Aluminum nitride powder, aluminum nitride sintered body, circuit board and bonded board
By optimizing aluminum nitride powders through specific Raman spectroscopy peaks and manufacturing controls, thermal conductivity is enhanced, addressing the limitations of existing materials in circuit boards and bonded substrates.
Patent Information
- Application Number
- JP2024005087
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-01-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-01-17
AI Technical Summary
Existing aluminum nitride powders used in circuit boards and bonded substrates do not achieve optimal thermal conductivity.
Aluminum nitride powders with specific Raman spectroscopy peak ranges and characteristics, along with controlled particle size, oxygen content, and manufacturing conditions, are developed to enhance thermal conductivity.
The improved aluminum nitride powders result in enhanced thermal conductivity, benefiting circuit boards and bonded substrates with superior heat dissipation properties.
Smart Images

Figure 0007581547000002 
Figure 0007581547000003 
Figure 0007581547000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum nitride powder, an aluminum nitride sintered body, a circuit board, and a bonded board. [Background technology]
[0002] Sintered bodies containing aluminum nitride powder are sometimes used for circuit boards and bonded substrates. Patent Document 1 describes an aluminum nitride powder having an oxygen content of 0.2 mass % or less and an average particle size of 10 to 50 μm, which is obtained by heating hollow aluminum nitride particles at 1900°C to 2200°C in a nitrogen-containing reducing atmosphere, with the aim of providing an aluminum nitride powder which has much lower oxygen content than conventional products and exhibits excellent high thermal conductivity when used as a filler for heat dissipation components. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-284315 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention provides an aluminum nitride powder having improved thermal conductivity. [Means for solving the problem]
[0005] The present inventors have conducted extensive research to solve the above problems. As a result, they have discovered that an aluminum nitride powder containing aluminum nitride particles has a wave number of 150 cm in a Raman spectrum measured under specific conditions. -1 More than 350cm -1 The following ranges (A) and 800 cm -1 More than 1000cm -1The inventors have found that aluminum nitride powder having peaks in the following ranges (B) can improve thermal conductivity, and have completed the present invention.
[0006] According to the present invention, there are provided an aluminum nitride powder, an aluminum nitride sintered body, a circuit board, and a bonded board, as described below.
[0007] [1] An aluminum nitride powder comprising aluminum nitride particles, In the Raman spectrum of the aluminum nitride powder measured under the following conditions, the wave number is 150 cm -1 More than 350cm -1 The following ranges (A) and 800 cm -1 More than 1000cm -1 Aluminum nitride powder having peaks in the following ranges (B): (conditions) Laser wavelength: 532nm Objective lens magnification: 20x Grating: 300Gr / mm Slit width: 50μm Exposure time: 1 second Number of exposures: 10 [2] In the Raman spectrum, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) X The wave number is 1250 cm -1 More than 1450cm -1 Peak intensity I of the maximum peak in the following range (C) C Ratio I C / I X The aluminum nitride powder according to [1], wherein the average molecular weight of the aluminum nitride powder is 0.020 or less. [3] The aluminum nitride powder according to [2], which has no peak in the range (C) in the Raman spectroscopy spectrum. [4] In the Raman spectrum, the wave number is 500 cm -1 More than 750cm-1 The peak intensity I of the maximum peak in the following range (X) X The wave number is 1500 cm -1 More than 1700cm -1 The peak intensity I of the maximum peak in the following range (D) D Ratio I D / I X The aluminum nitride powder according to any one of [1] to [3], wherein the value is 0.020 or less. [5] The aluminum nitride powder according to [4], which has no peak in the range (D) in the Raman spectroscopy spectrum. [6] In the Raman spectrum, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) X The peak intensity I of the maximum peak in the range (A) A Ratio I A / I X The aluminum nitride powder according to any one of [1] to [5], wherein is 0.020 or more and 0.200 or less. [7] In the Raman spectrum, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) X The peak intensity I of the maximum peak in the range (B) B Ratio I B / I X The aluminum nitride powder according to any one of [1] to [6], wherein is 0.030 or more and 0.400 or less. [8] In the Raman spectrum, the wave number is 500 cm -1 More than 750cm -1 The aluminum nitride powder according to any one of [1] to [7], further having two or more peaks in the following range (X): [9] The volume-based median diameter D of the aluminum nitride powder measured by the laser diffraction scattering method 50The aluminum nitride powder according to any one of [1] to [8], wherein the particle size is 0.50 μm or more and 5.00 μm or less.
[10] In the volume frequency particle size distribution of the aluminum nitride powder by the laser diffraction scattering method, the particle diameter D at which the cumulative value reaches 10% is 10 , 90% particle diameter D 90 , median diameter D 50 Regarding (D 90 -D 10 ) / D 50 The aluminum nitride powder according to any one of [1] to [9], wherein the value of is 3.00 or less.
[11] The aluminum nitride powder has a specific surface area of 1.00 m as measured by the BET single point method in accordance with ISO 9277. 2 / g or more 5.00m 2 The aluminum nitride powder according to any one of [1] to
[10] , wherein the aluminum nitride powder has a molecular weight of 1.0 to 1.5 μg / g or less.
