Thermally conductive sheet and its manufacturing method

By orienting thermally conductive filler in the thickness direction and using a controlled cutting process, the thermally conductive sheet achieves reduced thickness and thermal resistance, addressing the challenges of conventional methods and improving heat dissipation.

JP7582540B1Active Publication Date: 2024-11-13ZEON CORP
View PDF 8 Cites -1 Cited by

Patent Information

Application Number
JP2024053966
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2024-11-13
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

Conventional methods struggle to produce thermally conductive sheets with reduced thickness and thermal resistance while minimizing scratches, which are essential for effective heat dissipation in electronic components.

Method used

The thermally conductive sheet is manufactured by joining strips containing resin and thermally conductive filler in parallel, with the filler oriented in the thickness direction, and using a specific cutting blade with controlled rake and clearance angles to achieve a thickness of 15 μm to 90 μm and a low thermal resistance value.

Benefits of technology

This method results in a thermally conductive sheet with a small thickness, low thermal resistance, and improved handling properties, enhancing heat dissipation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582540000001_ABST
    Figure 0007582540000001_ABST
Patent Text Reader

Abstract

An object of the present invention is to provide a thermally conductive sheet that is thin and has a low thermal resistance value. The thermal conductive sheet is formed by joining strips containing a resin and a thermal conductive filler in parallel, the thermal conductive filler is oriented in the thickness direction of the thermal conductive sheet, the average thickness is 15 μm to 90 μm, and the density of scratches with a depth of 20% or more of the average thickness of the thermal conductive sheet, a width of 100 μm or more, and a length of 1000 μm or more is 5 scratches / 10000 mm 2 Below is a thermal conductive sheet.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermally conductive sheet and a method for producing the same. [Background technology]

[0002] In recent years, the amount of heat generated by electronic components such as plasma display panels (PDPs) and integrated circuit (IC) chips has increased as their performance has improved. As a result, it has become necessary to take measures to prevent malfunctions caused by temperature rises in electronic devices that use these components.

[0003] As a countermeasure against functional failures due to temperature rise of electronic components, a method is generally adopted in which a heat sink, a heat sink plate, a heat sink fin, or the like made of metal is attached to a heat generating body such as an electronic component to promote heat dissipation. When using a heat sink, a sheet-like member (thermal conductive sheet) having thermal conductivity is used to efficiently transfer heat from the heat generating body to the heat sink. For example, Patent Document 1 discloses a method for manufacturing a thermal conductive sheet, which includes a step of slicing the block body with the blade by sliding the block body while pressing it against the slide surface while supporting a blade whose tip portion protrudes from the slide surface, in which the blade contacts the block body with a first front surface having a length of a certain amount or more and a surface roughness of a certain amount or less. According to Patent Document 1, the thermal conductive sheet obtained by the above-mentioned method has both main surfaces that are smooth, has sufficient thickness accuracy, and is capable of transferring heat well in the thickness direction. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-140982 A Summary of the Invention [Problem to be solved by the invention]

[0005] Here, the thermal conductive sheet is required to exhibit superior thermal conductivity, and to achieve this, the thermal resistance value of the thermal conductive sheet itself can be reduced by making the thermal conductive sheet thinner. However, with the above-mentioned conventional methods, it is difficult to reduce the number of scratches on the manufactured thermally conductive sheet while also making the sheet thinner.

[0006] SUMMARY OF THE PRESENT EMBODIMENTS An object of the present invention is to provide a thermally conductive sheet that is thin and has a small thermal resistance value. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems, and have discovered that a thermally conductive sheet having a small thickness and a small thermal resistance can be obtained by controlling the average thickness within a predetermined range and the density of predetermined scratches to a certain value or less for a thermally conductive sheet formed by joining strips containing a resin and a thermally conductive filler in parallel, in which the thermally conductive filler is oriented in the thickness direction of the thermally conductive sheet, and have completed the present invention.

[0008] That is, the present invention has an object to advantageously solve the above-mentioned problems, and the present invention provides a thermally conductive sheet comprising: [1] strips containing a resin and a thermally conductive filler joined in parallel, the thermally conductive filler being oriented in the thickness direction of the thermally conductive sheet, the average thickness being 15 μm or more and 90 μm or less, the depth being 20% ​​or more of the average thickness of the thermally conductive sheet, the width being 100 μm or more, and the density of scratches being 1000 μm or more in length is 5 scratches / 10000 mm 2 The thermally conductive sheet is as follows: The thermally conductive sheet has a sufficiently small thickness and a sufficiently small thermal resistance value. The average thickness and density of scratches on the thermally conductive sheet can be measured according to the method described in the Examples of this specification.

[0009] [2] Here, the thermally conductive sheet of [1] above preferably has a tensile strength of 0.10 MPa or more. If the tensile strength is equal to or greater than the lower limit, the thermally conductive sheet is less likely to break and has excellent handleability. In this specification, the tensile strength of the thermal conductive sheet refers to the tensile strength when the thermal conductive sheet is assumed to have a thickness of 300 μm, and can be measured according to the method described in the Examples of this specification. By measuring the tensile strength of a thermal conductor sample that is thicker than the thermal conductive sheet of the present invention, it is possible to measure the strength derived from the composition of the thermal conductive sheet, regardless of the thickness of the thermal conductive sheet itself, and therefore the density and depth of scratches on the thermal conductive sheet.

[0010] [3] The present invention also provides a method for producing a thermally conductive sheet, comprising the steps of: supporting a block body containing a resin and a thermally conductive filler so that the block body is slidable on a sliding surface; supporting a cutting blade with a cutting edge protruding from the sliding surface; and sliding the block body on the sliding surface to slice the block body with the cutting blade to obtain a thermally conductive sheet, wherein the cutting blade has a flank, a first rake face that intersects with the flank and has a first rake angle, a second rake face that is adjacent to the first rake face and has a second rake angle, and a cutting edge formed by an intersection angle between the flank and the first rake angle, the second rake angle being greater than the first rake angle, and the clearance angle of the cutting blade being set to be 3° or more and 15° or less to slice the block body. According to the above-described manufacturing method, a thermally conductive sheet having a sufficiently small thickness and thermal resistance value can be obtained. In this specification, the block body refers to a laminate formed by laminating a plurality of primary sheets containing a resin and a thermally conductive filler in the thickness direction.

