Humidity measuring device, method for measuring equilibrium mass, method for obtaining equilibrium moisture content, and method for obtaining diffusion coefficient

The humidity measuring device facilitates simultaneous and rapid measurement of concrete equilibrium moisture content across multiple humidities, addressing the inefficiencies of traditional methods by using a novel device design for specimens and moisture agents.

JP7581090B2Active Publication Date: 2024-11-12TAIHEIYO CEMENT CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021039755
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-11
Publication Date
2024-11-12
Estimated Expiration
2041-03-11

AI Technical Summary

Technical Problem

Existing methods for obtaining equilibrium moisture content in concrete are time-consuming and prone to variations due to the use of multiple desiccators and test pieces, especially for concrete, which can take over 6 months to reach equilibrium, making them impractical.

Method used

A humidity measuring device with a housing that allows simultaneous measurement of multiple concrete specimens at different humidities using first and second arrangement parts for specimens and moisture agents, enabling quick and accurate equilibrium mass determination.

Benefits of technology

Enables rapid measurement of equilibrium moisture content in concrete at multiple humidities, reducing measurement time significantly and minimizing variations, allowing for efficient and precise moisture analysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581090000003
    Figure 0007581090000003
  • Figure 0007581090000004
    Figure 0007581090000004
  • Figure 0007581090000005
    Figure 0007581090000005
Patent Text Reader

Abstract

To provide a method, etc., with which it is possible to acquire the moisture content of concrete at a plurality of relative humidities in a short period at a time using one device.SOLUTION: The present invention includes a housing 11, the housing being constituted to allow the formation of a side wall 12, a closure part 14 having an opening 13 formed at one longitudinal end of the side wall and formed at the other longitudinal end of the side wall, a space part 15 situated between the opening to the closure part and enclosed by the inner wall surface of the side wall and the closure part, a plurality of first arrangement parts 16 in which a test piece of cementitious cured body is arranged, and a second arrangement part 17 in which a moisture releasing or a moisture absorbing agent is arranged. On the inner wall surface is formed an installation part in which a humidity measurer for measuring the humidity in a space partitioned by the test piece arranged in the first arrangement part can be installed, with the second arrangement part provided closer to the other end side than the first arrangement part.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an apparatus for measuring humidity in a space simulating the humidity environment inside concrete (hereinafter, sometimes abbreviated as "simulated space"), and a method for measuring equilibrium mass using the apparatus. Here, the equilibrium mass refers to the mass of a cementitious hardened body such as concrete when moisture absorption and release of the cementitious hardened body reach equilibrium. [Background technology]

[0002] In order to improve the long-term durability of concrete and extend its lifespan, it is important to know the moisture and humidity transfer characteristics inside concrete. One of the characteristic values ​​used to understand this moisture transfer characteristic is the equilibrium moisture content. The equilibrium moisture content is expressed as the ratio of the mass or volume of the evaporable moisture in a material to the mass or volume of the material when it is dry, when the material absorbs or releases water vapor around it and reaches equilibrium with the absorption and release of moisture. The diffusion coefficient obtained by substituting this equilibrium moisture content into the moisture flux equation of Fick's first law is a characteristic value required when performing simulations such as moisture transport analysis. In addition, by plotting multiple equilibrium moisture contents corresponding to multiple relative humidities, an equilibrium moisture content curve that represents the moisture absorption and desorption characteristics of a material can be obtained.

[0003] Currently, the method for obtaining the equilibrium moisture content is specified in JIS A 1475 "Method for measuring equilibrium moisture content of building materials" (Non-patent Document 1, Non-patent Document 2). This method involves placing a test specimen in a desiccator or chamber at a certain relative humidity, and calculating the equilibrium moisture content based on the moisture content when the moisture absorption and desorption of the test specimen reach equilibrium.