[12] The aluminum nitride powder according to any one of [1] to
[11] , wherein the amount of oxygen in the aluminum nitride powder is 0.50% by mass or more and 0.90% by mass or less as measured using an oxygen / nitrogen simultaneous analyzer.
[13] The aluminum nitride powder according to any one of [1] to
[12] , which contains hexagonal aluminum nitride primary particles.
[14] The aluminum nitride powder according to any one of [1] to
[13] , which has a thermal conductivity of 120 W / (m·K) or more, as measured by the following method: (method) A molding material is obtained by mixing 100 parts by mass of the aluminum nitride powder, 4 parts by mass of yttrium oxide powder, 3 parts by mass of aluminum oxide powder, 6 parts by mass of cellulose ether binder, 5 parts by mass of glycerin, and 10 parts by mass of ion-exchanged water. The molding material is then molded into a sheet, degreased by heating in air at 570°C for 5 hours, and then heated under nitrogen gas atmosphere at atmospheric pressure and 1800°C for 4 hours to obtain an aluminum nitride sintered body. The thermal conductivity of the aluminum nitride sintered body is then measured by a laser flash method at 23°C in accordance with JIS R1611:2010.
[15] An aluminum nitride sintered body comprising the aluminum nitride powder according to any one of [1] to
[14] .
[16]
[15] A circuit board comprising the aluminum nitride sintered body and a conductor portion.
[17]
[15] A bonded substrate comprising the aluminum nitride sintered body according to the present invention and a metal plate. Effect of the Invention
[0008] According to the present invention, it is possible to provide an aluminum nitride powder having improved thermal conductivity. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a perspective view showing a schematic example of a structure of the bonded substrate of the present embodiment. [Diagram 2] FIG. 2 is a perspective view showing a schematic example of the structure of the circuit board according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In the drawings, similar components are given similar symbols and descriptions thereof will be omitted as appropriate. In order to avoid complexity, when there are multiple identical components in the same drawing, only one of them may be labeled with a reference symbol, and not all of them. The drawings are for illustrative purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.
[0011] In this embodiment, the numerical range "A to B" indicates A or more and B or less, unless otherwise specified.
[0012] <Aluminum nitride powder> The aluminum nitride powder of the present embodiment is an aluminum nitride powder containing aluminum nitride particles, and in a Raman spectroscopy spectrum (S) measured under the following conditions, the wave number is 150 cm -1 More than 350cm -1 The following ranges (A) and 800 cm -1 More than 1000cm -1 It has peaks in the following ranges (B). (conditions) Laser wavelength: 532nm Objective lens magnification: 20x Grating: 300Gr / mm Slit width: 50μm Exposure time: 1 second Number of exposures: 10
[0013] According to the study by the present inventors, in aluminum nitride powder containing aluminum nitride particles, the wave number in the Raman spectrum of the aluminum nitride powder is 150 cm -1 More than 350cm -1 Peaks in the range below and 800 cm -1 More than 1000cm -1 It was found that there is a correlation between the peaks in the following ranges and thermal conductivity:
[0014] As a result of further investigations by the inventors based on the above findings, it was found that in a Raman spectrum measured under the conditions of a laser wavelength of 532 nm, an objective lens magnification of 20 times, a grating of 300 Gr / mm, a slit width of 50 μm, an exposure time of 1 second, and 10 exposures, the wave number was 150 cm -1 More than 350cm -1 The following ranges (A) and 800 cm-1 More than 1000cm -1 The inventors have found that the thermal conductivity of aluminum nitride powder can be improved by having peaks in the following ranges (B), and have completed the present invention.
[0015] The aluminum nitride powder of this embodiment preferably has a wave number of 500 cm in the Raman spectrum (S). -1 More than 750cm -1 It further has one or more peaks in the following range (X), more preferably it further has two or more peaks in the range (X), even more preferably it further has three or more peaks in the range (X), and even more preferably it further has three peaks in the range (X).
[0016] In the Raman spectrum (S) of the aluminum nitride powder of this embodiment, the peak intensity I of the maximum peak in the range (X) X is preferably the largest peak intensity among the peaks in the Raman spectrum (S).
[0017] In the Raman spectrum (S) of the aluminum nitride powder of this embodiment, the magnitude of the peak intensity of each peak is, for example, the peak intensity I of the maximum peak in the range (X). X It can be evaluated as a relative value to
[0018] In this specification, the wave number in the Raman spectrum (S) is P (cm -1 ) or more Q(cm -1 The peak intensity of the maximum peak in the range below P(cm -1 ) and Q(cm -1 ) is taken as the baseline, and the scattering intensity refers to the difference between the baseline and the maximum peak scattering intensity.
