is also challenging, as gold, platinum, palladium, and rhodium are easily encapsulated and lost. Furthermore, the gold extraction wastewater is difficult to treat, and the neutralization residue cannot be recycled.
Using a sodium-free, cyanide-free, nitrogen oxide-free, and sulfide-free aqueous phase system, combined with ion exchange technology and distillation concentration, the system achieves the regeneration and recycling of hydrochloric acid and water through steps such as chlorination dissolution, gold loading, reduction, low-temperature distillation, high-temperature distillation, and directional crystallization, thereby avoiding wastewater generation and improving the recovery rate of precious metals.
It achieves a high enrichment ratio and high recovery rate of precious metals, avoids wastewater generation, has a short process, and is suitable for the whole process of wastewater-free treatment of high selenium and low tellurium precious metal materials, and improves the separation efficiency of platinum, palladium and rhodium.
Smart Images

Figure CN119020594A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of comprehensive recovery of rare and precious metals, and specifically relates to a process for fully wet recovery of multiple metals from complex rare and precious materials. Background Art
[0002] During the non-ferrous metal smelting process, non-ferrous metals are enriched in the anode mud along with gold, platinum, palladium, rhodium, selenium, tellurium, etc. After the anode mud is treated by wet method, a product enriched with gold, platinum, palladium, rhodium, selenium and tellurium is often produced, such as crude gold powder and platinum-palladium concentrate. These products are intermediate products containing rare precious metals obtained by reducing the solution after chlorination of the anode mud for gold extraction.
[0003] Complex rare and precious materials containing gold, platinum, palladium, rhodium, selenium and tellurium are treated by the following conventional wet process: complex precious metal materials - aqueous solution chlorination dissolution - purification - reduction - gold powder (gold grade ≤ 99.9%), and the ammonium chloropalladate method is used to precipitate platinum, palladium and part of rhodium in the reduced liquid, and tellurium and selenium are recovered separately in the reduced liquid. Conventional processes can well separate tellurium bismuth and precious metals, but there are problems:
[0004] First, the low dissolution rate of platinum, palladium and rhodium during the chlorination gold separation process leads to dispersion, difficulty in enrichment and low subsequent recovery rate;
[0005] Second, the chlorinated slag is difficult to filter, and gold, platinum, palladium, and rhodium are easily entrained and lost;
[0006] Third, gold extraction wastewater is difficult to treat and requires the addition of a large amount of neutralizing agents to produce neutralized slag containing gold, platinum and palladium. The high-chloride and salt-containing wastewater after neutralization cannot be recycled. Summary of the invention
[0007] In view of this, in order to solve this problem, the present invention discloses a process for fully wet recovery of multiple metals from complex rare and precious materials, that is, there is no sodium salt, no cyanide, no nitrogen oxide, and no sulfide in the aqueous phase system, which creates conditions for the coordination of ion exchange technology and distillation concentration, realizes the regeneration cycle of hydrochloric acid and water, and outputs gold powder with a gold content of more than 99.99%, so that precious metals, especially from rare and precious materials with relatively high contents of platinum, palladium, and rhodium, can be processed to obtain a high enrichment ratio of these metals (the liquid phase enrichment ratio after the precious metals are dissolved is greater than 30), without generating wastewater in the whole process, with a short process and a high recovery rate of precious metals.
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] A process for fully wet recovery of multiple metals from complex rare and precious materials, comprising the following steps:
[0010] Step 1: Chlorination dissolution, add hydrochloric acid aqueous solution and complex rare and precious materials into the reactor for stirring reaction, heat up to 60-70°C, slowly add oxidant, add a small amount of complex rare and precious materials after the reaction is completed, stir to eliminate chlorine, stop stirring to clarify, extract the upper chlorinated liquid clarified liquid into gold loading, and the precipitated chlorinated slag is used as the raw material for recovering silver; the technical conditions are controlled as follows: hydrochloric acid aqueous solution concentration 5-7 mol / L, liquid-to-solid ratio 3-6:1, oxidation process temperature 80-95°C;
[0011] Step 2: gold loading, using two-stage countercurrent loading of gold, after the chlorinated solution is loaded, a gold-loaded liquid and a loaded liquid are obtained, the gold-loaded liquid is reduced, and static separation is performed after reduction to the end point to clarify the organic phase, and the precipitate is filtered to separate the reduced liquid and the sponge gold; the reduced liquid is evaporated and concentrated to produce a concentrated liquid 1 and a condensate;
[0012] Step 3: Cooling the concentrated solution 1 in step 2 to <30°C, stirring and crystallizing, filtering to obtain a crystallized solution and residual oxalic acid, wherein the crystallized solution is returned to the gold loading process in step 2, and the residual oxalic acid is returned to the reduction process of the gold loading solution in step 2;
[0013] Step 4: low temperature distillation, the liquid after loading in step 2 is subjected to low temperature distillation to distill out low acid condensate and high acid condensate, the high acid condensate is returned to step 1 as hydrochloric acid input, the low acid condensate enters step 6 for washing, and the residual liquid after distillation is the concentrated liquid 2;
[0014] Step 5: high temperature distillation, subjecting the concentrated solution 2 of step 4 to high temperature distillation to remove residual water to obtain a concentrated solution 3;
[0015] Step 6: Directional crystallization and centrifugal filtration: the concentrated solution 3 is subjected to direct crystallization and centrifugal filtration to obtain crystal residue and selenious acid;
[0016] Step 7: washing, the crystal slag is washed with cold water or the low-acid condensate produced in step 4, and filtered to obtain tellurium slag and palladium, platinum and rhodium rich solution.