[0004] However, the JIS method has the following problems when obtaining equilibrium moisture contents at multiple relative humidities. That is, when preparing desiccators and test specimens for the number of relative humidity levels, the equilibrium moisture content may change due to variations in the test specimens even at the same relative humidity. Also, when using one desiccator for the number of relative humidity levels, it takes a long time to reach equilibrium, so obtaining multiple equilibrium moisture contents takes that much time. In particular, when the test specimen is concrete, depending on the size of the specimen, it may take more than six months for the moisture content to reach equilibrium, which is not practical. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] JIS A 1475 "Method of measuring equilibrium moisture content of building materials" [Non-Patent Document 2] Central Testing Laboratory, "Testing for Equilibrium Moisture Content of Building Materials," Building Materials Testing Center, Building Materials Testing Information 5 '06 Summary of the Invention [Problem to be solved by the invention]

[0006] In view of the above-mentioned problems, the present invention aims to provide a humidity measuring device etc. that can obtain the mass of concrete at multiple humidities at once in a short period of time using a single device. [Means for solving the problem]

[0007] As a result of investigating humidity measuring devices and the like that meet the above-mentioned object, the present inventors have found that a humidity measuring device and the like having the following configuration can achieve the above-mentioned object, and have completed the present invention.

[0008] [1] A humidity measuring device for measuring the humidity of a cementitious hardened body, Equipped with a housing, The housing includes: A side wall; an opening formed on one end side of the side wall in a longitudinal direction, a blocking portion formed on the other end side of the side wall in the longitudinal direction; a space portion that is a space surrounded by an inner wall surface of the side wall and the closing portion, the space being a space between the opening portion and the closing portion; A plurality of first arrangement sections in which specimens of cementitious hardened bodies are arranged; A second arrangement portion in which a moisture release agent or a moisture absorbent is arranged is formed, The first arrangement section and the second arrangement section can be separated so that the housing is paired, and a plurality of recesses (grooves) are formed on the side surface constituting the housing, The inner wall surface is formed with an installation section capable of installing a humidity measuring device for measuring the humidity of a space partitioned by the specimen arranged in the first arrangement section, The second arrangement section is disposed closer to the other end than the first arrangement section. [2] The first arrangement portions are provided on the inner wall surface along the longitudinal direction of the side wall, A humidity measuring device as described in [1], wherein when the test specimen is placed, the test specimen is formed in a shape that can block the space in a vertical cross section in the longitudinal direction. [3] The humidity measuring device according to [1] or [2], wherein the blocking portion also serves as the second placement portion. [4] The humidity measuring device according to any one of [1] to [3], wherein the second arrangement section is a partial area of ​​the space section, and the partial area is larger than the space section between adjacent test specimens arranged in the first arrangement section. [5] The humidity measuring device according to any one of [1] to [4], wherein the housing is configured to be separable in the longitudinal direction. [6] The humidity measuring device according to any one of [1] to [5], wherein the inner wall surface of the side wall is formed so that the space is prismatic or cylindrical. [7] The humidity measuring device according to any one of [1] to [6], comprising the humidity measuring device. [8] A method for measuring equilibrium mass, comprising the steps of: (A) and (B) below; measuring the humidity in a space partitioned off by a specimen using a humidity meter provided in a humidity measuring apparatus described in any one of [1] to [7] above; and measuring the equilibrium mass of the specimen when the humidity reaches equilibrium. (A) A test specimen preparation process in which a plurality of plates are cut out from the cementitious hardened body, and the periphery of the plates is sealed with a sealing material to prepare a test specimen. (B) A process of arranging the specimen and the moisture releasing agent or moisture absorbing agent in the housing of the humidity measuring device. [9] The method for measuring a balance mass according to [8], wherein in the specimen preparation step, the thickness of each specimen cut out is 0.5 to 5 cm.

[10] The method for measuring a balance mass according to [8] or [9], wherein in the placing step, a desiccant is placed, and the desiccant is a liquid contained in a storage container.

[11] A method for obtaining an equilibrium moisture content, comprising calculating and obtaining the equilibrium moisture content using a balance mass described in any one of [8] to

[10] above.

[12] A method for obtaining a diffusion coefficient, comprising calculating the diffusion coefficient from the change in mass of the moisture release agent or moisture absorbent described in any one of [8] to

