Resin composition, coating composition and coated article

A resin composition with a branched compound, polycarbonate polyol, and functional inorganic particles addresses the wear and weathering issues of polycarbonate products, providing a durable and weather-resistant laminate.

JP7582385B2Active Publication Date: 2024-11-13MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023105257
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-06-27
Publication Date
2024-11-13
Estimated Expiration
2039-03-20

Smart Images

  • Figure 0007582385000001
    Figure 0007582385000001
  • Figure 0007582385000002
    Figure 0007582385000002
Patent Text Reader

Abstract

To provide a thermosetting resin composition that gives a laminate excellent in the appearance of a cured film, adhesion to a base material, chemical resistance and hardness.SOLUTION: A resin composition contains a compound A having a branched structure with a terminal being a hydroxy group, a polycarbonate polyol B, a polyisocyanate C, and an inorganic particle D. The inorganic particle D has a functional group that can react with a hydroxy group or an isocyanate group on the surface.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a coating composition, and a coated article. [Background technology]

[0002] In general, molded products made of polycarbonate resin, polymethyl methacrylate resin, and polystyrene resin are not only lightweight and excellent in moldability, but also have good transparency and excellent impact resistance compared to glass products. Therefore, polycarbonate resin, polymethyl methacrylate resin, and polystyrene resin are used as glass substitute materials for various lamp lenses, window materials, instrument covers, etc. In particular, the use of plastic materials for headlamp lenses is increasing due to the diversification of automobile designs, etc. In recent years, polycarbonate resin molded products with excellent impact resistance are used for window glass and sunroofs in order to reduce the weight of automobiles.

[0003] However, since the surface of polycarbonate resin molded products lacks wear resistance and scratch resistance, they are easily damaged by contact with other hard objects, friction, scratches, etc., and damage to the surface reduces the commercial value of the product.

[0004] When used as automotive components, weather resistance is also important because they are used outdoors. Polycarbonate resin has low weather resistance and is easily degraded by active energy rays such as ultraviolet rays contained in sunlight, causing molded products to yellow significantly and cracks to appear on the surface.

[0005] To compensate for such shortcomings of polycarbonate resin molded products, there is a method of applying a coating material composition, which is made by adding an ultraviolet absorber to a curing raw material such as an acrylic, melamine, urethane, or silicone, which has relatively good weather resistance, to the surface of the molded product and heating it to form a cured film, or a method of curing the material by irradiating it with active energy rays such as ultraviolet rays or electron beams to form a weather-resistant cured film. Among these, the method of curing a thermosetting paint in a heat drying oven has the advantage that it is easy to apply uniform heating regardless of the three-dimensional shape of the coated object, and the obtained cured film is likely to exhibit stable performance regardless of the location.

[0006] As a method for forming a thermosetting cured film on the surface of a resin molded article, coating with a paint containing a urethane resin composition is known.

[0007] For example, Patent Documents 1 and 2 describe urethane resin compositions containing a specific polyol compound, a polyisocyanate compound, and silica particles. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2013-01897 A [Patent Document 2] Japanese Patent Application Publication No. 10-45867 Summary of the Invention [Problem to be solved by the invention]

[0009] However, the urethane resin compositions described in Patent Documents 1 and 2 were insufficient in the appearance, abrasion resistance, hardness, and adhesion to substrates of the cured film.

[0010] The present invention has been made to solve the above-mentioned problems, and has an object to provide a thermosetting resin composition which can give a laminate having excellent appearance of a cured film, adhesion to a substrate, chemical resistance and hardness. [Means for solving the problem]

[0011] That is, the above object of the present invention can be achieved by the following means [1] to

[14] . [1] A resin composition comprising: a compound A having a branched structure with a hydroxyl group at the end; a polycarbonate polyol B; a polyisocyanate C; and inorganic particles D, the inorganic particles D having functional groups on their surfaces that can react with hydroxyl groups or isocyanate groups. [2] The resin composition according to [1], wherein the compound A is a polymer having a dendritic branched structure. [3] The resin composition according to [1] or [2], wherein the compound A is a hyperbranched polymer having a hydroxyl group at its terminal. [4] The resin composition according to any one of [1] to [3], wherein the content of the compound A is 10 mass % or more and 50 mass % or less in the total mass (100 mass %) of the compound A, the polycarbonate polyol B, the polyisocyanate C, and the inorganic particles D. [5] The resin composition according to any one of [1] to [4], wherein the compound A has a weight average molecular weight of 550 or more and 30,000 or less. [6] The resin composition according to any one of [1] to [5], wherein the compound A has a hydroxyl value of 20 mg·KOH / g or more and 1000 mg·KOH / g or less. [7] The resin composition according to any one of [1] to [6], wherein the polycarbonate polyol B is a compound having a ring structure in the molecule. [8] The resin composition according to any one of [1] to [7], wherein the polyisocyanate C is a tri- or higher functional isocyanate. [9] The resin composition according to any one of [1] to [8], wherein the functional group capable of reacting with a hydroxyl group or an isocyanate group of the inorganic particles D is any one of a mercapto group, an isocyanate group, and an epoxy group.

[10] The resin composition according to any one of [1] to [9], wherein the inorganic particles D are silica particles that have been surface-treated with a silane coupling agent having a functional group capable of reacting with a hydroxyl group or an isocyanate group.

[11] The resin composition according to any one of [1] to

[10] , wherein the content of the inorganic particles D in the total mass (100 mass%) of the compound A, the polycarbonate polyol B, the polyisocyanate C, and the inorganic particles D is 1 mass% or more and 40 mass% or less.

[12] The resin composition according to any one of [1] to

[11] , further comprising an ultraviolet absorber E which is at least one of compounds derived from a triazine-based compound, a benzophenone-based compound, a benzotriazole-based compound, a phenyl salicylate-based compound, a phenyl benzoate-based compound, or the like.