[0017] The chemical equation for the reaction in step 1 is as follows:
[0018] 7Au+3HClO4+25Cl - +21H - =7[AuCl4] -1 +12H2O
[0019] The beneficial effects are: it can avoid the chlorine-driving operation in the chlorination dissolution process of other technologies, which brings about the problems of long reaction time and poor on-site environment; by retaining the chlorination residue for rechlorination, the gold leaching effect during chlorination dissolution is improved, the number of filtration times of the chlorination residue is reduced, and the gold loss in the filtration process is avoided.
[0020] Preferably, the complex rare and precious material components include, by mass percentage: selenium 3-20%, tellurium 3-40%, gold ≥1%, platinum ≥0.1%, palladium ≥0.1%, rhodium ≥0.005%, and other impurities <30%. The selenium, tellurium, gold, platinum, palladium and rhodium all exist in the form of single phases.
[0021] Preferably, the specific operation of gold loading in step 1 is: controlling the flow ratio of the loading agent: the chlorinated liquid to be 1:0.8-8, using the loading reverse tower 1 and the loading tower 2, and adopting a two-stage loading reactor to countercurrently load the gold, and obtaining a gold-loaded liquid and a post-loaded liquid after loading, and sending the gold-loaded liquid into a reduction reactor for reduction, and performing static separation after reduction to the end point, standing for more than 10 minutes, separating the organic phase, and filtering the precipitate to separate the reduced liquid and the sponge gold; the reduced liquid is evaporated and concentrated to produce a concentrated liquid 1 and a condensate; the concentrated liquid 1 is returned to the reduction process, and the condensate is returned to step 1 to supplement the hydrochloric acid aqueous solution.
[0022] Preferably, the second-level loading reactor in step 2 includes a first-level loading reactor and a second-level loading reactor. A potentiometer is installed at the water phase outlet of the first-level loading reactor to monitor the potential value of the water phase. When the potential value is reduced to <520mV, the introduction of the chlorinated solution is stopped. At this time, the first-level gold-carrying liquid is pumped to the reduction reactor for reduction, and the second-level loading reactor is switched to the first-level loading reactor.
[0023] Upload the reaction below:
[0024] R+HAuCl4=[RH + ][AuCl4 - ]
[0025] Preferably, in step 2, the gold-carrying liquid is sent into a reactor for reduction, the temperature is controlled at 90-95° C., and the gold-carrying liquid contains less than 0.1 g / L of gold at the end of reduction; and the reducing agent is oxalic acid.
[0026] The reduction reaction is as follows:
[0027] 3H2C2O4+2[RH + ][AuCl4 - ]=2Au+6CO2+8H + +8Cl - +2R
[0028] Preferably, in step 4, the liquid temperature in the low-temperature distillation tower is controlled to be 60-75° C., and the pressure in the distillation tower is controlled to be 55-65 kPa.
[0029] Preferably, in step 5, the high temperature distillation temperature is 90-100° C., and the pressure in the evaporator is 60-80 kPa.
[0030] Preferably, the temperature of directional crystallization in step 6 is 75-80°C.
[0031] The principle of phase-fixed crystallization is: after high-temperature distillation, the free water and hydrochloric acid in the loaded liquid are distilled dry, and the remaining parts are platinum chloride, palladium chloride, rhodium chloride, tellurium chloride and selenious acid. When the temperature drops to 75-80°C, except for selenious acid, the others are precipitated in the form of solids. Directed crystallization separates precious metals and tellurium from selenium.
[0032] Preferably, the crystalline slag is washed with cold water to dissolve the soluble precious metal salts into the palladium, platinum and rhodium rich solution to separate them from tellurium. The obtained palladium, platinum and rhodium rich solution has a high concentration of precious metals and contains tellurium as an impurity. It can be used as a liquid raw material for separating and purifying palladium, platinum and rhodium. The palladium extraction, platinum extraction and reduction precipitation of rhodium can be used to separate and purify palladium, platinum and rhodium to obtain corresponding products or high-grade concentrates.
[0033] Preferably, in step 1, the oxidant is perchloric acid with a concentration of 26-30%, and the oxidant is added in an amount of 2.5-4 times the total amount of gold, selenium and tellurium in the input material.
[0034] Preferably, the carrier is a mixture of methyl isobutyl ketone (MIBK) and TBP, and the diluent is a mixture of one or both of n-dodecane and sulfonated kerosene and chloroform.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The present invention proposes a zero-discharge technology for wastewater, i.e., there is no sodium salt, no cyanide, no nitrogen oxides, and no sulfide in the aqueous phase system, which creates conditions for the coordination of ion exchange technology and distillation concentration and realizes the regeneration cycle of hydrochloric acid and water.
[0037] (2) The present invention has strong adaptability to complex materials containing gold, platinum, palladium, rhodium, selenium and tellurium, and is particularly suitable for materials with high selenium and low noble metal content. It can obtain a higher direct yield and recovery, and separate selenium and tellurium from the solution to obtain a higher concentration of platinum, palladium, rhodium and rhodium noble liquid, which is convenient for further extraction of these metals. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0039] Figure 1 This is a process flow chart for fully wet recovery of multiple metals from complex rare and precious materials disclosed in the present invention. DETAILED DESCRIPTION
[0040] Embodiments of the present invention are described below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but are not to be construed as limiting the present invention.