[0011] [4] In the method for manufacturing a thermally conductive sheet according to the above [3], it is preferable that the length of the first scooping face in the slicing direction is 0.1 mm or more. If the length of the first scooping face in the slicing direction is equal to or greater than the above lower limit, the occurrence of scratches caused by the thermally conductive sheet rubbing against the scooping face during slicing of the block body can be reduced.

[0012] [5] In the method for manufacturing a thermally conductive sheet according to the above [1] or [2], it is preferable that the flank of the cutting blade includes a first flank that intersects with the first rake face and has a first clearance angle, and a second flank that is adjacent to the first flank and has a second clearance angle, the second clearance angle being larger than the first clearance angle, and the first clearance angle corresponds to the clearance angle of the cutting blade. If the flank of the cutting blade satisfies the above, a thermally conductive sheet having a smaller thickness can be obtained. Effect of the Invention

[0013] According to the present invention, it is possible to provide a thermally conductive sheet that is thin and has a small thermal resistance value. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a diagram showing an example of a slicing device that can be used in the method for producing a thermally conductive sheet of the present invention. [Diagram 2] 5A to 5C are diagrams showing an example of a method for slicing a block body in the method for producing a thermally conductive sheet of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present invention will be described in detail. The thermally conductive sheet of the present invention can be used, for example, by being sandwiched between a heat generating body and a heat dissipating body when attaching the heat dissipating body to the heat generating body. That is, the thermally conductive sheet of the present invention can be used together with a heat dissipating body such as a heat sink, a heat dissipating plate, or a heat dissipating fin to form a heat dissipating device. The thermally conductive sheet of the present invention can be produced, for example, according to the method for producing a thermally conductive sheet of the present invention.

[0016] (Thermal Conduction Sheet) The thermally conductive sheet of the present invention is a thermally conductive sheet formed by joining strips containing a resin and a thermally conductive filler in parallel, and the thermally conductive filler is oriented in the thickness direction of the thermally conductive sheet. The thermally conductive sheet of the present invention has an average thickness of 15 μm to 90 μm, a depth of 20% or more of the average thickness of the thermally conductive sheet, a width of 100 μm or more, and a length of 1000 μm or more, and a density of scratches of 5 / 10000 mm 2 The above-mentioned thermally conductive sheet has a small thickness and a small thermal resistance value.

[0017] <Composition of the thermal conductive sheet> <<Resin>> The resin contained in the thermal conductive sheet is not particularly limited, and any resin can be used. For example, the resin can be either a liquid resin or a solid resin. The resin may be used alone or in combination of two or more types. For example, the thermal conductive sheet can contain at least one of a liquid resin and a solid resin, but from the viewpoint of further reducing the thickness and thermal resistance value of the thermal conductive sheet, it is preferable that the thermal conductive sheet contains both a liquid resin and a solid resin.

[0018] [Liquid resin] The liquid resin is not particularly limited as long as it is liquid at room temperature and normal pressure, and for example, a thermoplastic resin that is liquid at room temperature and normal pressure can be used. In the present invention, "normal temperature" refers to 23° C., and "normal pressure" refers to 1 atm (absolute pressure).

[0019] Examples of the liquid resin include fluororesin, silicone resin, acrylic resin, and epoxy resin. These may be used alone or in combination of two or more. Among them, silicone resin and fluororesin are preferred as the liquid resin, and fluororesin is more preferred. If at least one of silicone resin and fluororesin is used as the liquid resin, the flame retardancy of the thermal conductive sheet can be improved. If a fluororesin is used as the liquid resin, the heat resistance, oil resistance, and chemical resistance of the obtained thermal conductive sheet can be improved. Furthermore, if an acrylic resin is used as the liquid resin, the adhesion of the thermal conductive sheet to the metal is further increased, and the contact between the thermal conductive sheet and the metal member such as the heat sink can be sufficiently ensured even when the electronic component package or electronic device is deformed.

[0020] [Solid resin] The solid resin is not particularly limited as long as it is not liquid at room temperature and normal pressure. For example, a thermoplastic resin that is solid at room temperature and normal pressure, or a thermosetting resin that is solid at room temperature and normal pressure can be used.

[0021] {Thermoplastic resin that is solid at room temperature and pressure} Examples of thermoplastic resins that are solid at room temperature and pressure include acrylic resins such as poly(2-ethylhexyl acrylate), copolymers of acrylic acid and 2-ethylhexyl acrylate, polymethacrylic acid or its esters, and polyacrylic acid or its esters; silicone resins; fluororesins; polyethylene; polypropylene; ethylene-propylene copolymers; polymethylpentene; polyvinyl chloride; polyvinylidene chloride; polyvinyl acetate; ethylene-vinyl acetate copolymers; polyvinyl alcohol; polyacetal; polyethylene terephthalate; polybutylene terephthalate; polyethylene naphthalate; polystyrene; polyacrylonitrile. ; styrene-acrylonitrile copolymer; acrylonitrile-butadiene copolymer (nitrile rubber); acrylonitrile-butadiene-styrene copolymer (ABS resin); styrene-butadiene block copolymer or its hydrogenated product; styrene-isoprene block copolymer or its hydrogenated product; polyphenylene ether; modified polyphenylene ether; aliphatic polyamides; aromatic polyamides; polyamideimide; polycarbonate; polyphenylene sulfide; polysulfone; polyethersulfone; polyethernitrile; polyetherketone; polyketone; polyurethane; liquid crystal polymer; ionomer; etc. These may be used alone or in combination of two or more. In the present invention, rubber is included in the "resin".

[0022] {Thermosetting resin that is solid at room temperature and pressure} Examples of thermosetting resins that are solid at room temperature and normal pressure include natural rubber, butadiene rubber, isoprene rubber, nitrile rubber, hydrogenated nitrile rubber, chloroprene rubber, ethylene propylene rubber, chlorinated polyethylene, chlorosulfonated polyethylene, butyl rubber, halogenated butyl rubber, polyisobutylene rubber, epoxy resin, polyimide resin, bismaleimide resin, benzocyclobutene resin, phenolic resin, unsaturated polyester, diallyl phthalate resin, polyimide silicone resin, polyurethane, thermosetting polyphenylene ether, thermosetting modified polyphenylene ether, etc. These may be used alone or in combination of two or more.

