Spunbond nonwoven fabric, tape, and method for producing spunbond nonwoven fabric

The spunbond nonwoven fabric with controlled crystallization and melting peaks, core-sheath composite structure, and embossing ratio addresses the issue of high tear strength and poor hand tearability, providing a strong and easily tearable tape base material.

JP7582557B1Active Publication Date: 2024-11-13TORAY INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024520907
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-27
Publication Date
2024-11-13
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

Nonwoven fabrics with high tear strength lack hand tearability, and increasing crimped parts to improve hand tearability reduces mechanical strength, leading to inadequate performance as tape base materials.

Method used

A spunbond nonwoven fabric composed of polyethylene terephthalate resin fibers with specific crystallization and melting peaks, core-sheath composite structure, and controlled embossing compression ratio, enhancing mechanical strength while maintaining hand tearability.

Benefits of technology

The fabric achieves excellent mechanical strength and hand tearability, suitable for use as a tape base material with improved adhesion and reduced surface irregularities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582557000002
    Figure 0007582557000002
  • Figure 0007582557000001
    Figure 0007582557000001
Patent Text Reader

Abstract

An object of the present invention is to provide a nonwoven fabric that is excellent in mechanical strength and ease of being torn by hand. The present invention relates to a spunbond nonwoven fabric composed of fibers containing a polyethylene terephthalate resin as a main component, which has a crystallization peak in the range of 100°C or more and 150°C or less and a single melting peak in the range of 250°C or more and 270°C or less, as measured by differential scanning calorimetry, and has an embossed compression ratio of 5 area % or more and 30 area % or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to spunbond nonwoven fabrics and tapes. [Background technology]

[0002] Adhesive tapes are used in various fields such as building materials, vehicles, and medical applications, and paper, cloth, nonwoven fabric, film, etc. are used as tape substrates. Among them, paper is often used as tape substrates in fields that require so-called hand tearability, that is, the tape can be easily cut by hand when used by a worker. On the other hand, this paper-based tape may not have sufficient strength, so nonwoven fabric may be used instead. However, when nonwoven fabric is used, the tear strength is high and the hand tearability is poor, which is an issue.

[0003] Patent Document 1 proposes a nonwoven fabric tape substrate characterized by being made of a synthetic long fiber nonwoven fabric having fiber diameter, apparent density, basis weight, and partial heat-pressing rate within specific ranges, longitudinal tensile strength and breaking elongation above a certain level, and having linear or dashed line-shaped heat-pressing bonded parts that are perpendicular to the longitudinal direction and different from the heat-pressing bonded parts. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-180615 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the nonwoven fabric disclosed in Patent Document 1, the linear or broken line-shaped compression parts added after thermocompression can reduce the tear strength and improve the hand-tearability. However, in the nonwoven fabric subjected to the above-mentioned compression processing, the surface irregularities increase as the compression parts increase, so that when used as a tape substrate, the adhesion to the installation surface deteriorates. In addition, in order to improve the hand-tearability by increasing the compression parts, it is necessary to compress the nonwoven fabric until it becomes a film. As the film parts increase, the mechanical strength (tensile strength) of the nonwoven fabric decreases, so it cannot be said that it is sufficient in terms of achieving both mechanical strength and hand-tearability.

[0006] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a nonwoven fabric, and in turn a tape, which has excellent mechanical strength and excellent hand-tearability. [Means for solving the problem]

[0007] As a result of intensive research conducted by the present inventors to achieve the above object, it was discovered that by controlling the crystallization peak and melting peak of a spunbonded nonwoven fabric in a specific temperature range in differential scanning calorimetry, it is possible to obtain a spunbonded nonwoven fabric that is excellent in mechanical strength and hand-tearability. The present invention was completed based on these findings.

[0008] The present invention and its preferred embodiments include the following configurations.

[0009] [1] A spunbond nonwoven fabric composed of fibers whose main component is polyethylene terephthalate resin, which has a crystallization peak in the range of 100°C to 150°C and a single melting peak in the range of 250°C to 270°C when measured by differential scanning calorimetry, and has an embossed compression ratio of 5% to 30% by area.

[0010] [2] The nonwoven fabric described in [1] above, in which the fiber breakage rate per unit area in the non-bonded parts is 5.0% or more and 50.0% or less.