[0019] In the Raman spectrum (S) of the aluminum nitride powder of this embodiment, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) XThe wave number is 150 cm -1 More than 350cm -1 The peak intensity I of the maximum peak in the following range (A) A Ratio I A / I X From the viewpoint of further improving thermal conductivity, is preferably 0.020 or more and 0.200 or less, more preferably 0.025 or more and 0.150 or less, even more preferably 0.030 or more and 0.100 or less, even more preferably 0.040 or more and 0.070 or less, even more preferably 0.045 or more and 0.065 or less, and even more preferably 0.050 or more and 0.060 or less.
[0020] In the Raman spectrum (S) of the aluminum nitride powder of this embodiment, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) X The wave number is 800 cm -1 More than 1000cm -1 Peak intensity I of the maximum peak in the following range (B) B Ratio I B / I X From the viewpoint of further improving thermal conductivity, is preferably 0.030 or more and 0.400 or less, more preferably 0.040 or more and 0.300 or less, even more preferably 0.050 or more and 0.200 or less, even more preferably 0.060 or more and 0.150 or less, even more preferably 0.070 or more and 0.120 or less, and even more preferably 0.080 or more and 0.100 or less.
[0021] In the Raman spectrum (S) of the aluminum nitride powder of this embodiment, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) X The wave number is 1250 cm -1 More than 1450cm -1 Peak intensity I of the maximum peak in the following range (C) C Ratio I C / I XFrom the viewpoint of further improving the thermal conductivity, I is preferably 0.020 or less, more preferably 0.015 or less, even more preferably 0.010 or less, even more preferably 0.005 or less, and even more preferably 0.001 or less. In the Raman spectroscopy (S) of the aluminum nitride powder of this embodiment, I C / I X The lower limit of is not particularly limited, but may be, for example, 0.000 or more.
[0022] In the Raman spectrum (S) of the aluminum nitride powder of this embodiment, from the viewpoint of further improving thermal conductivity, the wave number is 1250 cm -1 More than 1450cm -1 It is more preferable that there is no peak in the following range (C).
[0023] In the Raman spectrum (S) of the aluminum nitride powder of this embodiment, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) X The wave number is 1500 cm -1 More than 1700cm -1 The peak intensity I of the maximum peak in the following range (D) D Ratio I D / I X From the viewpoint of further improving the thermal conductivity, I is preferably 0.020 or less, more preferably 0.015 or less, even more preferably 0.010 or less, even more preferably 0.005 or less, and even more preferably 0.001 or less. In the Raman spectroscopy (S) of the aluminum nitride powder of this embodiment, I C / I X The lower limit of is not particularly limited, but may be, for example, 0.000 or more.
[0024] In the Raman spectrum (S) of the aluminum nitride powder of this embodiment, from the viewpoint of further improving thermal conductivity, the wave number is set to 1500 cm -1 More than 1700cm -1 It is more preferable that there is no peak in the following range (D).
[0025] According to the study by the present inventors, in aluminum nitride powder containing aluminum nitride particles, the wave number in the Raman spectrum of the aluminum nitride powder is 1250 cm -1 More than 1450cm -1 Peaks in the range below and 1500 cm -1 More than 1700cm -1 It was found that there is a correlation between the peaks in the following ranges and thermal conductivity:
[0026] As a result of further investigations by the inventors based on the above findings, it was found that in a Raman spectrum measured under the conditions of a laser wavelength of 532 nm, an objective lens magnification of 20 times, a grating of 300 Gr / mm, a slit width of 50 μm, an exposure time of 1 second, and 10 exposures, the wavenumber was 1250 cm -1 More than 1450cm -1 Peak intensity I of the maximum peak in the following range (C) C or the wave number is 1500 cm -1 More than 1700cm -1 The peak intensity I of the maximum peak in the following range (D) D It has been found that the thermal conductivity of aluminum nitride powder can be improved by reducing the particle size.
[0027] From the viewpoint of further improving thermal conductivity, the aluminum nitride powder of the present embodiment preferably contains aluminum nitride primary particles, and more preferably contains hexagonal aluminum nitride primary particles.
[0028] From the viewpoint of further improving thermal conductivity, the content of aluminum nitride particles in the aluminum nitride powder of this embodiment is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and even more preferably 99 mass% or more, when the total amount of the aluminum nitride powder is 100 mass%. The upper limit of the content of aluminum nitride particles in the aluminum nitride powder of this embodiment is not particularly limited, but may be, for example, 100 mass% or less.
[0029] The volume-based median diameter D of the aluminum nitride powder of this embodiment measured by the laser diffraction scattering method 50 From the viewpoint of further improving the balance of sinterability and moldability, the particle size is preferably 0.50 μm or more and 5.00 μm or less, more preferably 0.80 μm or more and 4.00 μm or less, even more preferably 1.00 μm or more and 3.50 μm or less, and even more preferably 1.50 μm or more and 3.00 μm or less.