[0041] Example 1
[0042] 100 kg of rare and precious materials including 3.0% selenium, 37.3% tellurium, 1.16% gold, 0.107% platinum, 0.31% palladium and 0.0052% rhodium were added, and the operating steps of Example 1 were as follows:
[0043] Step 1: Chlorination dissolution, add 355kg of 36% hydrochloric acid in the reactor at a liquid-solid ratio of 5:1, then add water to prepare 500ml of 7mol / L hydrochloric acid solution, then start the agitator, slowly add complex rare and precious materials for stirring, heat to 60°C, slowly add 47kg of 28% perchloric acid, control the oxidation temperature to 82°C, after the reaction is completed, add 3kg of complex rare and precious materials for stirring to eliminate chlorine, stop stirring for clarification, extract the upper chlorinated liquid clarified liquid into the gold loading, and leave the precipitated chlorinated slag in the kettle to continue chlorination dissolution with the next batch of materials. After two cycles, filter to obtain 3.2kg of chlorinated slag as the raw material for recovering silver. The weight composition of the chlorinated slag is: 0.188% gold, 0.066% platinum, 0.0165% palladium, 0.0012% rhodium, 11.73% tellurium, 1.65% selenium, 28.67% silver, and 7.35% lead, and 461L of the chlorinated liquid clarified liquid is produced (containing 2.59g / L gold, 0.234g / L platinum, 0.693g / L palladium, 0.0112g / L rhodium, 82.7g / L tellurium, and 6.61g / L selenium).
[0044] Step 2: Recovery of gold: The loading agent is prepared according to MIBK: TBP: sulfonated kerosene: chloroform in a ratio of 30%: 10%: 50%: 10%. The chlorinated liquid in step 1 is loaded with gold in a two-stage (first and second stage) countercurrent manner according to a loading agent: chlorinated liquid flow ratio of 1:8. A potentiometer is installed at the outlet of the water phase of the first-stage loading reactor to monitor the potential value of the water phase. When the potential value drops to 508mV, the chlorinated liquid is stopped from being introduced. At this time, the first-stage gold loading liquid is pumped to the reduction reactor for reduction, and the second-stage loading is switched to the first-stage loading. After loading, 58L of gold-loaded liquid and 460.6L of post-loaded liquid are obtained. The gold-loaded liquid contains 20.58g / L of gold, and platinum, palladium, and rhodium are all less than 0.001g / L. It is sent to the reducer for reduction. The reducing agent is oxalic acid, which is prepared into 20L of 80g / l oxalic acid solution. The reduction temperature is 90°C. The gold-loaded liquid at the end of reduction contains 0.01g / L of gold. After reduction to the end point, static separation is performed. After standing for more than 10 minutes, the organic phase and the coarse gold powder mixed with the post-reduction liquid are separated by filtration to separate 19.5L of post-reduction liquid and 1.192kg of sponge gold, with a gold grade of 99.996%. The post-reduction liquid enters the evaporator for evaporation and concentration, and produces a concentrated liquid 1 (3L) and a condensate (16L). The concentrated liquid 1 returns to the reduction process, and the condensate returns to step 1.
[0045] Step 3: The concentrated solution 1 is cooled to 26°C and stirred for crystallization. After filtration, a crystallized solution and residual oxalic acid are obtained. The crystallized solution is returned to the gold loading process in step 2, and the residual oxalic acid is returned to the reduction process of the gold loading solution in step 2.
[0046] Step 4: Low temperature distillation: The loaded liquid in step 2 is pumped into a low temperature vacuum evaporator, the liquid temperature in the low temperature distillation tower is controlled at 65°C, the pressure in the distillation tower is controlled at 55 kPa, and 143.2 L of low acid condensate (containing 0.0001 g / L gold, 0.0001 g / L platinum, 0.0001 g / L palladium, 0.0001 g / L rhodium, 2.2 g / L tellurium, and 0.12 g / L selenium) and 113 L of high acid condensate (containing <0.0001 g / L gold, <0.0001 g / L palladium, <0.0001 g / L rhodium, 2.21 g / L tellurium, 0.1 g / L selenium, and 0.12 g / L H2O) are distilled out. + The high-acid condensate is returned to step 1 as hydrochloric acid, and the low-acid condensate enters step 6 for washing to produce a concentrated solution 2 (204.4 L), containing 0.0026 g / L gold, 0.527 g / L platinum, 1.56 g / L palladium, 0.0251 g / L rhodium, 184.86 g / L tellurium, and 14.77 g / L selenium.
[0047] Step 5: High-temperature distillation: The concentrated liquid 2 of step 4 is transferred to a high-temperature evaporator, the temperature is further increased to 96°C, the pressure in the evaporator is controlled to be 68 kPa, and the residual water is removed until crystals are produced to produce a concentrated liquid 3.
[0048] Step 6: directional crystallization and centrifugal filtration: The concentrated solution 3 (63 L) released in step 5 contains 0.0017 g / L of gold, 1.705 g / L of platinum, 4.93 g / L of palladium, 0.079 g / L of rhodium, 585.93 g / L of tellurium, and 45.0 g / L of selenium. The concentrated solution is cooled to 76°C and directional crystallized to obtain 58.45 kg of crystal slag (containing 0.0002% of gold, 0.184% of platinum, 0.53% of palladium, 0.0084% of rhodium, 62.78% of tellurium, and 0.39% of selenium) and 4.3 L of selenious acid (containing 0.0004 g / L of gold, 0.04 g / L of platinum, 0.159 g / L of palladium, 0.0067 g / L of rhodium, 50.64 g / L of tellurium, and 606.25 g / L of selenium).
[0049] Step 7: Wash the crystallized slag in step 6 with cold water or the low-acid condensate produced in step 4, control the pH value in the washing process to be 2-3, and filter after washing to obtain 63.4 kg of tellurium slag (containing gold <0.0001%, platinum <0.0001, palladium 0.001%, rhodium <0.0001%, tellurium 56.55%, selenium 0.19%) and palladium-platinum-rhodium rich solution (containing gold 0.004 g / L, platinum 4.52 g / L, palladium 13.11 g / L, rhodium 0.209 g / L, tellurium 35.76 g / L, selenium 4.491 g / L).