[0023] [Resin content] The resin content in the thermal conductive sheet is not particularly limited, but is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and is preferably 95% by mass or less, more preferably 85% by mass or less, and even more preferably 75% by mass or less. If the resin content is equal to or greater than the lower limit, the thermal conductive sheet can be easily formed. On the other hand, if the resin content is equal to or less than the upper limit, the thermal resistance value of the thermal conductive sheet can be further reduced.

[0024] [Liquid resin content] The content of the liquid resin in the resin (in other words, the proportion of the liquid resin in the total of the solid resin and the liquid resin) is not particularly limited, but is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, particularly preferably 60% by mass or more, and preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. If the content of the liquid resin in the resin is equal to or greater than the lower limit, the thickness and thermal resistance of the thermal conductive sheet can be further reduced while ensuring the flexibility of the thermal conductive sheet, while if the content of the liquid resin in the resin is equal to or less than the upper limit, the strength suitable for the primary sheet is imparted, making it easier to slice the block body, and the uniformity of the thickness of the obtained thermal conductive sheet can be further improved. In addition, the tensile strength of the sheet can be increased.

[0025] <<Thermal conductive filler>> The thermally conductive filler imparts excellent thermal conductivity to the thermally conductive sheet of the present invention. The thermally conductive filler is not particularly limited, and known thermally conductive fillers such as metal fillers and carbon fillers can be used. Among them, it is preferable to use carbon materials such as particulate carbon materials and fibrous carbon materials as the thermally conductive filler, and it is more preferable to use particulate carbon materials.

[0026] [Particulate carbon materials] The particulate carbon material is not particularly limited, and examples thereof include graphite such as artificial graphite, scaly graphite, exfoliated graphite, natural graphite, acid-treated graphite, expandable graphite, and expanded graphite; carbon black; etc. These may be used alone or in combination of two or more kinds.

[0027] Among the above, it is preferable to use expanded graphite as the particulate carbon material. By using expanded graphite, the thermal resistance value of the thermal conductive sheet can be further reduced. Here, the expanded graphite can be obtained by, for example, chemically treating graphite such as flake graphite with sulfuric acid or the like to obtain expandable graphite, expanding the same by heat treatment, and then pulverizing the same. Examples of the expanded graphite include EC1500, EC1000, EC500, EC300, EC100, and EC50 (all trade names) manufactured by Ito Graphite Industries Co., Ltd.

[0028] The particulate carbon material preferably has a volume average particle diameter of 10 μm or more, more preferably 15 μm or more, preferably 150 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less, and particularly preferably 60 μm or less. If the volume average particle diameter of the particulate carbon material is equal to or greater than the above lower limit, it is presumed that the heat transfer path of the particulate carbon material in the heat conductive sheet can be well formed, and the thermal conductivity in the thickness direction of the heat conductive sheet is increased. As a result, the thermal resistance value of the heat conductive sheet can be further reduced. On the other hand, if the volume average particle diameter of the particulate carbon material is equal to or less than the above upper limit, the thickness of the heat conductive sheet can be further reduced. In the present invention, the "volume average particle size" can be determined as the particle size (D50) at which the cumulative volume calculated from the small diameter side is 50% in the particle size distribution measured by a laser diffraction method using a laser diffraction / scattering type particle size distribution measurement device.

[0029] The particulate carbon material preferably has an aspect ratio (major axis / minor axis) of more than 1 and not more than 10, more preferably more than 1 and not more than 5. If the aspect ratio of the particulate carbon material is within the above range, it is presumed that the particulate carbon material is easily oriented well in the thickness direction in the thermal conductive sheet, and the thermal conductivity of the thermal conductive sheet in the thickness direction is increased. As a result, the thermal resistance value of the thermal conductive sheet can be further reduced. In the present invention, the "aspect ratio" can be determined by observing a particulate carbon material with a SEM (scanning electron microscope), measuring the maximum diameter (long diameter) and the particle diameter (short diameter) in a direction perpendicular to the maximum diameter for any 50 parts of the particulate carbon material, and calculating the average value of the ratio of the long diameter to the short diameter (long diameter / short diameter).

[0030] [Thermal conductive filler content] The content of the thermally conductive filler in the thermally conductive sheet is not particularly limited, but is preferably 30% by volume or more, more preferably 35% by volume or more, and particularly preferably 38% by volume or more, and is preferably 55% by volume or less, more preferably 50% by volume or less, even more preferably 45% by volume or less, and particularly preferably 43% by volume or less, based on the entire thermally conductive sheet. If the content of the thermally conductive filler is equal to or more than the lower limit, the thermal conductivity of the thermally conductive filler in the thickness direction is increased, and the thermal resistance value of the thermally conductive sheet can be further reduced. On the other hand, when the content of the thermally conductive filler is equal to or less than the above upper limit, the flexibility of the thermally conductive sheet is ensured, and the uniformity of the thickness of the thermally conductive sheet can be further improved.

[0031] The content of the thermally conductive filler in the thermally conductive sheet is not particularly limited, but is preferably 35% by mass or more, more preferably 40% by mass or more, particularly preferably 45% by mass or more, and preferably 65% ​​by mass or less, more preferably 55% by mass or less, particularly preferably 50% by mass or less, based on the entire thermally conductive sheet. If the content of the thermally conductive filler is equal to or greater than the lower limit, the thermal conductivity of the thermally conductive filler in the thickness direction is increased, and the thermal resistance value of the thermally conductive sheet can be further reduced. On the other hand, if the content of the thermally conductive filler is equal to or less than the upper limit, the flexibility of the thermally conductive sheet can be ensured while the uniformity of the thickness of the thermally conductive sheet can be further improved.