[0030] In the volume frequency particle size distribution of the aluminum nitride powder of this embodiment by the laser diffraction scattering method, the particle diameter D at which the cumulative value reaches 10% 10 From the viewpoint of further improving the balance of sinterability and moldability, the average particle size is preferably 0.10 μm or more and 3.00 μm or less, more preferably 0.20 μm or more and 2.00 μm or less, even more preferably 0.30 μm or more and 1.00 μm or less, even more preferably 0.35 μm or more and 0.80 μm or less, and even more preferably 0.40 μm or more and 0.60 μm or less.
[0031] In the volume frequency particle size distribution of the aluminum nitride powder of this embodiment by the laser diffraction scattering method, the particle diameter D at which the cumulative value reaches 90% 90 From the viewpoint of further improving the balance of sinterability and moldability, the average particle size is preferably 1.00 μm or more and 20.00 μm or less, more preferably 2.00 μm or more and 15.00 μm or less, even more preferably 2.50 μm or more and 10.00 μm or less, even more preferably 3.50 μm or more and 8.00 μm or less, and even more preferably 4.50 μm or more and 6.00 μm or less.
[0032] In the volume frequency particle size distribution of the aluminum nitride powder of this embodiment by the laser diffraction scattering method, the particle diameter D at which the cumulative value reaches 10% 10 , 90% particle diameter D 90 , median diameter D 50 Regarding (D 90 -D 10 ) / D 50From the viewpoint of further improving the balance between sinterability and moldability, the value of (D 90 -D 10 ) / D 50 The lower limit of the value is not particularly limited, and may be, for example, 0.10 or more, 0.50 or more, 1.00 or more, 1.30 or more, 1.50 or more, or 1.70 or more.
[0033] The specific surface area of the aluminum nitride powder of the present embodiment, as measured by the BET single-point method in accordance with ISO 9277, is preferably 1.00 m from the viewpoint of further improving the performance balance between sinterability and moldability. 2 / g or more 5.00m 2 / g or less, more preferably 1.30m 2 / g or more 4.00m 2 / g or less, more preferably 1.50m 2 / g or more 3.00m 2 / g or less, more preferably 1.70m 2 / g or more 2.70m 2 / g or less, more preferably 1.80m 2 / g or more 2.30m 2 / g or less.
[0034] From the viewpoint of further improving thermal conductivity, the amount of oxygen in the aluminum nitride powder of this embodiment measured using an oxygen / nitrogen simultaneous analyzer is, when the total amount of the aluminum nitride powder is taken as 100 mass%, preferably 0.50 mass% or more and 0.90 mass% or less, more preferably 0.55 mass% or more and 0.85 mass% or less, even more preferably 0.60 mass% or more and 0.80 mass% or less, and even more preferably 0.65 mass% or more and 0.75 mass% or less.
[0035] From the viewpoint of further improving thermal conductivity, the thermal conductivity of the aluminum nitride powder of this embodiment, measured by the method described below, is preferably 120 W / (m·K) or more, more preferably 130 W / (m·K) or more, even more preferably 140 W / (m·K) or more, even more preferably 150 W / (m·K) or more, even more preferably 155 W / (m·K) or more, and even more preferably 160 W / (m·K) or more. The upper limit of the thermal conductivity of the aluminum nitride powder of this embodiment, measured by the method described below, is not particularly limited, but may be, for example, 300 W / (m·K) or less, 250 W / (m·K) or less, or 200 W / (m·K) or less. (method) A molding material is obtained by mixing 100 parts by mass of aluminum nitride powder, 4 parts by mass of yttrium oxide powder, 3 parts by mass of aluminum oxide powder, 6 parts by mass of cellulose ether binder, 5 parts by mass of glycerin, and 10 parts by mass of ion-exchanged water. The molding material is then molded into a sheet, degreased by heating in air at 570°C for 5 hours, and then heated under nitrogen gas atmosphere at atmospheric pressure and 1800°C for 4 hours to obtain an aluminum nitride sintered body. The thermal conductivity of the aluminum nitride sintered body is then measured by the laser flash method at 23°C in accordance with JIS R1611:2010.
[0036] <Method of manufacturing aluminum nitride powder> The aluminum nitride powder of the present embodiment can be obtained by appropriately selecting raw materials, the ratio of each raw material, the manufacturing procedure, the manufacturing conditions, etc. Specifically, the aluminum nitride powder of the present embodiment is preferably A preparation step of preparing raw material powder; - an introduction step of introducing raw material powder into a sintering furnace; a nitriding step of sintering the raw material powder in a nitrogen atmosphere to obtain aluminum nitride powder; a recovery step of recovering the aluminum nitride powder from the sintering furnace; The aluminum nitride powder can be produced through the steps. In addition, the production of the aluminum nitride powder may include additional steps other than those described above.
[0037] <Preparation process> In the preparation step of this embodiment, a raw material powder is prepared. From the viewpoint of further improving thermal conductivity, the raw material powder of this embodiment preferably contains one or two types selected from the group consisting of metallic aluminum and α-alumina, and more preferably contains metallic aluminum. When the raw material powder of this embodiment contains α-alumina, it preferably further contains carbon black.