[0050] Comparative Example 1: Implementation method:
[0051] For the components of the waste acid treated in Example 1, an aqueous solution chlorination method is used to dissolve the precious metal-containing chlorinated solution - neutralize and adjust pH - reduce and precipitate gold - precipitate platinum and palladium with ammonium chloropalladate. The specific operation steps are as follows:
[0052] (1) According to a liquid-to-solid ratio of 5:1, 60 g / L hydrochloric acid and 15 kg sodium chlorate were added, the temperature was controlled at 95°C, and the mixture was stirred for 4 hours to dissolve, thereby obtaining 452 L of chlorinated liquid (containing 2.46 g / L gold, 0.65 g / L palladium, 0.33 g / L platinum, 0.01 g / L rhodium, 5.37 g / L selenium, and 79.72 g / L tellurium) and 18.6 kg of chlorinated slag (0.477% gold, 0.14% palladium, 0.0037% rhodium, 0.033% platinum, 13.24% tellurium, and 3.51% selenium).
[0053] (2) The chlorinated liquid obtained in step (1) was neutralized to pH=3 by adding sodium hydroxide, and filtered to obtain 449 L of neutralized liquid (containing 2.2 g / L gold, 0.22 g / L platinum, 0.63 g / L palladium, 0.01 g / L rhodium, 75.84 g / L tellurium, and 5.38 g / L selenium) and 3.4 kg of neutralized slag, containing 2.05% gold, 0.153% platinum, 0.322% palladium, 0.0009% rhodium, 58.3% tellurium, and 0.34% selenium.
[0054] (3) The neutralized liquid produced in step (2) was heated to 86-90° C., and 0.3 kg of oxalic acid was added for reduction to obtain about 0.988 kg of gold powder with a gold grade of 99.9%, and 445 L of reduced liquid was produced.
[0055] (4) Step (3) produces a reduced solution, controls the temperature at 57°C, slowly adds 8kg of sodium chlorate, produces 1.0kg of ammonium chloropalladate, containing 0.28% gold, 7.78% platinum, 24.72% palladium, 0.169% rhodium, 3.4% tellurium, and 1.1% selenium. Produces 445L of palladium precipitation solution, containing 0.519g / L gold, 0.061g / L platinum, 0.08g / L palladium, 0.0063g / L rhodium, 76.45 / L tellurium, and 5.1g / L selenium.
[0056] Effect comparison of embodiment 1:
[0057] Example 1 recovers 99.99% of gold powder from rare and precious materials containing 3.0% selenium, 37.3% tellurium, 1.16% gold, 0.107% platinum, 0.31% palladium, and 0.0052% rhodium, and recovers palladium, platinum, and rhodium rich liquid. The metal direct recovery rate is shown in Table 1. The direct recovery rate and recovery rate of each metal in Example 1 are better than those in Comparative Example 1. In addition, the method of Example 1 does not use reagents such as nitric acid, cyanide, sulfur dioxide, and alkali, and truly realizes the regeneration of acid, achieving the purpose of zero emission. Specific technical and economic indicators are shown in Table 1.
[0058] Table 1 Comparison of the effects of Example 1 and Comparative Example 1
[0059]
[0060] Example 2
[0061] For 100 kg of rare and precious materials containing 11.9% selenium, 17.8% tellurium, 15.0% gold, 0.146% platinum, 11.93% palladium, and 0.0064% rhodium, the operating steps of Example 2 are as follows:
[0062] Step 1: Chlorination dissolution: add 182.5 kg of 36% hydrochloric acid at a liquid-solid ratio of 3:1, add water into the reactor to prepare 300 L of hydrochloric acid solution containing 6 mol / L of hydrochloric acid, start stirring, slowly add complex rare and precious materials for stirring, heat to 65°C, slowly add 43 kg of 26% perchloric acid, control the oxidation process temperature at 88°C, after the reaction is completed, add 3 kg of complex rare and precious materials for stirring to eliminate chlorine, stop stirring for clarification, extract the upper chlorinated liquid clarified liquid into the gold loading, and leave the precipitated chlorinated slag in the reactor to continue chlorination dissolution with the next batch of materials. After three cycles, filter to obtain 2.7 kg of chlorinated slag, which is used as a raw material for recovering silver. The chlorinated slag obtained by filtration has the following components: 0.41% gold, 0.0011% platinum, 0.0957% palladium, 0.0041% rhodium, 11.65% tellurium, 1.82% selenium, 29.2% silver, 3.51% lead, and 296L of the chlorinated clarified liquid is produced (containing 41.52g / L gold, 0.51g / L platinum, 4.147g / L palladium, 0.0065g / L rhodium, 60.76g / L tellurium, 41.39g / L selenium).
[0063] Step 2: Recovery of gold: The loading agent is prepared according to MIBK: TBP: sulfonated kerosene: chloroform in a ratio of 35%: 5%: 55%: 5%. The chlorinated liquid in step 1 is loaded with gold in a two-stage (first and second stage) countercurrent manner according to a loading agent: chlorinated liquid flow ratio of 1:6. A potentiometer is installed at the outlet of the water phase of the first-stage loading reactor to monitor the potential value of the water phase. When the potential value drops to 512mV, the chlorinated liquid is stopped from being introduced. At this time, the first-stage gold loading liquid is pumped to the reduction reactor for reduction, and the second-stage loading is switched to the first-stage loading. After loading, 164L of gold-loaded liquid and 295L of post-loading liquid are obtained. The gold-loaded liquid contains 74.87g / L of gold, and platinum, palladium, and rhodium are all less than 0.001g / L. It is sent to the reducer for reduction. The reducing agent is oxalic acid, and 50L of 85g / l oxalic acid solution is prepared. The reduction temperature is 92°C. The gold-loaded liquid at the end of reduction contains 0.007g / L of gold. After reduction to the end point, static separation is performed. After standing for more than 10 minutes, the organic phase and the coarse gold powder mixed with the post-reduction liquid are separated by filtration to separate 49.6L of post-reduction liquid and 12.28kg of sponge gold, and its gold grade is 99.996%. The post-reduction liquid enters the evaporator for evaporation and concentration, and the concentrated liquid 1 (8L) and the condensate (41L) are produced. The concentrated liquid 1 returns to the reduction process, and the condensate returns to step 1.