[0032] In addition, the content of the thermally conductive filler in the thermally conductive sheet is not particularly limited, but is preferably 60 parts by mass or more, more preferably 70 parts by mass or more, particularly preferably 80 parts by mass or more, and preferably 220 parts by mass or less, more preferably 210 parts by mass or less, and particularly preferably 200 parts by mass or less per 100 parts by mass of resin. If the content of the thermally conductive filler per 100 parts by mass of resin is equal to or greater than the above lower limit, the thermal conductivity of the thermally conductive filler in the thickness direction is increased, and the thermal resistance value of the thermally conductive sheet can be further reduced. On the other hand, if the content of the thermally conductive filler per 100 parts by mass of resin is equal to or less than the above upper limit, the uniformity of the thickness of the thermally conductive sheet can be further improved while ensuring the flexibility of the thermally conductive sheet.

[0033] <Additives> The heat conductive sheet of the present invention may further contain known additives that can be used to form the heat conductive sheet, if necessary. The additives that can be contained in the heat conductive sheet are not particularly limited, and include, for example, plasticizers such as fatty acid esters such as sebacic acid esters; flame retardants such as red phosphorus flame retardants and phosphate ester flame retardants; toughness improvers such as urethane acrylates; moisture absorbents such as calcium oxide and magnesium oxide; adhesion improvers such as silane coupling agents, titanium coupling agents, and acid anhydrides; wettability improvers such as nonionic surfactants and fluorine surfactants; ion trapping agents such as inorganic ion exchangers, and antiaging agents such as phenolic antioxidants. The additives may be used alone or in combination of two or more.

[0034] If the thermal conductive sheet further contains an additive, the amount of the additive can be, for example, 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the above-mentioned resin, and it is preferable to set it to 10 parts by mass or less.

[0035] <Thermal Conduction Sheet Properties> The thermally conductive sheet of the present invention is formed by joining strips containing a resin and a thermally conductive filler in parallel. With such a thermally conductive sheet, it is easy to orient the thermally conductive filler in the thickness direction of the thermally conductive sheet, thereby improving the thermal conductivity of the thermally conductive sheet.

[0036] The thermally conductive sheet may have a structure in which strips containing a resin and a thermally conductive filler are connected in parallel in one direction approximately perpendicular to the thickness direction of the thermally conductive sheet (a direction at an angle of approximately 90° to the thickness direction). The width of the strip in this approximately perpendicular direction is not particularly limited, and can be, for example, 50 μm or more and 2000 μm or less. The width of the strip may depend on the thickness of the primary sheet in the manufacturing method described below. Therefore, a thermally conductive sheet having a strip width equal to or greater than the above lower limit has a reduced number of stacks, folds, or windings of the primary sheet. As a result, such a thermally conductive sheet has an improved block (laminate) formation speed described below, and improved productivity. On the other hand, a thermally conductive sheet having a strip width equal to or less than the above upper limit has improved thermal conductivity because the thermally conductive filler is well oriented in the thickness direction in the thermally conductive sheet, and the thermal resistance value of the thermally conductive sheet can be further reduced.

[0037] In the thermally conductive sheet, the thermally conductive filler is preferably oriented in the thickness direction of the thermally conductive sheet. Here, the orientation angle of the thermally conductive filler in the thermally conductive sheet is preferably 60° or more, and preferably 90° or less, with the direction parallel to the thickness direction of the thermally conductive sheet being 90°. If the orientation angle of the thermally conductive filler is within the above range, the thermally conductive filler is well oriented in the thickness direction in the thermally conductive sheet, so that the thermal conductivity is improved and the thermal resistance value of the thermally conductive sheet can be further reduced. In addition, when the thermally conductive filler has an aspect ratio (long axis / short axis) of more than 1, it is preferable that the long axis (major axis) of the thermally conductive filler is oriented in the thickness direction of the thermally conductive sheet at the above-mentioned orientation angle.

[0038] The thermal conductive sheet must have an average thickness of 15 μm or more, preferably 20 μm or more, more preferably 30 μm or more, and must have an average thickness of 90 μm or less, preferably 80 μm or less, and more preferably 70 μm or less. If the thickness of the thermal conductive sheet is equal to or greater than the lower limit, the strength of the thermal conductive sheet can be improved. On the other hand, if the thickness of the thermal conductive sheet is equal to or less than the upper limit, the thermal resistance of the thermal conductive sheet can be further reduced.

[0039] Moreover, the thermal conductive sheet preferably has a standard deviation of thickness of 3.5 μm or less, more preferably 3.0 μm or less, and even more preferably 2.7 μm or less. If the standard deviation of thickness is equal to or less than the above upper limit, a thermal conductive sheet with good thickness uniformity can be obtained. The lower limit of the standard deviation of thickness of the thermal conductive sheet is not particularly limited, but is, for example, 1 μm or more. The standard deviation of thickness refers to the standard deviation of the average thickness of multiple thermal conductive sheets manufactured by the same manufacturing method. The standard deviation of the thickness of the thermally conductive sheet can be adjusted by changing the type and content of materials (resin, thermally conductive filler, etc.) used in the production of the thermally conductive sheet, as well as the production conditions of the thermally conductive sheet. For example, the standard deviation of the thickness of the thermally conductive sheet can be reduced by producing the thermally conductive sheet using the thermally conductive sheet production method of the present invention described below. More specifically, in the thermally conductive sheet production method of the present invention, the standard deviation of the thickness of the thermally conductive sheet can be reduced by changing the content of the liquid resin, as well as the shape, clearance angle, and rake angle of the cutting blade.

[0040] The thermal conductive sheet has a density of 5 scratches per 10,000 mm with a depth of 20% or more of the average thickness of the thermal conductive sheet, a width of 100 μm or more, and a length of 1,000 μm or more. 2 Must be less than 4 pieces / mm 2 It is preferable that the number of particles is less than 3 / mm 2If the density of scratches is equal to or less than the upper limit, it is possible to obtain a thermally conductive sheet that is less likely to break and has excellent handleability. The density of scratches on the thermally conductive sheet is 0 scratches / mm 2 may be also possible. In addition, in the manufacturing method of the thermal conductive sheet of the present invention, the density of scratches in the thermal conductive sheet can be adjusted by changing the type and content ratio of materials (resin, thermal conductive filler, etc.) used in manufacturing the thermal conductive sheet, as well as the first and second rake angles of the cutting blade, the length along the slicing direction of the first rake face, etc.