[13] A coating composition comprising the resin composition according to any one of [1] to

[12] .

[14] A coated article having a cured film of the coating composition according to

[13] . Effect of the Invention

[0012] The resin composition of the present invention can provide a thermosetting resin composition capable of producing a laminate having excellent appearance of a cured film, adhesion to a substrate, chemical resistance and hardness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [Resin composition] The resin composition of the present invention contains a compound A having a branched structure terminated in a hydroxyl group, a polycarbonate polyol B, a polyisocyanate C, and inorganic particles D.

[0014] <Compound A having a branched structure with a terminal hydroxyl group> Compound A in the present invention has a branched structure and has two or more hydroxyl groups at the ends of the branched structure. By having a plurality of hydroxyl groups at the ends of the branched structure, the crosslink density of the cured film formed from the resin composition of the present invention is increased, and the abrasion resistance and hardness of the cured film are improved.

[0015] Examples of compound A include alcohols having a branched structure and polymers having a dendritic branched structure and terminal hydroxyl groups.

[0016] Even when the content of inorganic particles D is small, compound A is preferably a polymer having a dendritic branched structure having hydroxyl groups at its terminals, in that the abrasion resistance and hardness of the cured film are improved.

[0017] Examples of alcohols having a branched structure include methylpropanediol, trimethylolethane, trimethylolpropane, glycerol, polycaprolactone triol, erythritol, pentaerythritol, polycaprolactone tetraol, and diglycerin.

[0018] Examples of the polymer having a dendritic branched structure with terminal hydroxyl groups include dendrimers and hyperbranched polymers, with the hyperbranched polymers being preferred because they are easy to synthesize and can be easily produced on an industrial scale.

[0019] As dendrimers, there are used Boltorn (registered trademark; the same applies below) H20 (hydroxyl value: 490-520 mg KOH / g, weight average molecular weight (Mw): 2100 (catalog value)), Boltorn H311 (hydroxyl value: 230-260 mg KOH / g, weight average molecular weight (Mw): 5700 (catalog value)), Boltorn H2004 (hydroxyl value: 105-125 mg KOH / g, weight average molecular weight (Mw): 3200 (catalog value)), Boltorn P500 (hydroxyl value: 560-630 mg KOH / g, weight average molecular weight (Mw): 1800 (catalog value)), Boltorn P1000 (hydroxyl value: 430-490 mg KOH / g, weight average molecular weight (Mw): 1500 (catalog value)), Boltorn Examples include U3000 (hydroxyl value 15 mg KOH / g, weight average molecular weight (Mw) 6500 (catalog value)), Boltorn W3000 (hydroxyl value 15 mg KOH / g, weight average molecular weight (Mw) 9000 (catalog value)).

[0020] Examples of hyperbranched polymers include BASF's Basonol (registered trademark; the same applies below) HPE 1170B (hydroxyl value 280 mg KOH / g, weight average molecular weight (Mw) 1800 (catalog value)), Basonol HPE 021 (hydroxyl value 190 mg KOH / g, weight average molecular weight (Mw) 1400 (catalog value)), Basonol HPE-026 (hydroxyl value 180 mg KOH / g, weight average molecular weight (Mw) 2600 (catalog value)), and Basonol HPE-046 (hydroxyl value 250 mg KOH / g, weight average molecular weight (Mw) 4800 (catalog value)). The compound A may be used alone or in combination of two or more kinds.

[0021] The molecular weight of the compound A (when the compound A is a polymer, this means the weight average molecular weight) is preferably 550 or more and 30,000 or less, more preferably 600 or more and 10,000 or less, and further preferably 800 or more and 5,000 or less. When the molecular weight of the compound A is equal to or more than the lower limit, the adhesion between the cured film and the substrate and the hardness of the cured film are likely to be improved.When the weight average molecular weight of the compound A is equal to or less than the upper limit, the appearance of the cured film is likely to be good.

[0022] When the compound A is a polymer, the weight average molecular weight is a weight average molecular weight (Mw) calculated in terms of standard polystyrene measured by gel permeation chromatography (GPC).

[0023] The compound A preferably has three or more hydroxyl groups per molecule. By having three or more hydroxyl groups per molecule, the crosslink density of the cured film increases, and the abrasion resistance and hardness tend to improve.

[0024] The hydroxyl value of the compound A is preferably from 20 to 1000 mg·KOH / g, more preferably from 50 to 600 mg·KOH / g, and even more preferably from 100 to 400 mg·KOH / g. When the hydroxyl value of the compound A is equal to or greater than the lower limit, the hardness of the cured film is likely to be improved.When the hydroxyl value of the compound A is equal to or less than the upper limit, the solubility of the resin composition of the compound A in a non-polar solvent and the compatibility with multiple components such as the polycarbonate polyol B and the compound D are likely to be good.

[0025] The content of the compound A in the resin composition of the present invention is preferably 10% by mass or more and 50% by mass or less, more preferably 15% by mass or more and 45% by mass or less, and even more preferably 20% by mass or more and 40% by mass or less, based on the total mass (100% by mass) of the compound A, the polycarbonate polyol B, the polyisocyanate C, and the inorganic particles D. When the content of the compound A is equal to or less than the upper limit, the abrasion resistance and hardness of the obtained cured film are likely to be improved.When the content of the compound A is equal to or more than the lower limit, the appearance of the obtained cured film and the drying property after the formation of the cured film are likely to be improved.

[0026] <Polycarbonate polyol B> In the present invention, by including the polycarbonate polyol B, the adhesion to the substrate is improved.

[0027] The polycarbonate polyol B may have a polycarbonate structure in the molecule and two or more hydroxyl groups at the terminals, but it is preferable that the terminals are primary hydroxyl groups. From the viewpoint of weather resistance, the polycarbonate polyol B is preferably an aliphatic polycarbonate polyol.