[0064] Step 3: The concentrated solution 1 is cooled to 25°C and stirred for crystallization. After filtration, a crystallized liquid and residual oxalic acid are obtained. The crystallized liquid is returned to the gold loading process in step 2, and the residual oxalic acid is returned to the reduction process of the gold loading liquid in step 2.
[0065] Step 4: Low temperature distillation: The loaded liquid in step 2 is pumped into a low temperature vacuum evaporator, the liquid temperature in the low temperature distillation tower is controlled to be 70°C, the pressure in the distillation tower is controlled to be 61 kPa, and 124 L of low acid condensate (containing 0.0001 g / L gold, 0.0001 g / L platinum, 0.0001 g / L palladium, 0.0001 g / L rhodium, 0.0001 g / L tellurium, 0.876 g / L selenium) and 104 L of high acid condensate (containing <0.0001 g / L gold, <0.0001 g / L palladium, <0.0001 g / L rhodium, 1.34 g / L tellurium, 1.41 g / L selenium, 0.877 g / L H) are distilled out. + The high-acid condensate is returned to step 1 as hydrochloric acid, and the low-acid condensate enters step 6 for washing to produce a concentrated solution 2 (67L), containing 0.0147g / L gold, 2.227g / L platinum, 18.31g / L palladium, 0.096g / L rhodium, 263.67g / L tellurium, and 178.67g / L selenium.
[0066] Step 5: High-temperature distillation: The concentrated liquid 2 of step 4 is transferred to a high-temperature evaporator, the temperature is further increased to 96°C, the pressure in the evaporator is controlled to be 68 kPa, and the residual water is removed until crystals are produced to produce a concentrated liquid 3.
[0067] Step 6: directional crystallization and centrifugal filtration: The concentrated solution 3 (32 L) released in step 5 contains 0.306 g / L of gold, 4.66 g / L of platinum, 38.245 g / L of palladium, 0.200 g / L of rhodium, 545.35 g / L of tellurium, and 372.67 g / L of selenium. The concentrated solution is cooled to 73°C and directional crystallized to obtain 27.36 kg of crystal slag (containing 0.035% of gold, 0.544% of platinum, 4.467% of palladium, 0.023% of rhodium, 63.407% of tellurium, and 3.504% of selenium) and 16.83 L of selenious acid (containing 0.0004 g / L of gold, 0.04 g / L of platinum, 0.159 g / L of palladium, 0.0067 g / L of rhodium, 50.64 g / L of tellurium, and 606.25 g / L of selenium);
[0068] Step 7: Wash the crystallized slag in step 6 with cold water or the low-acid condensate produced in step 4, control the pH value in the washing process to be 2-3, and filter after washing to obtain 63.4 kg of tellurium slag (containing gold <0.0001%, platinum <0.0001, palladium 0.001%, rhodium <0.0001%, tellurium 56.55%, selenium 0.19%) and palladium-platinum-rhodium rich solution (containing gold 0.004 g / L, platinum 4.52 g / L, palladium 13.11 g / L, rhodium 0.209 g / L, tellurium 35.76 g / L, selenium 4.491 g / L).
[0069] Comparative Example 2: Implementation method:
[0070] For the components of the waste acid treated in Example 2, an aqueous solution chlorination method is used to dissolve the precious metal-containing chlorinated solution - neutralize and adjust pH - reduce and precipitate gold - precipitate platinum and palladium with ammonium chloropalladate. The specific operation steps are as follows:
[0071] (1) According to the liquid-to-solid ratio of 3:1, 80 g / L hydrochloric acid and 15 kg sodium chlorate were added, the temperature was controlled at 95°C, and the mixture was stirred for 4 hours to dissolve, thereby obtaining 297 L of chlorinated liquid (containing 48.9 g / L gold, 3.84 g / L palladium, 0.463 g / L platinum, 0.0197 g / L rhodium, 32.14 g / L selenium, and 56.87 g / L tellurium) and 16.3 kg of chlorinated slag (5.99% gold, 0.551% palladium, 0.0046% rhodium, 0.076% platinum, 8.64% tellurium, and 16.9% selenium).
[0072] (2) The chlorinated liquid obtained in step (1) was neutralized to pH = 2 by adding sodium hydroxide, and filtered to obtain 278 L of neutralized liquid (containing 51.96 g / L of gold, 4.212 g / L of palladium, 0.514 g / L of platinum, 0.0236 g / L of rhodium, 61.746 g / L of tellurium, and 5.38 g / L of selenium) and 4.8 kg of neutralized slag, containing 21.95% of gold, 4.7% of palladium, 0.15% of platinum, 0.0011% of rhodium, 23.64% of tellurium, and 0.34% of selenium.
[0073] (3) The neutralized liquid produced in step (2) was heated to 90°C, and 5 kg of oxalic acid was added to reduce the liquid to obtain about 14.446 kg of gold powder with a gold grade of 99.9%, and 273 L of reduced liquid was produced.