[0041] The thermally conductive sheet preferably has a tensile strength of 0.10 MPa or more, more preferably 0.11 MPa or more, even more preferably 0.12 MPa or more, and preferably 0.50 MPa or less. If the tensile strength is equal to or greater than the lower limit, a thermally conductive sheet that is less likely to break and has excellent handleability can be obtained. If the tensile strength is equal to or less than the upper limit, the block body can be easily sliced, and the thickness of the thermally conductive sheet can be further reduced. The tensile strength of the thermally conductive sheet can be adjusted by changing the type and content of materials (resin, thermally conductive filler, etc.) used in producing the thermally conductive sheet, as well as the production conditions of the thermally conductive sheet.

[0042] In the present invention, the tensile strength of the thermal conductive sheet refers to the tensile strength in a direction perpendicular to the slicing direction of the block body containing the resin and the thermal conductive filler (the short direction of the strips joined in parallel in the thermal conductive sheet) in the manufacturing method of the thermal conductive sheet of the present application described later. Since the tensile strength is an attribute highly dependent on the sheet thickness, it cannot be simply compared between sheets of various thicknesses. Therefore, in the present invention, the tensile strength was measured by preparing a thermal conductor sample thicker than the thermal conductive sheet of the present invention (for example, 300 μm thick) from the composition that is the raw material of the thermal conductive sheet of the present invention, as described in the examples of this specification, using a general tensile tester or the like. By measuring the tensile strength of a thermal conductor sample that is thicker than the thermal conductive sheet of the present invention, it is possible to measure the strength derived from the composition of the thermal conductive sheet, independent of the thickness of the thermal conductive sheet itself, and thus the density and depth of scratches on the thermal conductive sheet. Specifically, the composition of the thermal conductive sheet refers to the content of the thermal conductive filler and the resin composition (the ratio of liquid resin to solid resin), etc., and by changing these, the strength derived from the composition of the thermal conductive sheet can be controlled.

[0043] (Method of manufacturing thermal conductive sheet) The thermally conductive sheet of the present invention described above can be manufactured, for example, by using the manufacturing method of the thermally conductive sheet of the present invention. Here, the manufacturing method of the thermally conductive sheet of the present invention includes at least a step of supporting a block body containing a resin and a thermally conductive filler slidably on a slide surface, and, in a state in which a cutting blade is supported with the cutting blade arranged so that the cutting edge protrudes from the slide surface, sliding the block body on the slide surface and slicing the block body with the cutting blade to obtain a thermally conductive sheet (hereinafter also referred to as a slicing step). Furthermore, according to the method for producing a thermally conductive sheet of the present invention, a thermally conductive sheet having a small thickness and a small thermal resistance value can be obtained.

[0044] 1 shows a slicing device for carrying out a manufacturing method according to one embodiment of the present invention. Note that the slicing device shown in the figure is just one example, and the slicing device used in the manufacturing method of the present invention is not limited to the embodiment shown in the figure, and the size and relative positions of each component are also just one example and are not limited to the embodiment shown in the figure. The slicing device has a cutting blade (30) attached to a slide table having a slide surface (20) that slidably supports a block body (10). In FIG. 1, the slicing device and the block body (10) are shown as a cross-sectional view cut along a plane parallel to the plane of the drawing. The cutting blade (30) has a clearance surface (31), a first rake surface (32a) that intersects with the clearance surface (31) and has a first rake angle (θa1), a second rake surface (32b) that is adjacent to the first rake surface (32a) and has a second rake angle (θa2), and a cutting edge (33) that is an intersection angle between the clearance surface (31) and the first rake surface (32a). Here, the second rake angle (θa2) is larger than the first rake angle (θa1). The clearance angle (θb) of the cutting blade is set to be 3° or more and 15° or less. The flank (31) of the cutting blade preferably includes a first flank (31a) intersecting the first rake face (32a) and having a first clearance angle (θb1), and a second flank (31b) adjacent to the first flank and having a second clearance angle (θb2). The second clearance angle (θb2) is preferably larger than the first clearance angle (θb1). In this case, the first clearance angle (θb1) corresponds to the clearance angle (θb) of the cutting blade.

[0045] <Slicing process> In the slicing process, as described above, the block body is slidably supported by the sliding surface while the cutting blade is supported with its tip protruding from the sliding surface. In this state, the block body is slid on the sliding surface and sliced ​​by the cutting blade to cut out the thermally conductive sheet from the block body.

[0046] <<Block letters>> The block body includes a resin and a thermally conductive filler, and may further include an optional additive. The block body is not particularly limited, but is preferably a laminate described below.

[0047] [Resin, thermally conductive filler, and additives] The suitable types, properties and content ratios of the resin and thermally conductive filler contained in the block body, as well as the optional additives contained therein, can be the same as the suitable types, properties and content ratios described above for the thermally conductive sheet of the present invention.

[0048] <<Cutting blade>> The cutting blade used to slice the block body described above has a cutting edge located at one end in the extension direction, and is usually used so that the extension direction of the cutting blade is the slicing direction. The cutting blade has a flank, a first rake face that intersects with the flank and has a first rake angle, a second rake face that is adjacent to the first rake face and has a second rake angle, and a cutting edge formed by the intersection angle between the flank and the first rake angle, the second rake angle being larger than the first rake angle. By having the first rake face and the second rake face that have the above-mentioned relationship, the occurrence of scratches caused by the sliced ​​heat conductive sheet rubbing against the rake face when slicing the block body can be reduced.

[0049] The first rake angle of the cutting blade is preferably 40° or more, more preferably 55° or more, and is preferably 75° or less, more preferably 65° or less. If the first rake angle is equal to or greater than the above lower limit, the occurrence of scratches caused by the sliced ​​thermally conductive sheet rubbing against the rake face when slicing the block body can be reduced. Also, if the first rake angle is equal to or less than the above upper limit, the clearance angle of the cutting blade can be prevented from becoming too small, and the block body can be prevented from riding up onto the cutting blade when slicing the block body, thereby making it possible to obtain a thermally conductive sheet with a small thickness by slicing.

[0050] The angle between the first and second rake faces is preferably 1° or more, more preferably 5° or more. There is no particular upper limit to the angle between the first and second rake faces, but it is generally preferably 20° or less.