[0038] When the raw material powder of this embodiment contains metallic aluminum, the content of metallic aluminum in the raw material powder is preferably 95 mass% or more and 100 mass% or less, and more preferably 99 mass% or more and 100 mass% or less, when the total amount of the raw material powder is taken as 100 mass%, from the viewpoint of further improving thermal conductivity.
[0039] When the raw material powder of this embodiment contains α-alumina, the content of α-alumina in the raw material powder is preferably 50 mass% or more and 65 mass% or less, and more preferably 55 mass% or more and 60 mass% or less, when the total amount of the raw material powder is taken as 100 mass%, from the viewpoint of further improving thermal conductivity. By setting the content of α-alumina in the raw material powder within the above range, the thermal conductivity of the resulting aluminum nitride powder can be further improved.
[0040] When the raw material powder of this embodiment contains metallic aluminum, the raw material powder preferably contains atomized powder of metallic aluminum from the viewpoint of further improving the production safety.
[0041] When the raw material powder of this embodiment contains metallic aluminum, the average particle size of the raw material powder is preferably 17 μm or more and 23 μm or less, more preferably 19 μm or more and 21 μm or less, from the viewpoint of further improving the balance between thermal conductivity and production safety. By adjusting the average particle size of the raw material powder to be equal to or less than the above upper limit, the thermal conductivity of the resulting aluminum nitride powder can be further improved.
[0042] When the raw material powder of this embodiment contains metallic aluminum, the oxygen content of the raw material powder is preferably 0.10 mass % or more and 0.25 mass % or less, and more preferably 0.20 mass % or more and 0.25 mass % or less, when the total amount of the raw material powder is taken as 100 mass %, from the viewpoint of further improving thermal conductivity. By controlling the oxygen content in the raw material powder to the above upper limit or less, the thermal conductivity of the resulting aluminum nitride powder can be further improved.
[0043] When the raw material powder of the present embodiment contains α-alumina, the average particle size of the raw material powder is preferably 0.1 μm or more and 1.5 μm or less, more preferably 0.5 μm or more and 1.0 μm or less, and the specific surface area of the raw material powder is preferably 2 m 2 / g or more 8m 2 / g or less, more preferably 4m 2 / g or more 6m 2 / g or less.
[0044] In the preparation step of this embodiment, when the raw material powder contains α-alumina and carbon black, it is preferable to mix α-alumina and carbon black. The mixing method may be dry mixing using a known device such as a blender or mixer, or dry mixing using a known dry grinder.
[0045] <Introduction process> In the introducing step of this embodiment, the raw material powder is introduced into a firing furnace. In the present embodiment, when the raw material powder contains metallic aluminum, the raw material powder is preferably introduced into the sintering furnace by being sprayed together with nitrogen gas from a nozzle. The speed at which the raw material powder and nitrogen gas are sprayed into the sintering furnace is preferably 12 m / s or more and 18 m / s or less, more preferably 14 m / s or more and 16 m / s or less. By setting the rate at which the raw material powder and nitrogen gas are sprayed into the sintering furnace within the above range, the thermal conductivity of the resulting aluminum nitride powder can be further improved.
[0046] When the raw material powder of this embodiment contains metallic aluminum, the mass of the raw material powder introduced into the sintering furnace per unit time is preferably 12 kg or more and 18 kg or less, more preferably 14 kg or more and 16 kg or less, from the viewpoint of further improving thermal conductivity.
[0047] When the raw material powder of this embodiment contains metallic aluminum, the volume of nitrogen gas introduced into the sintering furnace per unit time is preferably 15 m from the viewpoint of further improving thermal conductivity. 3 More than 25m 3 Less than or equal to 18m, preferably 3 More than 22m 3 The following is the result.
[0048] <Nitriding process> In the nitriding step of this embodiment, the raw material powder is sintered in a nitrogen atmosphere to obtain aluminum nitride powder. In the nitriding step of this embodiment, it is preferable to sinter the raw material powder in an atmosphere in which nitrogen gas flows in a sintering furnace.
[0049] The firing temperature in the nitriding step of the present embodiment is preferably 1500° C. or higher and 2000° C. or lower, more preferably 1900° C. or higher and 2000° C. or lower, from the viewpoint of further improving thermal conductivity. By setting the firing temperature in the nitriding step within the above range, the thermal conductivity of the resulting aluminum nitride powder can be further improved.
[0050] The purity of the nitrogen gas used in the nitriding step of this embodiment is preferably 99 vol. % or more and 100 vol. % or less, more preferably 99.9 vol. % or more and 100 vol. % or less, from the viewpoint of further improving thermal conductivity.
[0051] When the raw material powder of this embodiment contains metallic aluminum, the inner diameter of the sintering furnace used in the nitriding step is preferably 350 mm or more and 450 mm or less, more preferably 380 mm or more and 420 mm or less, from the viewpoint of further improving the balance between thermal conductivity and productivity.
[0052] When the raw material powder of this embodiment contains α-alumina, it is preferable to carry out an oxidation treatment after the nitriding step of this embodiment in an air atmosphere under conditions of 650° C. to 750° C. and 10 hours to 14 hours.