[0074] (4) Step (3) produces a reduced solution, controls the temperature at 59°C, slowly adds 6kg of sodium chlorate, produces 4.2kg of ammonium chloropalladate, containing 0.281% gold, 24.73% palladium, 3.0% platinum, 0.083% rhodium, 0.41% tellurium, and 0.22% selenium. , produces a palladium precipitation solution, containing 1.86g / L gold, 0.06g / L platinum, 0.49g / L palladium, 0.011g / L rhodium, 63.517g / L tellurium, and 34.7g / L selenium.
[0075] Effect comparison of Example 2:
[0076] 99.99% of gold powder was recovered from rare and precious materials containing 11.9% selenium, 17.8% tellurium, 15.0% gold, 0.146% platinum, 11.93% palladium, and 0.0064 rhodium, and palladium, platinum, and rhodium rich liquid was recovered. The metal direct recovery rate is shown in Table 2. The direct recovery rate and recovery rate of each metal in Example 2 are better than those in Comparative Example 2. In addition, the method of Example 2 is adopted without using reagents such as nitric acid, cyanide, sulfur dioxide, and alkali, which truly realizes the regeneration of acid and achieves the purpose of zero emission. The specific technical and economic indicators of the implementation are shown in Table 2.
[0077] Table 2 Comparison of the effects of Example 2 and Comparative Example 2
[0078]
[0079] Example 3
[0080] For 100 kg of rare and precious materials containing 19.2% selenium, 3.2% tellurium, 51.1% gold, 0.35% platinum, 2.17% palladium, and 0.0071% rhodium, the operating steps of Example 3 are as follows:
[0081] Step 1: Chlorination dissolution, according to the liquid-solid ratio of 6:1, add 365kg of 36% hydrochloric acid, add water to the reactor to prepare 600L of hydrochloric acid solution containing 6mol / L hydrochloric acid, start stirring, slowly add complex rare and precious materials for stirring, add aqueous solution containing hydrochloric acid and complex rare and precious materials to the reactor for stirring reaction, heat to 70°C, slowly add 48kg of 30% perchloric acid, control the temperature of the oxidation process at 95°C. After the reaction is completed, add 3kg of complex rare and precious materials for stirring and dechlorination, stop stirring for clarification, extract the upper chlorination liquid clarified liquid into the gold loading, and leave the precipitated chlorination residue in the kettle to continue chlorination dissolution with the next batch of materials. After 4 cycles, filter to obtain 2.4kg of chlorination residue as the raw material for recovering silver. The composition of the chlorinated slag obtained by filtration is: 1.98% gold, 0.003% platinum, 0.196% palladium, 0.005% rhodium, 2.37% tellurium, 3.3% selenium, 34.1% silver, 2.92% lead, and 597L of the chlorinated liquid clarified liquid is produced (containing 88.20g / L gold, 0.60g / L platinum, 3.74 / L palladium, 0.012g / L rhodium, 5.43g / L tellurium, 33.03g / L selenium).
[0082] Step 2: Recovery of gold: The loading agent is prepared according to MIBK: TBP: sulfonated kerosene: chloroform in a ratio of 40%: 5%: 50%: 5%. The chlorinated liquid described in step 1 is loaded with gold in a two-stage (first and second stage) countercurrent manner according to the loading agent: chlorinated liquid flow ratio of 1: 0.8. A potentiometer is installed at the outlet of the water phase of the first-stage loading reactor to monitor the potential value of the water phase. When the potential value drops to 503mV, the chlorinated liquid is stopped from being introduced. At this time, the first-stage gold loading liquid is pumped to the reduction reactor for reduction, and the second-stage loading is switched to the first-stage loading. After loading, 745L of gold-loaded liquid and 596L of post-loading liquid are obtained. The gold-loaded liquid contains 70.55g / L of gold, and platinum, palladium, and rhodium are all less than 0.001g / L. It is sent to the reducer for reduction. The reducing agent is oxalic acid, and 62L of 85g / L oxalic acid solution is prepared. The reduction temperature is 93°C. The gold-loaded liquid at the end of reduction contains 0.014g / L of gold. After reduction to the end point, static separation is performed. After standing for more than 10 minutes, the organic phase and the coarse gold powder mixed with the post-reduction liquid are separated by filtration to separate 61L of post-reduction liquid and 52.647kg of sponge gold, and the gold grade is 99.996%. The post-reduction liquid enters the evaporator for evaporation and concentration, and the concentrated liquid 1 (37L) and the condensate (706L) are produced. The concentrated liquid 1 returns to the reduction process, and the condensate returns to step 1.
[0083] Step 3: The concentrated solution 1 is cooled to 24°C and stirred for crystallization. After filtration, a crystallized solution and residual oxalic acid are obtained. The crystallized solution is returned to the gold loading process in step 2, and the residual oxalic acid is returned to the reduction process of the gold loading solution in step 2.
[0084] Step 4: Low temperature distillation: The loaded liquid in step 2 is pumped into a low temperature vacuum evaporator, the liquid temperature in the low temperature distillation tower is controlled at 62°C, the pressure in the distillation tower is controlled at 58 kPa, and 325 L of low acid condensate (containing 0.0001 g / L gold, 0.0001 g / L platinum, 0.0001 g / L palladium, 0.0001 g / L rhodium, 0.0001 g / L tellurium, 0.08 g / L selenium 0.539 g / L) and 184 L of high acid condensate (containing <0.0001 g / L gold, <0.0001 g / L palladium, <0.0001 g / L rhodium, 0.211 g / L tellurium, 1.50 g / L selenium, H + The high-acid condensate is returned to step 1 as hydrochloric acid input, and the low-acid condensate enters step 6 for washing to produce a concentrated solution 2 (87L), containing 0.042g / L gold, 4.116g / L platinum, 25.68g / L palladium, 0.082g / L rhodium, 36.39g / L tellurium, and 221.04g / L selenium.