[0051] The length of the cutting blade along the slicing direction of the first scooping face is preferably 0.1 mm or more, and is preferably 5.0 mm or less, more preferably 3.0 mm or less, even more preferably 1.5 mm or less, and particularly preferably 1.0 mm or less. If the length of the first scooping face along the slicing direction is within the above range, the occurrence of scratches caused by the thermally conductive sheet rubbing against the scooping face when slicing the block body can be reduced.

[0052] In addition, when performing the slicing step, the clearance angle of the cutting blade is set to 3° or more and 15° or less. The clearance angle is preferably 4° or more, more preferably 5° or more, and is preferably 13° or less, and more preferably 10° or less. If the clearance angle is equal to or greater than the lower limit, the block body can be prevented from riding on the cutting blade when slicing the block body, and a thin thermally conductive sheet can be obtained by slicing. If the clearance angle is equal to or less than the upper limit, the rake angle of the cutting blade can be prevented from becoming too small, and the occurrence of scratches on the sliced ​​thermally conductive sheet caused by rubbing against the rake face when slicing the block body can be reduced.

[0053] Furthermore, the flank of the cutting blade preferably includes a first flank that intersects with the first rake face and has a first clearance angle, and a second flank that is adjacent to the first flank and has a second clearance angle, and the second clearance angle is preferably larger than the first clearance angle. Here, the first clearance angle corresponds to the clearance angle of the cutting blade. By the cutting blade having the first and second clearance faces having the above relationship, a thermally conductive sheet having a smaller thickness can be obtained by slicing. In the present invention, a cutting blade having both a first scooping face and a second scooping face, and a first flank face and a second flank face may be referred to as a "double-edged" cutting blade, and a cutting blade having only either the first scooping face and the second scooping face, or the first flank face and the second flank face may be referred to as a "single-edged" cutting blade.

[0054] The angle between the first flank and the second flank is preferably 0.5° or more, and more preferably 1° or more. There is no particular upper limit to the angle between the first flank and the second flank, but it is generally preferably 10° or less.

[0055] Furthermore, the cutting edge angle (the angle between the first rake face and the flank face) of the cutting edge is not particularly limited, and can be, for example, 10° or more and 35° or less.

[0056] The material of the cutting blade is not particularly limited, but from the viewpoint of reducing the thickness of the thermally conductive sheet and improving the uniformity of the thickness, it is preferable that the cutting blade be made of a metal such as ceramic, cemented carbide, high-speed tool steel (high-speed steel), steel, etc., and cemented carbide is more preferable in terms of the balance of hardness of the blade itself and the ease of processing the blade.

[0057] <<Slice>> The slicing of the resin block using the above-mentioned cutting blade is not particularly limited, but is preferably performed while applying pressure to the resin block, and more preferably while applying a pressure of 0.1 MPa or more and 1.0 MPa or less.

[0058] In order to easily slice the resin block, the temperature of the resin block during slicing is preferably set to be in the range of -20°C to 40°C.

[0059] Furthermore, the slicing speed of the resin block is not particularly limited, but is preferably 50 mm / sec or more, more preferably 60 mm / sec or more, and even more preferably 70 mm / sec or more. If the slicing speed is set to be equal to or higher than the above lower limit, the productivity of the resin sheet can be increased and the uniformity of the thickness of the obtained resin sheet can be further improved. The slicing speed of the resin block is usually 600 mm / sec or less. If the slicing speed is set to be equal to or lower than the above upper limit, the block body can be prevented from riding on the cutting blade when slicing, thereby obtaining a thermally conductive sheet with an even smaller thickness by slicing.

[0060] <Other processes> Other steps that may be optionally included in the method for producing a thermally conductive sheet of the present invention are not particularly limited. For example, in the manufacturing method of the thermally conductive sheet of the present invention, before the above-mentioned slicing step, a step (stacking step) can be carried out in which multiple primary sheets containing resin and thermally conductive filler are stacked in the thickness direction, or the primary sheets are folded or rolled to obtain a block body. In the method for producing a thermally conductive sheet of the present invention, a step of heating the block body (heating step) can be carried out prior to the above-mentioned slicing step. The lamination step and the heating step as other steps will be described in detail below.

[0061] <<Lamination process>> As described above, in the lamination process, a plurality of primary sheets are laminated in the thickness direction, or the primary sheets are folded or rolled to obtain a block body that is a laminate. The thermally conductive sheet manufactured through the lamination process has a configuration in which slices of the primary sheets that constituted the laminate are joined in parallel, and the thermally conductive filler is oriented in the thickness direction, so that the thermal conductivity in the thickness direction is excellent.

[0062] [1st sheet] The primary sheet includes a resin and a thermally conductive filler, and may optionally further include additives.

[0063] The suitable types, properties and content ratios of the resin and thermally conductive filler contained in the primary sheet, as well as the optional additives contained therein, can be the same as the suitable types, properties and content ratios described above for the block body and the thermally conductive sheet of the present invention.

[0064] The thickness (average thickness) of the primary sheet is not particularly limited, and can be, for example, 50 μm or more and 2000 μm or less. The "thickness (average thickness)" of the primary sheet can be measured in the same manner as the "average thickness" of the thermally conductive sheet.

[0065] The method for preparing the primary sheet is not particularly limited. The primary sheet can be obtained, for example, by molding a composition containing a resin, a thermally conductive filler, and an optional additive by a known molding method such as press molding, rolling molding, or extrusion molding. In this way, when producing the primary sheet, by performing a pressing operation in the sheet surface direction, a structure can be formed in which the thermally conductive filler is oriented in a direction perpendicular to the sheet thickness direction (i.e., the sheet surface direction) in the primary sheet.

[0066] [Formation of blocks by lamination, etc.] The formation of a block body by stacking the primary sheets is not particularly limited, and may be performed using a stacking device or manually. The formation of a block body by folding a thermally conductive sheet is not particularly limited, and may be performed by folding the primary sheet at a fixed width using a folding machine. The formation of a block body by winding the primary sheet is not particularly limited, and may be performed by winding the primary sheet around an axis parallel to the short side or long side of the primary sheet.