[0053] <Recovery process> In the recovery step of this embodiment, aluminum nitride powder is recovered from inside the sintering furnace. When the raw material powder of this embodiment contains metallic aluminum, the recovery step is preferably carried out by sucking the produced aluminum nitride powder from the bottom of the sintering furnace with a blower and collecting it with a bag filter.
[0054] <Aluminum nitride sintered body> The aluminum nitride sintered body of the present embodiment contains the aluminum nitride powder of the present embodiment. Since the aluminum nitride powder of this embodiment has improved thermal conductivity, the aluminum nitride sintered body of this embodiment also has improved thermal conductivity and can be suitably used for circuit boards and bonded boards.
[0055] <Bonded substrate> The bonded substrate of the present embodiment includes the aluminum nitride sintered body of the present embodiment and a metal plate. Hereinafter, the bonded substrate of this embodiment will be described with reference to FIG. 1, which is a perspective view showing a schematic example of the structure of the bonded substrate of this embodiment.
[0056] The bonded substrate 200 includes a pair of metal plates 110 arranged to face each other, and a plate-shaped aluminum nitride sintered body 100 between the pair of metal plates 110. An example of the metal plate 110 is a copper plate. The aluminum nitride sintered body 100 and the metal plate 110 may have the same shape and size or may have different shapes and sizes. The main surfaces of the metal plate 110 and the aluminum nitride sintered body 100 may be bonded to each other by, for example, a brazing material.
[0057] The bonded substrate 200 can sufficiently prevent foreign matter from being caught between the metal plate 110 and the aluminum nitride sintered body 100. In addition, since the aluminum nitride sintered body 100 has improved thermal conductivity, the bonded substrate 200 has excellent thermal conductivity.
[0058] In the bonded substrate 200, one of the pair of metal plates 110 may be a heat dissipation material, and the other may be processed into a conductor portion. The conductor portion may be formed by etching the metal plate 110 using a resist. This makes it possible to form a circuit board that has excellent thermal conductivity and is capable of sufficiently suppressing leakage current and the like.
[0059] <Circuit board> The circuit board of the present embodiment includes the aluminum nitride sintered body of the present embodiment and a conductor portion. Hereinafter, the circuit board of this embodiment will be described with reference to FIG. 2, which is a perspective view showing a schematic example of the structure of the circuit board of this embodiment.
[0060] The circuit board 300 includes a plate-shaped aluminum nitride sintered body 100, a conductor portion 20 on one main surface 100A, and a metal plate 110 on the other main surface. The conductor portion 20 and the main surface 100A of the aluminum nitride sintered body 100 may be joined by, for example, a brazing material. When the circuit board 300 is used in a product such as a power module, the conductor portion 20 may form a part of the circuit, and the metal plate 110 may function as a heat dissipation material. The circuit board 300 may also have a cooling fin instead of the metal plate 110.
[0061] The circuit board 300 can sufficiently prevent foreign matter from being caught between the conductor portion 20 and the metal plate 110 and the aluminum nitride sintered body 100. In addition, since the aluminum nitride sintered body 100 has improved thermal conductivity, the circuit board 300 has excellent thermal conductivity.
[0062] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. For example, the shapes and structures of the bonded substrate and the circuit substrate of this embodiment are not limited to those shown in Fig. 1 and Fig. 2. For example, the circuit substrate may have conductors attached to both main surfaces of the aluminum nitride sintered body 100. Instead of forming the conductors 20 by etching the metal plate 110, the conductors 20 may be formed by spraying metal powder and subjecting the metal powder to heat treatment. EXAMPLES
[0063] The embodiments of the present invention will be described in detail based on examples. However, the present invention is not limited to only the examples.
[0064] Example 1 In a 1820℃ furnace made of boron nitride with an inner diameter of 400 mm and a total length of 3000 mm, 15 kg of metallic aluminum powder (atomized powder, average particle size 19.8 μm, oxygen content 0.25 mass%) and 20.9 m of powder were fed per hour through a nozzle. 3 Nitrogen gas (normal) was sprayed at a speed of 15 m / s. The temperature inside the furnace during the reaction was kept at 1950°C by the heat of the nitriding reaction. The aluminum nitride powder produced was sucked from the bottom of the furnace by a blower and collected in a bag filter to obtain the aluminum nitride powder of Example 1.
[0065] Example 2 α-alumina (average particle size 0.8 μm, specific surface area 5.0 m 2 / g) 200 kg, and carbon black (specific surface area 110 m 2 The aluminum nitride powder (150 kg) was mixed for 0.5 hours in a mixer equipped with stirring blades. The mixture was mixed for 2 hours in a batch-type rotary ball mill, and then nitrided in a nitrogen atmosphere at a firing temperature of 1600°C for 10 hours. The aluminum nitride powder was then oxidized in an air atmosphere at 700°C for 12 hours to obtain 140 kg of aluminum nitride powder of Example 2.