[0028] Examples of the aliphatic polycarbonate polyol include Kuraray Polyol (registered trademark; the same applies below) C-1090 (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog value)) manufactured by Kuraray Co., Ltd., Kuraray Polyol C-2090 (hydroxyl value 56.1 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value)), Kuraray Polyol C-3090 (hydroxyl value 37 mg KOH / g, weight average molecular weight (Mw) 3000 (catalog value)), and Duranol ( Registered trademark. The same applies below) T-5651 (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog value)), Duranol T-5652 (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value)), Duranol T-4691 (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog value)), Duranol T-4692 (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value)), Duranol T -4671 (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog value)), Duranol G-4672 (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value)), Duranol G-3450J (hydroxyl value 140 mg KOH / g, weight average molecular weight (Mw) 800 (catalog value)), Duranol G-3452 (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value)), Mitsubishi Chemical Corporation Benebiol (registered Trademark. The same applies below) NL1010DB (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog value)), Benebiol NL2010DB (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value)), Benebiol NL1000B (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog value)), Benebiol NL2000B (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value)), Benebiol All NL1050B (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog value)), Benebiol NL2050B (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value)), Benebiol HS0840B (hydroxyl value 140 mg KOH / g, weight average molecular weight (Mw) 800 (catalog value)), Benebiol HS0850B (hydroxyl value 140 mg KOH / g, weight average molecular weight (Mw) 800 (catalog value)), Ube Industries ETERNALCOLL (registered trademark; the same applies below) UHC50-100 (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog value)), ETERNALCOLL UHC50-200 (hydroxyl value 56 mg KOH / g, weight average molecular weight (Mw) 2000 (catalog value)), ETERNALCOLL Examples include UC-100 (hydroxyl value 112 mg KOH / g, weight average molecular weight (Mw) 1000 (catalog value)), ETERNALCOLL UM-90 (hydroxyl value 125 mg KOH / g, weight average molecular weight (Mw) 900 (catalog value)).

[0029] From the viewpoint of increasing the hydrophobicity of the cured film and improving the chemical resistance and adhesion, an aliphatic polycarbonate polyol having a ring structure is preferred as the aliphatic polycarbonate polyol B. As the aliphatic polycarbonate polyol having a ring structure, Benebiol HS0840B and Benebiol HS0850B manufactured by Mitsubishi Chemical Corporation, ETERNALCOLL UC-100 and ETERNALCOLL UM-90 manufactured by Ube Industries, Ltd. are preferred. The polycarbonate polyol B may be used alone or in combination of two or more kinds.

[0030] The weight average molecular weight (Mw) of the polycarbonate polyol B is preferably 300 or more and 10,000 or less, more preferably 400 or more and 8,000 or less, and even more preferably 500 or more and 7,500 or less. When the weight average molecular weight (Mw) of the polycarbonate polyol B is equal to or higher than the lower limit, the appearance is likely to be maintained at a high quality for a long period of time. When the weight average molecular weight (Mw) of the polycarbonate polyol B is equal to or lower than the upper limit, the scratch resistance of the cured film is likely to be improved.

[0031] The content of polycarbonate polyol B in the resin composition of the present invention is preferably 5% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 30% by mass or less, and even more preferably 7% by mass or more and 20% by mass or less, based on the total mass (100% by mass) of compound A, polycarbonate polyol B, polyisocyanate C, and inorganic particles D. When the content of polycarbonate polyol B is equal to or less than the upper limit, the weather resistance, chemical resistance, and adhesion to a substrate of the obtained cured film are likely to be improved.When the content of polycarbonate polyol B is equal to or more than the lower limit, the hardness of the obtained cured film is likely to be improved.

[0032] <Polyisocyanate C> The polyisocyanate C in the present invention reacts with the hydroxyl groups of the compound A and the polycarbonate polyol B to form urethane bonds, thereby increasing the crosslink density of the cured film and improving the weather resistance, chemical resistance and hardness of the cured film.

[0033] Examples of the polyisocyanate C include bifunctional isocyanates such as hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, and 4,4-dicyclohexyl diisocyanate, and trifunctional or higher isocyanates such as biuret compounds, trimethylolpropane adduct compounds, isocyanurate compounds, and allophanate compounds synthesized using the above bifunctional isocyanates as a starting material.

[0034] As the trifunctional or higher isocyanate, a burette of hexamethylene diisocyanate manufactured by Asahi Kasei Corporation (trade name: Duranate (registered trademark; the same applies below) 24A-100 ), hexamethylene diisocyanate adduct (product name: Duranate P-301-75E), hexamethylene diisocyanate isocyanurate (product name: Duranate TPA-100), blocked isocyanate (product name: Duranate MF-K60X), Mitsui Chemicals' 1,3-bis(isocyanatomethyl)cyclohexane trimethylolpropane adduct (product name: Takenate (registered trademark; the same applies below) D-120N), 1,3-bis(isocyanatomethyl)cyclohexane ) cyclohexane isocyanurate (trade name: Takenate D-127N), trimethylolpropane adduct of isophorone diisocyanate (trade name: Takenate D-140N), allophanate of hexamethylene diisocyanate manufactured by Sumika Covestro Urethane Co., Ltd. (trade name: Desmodur (registered trademark; the same applies below) XP2679), and isocyanurate of isophorone diisocyanate manufactured by EVONIK (trade name: Desmodur T-1890 / 100).

[0035] The polyisocyanate C is preferably a tri- or higher functional isocyanate from the viewpoints of increasing the crosslink density of the cured film and improving the weather resistance, stain resistance, and hardness of the cured film. The polyisocyanate C may be used alone or in combination of two or more kinds.