[0085] Step 5: High-temperature distillation: The concentrated liquid 2 of step 4 is transferred to a high-temperature evaporator, the temperature is further increased to 98°C, the pressure in the evaporator is controlled to be 71 kPa, and the residual water is removed until crystals are produced to produce a concentrated liquid 3.
[0086] Step 6: directional crystallization and centrifugal filtration: The concentrated solution 3 (62 L) released in step 5 contains 0.058 g / L gold, 5.78 g / L platinum, 36.01 g / L palladium, 0.114 g / L rhodium, 48.62 g / L tellurium and 309.66 g / L selenium. It is cooled to 71°C and directional crystallized to obtain 27.36 kg of crystal slag (containing 0.035% gold, 0.544% platinum, 4.467% palladium, 0.023% rhodium, 63.407% tellurium and 3.504% selenium) and 16.83 L of selenious acid (containing 0.0004 g / L gold, 0.04 g / L platinum, 0.159 g / L palladium, 0.0067 g / L rhodium, 50.64 g / L tellurium and 606.25 g / L selenium).
[0087] Step 7: Wash the crystallized slag in step 6 with cold water or the low-acid condensate produced in step 4, control the pH value in the washing process to be 2-3, and filter after washing to obtain 5.8 kg of tellurium slag (containing gold <0.0001%, platinum <0.0001, palladium 0.001%, rhodium <0.0001%, tellurium 50.48%, selenium 14.24%) and palladium-platinum-rhodium rich solution (containing gold 0.117 g / L, platinum 13.70 g / L, palladium 85.52 g / L, rhodium 0.269 g / L, tellurium 2.65 g / L, selenium 27.61 g / L).
[0088] Comparative Example 3: Implementation method:
[0089] For the components of the waste acid treated in Example 3, an aqueous solution chlorination method is used to dissolve the precious metal-containing chlorinated solution - neutralize and adjust pH - reduce and precipitate gold - precipitate platinum and palladium with ammonium chloropalladate. The specific operation steps are as follows:
[0090] (1) According to the liquid-to-solid ratio of 6:1, 60 g / L hydrochloric acid and 22 kg sodium chlorate were added, the temperature was controlled at 90°C, and the mixture was stirred for 4 hours to dissolve, thereby obtaining 596 L of chlorinated liquid (containing 82.85 g / L gold, 0.554 g / L platinum, 3.84 g / L palladium, 0.011 g / L rhodium, 5.11 g / L tellurium, and 25.78 g / L selenium) and 14.2 kg of chlorinated slag (23.38% gold, 0.21% platinum, 1.15% palladium, 0.0059% rhodium, 1.79% tellurium, and 31.23% selenium).
[0091] (2) The chlorinated liquid obtained in step (1) was neutralized to pH = 2 by adding sodium hydroxide, and filtered to obtain 278 L of neutralized liquid (containing 51.96 g / L of gold, 0.514 g / L of platinum, 4.212 g / L of palladium, 0.0236 g / L of rhodium, 61.746 g / L of tellurium, and 5.38 g / L of selenium), and 9.2 kg of neutralized slag, containing 36.50% of gold, 0.136% of platinum, 0.835% of palladium, 0.0006% of rhodium, 1.72% of tellurium, and 2.51% of selenium.
[0092] (3) The neutralized liquid produced in step (2) was heated to 90° C., and 15 kg of oxalic acid was added for reduction to obtain about 46.02 kg of gold powder with a gold grade of 99.9% (after washing), and 593 L of reduced liquid was produced.
[0093] (4) Step (3) produces a reduced solution, controls the temperature at 59°C, slowly adds 6kg of sodium chlorate, produces 7.2kg of ammonium chloropalladate, containing 0.015% gold, 24.62% palladium, 3.90% platinum, 0.0476% rhodium, 0.04% tellurium, and 0.21% selenium. , produces 591L of palladium precipitation solution, containing 0.126g / L gold, 0.061g / L platinum, 0.38g / L palladium, 0.005g / L rhodium, 4.48g / L tellurium, and 25.60g / L selenium.
[0094] Effect comparison of Example 3:
[0095] 99.99% of gold powder was recovered from rare and precious materials containing 19.2% selenium, 3.2% tellurium, 51.1% gold, 0.35% platinum, 2.17% palladium, and 0.0071% rhodium, and palladium, platinum, and rhodium rich liquid was recovered. The direct recovery rates of each metal are shown in Table 3. The direct recovery rates and recovery rates of each metal in Example 3 are better than those in Comparative Example 3. In addition, the method of Example 3 is adopted without using reagents such as nitric acid, cyanide, sulfur dioxide, and alkali, which truly realizes the regeneration of acid and achieves the purpose of zero emission. The specific technical and economic indicators for implementation are shown in Table 3.
[0096] Table 3 The effects of Example 3 and Comparative Example 3 are compared in the following table:
[0097]
[0098] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples are used to further illustrate the technical features disclosed in the present invention, but they should not be construed as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without inventive work are also considered to fall within the scope of protection of the present invention.