[0066] <Raman Spectrum> Using a Raman spectroscopic analyzer (Horiba, Ltd., Raman microscope XploRA), the Raman spectroscopic spectrum of the aluminum nitride powder of each example was measured under the conditions of a laser wavelength of 532 nm, an objective lens magnification of 20x, a grating of 300 Gr / mm, a slit width of 50 μm, an exposure time of 1 second, and 10 exposures.
[0067] <Peak intensity> From the obtained Raman spectrum, the wave number was 150 cm -1 More than 350cm -1 The following range (A): 800 cm -1 More than 1000cm -1 The following range (B): 1250 cm -1 More than 1450cm -1 The following range (C), 1500 cm -1 More than 1700cm -1 The following ranges (D) and 500 cm -1 More than 750cm -1 Each maximum peak of scattering intensity present in each of the following ranges (X) was identified, and the peak position (wave number) and peak intensity of each maximum peak were measured. Then, the peak intensity of the maximum peak in the range (A) is I A , the peak intensity of the maximum peak in range (B) is I B , the peak intensity of the maximum peak in the range (C) is I C , the peak intensity of the maximum peak in the range (D) is I D , the peak intensity of the maximum peak in the range (X) is I X When I A / I X , I B / I X , I C / I X and I D / I X The values of were calculated, and the results are shown in Table 1. In addition, in cases where the scattering intensity in range (C) or range (D) is generally low and the maximum peak cannot be identified, the peak position and IC / I X , I D / I X The value of is not stated.
[0068] <Particle size> Using a particle size distribution measuring device (MT3000II manufactured by Nikkiso Co., Ltd.), the volume frequency particle size distribution of the aluminum nitride powder of each example was measured by a laser diffraction scattering method in accordance with JIS R1629:1997. From the obtained volume frequency particle size distribution, the median diameter D 50 , the particle diameter at which the cumulative value reaches 10% D 10 , the particle diameter at which the cumulative value reaches 90% D 90 and (D 90 -D 10 ) / D 50 The results are shown in Table 1.
[0069] <Specific surface area> The specific surface area of the aluminum nitride powder of each example was measured using a specific surface area measuring device (MONOSORB, manufactured by Yuasa Ionics Co., Ltd.) by the BET single point method in accordance with ISO 9277. The results are shown in Table 1.
[0070] <Amount of oxygen> The oxygen content (mass%) of the aluminum nitride powder of each example was measured using an oxygen / nitrogen simultaneous analyzer (EMGA920, manufactured by Horiba, Ltd.) The results are shown in Table 1.
[0071] <Thermal conductivity> For the aluminum nitride powder of each example, 100 parts by mass of aluminum nitride powder, 4 parts by mass of yttrium oxide powder, 3 parts by mass of aluminum oxide powder, 6 parts by mass of cellulose ether binder, 5 parts by mass of glycerin, and 10 parts by mass of ion-exchanged water were mixed to obtain a molding material. The molding material was then molded into a sheet, heated in air at 570°C for 5 hours to be degreased, and then heated under nitrogen gas atmosphere, atmospheric pressure, and 1800°C for 4 hours to obtain an aluminum nitride sintered body. Next, the thermal conductivity of the aluminum nitride sintered body was measured by the laser flash method at 23°C in accordance with JIS R1611:2010. The results are shown in Table 1.
[0072] [Table 1] [Explanation of symbols]
[0073] 20 Conductor 100 Aluminum nitride sintered body 110 Metal plate 200 Bonded Substrate 300 Circuit Board
Claims
1. An aluminum nitride powder comprising aluminum nitride particles, In the Raman spectrum of the aluminum nitride powder measured under the following conditions, the wave number is 150 cm -1 More than 350cm -1 The following range (A) and 800 cm -1 More than 1000cm -1 Each of the peaks is in the following range (B): In the Raman spectrum, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) X The wave number for this is 1250 cm -1 1450cm or more -1 The peak intensity I of the maximum peak in the following range (C) C Ratio I C / I X The aluminum nitride powder has a refractive index of 0.020 or less. (conditions) Laser wavelength: 532 nm Objective lens magnification: 20x Grating: 300Gr / mm Slit width: 50 μm Exposure time: 1 second Number of exposures: 10
2. The aluminum nitride powder according to claim 1 , wherein the Raman spectroscopy spectrum does not have a peak in the range (C).
3. An aluminum nitride powder comprising aluminum nitride particles, In the Raman spectrum of the aluminum nitride powder measured under the following conditions, the wave number is 150 cm -1 More than 350cm -1 The following range (A) and 800 cm -1 More than 1000cm -1 Each of the peaks is in the following range (B): In the Raman spectrum, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) X The wave number is 1500 cm -1 More than 1700cm -1 The peak intensity I of the maximum peak in the following range (D) D Ratio I D / I X The aluminum nitride powder has a refractive index of 0.020 or less. (conditions) Laser wavelength: 532 nm Objective lens magnification: 20x Grating: 300Gr / mm Slit width: 50 μm Exposure time: 1 second Number of exposures: 10
4. The aluminum nitride powder according to claim 3 , wherein the Raman spectroscopy spectrum does not have a peak in the range (D).