[10] above and the change in mass of a test specimen. Effect of the Invention

[0009] By using the humidity measuring device of the present invention, the equilibrium mass of the cementitious hardened body at a plurality of humidities can be measured at once in a short period of time, so that the equilibrium moisture content of the cementitious hardened body can be easily obtained. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram (cross-sectional view) illustrating an example of a humidity measuring device of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing an example of a state in which multiple test specimens are cut out from a cementitious hardened body, and a schematic diagram (cross-sectional view) showing an example of a humidity measuring device in which test specimens, a humidity measuring instrument, and a moisture releasing agent or a moisture absorbing agent are arranged. [Diagram 3]FIG. 13 is a schematic diagram showing an example of a process of placing a specimen in a first placement section of a divided housing and then stacking the housings. [Figure 4] FIG. 1 is a schematic diagram (cross-sectional view) showing an example of a divided housing, in which (a) shows a divided housing with a test piece placed therein, and (b) shows a divided housing without a test piece placed therein. [Diagram 5] FIG. 2 is a perspective view showing an example of a divided housing, in which (a) shows a divided housing with a test piece placed therein, and (b) shows a divided housing without a test piece placed therein. [Figure 6] 1 is a diagram showing an example of an equilibrium volumetric moisture content curve created using the equilibrium volumetric moisture content obtained by the method for obtaining equilibrium moisture content of the present invention. FIG. [Figure 7] FIG. 1 is a plot of mass reduction rates of test specimens. [Figure 8] FIG. 1 is a plot of diffusion coefficient versus equilibrium volumetric water content. [Figure 9] FIG. 1 is a plot of equilibrium volumetric moisture content versus relative humidity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] As described above, the present invention relates to a humidity measuring device, a method for measuring a balance mass, a method for obtaining an equilibrium moisture content, and a method for obtaining a diffusion coefficient. Hereinafter, the present invention will be described in detail with respect to the humidity measuring device, the method for measuring a balance mass, the method for obtaining an equilibrium moisture content, and the method for obtaining a diffusion coefficient.

[0012] 1.Humidity measuring device The humidity measuring device 1 of the present invention comprises a housing 11, which has a side wall 12, an opening 13 formed at one end of the side wall 12 in the longitudinal direction, and a blocking portion 14 formed at the other end of the side wall 12 in the longitudinal direction. The outer shape of the housing 11 is not particularly limited, but is preferably a prismatic or cylindrical shape from the viewpoint of ease of manufacturing and handling the housing. The inner wall surface of the side wall 12 of the housing 11 is formed so that the space portion 15 is prismatic or cylindrical. The material of the housing 11 is not particularly limited, but is preferably a resin such as an acrylic resin or a polyvinyl chloride resin, because it is easy to process the first arrangement section 16 and the second arrangement section 17. The housing 11 is preferably configured to be separable in the longitudinal direction to facilitate installation of the specimen 21. The opening 13 is in contact with the outside air and serves as a flow path for moisture. The blocking portion 14 formed on the other end side is, for example, a bottom surface, and a mounting base (second arrangement portion 17) may be placed on the bottom surface, or the second arrangement portion 17 may be integrally molded with the housing 11.

[0013] The humidity measuring device 1 also has a space 15, which is a space surrounded by the inner wall surface of the side wall 12 and the closing portion 14, and is the space between the opening 13 and the closing portion 14. The inner wall surface of the side wall 12 of the housing 11 is preferably formed so that the space 15 is prismatic or cylindrical. If the space 15 is formed in this manner so as to be prismatic or cylindrical, implementation becomes easier because the shapes of prismatic or cylindrical formwork and cylindrical concrete cores are common. The blocking portion 14 may also serve as the second arrangement portion 17 . When the space 15 is divided into a plurality of spaces by the test specimen 21, the spaces become spaces simulating the humidity environment inside the cementitious hardened material such as concrete used to prepare the test specimen 21.

[0014] The inner wall surface of the side wall 12 is configured to form a plurality of first arrangement sections 16 in which test specimens 21 of the cementitious hardened body 2 are arranged, and a second arrangement section 17 in which a moisture releasing agent or moisture absorbing agent 22 is arranged. An installation section 19 is formed on the inner wall surface, in which a humidity measuring device 18 for measuring the humidity of the space partitioned by the test specimen 21 arranged in the first arrangement section 16 can be installed, and the second arrangement section 17 is provided on the other end side relative to the first arrangement section 16.