[0011] [3] A tape comprising the spunbond nonwoven fabric according to [1] or [2] above. [4] A method for producing the spunbonded nonwoven fabric according to the above item [1] or [2], comprising the following steps (a) to (c) in this order: Step (a): A step of spinning a core-sheath type composite fiber in which a low-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less and having an intrinsic viscosity (IV) that is 0.05 or more and 0.25 or less lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin is disposed around the high-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less. Step (b): A step of drawing and stretching the spun core-sheath type composite fiber by an ejector and depositing it on a moving net conveyor to form a fiber web. Step (c): A step of thermally compressing the fiber web to an embossing rate in the range of 5 area % or more and 30 area % or less. Effect of the Invention

[0012] According to the present invention, there is provided a nonwoven fabric which has excellent mechanical strength and hand-tearability. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a scanning electron micrograph of a non-bonded portion containing torn fibers in a spunbonded nonwoven fabric of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The spunbond nonwoven fabric of the present invention is a spunbond nonwoven fabric composed of fibers mainly composed of polyethylene terephthalate resin, and has a crystallization peak in the range of 100° C. to 150° C. and a single melting peak in the range of 250° C. to 270° C. as measured by differential scanning calorimetry, and an embossing compression rate of 5 area % to 30 area %. The components are described in detail below, but the present invention is not limited to the scope described below as long as it does not deviate from the gist of the invention, and various modifications are possible without departing from the gist of the invention.

[0015] [Polyethylene terephthalate resin] First, the spunbond nonwoven fabric of the present invention is composed of fibers containing polyethylene terephthalate resin as a main component.

[0016] The melting point of the polyethylene terephthalate resin is preferably 250°C or higher and 270°C or lower. By setting the melting point of the polyethylene terephthalate resin to 250°C or higher, it becomes easier to obtain heat resistance that can withstand practical use. Furthermore, by setting the melting point of the polyethylene terephthalate resin to 270°C or lower, it becomes easier to cool the yarn discharged from the spinneret, and it becomes easier to suppress fusion between fibers and perform stable spinning even with a thin fiber diameter. Here, the melting point of the polyethylene terephthalate resin refers to the maximum melting peak temperature obtained by measuring the polyethylene terephthalate resin by differential scanning calorimetry (DSC).

[0017] The intrinsic viscosity (IV) of the polyethylene terephthalate resin is preferably 0.40 or more and 0.70 or less. By making the intrinsic viscosity of the polyethylene terephthalate resin 0.40 or more, more preferably 0.45 or more, and even more preferably 0.50 or more, it is possible to suppress a decrease in the strength of the fibers constituting the nonwoven fabric. On the other hand, by making the intrinsic viscosity of the polyethylene terephthalate resin 0.70 or less, it is possible to stably spin even fine fibers, and to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.

[0018] Additives such as crystal nucleating agents, matting agents, lubricants, pigments, mildewproofing agents, antibacterial agents, flame retardants, metal oxides, aliphatic bisamides and / or alkyl-substituted aliphatic monoamides, and hydrophilic agents can be added to the polyethylene terephthalate resin as long as they do not impair the effects of the present invention. Among them, metal oxides such as titanium oxide have the effect of improving spinnability by reducing surface friction of fibers and preventing fusion between fibers, and also improving the fusion properties of the nonwoven fabric by increasing thermal conductivity during fusion molding of the nonwoven fabric with a heated roll, thereby making it possible to obtain a spunbond nonwoven fabric with superior mechanical strength.

[0019] [fiber] The fibers constituting the nonwoven fabric are preferably core-sheath type composite fibers.

[0020] Furthermore, the intrinsic viscosity (IV) of the polyethylene terephthalate resin of the sheath component is preferably lower than the intrinsic viscosity (IV) of the polyethylene terephthalate resin of the core component by 0.05 or more and 0.25 or less. Hereinafter, the polyethylene terephthalate resin of the sheath component in this embodiment is also called "low-viscosity polyethylene terephthalate resin", and the polyethylene terephthalate resin of the core component is also called "high-viscosity polyethylene terephthalate resin". The intrinsic viscosity of the low-viscosity polyethylene terephthalate resin is lower than the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin by 0.05 or more, more preferably 0.08 or more, and even more preferably 0.10 or more, so that spinning stress is concentrated on the core component during spinning, promoting the orientation of the core component and suppressing the orientation of the sheath component. As a result, a fiber having high single fiber strength and excellent thermal adhesion can be obtained, making it easier to obtain a nonwoven fabric having excellent mechanical strength. On the other hand, when the intrinsic viscosity of the low-viscosity polyethylene terephthalate resin is lower than the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin by 0.25 or less, preferably 0.20 or less, the single fiber strength of the core-sheath type composite fiber can be improved.

[0021] The intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin is preferably 0.55 or more and 0.70 or less. By making the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin 0.55 or more, it is possible to prevent a decrease in single fiber strength. Furthermore, by making the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin 0.70 or less, it is possible to stably spin even fine fibers, and to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.