5. An aluminum nitride powder comprising aluminum nitride particles, In the Raman spectrum of the aluminum nitride powder measured under the following conditions, the wave number is 150 cm -1 More than 350cm -1 The following range (A) and 800 cm -1 More than 1000cm -1 Each of the peaks is in the following range (B): The volume-based median diameter D of the aluminum nitride powder measured by the laser diffraction scattering method 50 The aluminum nitride powder has a particle size of 0.50 μm or more and 5.00 μm or less. (conditions) Laser wavelength: 532 nm Objective lens magnification: 20x Grating: 300Gr / mm Slit width: 50 μm Exposure time: 1 second Number of exposures: 10
6. An aluminum nitride powder comprising aluminum nitride particles, In the Raman spectrum of the aluminum nitride powder measured under the following conditions, the wave number is 150 cm -1 More than 350cm -1 The following range (A) and 800 cm -1 More than 1000cm -1 Each of the peaks is in the following range (B): The particle diameter D at which the cumulative value reaches 10% in the volume frequency particle size distribution by the laser diffraction scattering method of the aluminum nitride powder is 10 , 90% particle diameter D 90 , median diameter D 50 Regarding (D 90 -D 10 ) / D 50 The aluminum nitride powder has a value of 3.00 or less. (conditions) Laser wavelength: 532 nm Objective lens magnification: 20x Grating: 300Gr / mm Slit width: 50 μm Exposure time: 1 second Number of exposures: 10
7. An aluminum nitride powder comprising aluminum nitride particles, In the Raman spectrum of the aluminum nitride powder measured under the following conditions, the wave number is 150 cm -1 More than 350cm -1 The following range (A) and 800 cm -1 More than 1000cm -1 Each of the peaks is in the following range (B): The aluminum nitride powder has a specific surface area of 1.00 m as measured by the BET single point method in accordance with ISO 9277. 2 / g or more 5.00m 2 / g or less. (conditions) Laser wavelength: 532 nm Objective lens magnification: 20x Grating: 300Gr / mm Slit width: 50 μm Exposure time: 1 second Number of exposures: 10
8. An aluminum nitride powder comprising aluminum nitride particles, In the Raman spectrum of the aluminum nitride powder measured under the following conditions, the wave number is 150 cm -1 More than 350cm -1 The following range (A) and 800 cm -1 More than 1000cm -1 Each of the peaks is in the following range (B): The aluminum nitride powder has an oxygen content of 0.50% by mass or more and 0.90% by mass or less as measured using an oxygen / nitrogen simultaneous analyzer. (conditions) Laser wavelength: 532 nm Objective lens magnification: 20x Grating: 300Gr / mm Slit width: 50 μm Exposure time: 1 second Number of exposures: 10
9. In the Raman spectrum, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) X The peak intensity I of the maximum peak in the range (A) A Ratio I A / I X The aluminum nitride powder according to any one of claims 1 to 8, wherein the alumina content is 0.020 or more and 0.200 or less.
10. In the Raman spectrum, the wave number is 500 cm -1 More than 750cm -1 The peak intensity I of the maximum peak in the following range (X) X The peak intensity I of the maximum peak in the range (B) B Ratio I B / I X The aluminum nitride powder according to any one of claims 1 to 8, wherein the alumina content is 0.030 or more and 0.400 or less.
11. In the Raman spectrum, the wave number is 500 cm -1 More than 750cm -1 The aluminum nitride powder according to any one of claims 1 to 8, further having two or more peaks in the following range (X):
12. The aluminum nitride powder according to any one of claims 1 to 8, which has a thermal conductivity of 120 W / (m·K) or more, as measured by the following method: (method) A molding material is obtained by mixing 100 parts by mass of the aluminum nitride powder, 4 parts by mass of yttrium oxide powder, 3 parts by mass of aluminum oxide powder, 6 parts by mass of cellulose ether binder, 5 parts by mass of glycerin, and 10 parts by mass of ion-exchanged water. The molding material is then molded into a sheet, heated in air at 570°C for 5 hours to be degreased, and then heated under a nitrogen gas atmosphere at atmospheric pressure and 1800°C for 4 hours to obtain an aluminum nitride sintered body. The thermal conductivity of the aluminum nitride sintered body is then measured by a laser flash method at 23°C in accordance with JIS R1611:2010.
13. An aluminum nitride sintered body comprising the aluminum nitride powder according to any one of claims 1 to 8.
14. A circuit board comprising the aluminum nitride sintered body according to claim 13 and a conductor portion.
15. A bonded substrate comprising the aluminum nitride sintered body according to claim 13 and a metal plate.
Citation Information
Patent Citations
Thermally reduced ceramic material and production thereof
JP1989197306A
Aluminum nitride and device for producing semiconductor
JP1997048669A
Resistor and its manufacturing method and its holding device
JP2003040674A
Aluminum nitride powder and resin composition
JP2007284315A
Method for producing aluminum nitride
JP2017145182A