[0067] <<Heating process>> Here, for example, the block body obtained through the lamination step described above may be subjected to the slicing step as it is, or may be subjected to the slicing step after being further heated. The heating temperature in the heating step may be, for example, 50° C. or higher and 170° C. or lower, and the heating time may be, for example, 1 minute or higher and 8 hours or lower. By passing through the heating step, it is possible to adjust the adhesion of the block body in the lamination direction. For example, when the block body contains a thermoplastic resin, it is possible to increase the adhesion of the block body in the lamination direction by carrying out the heating step. EXAMPLES

[0068] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, the units "%" and "parts" expressing amounts are by mass unless otherwise specified. In the examples and comparative examples, various measurements and evaluations were carried out by the following methods.

[0069] <Physical property measurement and evaluation> <<Average thickness and standard deviation of thickness of thermal conductive sheet>> Using a film thickness gauge (manufactured by Mitutoyo Corporation, product name "Digimatic Indicator"), the thickness was measured at five points, approximately the center and each of the four corners (squares), of the thermal conductive sheet, and the average value (μm) of the measured thicknesses was calculated. In addition, the average thickness of 100 slices of the thermally conductive sheet was measured as described above, and the standard deviation (μm) was calculated.

[0070] <<Density of scratches>> The obtained thermally conductive sheet (150mm x 150mm x 0.06mm) was placed on an inspection stage (transparent acrylic plate of 200mm x 200mm), and light was irradiated from an irradiation angle of 40° to the perpendicular line of the surface of the thermally conductive sheet (50° to the surface of the thermally conductive sheet) using a white LED bar light (model number "LDL2-275X" manufactured by CCS; color temperature 7,800K; power consumption 27W). Then, while irradiating light, an 8K monochrome CMOS line camera (manufactured by Basler; model number "raL8192-12gm"; 8192pix x 1pix) installed directly above the thermally conductive sheet (i.e., an imaging angle of 90° to the surface of the thermally conductive sheet) and the white LED bar light were scanned parallel to the surface of the thermally conductive sheet, and the surface of the thermally conductive sheet was photographed with the camera to obtain a digital image of the surface of the thermally conductive sheet. After that, the digital image was subjected to image processing such as smoothing and edge detection in an image processing unit (original software) to detect scratches, and the number of scratches, their width, length, and scratch position coordinates were obtained. Next, the inspected thermal conductive sheet was removed from the inspection stage and placed on the stage of a laser microscope (Keyence Corporation, product name "VK-X2000"). The location corresponding to the coordinates of the scratch obtained in the above inspection was measured at 10x magnification over a height range of 200μm to obtain a profile of the scratch in the depth direction. The scratch depth was measured from the obtained profile. From the width, length, and depth of the scratches obtained, the number of scratches whose depth is 20% or more of the average thickness of the thermal conductive sheet measured, whose width is 100 μm or more, and whose length is 1000 μm or more was calculated, and the number of scratches was calculated by dividing the size of the thermal conductive sheet by 10,000 mm. 2 The number of scratches per unit area was calculated and defined as the scratch density.

[0071] <<Tensile strength>> A thermally conductive sheet sliced ​​to a thickness of 300 μm was punched out using a dumbbell No. 2 (dumbbell-shaped, width 3 mm, length 70 mm) conforming to JIS K7113 to prepare a sample. Using a tensile tester (manufactured by Shimadzu Corporation, product name "AG-IS20kN"), the sample was pulled in the direction perpendicular to the slicing direction (the short direction of the strips joined in parallel within the thermally conductive sheet) under the following conditions: load cell: 50 N, chuck distance: 35 mm, speed: 50 mm / min, temperature: 23°C, and the breaking strength (tensile strength) was measured. The average value of the measured values ​​of the three sample pieces was regarded as the tensile strength of the thermally conductive sheet.

[0072] <<Bulk thermal resistance value>> The thermal resistance value of the thermal conductive sheet was measured using a thermal resistance tester (manufactured by Hitachi Technology & Services Co., Ltd., product name "Resin Material Thermal Resistance Measuring Device"). Here, apart from the thermal conductive sheets of the examples and comparative examples, thermal conductive sheets of 50 μm, 100 μm, and 200 μm cut into approximately 1 cm squares were prepared as samples, and the thermal resistance value (°C / W) of these samples was measured when a pressure of 0.3 MPa was applied at a sample temperature of 50°C. From the obtained thermal resistance value, an approximation of y=ax+b was calculated, where y is the thermal resistance value and x is the thickness of the thermal conductive sheet, and b was taken as the interface thermal resistance value of the thermal conductive sheet. Then, the value of b was subtracted from the thermal resistance value measured in the same manner for the thermal conductive sheets of the examples and comparative examples to take the bulk thermal resistance value.

[0073] <<Handling>> The handleability was evaluated based on the measurement results of the density of scratches and the tensile strength of the thermal conductive sheet as follows: The lower the density of scratches, the better the handleability, and the higher the tensile strength, the better the handleability. [Table 1]

[0074] Example 1 <Preparation of Composition> 40 parts of a thermoplastic fluororesin (manufactured by Daikin Industries, Ltd., trade name "Daiel G-101") that is liquid at room temperature and normal pressure as a fluororesin, 20 parts of a thermoplastic fluororesin (manufactured by 3M Japan Ltd., trade name "Dyneon FC2211") that is solid at room temperature and normal pressure, 40 parts of a hydroxyl group-containing liquid acrylic polymer (manufactured by Toagosei Co., Ltd., trade name "ARUFON (registered trademark) UH-2190") that is liquid at room temperature and normal pressure as an acrylic resin, and 90 parts of expanded graphite (manufactured by Ito Graphite Industries Co., Ltd., trade name "EC-300", volume average particle size: 50 μm) as a thermally conductive filler were stirred and mixed for 5 minutes using a Hobart mixer (manufactured by Kodaira Manufacturing Co., Ltd., trade name "ACM-5LVT type"). The mixture obtained was vacuum degassed for 30 minutes and put into a crusher and crushed for 10 seconds to obtain a composition.

[0075] <Formation of the primary sheet> Next, 1 kg of the obtained composition was sandwiched between sandblasted PET films (protective films) having a thickness of 50 μm, and roll-molded (primary pressing) under conditions of a roll gap of 600 μm, a roll temperature of 50° C., a roll linear pressure of 50 kg / cm, and a roll speed of 1 m / min to obtain a primary sheet having a thickness of 800 μm.