[0015] The first arrangement portion 16 is provided on the inner wall surface along the longitudinal direction of the side wall 12 in a plurality of portions, and is formed in a shape that allows the specimen 21 to block the space 15 in a vertical cross section in the longitudinal direction when the specimen 21 is arranged thereon. Here, the first arrangement portion 16 is formed in a shape that allows the specimen 21 to block the space 15 means that, for example, when the first arrangement portion 16 is a groove and the vertical cross section is circular, the groove is formed over the entire circumference, not just a part of the circumference. The first arrangement portion 16 may have any shape that allows the specimen 21 to be placed therein and block the space 15, and may be, for example, a recess (groove) or a protrusion. For example, when the housing 11 is configured to be separable, each of the divided housings 11 is provided with a recess (groove) or a protrusion, and when the divided housings 11 are overlapped, these recesses (grooves) or protrusions are configured to be continuous in the vertical cross section direction, thereby forming the first arrangement portion 16. The second arrangement section 17 is a partial area of ​​the space 15, and this partial area is larger than the space 15 between the adjacent test specimens 21 arranged in the first arrangement section 16. The reason why the second arrangement section 17 is made larger is that when the humidity measurement period is long, a large amount of moisture absorbent or the like is required, and even such a large-volume moisture absorbent or the like can be arranged in the second arrangement section 17 by making it a larger area.

[0016] Furthermore, an installation section 19 is formed on the inner wall surface, in which a humidity measuring device 18 for measuring the humidity within the space partitioned by the multiple test specimens 21 arranged in the first arrangement section 16 can be installed. The installation portion 19 may be, but is not limited to, an insertion hole penetrating the side wall 12. For example, in the case of a configuration in which the humidity measuring device 18 is attached to the detection portion of the humidity measuring device 18 by gluing the detection portion in advance, the adhesion portion between the inner wall surface of the housing 11 and the detection portion corresponds to the installation portion 19. The humidity measuring device 1 may further include the humidity measuring device 18 at the installation section 19 .

[0017] 2. Humidity measurement method In the humidity measurement method, after the steps (A) and (B) are performed, the humidity in the space partitioned by the test specimen 21 is measured by the humidity measuring device 18 provided in the humidity measuring device 1, and the equilibrium mass of the test specimen 21 is measured when the humidity reaches equilibrium. Each step will be described below.

[0018] (A) Test specimen preparation process This step involves cutting out a plurality of plates from the cementitious hardened body 2, and then sealing the periphery of each plate with a sealing member to prepare a test specimen 21. The cementitious hardened body 2 may be concrete or mortar. The cement, aggregate, and admixture used in the cementitious hardened body 2 are not particularly limited, and may be ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, blast-furnace cement, ecocement, rapid-hardening cement, river gravel, mountain gravel, crushed stone, river sand, mountain sand, land sand, sea sand, crushed sand, silica sand, blast-furnace slag, fly ash, and silica fume. The shape of the specimen 21 is a disk shape if the shape of the space 15 is cylindrical, and a square plate shape if the shape of the space 15 is prismatic. The thickness of the specimen 21 is not particularly limited, but is particularly preferably 0.5 cm or more since the specimen 21 is less likely to break when cut out, and 5 cm or less since the period until equilibrium is reached is relatively short. Moreover, since the sealing member is used to prevent moisture leakage at the contact point between the first arrangement portion 16 and the specimen 21, it is not particularly limited as long as it has a sealing function, and examples of the sealing member include a rubber ring, etc. To further strengthen the sealing function, it is preferable to fill the first arrangement portion 16 with silicon oil, etc.