[0036] From the viewpoint of the performance of the cured film, the compounding ratio of the polyisocyanate C to the compound A and the polycarbonate polyol B is preferably such that NCO / OH [the number of moles of isocyanate groups in the polyisocyanate C / the number of moles of hydroxyl groups in the compound A and the polycarbonate polyol B] is 0.5 or more and 2.0 or less, more preferably 0.7 or more and 1.8 or less, and even more preferably 1.0 or more and 1.6 or less.

[0037] When the equivalent ratio of the isocyanate group of the polyisocyanate C is equal to or greater than the lower limit, the curing rate of the resin composition can be increased, and the crosslink density of the cured film of the resin composition can be increased, so that the hardness and water resistance of the cured film can be improved.When the equivalent ratio of the isocyanate group of the polyisocyanate C is equal to or less than the upper limit, the drying property and adhesion of the cured film of the resin composition after it is formed can be improved.

[0038] <Inorganic particles D> The inorganic particles D in the present invention have, on the surface, functional groups capable of reacting with hydroxyl groups or isocyanate groups.

[0039] Since the inorganic particles D have on their surfaces functional groups capable of reacting with hydroxyl groups or isocyanate groups, the inorganic particles D are fixed to the resin component, and the abrasion resistance of the cured film is improved.

[0040] Examples of the functional group capable of reacting with a hydroxyl group include an isocyanate group, an epoxy group, a carboxyl group, etc. Examples of the functional group capable of reacting with an isocyanate group include a mercapto group, a hydroxyl group, an amino group, a carboxyl group, an isocyanate group, etc.

[0041] The functional group capable of reacting with the hydroxyl group or isocyanate group of the inorganic particles D is preferably a mercapto group, an isocyanate group, an amino group, or an epoxy group, because they have high reactivity with the hydroxyl group or isocyanate group.

[0042] The inorganic particles D can be obtained, for example, by surface-treating silica particles that do not have functional groups on their surfaces that can react with hydroxyl groups or isocyanate groups with a silane coupling agent that has functional groups that can react with hydroxyl groups or isocyanate groups.

[0043] Examples of silica particles that do not have a functional group on the surface that can react with a hydroxyl group or an isocyanate group include methanol-dispersed silica sol (MA-ST, MA-ST-M), isopropyl alcohol-dispersed silica sol (IPA-ST, IPA-ST-L, IPA Commercially available products such as silica sol dispersed in ethylene glycol (EG-ST, EG-ST-L), silica sol dispersed in dimethylacetamide (DMAC-ST, DMAC-ST-L), silica sol dispersed in xylene / butanol (XBA-ST), silica sol dispersed in methyl ethyl ketone (MEK-ST, MEK-ST-L, MEK-ST-ZL, MEK-ST-UP), silica sol dispersed in methyl isobutyl ketone (MIBK-ST), and silica sol dispersed in propylene glycol monomethyl ether acetate (PMA-ST) can be used.

[0044] Examples of silane coupling agents having a functional group capable of reacting with a hydroxyl group or an isocyanate group include silane compounds having a glycidyl group such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltriethoxysilane, and 3-glycidoxypropylmethyldiethoxysilane; 1-mercaptomethyltrimethoxysilane, 1-mercaptomethylmethyldimethoxysilane, 1-mercaptomethyltriethoxysilane, and 1-mercaptomethylmethyldiethoxysilane; silane compounds having a mercapto group, such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-aminopropyltriethoxysilane; silane compounds having an amino group, such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, and 3-aminopropyltriethoxysilane; and 3-isocyanatepropyltriethoxysilane.

[0045] In addition, examples of commercially available dispersions of the inorganic particles D include MEK-EC-2130Y, MEK-EC-6150P, and MEK-EC-7150P manufactured by Nissan Chemical Industries, Ltd. The inorganic particles D may be used alone or in combination of two or more kinds.

[0046] The content of the inorganic particles D in the resin composition of the present invention is preferably from 1 mass % to 40 mass % inclusive, more preferably from 1 mass % to 30 mass % inclusive, and even more preferably from 1 mass % to 10 mass % inclusive, based on the total mass (100 mass %) of the compound A, the polyisocyanate B, and the inorganic particles C.

[0047] When the content of the inorganic particles D is equal to or less than the upper limit, it is easy to maintain a high appearance for a long period of time and to reduce the cost of the coating material.When the content of the inorganic particles D is equal to or more than the lower limit, it is easy to improve the abrasion resistance and hardness of the obtained cured film.

[0048] The average particle size of the inorganic particles D is preferably from 2 nm to 300 nm, more preferably from 2 nm to 100 nm, further preferably from 4 nm to 100 nm, and particularly preferably from 4 nm to 50 nm. When the average particle size of the inorganic particles D is equal to or larger than the lower limit, the abrasion resistance is easily improved. When the average particle size of the inorganic particles D is equal to or smaller than the upper limit, the transparency of the cured film of the resin composition is easily maintained.

[0049] The average particle size of the inorganic particles D is a value calculated from a specific surface area measured by a BET adsorption method (based on JIS Z8830).

[0050] <Ultraviolet absorber E> The ultraviolet absorber E in the present invention can impart the effect of absorbing ultraviolet rays contained in sunlight to the cured film of the resin composition, and can improve the weather resistance of the cured film.

[0051] The ultraviolet absorber E is not particularly limited as long as it can absorb ultraviolet rays, but it is preferable that the ultraviolet absorber E is capable of dissolving uniformly in the resin composition of the present invention and provides a cured film having good weather resistance.

[0052] The ultraviolet absorber E is preferably at least one ultraviolet absorber selected from the group consisting of triazine-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, phenyl salicylate-based ultraviolet absorbers, and phenyl benzoate-based ultraviolet absorbers.

[0053] Benzophenone-based UV absorbers are preferred because they can be contained in large amounts in the coating composition containing the resin composition. Also, triazine-based UV absorbers and benzotriazole-based UV absorbers are preferred because they can prevent yellowing of substrates such as polycarbonate. Furthermore, UV absorbers having a hydroxyl group capable of reacting with an isocyanate group are more preferred because they are less likely to bleed out from the cured film.