[0022] The mass ratio of the sheath component in the core-sheath type composite fiber is preferably 10% by mass or more and 80% by mass or less. By making the mass ratio of the sheath component 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, the sheath components are firmly fused together during thermal bonding, and a spunbonded nonwoven fabric having sufficient strength for practical use can be obtained. On the other hand, by making the ratio of the sheath component 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, the proportion of the highly oriented core component is increased, the single fiber strength of the core-sheath type composite fiber is improved, and a spunbonded nonwoven fabric having sufficient strength for practical use can be obtained.

[0023] The composite form of the sheath-core composite fiber may be, for example, a concentric sheath-core type, an eccentric sheath-core type, an islands-in-the-sea type, etc. Among these, the sheath-core type composite form is preferred, and the concentric sheath-core type composite form is more preferred, since it has excellent spinnability and can be used to produce a spunbonded nonwoven fabric having excellent mechanical strength by uniformly bonding the fibers together by thermal bonding.

[0024] The fibers preferably have an average single fiber diameter of 6.0 μm or more and 20.0 μm or less. By making the average single fiber diameter 6.0 μm or more, more preferably 7.0 μm or more, and even more preferably 8.0 μm or more, it is possible to prevent a decrease in spinnability, improve production stability, and obtain a spunbond nonwoven fabric having excellent mechanical strength. On the other hand, by making the average single fiber diameter 20.0 μm or less, more preferably 18.0 μm or less, and even more preferably 16.0 μm or less, it is possible to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.

[0025] In the present invention, the average single fiber diameter (μm) is determined by the following method. (i) Ten small sample pieces of 10 mm x 10 mm are randomly taken from the spunbond nonwoven fabric. (ii) The surface of the collected small sample is photographed using a scanning electron microscope or the like at a magnification range of 500 to 2000 times so that the fiber thickness can be measured. (iii) From the photographs of each small sample, 10 fibers are randomly selected (100 fibers in total) and their thickness is measured. Assuming that the cross section of the fiber is circular, the thickness is taken as the fiber diameter. (iv) The average single fiber diameter is calculated by rounding off the arithmetic average value to one decimal place.

[0026] [Spunbond nonwoven fabric] The spunbonded nonwoven fabric of the present invention has a crystallization peak in the range of 100°C to 150°C by differential scanning calorimetry. When the spunbonded nonwoven fabric has a crystallization peak temperature in the above range, the fusion of fibers during embossing and compression is promoted, resulting in a spunbonded nonwoven fabric with excellent tensile strength, and furthermore, the fibers in the non-compressed parts are torn by heat, resulting in a spunbonded nonwoven fabric with low tear strength and excellent hand-cuttability. On the other hand, in the case of a spunbonded nonwoven fabric that does not have a crystallization peak, not only is fusion of fibers unlikely to occur, resulting in a nonwoven fabric with low tensile strength, but also, since the fibers in the non-compressed parts are not torn, the fibers are difficult to tear, resulting in a spunbonded nonwoven fabric with poor hand-cuttability.

[0027] Furthermore, the spunbond nonwoven fabric has a single melting peak in the range of 250° C. to 270° C. as measured by differential scanning calorimetry. By having a single melting peak in the above range, the fibers can be firmly thermally bonded together at a sufficient temperature without causing operational problems such as low-melting point components melting and sticking to a heated roll during thermal bonding, and a spunbond nonwoven fabric having sufficient strength for practical use can be obtained.

[0028] Here, the crystallization peak temperature Tc (°C) and melting peak temperature Tm (°C) of the spunbond nonwoven fabric are obtained by differential scanning calorimetry (DSC), and the values ​​calculated according to the following procedure are adopted. (1) Take a small piece of spunbond nonwoven fabric, measuring 0.5 to 5 mg. (2) Using differential scanning calorimetry (DSC), the temperature is raised from room temperature to 280°C at a rate of 16°C / min to obtain a DSC curve. (3) The peak top temperature of the crystallization exothermic peak is read from the DSC curve and regarded as the crystallization peak temperature Tc (°C) of the spunbond nonwoven fabric, and the peak top temperature of the melting endothermic peak is read and regarded as the melting peak temperature Tm (°C) of the spunbond nonwoven fabric.

[0029] The spunbonded nonwoven fabric has an embossing rate of 5% by area or more and 30% by area or less. By making the embossing rate 5% by area or more, more preferably 8% by area or more, and even more preferably 10% by area or more, it is possible to obtain a strength sufficient for practical use as a spunbonded nonwoven fabric. On the other hand, by making the embossing rate 30% by area or less, more preferably 25% by area or less, and even more preferably 20% by area or less, it is possible to reduce the unevenness of the nonwoven fabric surface and obtain sufficient adhesion when used as a tape.