[0019] (B) Placement process of the test specimen and the moisture release agent or moisture absorbent This step is an arrangement step of arranging the specimen 21 and the moisture release agent or moisture absorbent 22 in the housing 11 of the humidity measuring device 1. This step may also include a step of arranging a plurality of the specimens 21 in a first arrangement section 16 formed in the housing 11 in a state in which the housing 11 is divided in the longitudinal direction, arranging the moisture release agent or moisture absorbent 22 in a second arrangement section 17 formed in the housing 11, and then overlapping the housings 11 to seal the specimens 21 and the moisture release agent or moisture absorbent 22. When the moisture release agent 22 is used, the test piece 21 absorbs moisture, and when the moisture absorbent 22 is used, the test piece 21 releases moisture. In this way, the humidity measurement method of the present invention can easily measure the humidity in the moisture absorption process or moisture release process by the simple operation of using the moisture release agent or moisture absorbent 22. The moisture release agent 22 and the moisture absorbent 22 are not particularly limited as long as they have a predetermined moisture release function or moisture absorption function. For example, they may be liquid or solid. When a liquid is used, it is placed in a storage container such as a petri dish. The liquid may be, for example, water or a saturated salt solution, and examples of the saturated salt solution include a zinc chloride solution, a magnesium chloride solution, and a magnesium nitrate solution. The saturated salt solution can keep the relative humidity in a sealed container constant. The solid may be, for example, silica gel or quicklime. The humidity measuring device 18 is not particularly limited and may be a commercially available humidity sensor, for example, IST HYT939 (manufactured by Syscom), etc. In addition, when the installation part 19 is an insertion hole, it is preferable to close it with a rubber plug or the like when the humidity sensor is not inserted. One of the technical features of the humidity measurement method of the present invention is that it measures the humidity in a space partitioned off by the test specimen 21 as a space simulating the humidity environment inside concrete. As an effect of this, since multiple measurements can be performed at once with one measurement device, test results can be obtained earlier than with conventional measurement methods that use one desiccator in multiple applications, and measurement variations between devices that occur when multiple desiccators are used are not generated, allowing for accurate measurements. In addition, as illustrated in Figure 2, humidity can be measured easily and accurately without the humidity meter 18 coming into contact with moisture.

[0020] 3. How to obtain equilibrium moisture content The equilibrium moisture content is calculated using the balance mass by the following formula (1) or (2): Ww = 100 × (Me - Mc) / Mc (1) Wv = 100 × (Me-Mc) / V (2) In formula (1), Ww represents the equilibrium mass moisture content of the specimen 21, Me represents the mass of each specimen 21 when the humidity reaches equilibrium, Mc represents the mass of each specimen 21 that has dried to a constant weight, and in formula (2), Wv represents the equilibrium volumetric moisture content of each specimen 21, Me represents the mass of each specimen 21 when the humidity reaches equilibrium, Mc represents the mass of each specimen 21 that has dried to a constant weight, and V represents the volume of each specimen 21.

[0021] 4. How to obtain the diffusion coefficient The method of obtaining this is to obtain the equilibrium moisture content gradient by dividing the difference in the equilibrium volumetric moisture content of adjacent specimens 21 at that time and the moisture flux, which is the amount of moisture passing through each specimen 21 per unit time and unit area, from the change in mass of the moisture release agent or moisture absorbent 22 and the change in mass of the specimen 21, by the thickness of the specimen 21, and then using the moisture flux and the equilibrium volumetric moisture content gradient to calculate the diffusion coefficient according to the following equation (3). D = J / (dWv / dX) (3) In equation (3), D is the diffusion coefficient (cm 2 / day), and J is the moisture flux (g / cm2 ·day), and dWv / dX is the equilibrium volumetric water content gradient ((g / cm 3 ) / cm). The change in mass is determined by measuring the mass of each test specimen 21 at least at the start of the measurement and when the humidity reaches equilibrium, and at that time, the sealing member of the test specimen 21 may be either attached or detached. In this description, the diffusion coefficient is calculated using the above formula (3), but the method of obtaining the diffusion coefficient is not limited to this. For example, a value as shown in the following formula (4) may be used. TIFF0007581090000001.tif13149In equation (4), D is the diffusion coefficient, W is the water content, W0 is 100%, and λ is the Boltzmann variable, which is the distance from the drying surface divided by the square root of the drying period. EXAMPLES

[0022] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. 1.Materials used (1) Ordinary Portland cement (abbreviation: C) Manufactured by Pacific Cement Corporation. (2) Mountain sand (abbreviation: S) Surface dry density is 2.56g / cm 3 It is. (3) Crushed sandstone (Abbreviation: G) Surface dry density is 2.66g / cm 3 It is. (4) Tap water (abbreviation: W) (5) AE water reducing agent (abbreviation: AD) The product name is Pozzolith No. 70 (registered trademark) and is manufactured by BASF. (6) Air Entrainer (AE) The product name is MasterAir 404 [registered trademark] and is manufactured by BASF.

[0023] 2. Preparation of specimen According to the composition shown in Table 1, the above materials were all charged at once into a 50-liter pan-type mixer, mixed for 2 minutes, and then cast into a formwork with an inner diameter of 10 cm and a height of 20 cm to obtain a cementitious hardened body 2 (concrete). Next, the hardened body was sealed and cured at 20°C for 28 days, and then removed from the form, and cut out as shown in Figure 2 to prepare 10 test pieces 21 with a thickness of 1 cm. Next, the circumference of the test piece 21 was covered with a sealing member (rubber ring) to obtain ten test pieces 21.