[0054] In the present invention, the ultraviolet absorbent E is preferably an ultraviolet absorbent having a maximum absorption wavelength in the range of 240 to 380 nm.

[0055] Examples of the ultraviolet absorber E include benzophenone-based ultraviolet absorbers such as 2-hydroxybenzophenone, 5-chloro-2-hydroxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, and 2,2'-dihydroxy-4,4'-dimethoxybenzophenone; benzotriazole-based ultraviolet absorbers such as 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, and 2-(2-hydroxy-5-(2-methacryloyloxyethyl)phenyl)-2H-benzotriazole; [4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy hydroxyphenyltriazine-based ultraviolet absorbers such as 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine; phenyl salicylate, p-tert-butylphenyl salicylate, p-(1,1,3,3-tetramethylbutyl)phenyl salicylate, 3-hydroxyphenyl benzoate, and phenylene-1,3-dibenzoate.These may be used alone or in combination of two or more.

[0056] The content of the ultraviolet absorber E in the resin composition of the present invention is preferably 5% by mass or more and 40% by mass or less, and more preferably 10% by mass or more and 30% by mass or less, based on the total mass (100% by mass) of the compound A, the polycarbonate polyol B, the polyisocyanate C, and the inorganic particles D. When the content of the ultraviolet absorber is equal to or more than the lower limit, the weather resistance of the cured film is likely to be improved. When the content of the infrared absorbing agent is equal to or less than the upper limit, the curability of the coating composition and the toughness, heat resistance and abrasion resistance of the cured film tend to be improved.

[0057] <Other ingredients> The resin composition of the present invention may contain other components in addition to the compound A, the polycarbonate polyol B, the polyisocyanate C, the inorganic particles D, and the UV absorber E, so long as the effects of the present invention are not impaired.

[0058] The resin composition of the present invention may contain, in addition to the ultraviolet absorber E, a weather resistance imparting agent such as a light stabilizer in order to improve the weather resistance of the cured film.

[0059] As the light stabilizer, for example, a hindered amine light stabilizer can be used. The hindered amine light stabilizer can further improve the weather resistance of the cured film by using it in combination with an ultraviolet absorber.

[0060] Examples of the hindered amine-based light stabilizer include a condensate of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, and β,β,β,β-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5,5])undecane)diethanol (trade name: Adeka STAB (registered trademark; the same applies below) LA-63P), manufactured by ADEKA Corporation; Condensation product of 2,2,6,6-pentamethyl-4-piperidinol and β,β,β,β-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5,5])undecane)diethanol (trade name: Adeka STAB LA-68P, manufactured by BASF), condensation product of 1,1-dimethylethyl hydroperoxide and octane, bis(2,2,6,6-tetramethyl-1-(octane) decanedioate 2,4-bis[N-butyl-N-(1-phenyloxy)-4-piperidinyl]malonate (trade name: Tinuvin 144), 2-butyl-2-[3,5-di(tert-butyl)-4-hydroxybenzyl]malonate bis(1,2,2,6,6-pentamethyl-4-piperidyl) (trade name: Tinuvin 144), 2,4-bis[N-butyl-N-(1-phenyloxy)-4-piperidinyl]malonate ... cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)amino]-6-(2-hydroxyethylamine)-1,3,5-triazine (trade name: Tinuvin 152), a mixture of bis(1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate and methyl(1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate (trade name: Tinuvin 292), and the like. The hindered amine light stabilizers may be used alone or in combination of two or more kinds.

[0061] The content of the hindered amine light stabilizer in the resin composition of the present invention is preferably 0.1 mass% or more and 5 mass% or less, and more preferably 0.5 mass% or more and 2 mass% or less, relative to the total mass (100 mass%) of the compound A, the polyisocyanate B, and the inorganic particles C.

[0062] When the content of the hindered amine light stabilizer is equal to or greater than the lower limit, the weather resistance of the coating film is likely to be improved.When the content of the hindered amine light stabilizer is equal to or less than the upper limit, the curability of the coating composition and the toughness, heat resistance, and abrasion resistance of the cured film are likely to be improved.

[0063] <Method of producing resin composition> The resin composition of the present invention can be produced by uniformly mixing the compound A, the polycarbonate polyol B, the polyisocyanate C, and the inorganic particles D. If necessary, the other components described above may be added. The mixing method is not limited as long as it is a normal mixer capable of uniformly mixing the components, and any known mixer can be used.

[0064] [Paint composition] The coating composition of the present invention includes the resin composition of the present invention. If necessary, a curing-accelerating catalyst, an organic solvent, an antioxidant, an anti-yellowing agent, a bluing agent, a pigment, a leveling agent, an antifoaming agent, a thickener, an anti-settling agent, an antistatic agent, an anti-fogging agent, and the like are blended into the resin composition of the present invention.

[0065] <Curing accelerating catalyst> The coating composition of the present invention can be cured at room temperature or by heating, and may contain a curing-accelerating catalyst as required.

[0066] The curing-accelerating catalyst is not particularly limited, and examples of the curing-accelerating catalyst that can be used include monoamines such as triethylamine and N,N-dimethylcyclohexylamine, diamines such as tetramethylethylenediamine, other triamines, cyclic amines, alcohol amines such as dimethylethanolamine, ether amines, and other amines; potassium acetate, potassium 2-ethylhexanoate, calcium acetate, lead octoate, dibutyltin dilaurate, tin octoate, bismuth neodecanoate, bismuth oxycarbonate, bismuth 2-ethylhexanoate, zinc octoate, zinc neodecanoate, phosphine, phosphophosphoric acid, and other commonly used metal catalysts. These may be used alone or in combination of two or more kinds.