[0099] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
[0100] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A process for fully wet recovery of multiple metals from complex rare and precious materials. It is characterized in that The following steps are involved: Step 1: Chlorination dissolution, add hydrochloric acid aqueous solution and complex rare and precious materials into the reactor for stirring reaction, heat up to 60-70°C, slowly add oxidant, add a small amount of complex rare and precious materials after the reaction is completed, stir to eliminate chlorine, stop stirring to clarify, extract the upper chlorinated liquid clarified liquid into gold loading, and the precipitated chlorinated slag is used as the raw material for recovering silver; the technical conditions are controlled as follows: hydrochloric acid aqueous solution concentration 5-7 mol / L, liquid-to-solid ratio 3-6:1, oxidation process temperature 80-95°C; Step 2: gold loading, using two-stage countercurrent loading of gold, after the chlorinated solution is loaded, a gold-loaded liquid and a loaded liquid are obtained, the gold-loaded liquid is reduced, and static separation is performed after reduction to the end point to clarify the organic phase, and the precipitate is filtered to separate the reduced liquid and the sponge gold; the reduced liquid is evaporated and concentrated to produce a concentrated liquid 1 and a condensate; Step 3: Cooling the concentrated solution 1 in step 2 to <30°C, stirring and crystallizing, filtering to obtain a crystallized solution and residual oxalic acid, wherein the crystallized solution is returned to the gold loading process in step 2, and the residual oxalic acid is returned to the reduction process of the gold loading solution in step 2; Step 4: low temperature distillation, the liquid after loading in step 2 is subjected to low temperature distillation to distill out low acid condensate and high acid condensate, the high acid condensate is returned to step 1 as hydrochloric acid input, the low acid condensate enters step 6 for washing, and the residual liquid after distillation is the concentrated liquid 2; Step 5: high temperature distillation, subjecting the concentrated solution 2 of step 4 to high temperature distillation to remove residual water to obtain a concentrated solution 3; Step 6: Directional crystallization and centrifugal filtration: the concentrated solution 3 is subjected to direct crystallization and centrifugal filtration to obtain crystal residue and selenious acid; Step 7: washing, the crystal slag is washed with cold water or the low-acid condensate produced in step 4, and filtered to obtain tellurium slag and palladium, platinum and rhodium rich solution.
2. According to claim 1, a process for fully wet recovery of multiple metals from complex rare and precious materials, It is characterized in that The complex rare and precious material components include, by mass percentage: selenium 3-20%, tellurium 3-40%, gold ≥1%, platinum ≥0.1%, palladium ≥0.1%, rhodium ≥0.005%, and other impurities <30%. The selenium, tellurium, gold, platinum, palladium, and rhodium all exist in the form of single phases.
3. According to claim 1, a process for fully wet recovery of multiple metals from complex rare and precious materials, It is characterized in that The specific operation of gold loading in step 1 is as follows: controlling the flow ratio of loading agent: chlorinated liquid to be 1:0.8-8, using loading reverse tower 1 and loading tower 2, adopting a two-stage loading reactor to countercurrently load gold, and obtaining gold-loaded liquid and loaded liquid after loading, the gold-loaded liquid is sent to a reduction reactor for reduction, and static separation is performed after reduction to the end point, and the organic phase is clarified, and the precipitate is filtered to separate the reduced liquid and sponge gold; the reduced liquid is evaporated and concentrated to produce a concentrated liquid 1 and a condensate; the concentrated liquid 1 is returned to the reduction process, and the condensate is returned to step 1 to supplement the hydrochloric acid aqueous solution.
4. The process for fully wet recovery of multiple metals from complex rare and precious materials according to claim 1, It is characterized in that In the step 2, the second-level loading reactor includes a first-level loading reactor and a second-level loading reactor. A potentiometer is installed at the water phase outlet of the first-level loading reactor to monitor the potential value of the water phase. When the potential value decreases to <520mV, the introduction of the chlorinated solution is stopped. At this time, the first-level gold-carrying liquid is pumped to the reduction reactor for reduction, and the second-level loading reactor is switched to the first-level loading reactor.
5. The process for fully wet recovery of multiple metals from complex rare and precious materials according to claim 1, It is characterized in that In step 2, the gold-carrying liquid is sent into the reactor for reduction, the temperature is controlled at 90-95° C., and the gold-carrying liquid contains less than 0.1 g / L of gold at the end of reduction; the reducing agent is oxalic acid.
6. The process for fully wet recovery of multiple metals from complex rare and precious materials according to claim 1, It is characterized in that In step 3, the liquid temperature in the low-temperature distillation tower is controlled to be 60-75° C., and the pressure in the distillation tower is controlled to be 55-65 kPa.
7. The process for fully wet recovery of multiple metals from complex rare and precious materials according to claim 1, It is characterized in that In step 4, the high temperature distillation temperature is 90-100° C., and the pressure in the evaporator is 60-80 kPa.
8. The process for fully wet recovery of multiple metals from complex rare and precious materials according to claim 1, It is characterized in that The temperature of the directional crystallization in step 4 is 75-80°C.
9. The process for fully wet recovery of multiple metals from complex rare and precious materials according to claim 1, It is characterized in that In step 1, the oxidant is perchloric acid with a concentration of 26-30%. The oxidant is added in an amount of 2.5-4 times the total amount of gold, selenium and tellurium in the input materials.
10. The process for fully wet recovery of multiple metals from complex rare and precious materials according to claim 1, It is characterized in that The carrier is a mixture of methyl isobutyl ketone (MIBK) and TBP, and the diluent is a mixture of one or both of n-dodecane and sulfonated kerosene and chloroform.
Citation Information
Patent Citations
Method of reclaiming platinum from selenium-containing waste liquid using hydrazine
CN101045962A
Process for extracting, separating and purifying Ag, Au, Pd and Pt
CN101748276A
Method for refining gold and silver
CN114410981A
Method for recovering valuable metals from complex copper anode slime selenium steaming slag
CN114892007A
Method for separating Te from Rh solution
CN1837384A
Cited By
Hydrometallurgical process for recovering a plurality of metals from complex rare and precious material
GB2645310A
Hydrometallurgical process for recovering a plurality of metals from complex rare and precious material
WO2026037437A1