[0024] [Table 1]

[0025] 3. Measurement of Balance Mass and Obtaining Equilibrium Volumetric Moisture Content Next, as shown in Figures 2, 4, and 5, the 10 test specimens 21 and a container (peter dish) containing distilled water were placed in the first placement section 16 (groove) and the second placement section 17 (bottom surface) of the divided acrylic housing 11, respectively, and then the housing 11 and the housing 11 with 10 humidity meters 18 (humidity sensors IST HYT939, manufactured by Syscom) inserted into the installation sections 19 (insertion holes) were stacked together to form 10 simulated spaces and openings 13. Next, the humidity measuring device 1 was stored in an environment with a relative humidity of 12%, and the relative humidity in these 10 simulated spaces was measured. When the humidity reached equilibrium, each specimen 21 was taken out of the humidity measuring device 1, the rubber ring of the specimen 21 was immediately removed, and the mass (equilibrium mass) of each specimen 21 was measured. Here, the "when the humidity reached equilibrium" refers to when the change in relative humidity per day was 0.1% or less. In addition, while the equilibrium mass of one specimen 21 was being measured, the remaining nine specimens 21 were temporarily stored in sealed bags to prevent drying in the air. Furthermore, each specimen 21 was dried at 105° C. for 24 hours, and the dry mass of each specimen 21 was measured. The equilibrium volumetric moisture content was calculated using the equilibrium mass, dry mass, and formula (2). The volume of the specimen 21 was 78.5 cm 3 was used. An equilibrium volumetric moisture content curve created using the obtained equilibrium volumetric moisture content is shown in Fig. 6. The relative humidity corresponding to the equilibrium moisture content of each specimen 21 is the average value of the relative humidities of the two spaces sandwiching the specimen 21. In other words, the measured value of the equilibrium mass corresponds to the equilibrium mass at the average value of the relative humidities of the two spaces sandwiching the specimen 21 to be measured.

[0026] As shown in FIG. 6, according to the measurement method of the present invention, the equilibrium mass of the specimen 21 at a plurality of relative humidities can be measured at once using one device, so that the equilibrium moisture content can be easily obtained and the equilibrium moisture content curve can be created in a short time. FIG. 9 also shows the results of the equilibrium moisture content curve obtained by storing the specimen 21 having a thickness of 1 cm in a desiccator conditioned to relative humidities of 12, 33, 45, 59, 74, 85, and 96% in accordance with JIS A 1475 "Method of measuring equilibrium moisture content of building materials". The equilibrium moisture content curve of the present invention uses the average value of the relative humidities of the two spaces sandwiching the specimen 21, and as shown in FIG. 9, it can be seen that the measurement results by the measurement method of JISA1475 can be reproduced with high accuracy. FIG. 7 shows the mass loss rate of the specimen 21 at a position 3 cm from the opening 13 excluding the space 15 during the drying period. As shown in FIG. 7, when a concrete specimen of 10×10×40 cm specified by JIS A 1129 "Method of measuring change in length of mortar and concrete" (indicated as "JIS method" in FIG. 7) is stored in an environment of relative humidity of 60%, it takes more than 180 days to reach equilibrium, whereas in the present invention, the equilibrium state is reached in about 120 days for drying, and the measurement period can be significantly shortened, so that the present invention is highly practical and convenient. Note that FIG. 7 is only one example, and the mass loss rate of the specimen 21 at 1 cm, 2 cm, 4 cm, and 5 cm from the opening 13 excluding the space 15 can also be significantly shortened compared to the JIS method.