[0067] The content of the curing-accelerating catalyst is preferably from 0.001 to 10% by mass, more preferably from 0.01 to 5% by mass, and even more preferably from 0.1 to 1% by mass, relative to the mass (100% by mass) of polyisocyanate B. The release agent, flow control agent, and leveling agent are not particularly limited, but examples thereof include silicone, wax, stearates, polysiloxanes such as BYK-300 (manufactured by BYK Chemicals), and fluorine-based surfactants such as Megafac F-477 (manufactured by DIC Corporation).

[0068] <Organic solvent> In order to adjust the workability during coating, the coating composition of the present invention preferably contains an organic solvent in an amount of 1 to 90% by weight based on the mass (100% by weight) of the coating composition, more preferably 20 to 80% by weight, and even more preferably 40 to 70% by weight.

[0069] The organic solvent to be used is not particularly limited, but examples thereof include alcohols such as methanol, ethanol, isopropyl alcohol, n-butanol, diacetone alcohol, 2-methoxyethanol (methyl cellosolve), 2-ethoxyethanol (ethyl cellosolve), 2-butoxyethanol (butyl cellosolve), and tertiary amyl alcohol; esters such as ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, and butyl formate; ketones such as methyl ethyl ketone, methyl isobutyl ketone, acetone, cyclohexanone, and diisobutyl ketone; amides such as dimethylformamide and dimethylacetamide; ethers such as diethyl ether, methoxytoluene, 1,2-dimethoxyethane, 1,2-dibutoxyethane, 1,1-dimethoxymethane, 1,1-dimethoxyethane, 1,4-dioxane, and tetrahydrofuran; aliphatic hydrocarbons such as pentane, hexane, heptane, cyclohexane, and methylcyclohexane; and aromatic hydrocarbons such as toluene, xylene, and benzene.

[0070] Among these, non-alcohol-based solvents are preferred, since they are not reactive with polyisocyanate C and do not deteriorate the physical properties of the cured film. These may be used alone or in combination of two or more kinds.

[0071] [Painted items] The coated article of the present invention has a cured film of the coating composition of the present invention. The coated article of the present invention can be obtained by applying the coating composition of the present invention to a substrate by a known coating method, and then curing the coating composition of the present invention applied to the substrate.

[0072] Examples of the substrate include metals such as zinc-plated steel sheet, zinc alloy-plated steel sheet, stainless steel sheet, and tin-plated steel sheet, polymethyl methacrylate resin, polycarbonate resin, polyester resin, polystyrene resin, ABS resin, AS resin, polyamide resin, polyarylate resin, polymethacrylimide resin, and polyallyl diglycol carbonate resin.

[0073] In particular, the coated article of the present invention is effective in improving the abrasion resistance of the surface of a substrate when polymethyl methacrylate resin, polycarbonate resin, polystyrene resin, or polymethacrylimide resin is used as the substrate.

[0074] The coating composition of the present invention can be applied to a substrate by a known method such as brush coating, bar coating, spray coating, dip coating, spin coating, curtain coating, or the like.

[0075] The curing temperature when curing the coating composition of the present invention applied to a substrate may be appropriately set taking into consideration the heat resistance and thermal deformation properties of the substrate, and is preferably from 20°C to 200°C, more preferably from 60°C to 150°C, and even more preferably from 80°C to 120°C.

[0076] The curing time for curing the coating composition of the present invention applied to a substrate is preferably several minutes to several tens of minutes.

[0077] The thickness of the cured film of the coating composition of the present invention in the coated article of the present invention is preferably 3 μm or more and 50 μm or less.

[0078] When the thickness of the cured film in the coated article of the present invention is equal to or greater than the lower limit, the abrasion resistance and hardness of the cured film are good, and the appearance is easily maintained for a long period of time. When the thickness of the cured film in the coated article of the present invention is equal to or less than the upper limit, cracks are easily suppressed. EXAMPLES

[0079] The present invention will be described in more detail below with reference to examples and comparative examples. In the examples, unless otherwise specified, "parts" refers to "parts by mass". Each evaluation was carried out in the following manner.

[0080] <Weight average molecular weight> The weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC) under the following conditions, and calculated in terms of standard polystyrene. Equipment: Tosoh Corporation high-speed GPC equipment HLC-8320GPC type UV detector: Tosoh UV-8320 Flow rate: 0.35mL / min Inlet temperature: 40℃ Oven temperature: 40℃ RI temperature: 40℃ UV wavelength: 254nm Sample injection volume: 10 μL Columns: Three columns connected in the order of (1) to (3). (1) Tosoh TSKgel superHZM-M (4.6mm ID x 15cm L) (2) Tosoh TSKgel superHZM-M (4.6mm ID x 15cm L) (3) Tosoh TSKgel HZ2000 (4.6mm ID x 15cm L) Guard column: Tosoh TSKguardcolumn SuperHZ-L (4.6mm ID x 3.5cm L) Solvent: THF (stabilized with BHT) Sample concentration: Resin content adjusted to 0.2% by mass

[0081] <Evaluation sample> Each of the coating compositions shown in Tables 1 and 2 was spray-coated onto a 3 mm thick polycarbonate resin plate (manufactured by Mitsubishi Engineering Plastics Corporation, product name: "IUPILON ML-300") so that the coating film after curing would be 10 μm thick. The plate was then heated at 120° C. for 30 minutes to form a coating film on the polycarbonate resin plate, which was then evaluated.

[0082] <Appearance> The appearance of the coating film was evaluated by measuring the diffuse transmittance (haze value) using a haze meter (HM-65W, manufactured by Murakami Color Research Laboratory Co., Ltd.) in accordance with JIS K7136: 2000. Haze less than 1% was judged as ○ (good), and haze 1% or more was judged as × (bad).