[0076] <Lamination process> The obtained primary sheet was cut to a size of 150 mm length x 150 mm width x 800 μm thickness, and 200 sheets were stacked in the thickness direction of the primary sheet. Further, the sheet was pressed in the stacking direction at a temperature of 120°C and a pressure of 0.1 MPa for 3 minutes to obtain a block body (laminate) with a height of approximately 160 mm.

[0077] <Formation of heat conductive sheet> Thereafter, the side (surface along the lamination direction) of the secondary pressurized block body (laminate) was pressed with a pressure of 0.3 MPa, and the block body was sliced ​​at an angle of 90° to the lamination direction (in other words, in a direction perpendicular to the normal line of the main surface of the laminated primary sheets) at a speed of 80 mm / sec using a wood slicer (manufactured by Marunaka Iron Works Co., Ltd., product name "Super Finish Planer Super Mecha S") with the temperature in the processing space of the slicer at 15°C, to obtain a thermally conductive sheet of length 150 mm x width 150 mm x thickness 45 μm. As shown in FIG. 2, the slicing direction (A) of the block body (10) is perpendicular to the lamination direction (B) of the primary sheet (11). The first and second clearance angles, first and second rake angles, shape, and length of the first rake face of the cutting blade used for slicing are as shown in Table 2. The thermally conductive sheet thus obtained was subjected to various measurements and evaluations according to the methods described above. The results are shown in Table 2.

[0078] (Examples 2-4 and Comparative Examples 1-5) Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that the types and amounts of materials mixed when preparing the composition, as well as the shape, clearance angle, and rake angle of the cutting blade were changed as shown in Table 2. However, for Comparative Examples 2 and 4, the slicing process was carried out with the intention of producing a thermally conductive sheet as a thin film (thickness 90 μm or less), but the block body got on the cutting blade and could not be sliced ​​at the above thickness, so that the thermally conductive sheet could not be measured or evaluated. The results are shown in Table 2.

[0079] The modified nitrile rubber used was acrylonitrile-butadiene rubber (manufactured by Nippon Zeon Co., Ltd., product name "Nipol 1072J") which is solid at room temperature and normal pressure. The liquid nitrile rubber used was acrylonitrile-butadiene rubber (manufactured by Nippon Zeon Co., Ltd., product name "Nipol 1312") which is liquid at room temperature and normal pressure. The epoxy resin used was bisphenol A diglycidyl ether (manufactured by Mitsubishi Chemical Corporation, product name "jER") which is liquid at room temperature and normal pressure. The antioxidant used was a combination of an aromatic secondary amine antioxidant (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Nocrac CD") and a benzimidazole antioxidant (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Nocrac MBZ") Moreover, in cases where the cutting blade did not have a second rake face, the angle between the first rake face and the second rake face was recorded as 0°.

[0080] [Table 2]

[0081] From Table 2, the average thickness is 15 μm or more and 90 μm or less, and the density of the specified scratches is 5 pieces / 10,000 mm 2 It can be seen that the thermally conductive sheet of Example 1-4 below has a smaller thickness and thermal resistance value than the thermally conductive sheet of Comparative Example 1-5. Also, the thermally conductive sheet of Example 1-4 has fewer scratches and a larger tensile strength than the thermally conductive sheet of Comparative Example 1-5, and is therefore easier to handle. [Industrial Applicability]

[0082] According to the present invention, it is possible to provide a thermally conductive sheet that is thin and has a small thermal resistance value. [Explanation of symbols]

[0083] 10 Block Letters 11 First sheet 20 Slide surface 30 cutting blade 31 Flank 31a First relief face 31b Second relief face 32a First scooping face 32b Second scooping face 33 Cutting Edge θa1 First rake angle θa2 Second rake angle θb1 First clearance angle θb2 Second clearance angle A Block slice direction B Stacking direction of the primary sheet C Orientation direction of thermally conductive filler

Claims

1. A thermally conductive sheet comprising strips each containing a resin and a thermally conductive filler joined in parallel, the thermally conductive filler is oriented in the thickness direction of the thermally conductive sheet, The average thickness is 15 μm or more and 90 μm or less, The density of scratches having a depth of 20% or more of the average thickness of the thermal conductive sheet, a width of 100 μm or more, and a length of 1000 μm or more is 5 / 10000 mm 2 Below is the A thermally conductive sheet (excluding a thermally conductive sheet having a surface roughness Sz of 3.5 μm or less).

2. The thermal conductive sheet according to claim 1 , wherein the thermal conductive sheet has a tensile strength of 0.10 MPa or more.

3. A method for producing a thermally conductive sheet, comprising: supporting a block body containing a resin and a thermally conductive filler slidably on a slide surface; supporting a cutting blade disposed so that a cutting edge protrudes from the slide surface; and sliding the block body on the slide surface while supporting the block body, and slicing the block body with the cutting blade to obtain a thermally conductive sheet, The cutting blade is The relief surface and a first rake face intersecting the flank face and having a first rake angle; a second rake face adjacent to the first rake face and having a second rake angle; a cutting edge formed by an intersection angle between the flank and the first rake face; Equipped with the second rake angle is greater than the first rake angle; The clearance angle of the cutting blade is set to 3° or more and 15° or less to slice the block body. A method for manufacturing a thermal conductive sheet.

4. The method for producing a thermal conductive sheet according to claim 3 , wherein the length of the first cutting face in the slicing direction is 0.1 mm or more.

5. The flank surface of the cutting blade is a first flank surface intersecting the first rake face and having a first clearance angle; a second flank adjacent the first flank and having a second clearance angle; Equipped with the second clearance angle is greater than the first clearance angle; the first clearance angle corresponds to the clearance angle of the cutting blade; A method for producing the thermal conductive sheet according to claim 3 or 4.

Citation Information

Patent Citations

  • Thermoconductive sheet, method for producing the same, and heat-releasing device using the same

    JP2010132856A

  • Heat conductive sheet and production process therefor

    JP2017043655A

  • Thermally conductive sheet and method for producing the same

    JP2018067695A

  • Heat conductive sheet and method of manufacturing the same

    JP2020140982A

  • Heat conductive sheet and manufacturing method thereof

    JP2021005595A