[0027] 4. Obtaining the Diffusion Coefficient When the equilibrium mass of each specimen 21 was measured, the mass of the container containing the distilled water was also measured. The change in mass of each specimen 21 and the container was obtained from the difference between the mass of each specimen 21 and the container at the start of the measurement and the mass of each specimen 21 when the humidity reached equilibrium. Next, from the change in mass of each specimen 21 and the container, the moisture flux, which is the amount of moisture passing through each specimen 21 per unit time and unit area, and the difference in the equilibrium volumetric moisture content of the adjacent specimens 21 at that time were divided by the thickness of the specimen 21 to obtain the equilibrium volumetric moisture content gradient. Then, the diffusion coefficient was calculated and obtained by using the moisture flux and the equilibrium volumetric moisture content gradient according to the above formula (3). Figure 8 shows a graph of the diffusion coefficient with respect to the equilibrium volumetric moisture content. According to the method for obtaining a diffusion coefficient of the present invention, the diffusion coefficient with respect to the equilibrium volumetric moisture content can be easily obtained in a short period of time. [Explanation of symbols]

[0028] 1 Humidity measuring device 11. Cabinet 12 Side wall 13 Opening 14 Occlusion 15 Space section 16 1st placement part 17 Second placement part 18 Humidity meter 19 Installation part 2. Hardened cementitious material 21 Specimen 22 Moisture release or moisture absorption agents

Claims

1. A humidity measuring device for measuring the humidity of a cementitious hardened body, comprising: Equipped with a housing, The housing includes: A side wall; an opening formed on one end side of the side wall in a longitudinal direction, a blocking portion formed on the other end side of the side wall in the longitudinal direction; a space portion that is a space surrounded by an inner wall surface of the side wall and the closing portion, the space being a space between the opening portion and the closing portion; A plurality of first arrangement sections in which specimens of cementitious hardened bodies are arranged; A second arrangement portion in which a moisture release agent or a moisture absorbent is arranged is formed, The first arrangement portion and the second arrangement portion can be separated so that the housing is paired, and a plurality of recesses (grooves) are formed on the side surface constituting the housing, The inner wall surface is formed with an installation section capable of installing a humidity measuring device for measuring humidity in a space partitioned by the specimen placed in the first arrangement section, The second arrangement portion is disposed closer to the other end than the first arrangement portion.

2. The first arrangement portions are provided on the inner wall surface along a longitudinal direction of the side wall, 2. The humidity measuring device according to claim 1, wherein the test piece is formed in a shape that allows the test piece to block the space in a vertical cross section in the longitudinal direction when the test piece is placed thereon.

3. The humidity measuring device according to claim 1 , wherein the blocking portion also serves as the second arrangement portion.

4. The humidity measuring device according to any one of claims 1 to 3, wherein the second arrangement section is a partial area of ​​the space section, and the partial area is larger than the space section between adjacent test specimens arranged in the first arrangement section.

5. The humidity measuring device according to claim 1 , wherein the housing is configured to be separable in the longitudinal direction.

6. The humidity measuring device according to claim 1 , wherein an inner wall surface of the side wall is formed so that the space has a prismatic or cylindrical shape.

7. The humidity measuring device according to claim 1 , further comprising the humidity measuring device.

8. A method for measuring equilibrium mass, comprising the steps of: measuring the humidity in a space partitioned off by a specimen using a humidity measuring instrument provided in a humidity measuring device described in any one of claims 1 to 7, after undergoing the steps (A) and (B) below; and measuring the equilibrium mass of the specimen when the humidity reaches equilibrium. (A) A test specimen preparation step in which a plurality of plates are cut out from a cementitious hardened body, and then the periphery of the plate is sealed with a sealing material to prepare a test specimen. (B) A step of arranging the test specimen and the moisture releasing agent or moisture absorbing agent in the housing of the humidity measuring device.

9. 9. The method for measuring a balance mass according to claim 8, wherein in the specimen preparation step, each of the specimens cut out has a thickness of 0.5 to 5 cm.

10. 10. The method for measuring a balance mass according to claim 8, wherein in the placing step, a moisture-releasing agent is placed, and the moisture-releasing agent is a liquid contained in a storage container.

11. A method for obtaining an equilibrium moisture content, comprising calculating and obtaining an equilibrium moisture content using the balance mass according to any one of claims 8 to 10.

12. A method for obtaining a diffusion coefficient, comprising calculating and obtaining a diffusion coefficient from a change in mass of the moisture release agent or moisture absorbent according to any one of claims 8 to 10 and a change in mass of a test specimen.

Citation Information

Patent Citations

  • Measuring method of relative humidity in concrete

    JP2020106332A

  • Positive photosensitive resin composition, method for forming patterned resist film, and patterned resist film