[0083] <Adhesion> The adhesion resistance of the coating film was evaluated by the following procedure. 100 squares were made on the surface of the coating film by cutting 1.5 mm apart vertically and horizontally, reaching 11 substrates, with a cutter, and cellophane adhesive tape (25 mm wide, Nichiban Co., Ltd.) was pressed onto the squares and then rapidly peeled off upwards. Adhesion was evaluated by the number of remaining squares / total number of squares (100) and visual observation according to the following criteria. ○: 100 / 100 (no peeling or chipping). ×: 0 / 100~99 / 100 (peeling occurs).

[0084] <Chemical resistance> The chemical resistance of the coating was evaluated by dropping 2mL of brake fluid oil (TOYOTA genuine DOT-3) onto the evaluation sample, leaving it to stand for 24 hours in an environment of 23°C, and then wiping off the oil and visually inspecting the appearance of the coating. ○: No traces of chemicals are visible (good) △: Chemical traces are faintly visible (slightly poor) ×: Chemical traces are visible (defective)

[0085] <Scratch resistance> The scratch resistance of the coating was evaluated using a flat surface abrasion tester (KASAI scratch tester) with steel wool #000 placed on the evaluation sample at 250g / 1.1cm 2 After 50 reciprocating strokes under a load of 1000 rpm using a rubbing tester, the diffuse transmittance (haze value) was measured using a haze meter (HM-65W, manufactured by Murakami Color Research Laboratory Co., Ltd.). The scratch resistance was evaluated based on the value (Δ haze value) obtained by subtracting the initial haze value from the measured haze value. ◎: Increase in haze value = less than 1.0% ○: Increased haze value = 1.0% or more, less than 2.0% ×: Increase in haze value = 2.0% or more

[0086] <Pencil hardness> The hardness of the coating was evaluated by pencil hardness in accordance with ISO / DIS 15184. After that, the highest hardness that did not cause any scratches was adopted as the pencil hardness of the coating film.

[0087] (Production Example 1) Production method of inorganic particle dispersion D-1 To flask A were added 1.2 g of 3-mercaptopropyltrimethoxysilane manufactured by Tokyo Chemical Industry Co., Ltd., 0.6 g of distilled water, and 2.1 g of tetrahydrofuran, and the mixture was stirred at 30° C. for 3 hours to obtain a silanol solution. 100 g of methyl isobutyl ketone-dispersed silica sol (product name: "MIBK-ST", solvent: methyl isobutyl ketone, solid content: 30% by mass, average particle size: 15 nm) manufactured by Nissan Chemical Industries, Ltd. was added to flask B, and the temperature was raised to 70°C. The silanol solution in Flask A was added dropwise to Flask B, and after completion of the addition, the mixture was stirred at 70° C. for 1 hour to obtain a dispersion D-1 (solid content 20%) of inorganic particles having a mercapto group.

[0088] (Production Example 2) Production method of inorganic particle dispersion D-2 To flask A were added 1.2 g of 3-methacryloylpropyltrimethoxysilane manufactured by Tokyo Chemical Industry Co., Ltd., 0.6 g of distilled water, and 2.1 g of tetrahydrofuran, and the mixture was stirred at 30° C. for 3 hours to obtain a silanol solution. 100 g of methyl isobutyl ketone-dispersed silica sol (product name: "MIBK-ST", solvent: methyl isobutyl ketone, solid content: 30% by mass, average particle size: 15 nm) manufactured by Nissan Chemical Industries, Ltd. was added to flask B, and the temperature was raised to 70°C. The silanol solution in Flask A was added dropwise to Flask B, and after completion of the addition, the mixture was stirred at 70° C. for 1 hour to obtain a dispersion D-2 (solid content 20%) of inorganic particles having methacryloyl groups.

[0089] Example 1 As the compound A having a hydroxyl group, 100 parts of Basonol (registered trademark) HPE1170B manufactured by BASF (components will be described later; the same applies below), as the polycarbonate polyol B, 30 parts of Kuraray Polyol C-1090 manufactured by Kuraray Co., Ltd., as the polycarbonate polyol B, 159 parts of Duranate MHG-80B manufactured by Asahi Kasei Corporation, as the polyisocyanate C, 70 parts of inorganic particle dispersion D-1 as the inorganic particle D, and Tinuvin 40 manufactured by BASF as the ultraviolet absorber were used. The mixture was mixed uniformly and then diluted with cyclohexanone and MIBK to a solids concentration of approximately 32%. The evaluation results of the resulting coating compositions are shown in Table 1.

[0090] (Examples 2 to 13 and Comparative Examples 1 to 8) Coating compositions were prepared in the same manner as in Example 1 using the compositions shown in Tables 1 and 2. The evaluation results of the resulting coating compositions are shown in Tables 1-2. The values ​​in the table indicate parts by mass, and the values ​​in parentheses indicate solid content values ​​(parts by mass).

[0091] [Table 1]

[0092] [Table 2]

[0093] The ingredients in the table are as follows: ·Basonol HPE 1170B: BASF hyperbranched polymer with terminal hydroxyl groups, solids content 70%, water Acid value: 280 mg KOH / g, weight average molecular weight (Mw): 1800. ·Basonol HPE 1265B: Hyperbranched polymer with hydroxyl groups at the ends, manufactured by BASF, solid content 65%, hydroxyl value: 190 mg KOH / g, weight average molecular weight (Mw): 2600. Kuraray Polyol C-1090: Polycarbonate diol with hydroxyl groups at both ends manufactured by Kuraray Co., Ltd., solid content 100%, hydroxyl value: 112 mg KOH / g, number average molecular weight (Mn): 1000. Duranol T-5651: Polycarbonate diol with hydroxyl groups at both ends manufactured by Asahi Kasei Corporation, solid content 100%, hydroxyl value: 112 mg KOH / g, number average molecular weight (Mn): 1000. Benebiol HS0840B: Polycarbonate diol with hydroxyl groups on both ends, manufactured by Mitsubishi Chemical Corporation, solid content 100%, hydroxyl value: 140 mg KOH / g, number average molecular weight (Mn): 800. ETERNACOLL UM-90(3 / 1): Polycarbonate diol with hydroxyl groups at both ends, manufactured by Ube Industries, Ltd., solid content 100%, hydroxyl value: 125 mg KOH / g, number average molecular weight (Mn): 900. Kuraray Polyol P-1050: Polyester diol with hydroxyl groups at both ends, manufactured by Kuraray Co., Ltd., solid content 100%, hydroxyl value: 112 mg KOH / g, number average molecular weight (Mn): 1000. NISSO‐PB G-1000: Polybutadiene diol with hydroxyl groups at both ends, manufactured by Nippon Soda Co., Ltd., solid content 100%, hydroxyl value: 73 mg KOH / g, number average molecular weight (Mn): 1,400. PTMG-1050: Polyether diol with hydroxyl groups on both ends, manufactured by Mitsubishi Chemical Corporation, solid content 100%, hydroxyl value: 112 mg KOH / g, number average molecular weight (Mn): 1000. Duranate MHG-80B: Isocyanurate of hexamethylene diisocyanate and isophorone diisocyanate manufactured by Asahi Kasei Corporation, solids content 80%, 3.60 mmol / g. Vestanate T-1890 / 100: Isocyanurate of isophorone diisocyanate manufactured by EVONIK, 100% solids, 4.12 mmol / g. Duranate 24A-100: Hexamethylene diisocyanate burette manufactured by Asahi Kasei Corporation, solids content 100%, 5.60 mmol / g. Takenate D-131N: Polyisocyanurate of xylylene diisocyanate manufactured by Mitsui Chemicals, Inc., solids content 75.6%, 3.36 mmol / g. MEK-ST: MEK-dispersed silica sol manufactured by Nissan Chemical Industries (solid content 30%, average particle size of silica particles: 10 nm to 15 nm, non-reactive inorganic particles) · Tinuvin 405: 2-[4-(2-hydroxy-3-(2'-ethyl)hexyl)oxy-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 100% solids, manufactured by BASF. Tinuvin 152: 2,4-Bis[N-butyl-N-(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)amino]-6-(2-hydroxyethylamine)-1,3,5-triazine, 100% solids, from BASF BYK-370: A silicone-based surface conditioner manufactured by BYK Japan Co., Ltd.

[0094] As shown in Table 2, in Comparative Example 1, since the compound A having a branched structure with a terminal hydroxyl group was not contained, the chemical resistance, scratch resistance, and pencil hardness were insufficient. In Comparative Examples 2 to 5, since the polycarbonate polyol B was not contained, the adhesion was insufficient. Comparative Examples 6 to 8 used inorganic particles that did not have a functional group capable of reacting with a hydroxyl group or an isocyanate group on the surface, and therefore the scratch resistance was insufficient. [Industrial Applicability]

[0095] INDUSTRIAL APPLICABILITY The resin composition of the present invention is excellent in appearance, abrasion resistance, hardness, etc., and can therefore be suitably used for applications such as various lamp lenses for automobiles and hard coats for glazing.

Claims

1. A resin composition comprising compound A having a branched structure with hydroxyl groups at the terminals, polycarbonate polyol B, polyisocyanate C, and inorganic particles D, wherein compound A is a hyperbranched polymer having hydroxyl groups at the terminals, compound A has a hydroxyl value of 20 mg KOH / g or more and 1000 mg KOH / g or less, and inorganic particles D have functional groups on their surfaces that can react with hydroxyl groups or isocyanate groups of a resin component.

2. The resin composition according to claim 1 , wherein the compound A is a polymer having a dendritic branched structure.

3. The content of the compound A is 10 mass% or more and 50 mass% or less in the total mass (100 mass%) of the compound A, the polycarbonate polyol B, the polyisocyanate C, and the inorganic particles D. The resin composition according to claim 1 or 2.

4. The resin composition according to any one of claims 1 to 3, wherein the compound A has a weight average molecular weight of 550 or more and 30,000 or less.

5. The resin composition according to any one of claims 1 to 4, wherein the polycarbonate polyol B is a compound having a ring structure in the molecule.

6. The resin composition according to any one of claims 1 to 5, wherein the polyisocyanate C is a trifunctional or higher isocyanate.

7. The resin composition according to any one of claims 1 to 6, wherein the functional group capable of reacting with a hydroxyl group or an isocyanate group of the inorganic particles D is any one of a mercapto group, an isocyanate group, and an epoxy group.

8. The resin composition according to any one of claims 1 to 7, wherein the inorganic particles D are silica particles surface-treated with a silane coupling agent having a functional group capable of reacting with a hydroxyl group or an isocyanate group.

9. The content of the inorganic particles D in the total mass (100 mass%) of the compound A, the polycarbonate polyol B, the polyisocyanate C, and the inorganic particles D is 1 mass% or more and 40 mass% or less. The resin composition according to any one of claims 1 to 8.

10. The resin composition according to any one of claims 1 to 9, comprising an ultraviolet absorber E which is at least one of compounds derived from triazine-based, benzophenone-based, benzotriazole-based, phenyl salicylate-based, and phenyl benzoate-based compounds.

11. A coating composition comprising the resin composition according to any one of claims 1 to 10.

12. A coated article having a cured film of the coating composition according to claim 11.

Citation Information

Patent Citations

  • Thermosetting resin composition

    JP1998045867A

  • Thermosetting resin composition containing carboxy group-containing urethane resin and cured material thereof

    JP2008201847A

  • Coating material composition and method for forming coating film using the same

    JP2013001897A

  • Curable heat-dissipating composition

    WO2012157627A1