[0030] The embossing rate here refers to the ratio of the area of ​​the bonded portion to the entire area of ​​the spunbonded nonwoven fabric. Specifically, when heat-bonding is performed using a pair of rolls with projections and recesses, it refers to the ratio of the area of ​​the entire spunbonded nonwoven fabric where the projections of the upper roll and the projections of the lower roll overlap and contact the fiber web (bonded portion). When heat-bonding is performed using a roll with projections and a flat roll, it refers to the ratio of the area of ​​the entire spunbonded nonwoven fabric where the projections of the roll with projections and recesses contact the fiber web (bonded portion).

[0031] The spunbonded nonwoven fabric preferably has a fiber fraying rate per unit area in the non-bonded portion of 5.0% or more and 50.0% or less. By having a fiber fraying rate of 5.0% or more, more preferably 7.0% or more, and even more preferably 10.0% or more, the tear strength is reduced, and the fabric can be sufficiently hand-cuttable for practical use as a tape substrate. On the other hand, by having a fiber fraying rate of 50.0% or less, more preferably 40.0% or less, and even more preferably 30.0% or less, excessive fiber fraying can be suppressed, and a decrease in tensile strength can be suppressed. In the present invention, the fiber fraying rate refers to a value measured and calculated by the following method. (i) Take small samples from the nonwoven fabric, 10 for observation of the front surface and 10 for observation of the back surface (20 samples in total). (ii) The collected small sample is subjected to a scanning electron microscope (SEM, for example, Keyence Corporation's "VHX-D500") at a magnification of 2000 times and an area of ​​22000 μm. 2 Take a photo of. (iii) In the photographs of each small sample, the total number of fibers (N) and the number of fibers (n) having frayed areas (3) of 10 μm or more in the longitudinal direction of the fibers as shown in FIG. 1 are counted, and the fiber fraying rate is calculated using the following formula. Fiber fraying rate (%) = (n / N) x 100 (iv) Calculate the arithmetic average of 10 small samples on each of the front and back surfaces, round off to one decimal place, compare the fraying rates of the front and back surfaces, and take the larger value as the fiber fraying rate of the spunbond nonwoven fabric.

[0032] The spunbond nonwoven fabric of the present invention has a tensile strength per unit area of ​​5.00 (N / 5cm) / (g / m 2 It is preferable that the tensile strength is 5.00 (N / 5cm) / (g / m 2 ) or more, more preferably 5.50 (N / 5cm) / (g / m 2 ) or more, more preferably 5.80 (N / 5cm) / (g / m 2 ) or more, a minimum tensile strength required for a tape substrate can be obtained, which is preferable from the standpoint of tape processability.

[0033] In the present invention, the tensile strength per unit area of ​​the spunbond nonwoven fabric ((N / 5cm) / (g / m 2 )) shall be the value determined by the following method in accordance with JIS L1913:2010 "Testing methods for general long-fiber nonwoven fabrics", 6.3 "Tensile strength and elongation". (i) Three samples measuring 30 cm x 5.0 cm are taken from the nonwoven fabric at equal intervals in both the MD and CD directions. (ii) A load is applied until the sample breaks, with a grip distance of 20 cm and a tensile speed of 100±10 mm / min. (iii) The strength of the sample at maximum load is taken as the tensile strength (N / 5 cm), and the average of three points in each of the MD and CD directions is calculated. The sum of these average values ​​is the tensile strength of the spunbond nonwoven fabric. (iv) The tensile strength per unit area of ​​the spunbond nonwoven fabric ((N / 5cm) / (g / m 2 )) and round off to the third decimal place. Tensile strength per unit area of ​​spunbond nonwoven fabric ((N / 5cm) / (g / m 2 )) = [tensile strength of spunbond nonwoven fabric (N / 5cm)] / weight (g / m 2 ).

[0034] The spunbond nonwoven fabric of the present invention has a tear strength per unit area of ​​0.10 N / (g / m 2 ) or more 1.00N / (g / m 2 It is preferable that the tear strength is 0.10 N / (g / m) or less.2 ) or more, more preferably 0.15N / (g / m 2 ) or more, the tape substrate can have a minimum tear strength, which is preferable from the viewpoint of tape processability. 2 ) or less, more preferably 0.90N / (g / m 2 ) or less, more preferably 0.80 N / (g / m 2 ) or less, the hand tearability after tape processing can be more effectively improved.

[0035] In the present invention, the tear strength per unit area of ​​the spunbond nonwoven fabric is determined by measuring the tear strength per unit area using a constant-speed extension tensile tester (e.g., Baldwin's RTG-1250) in accordance with JIS L1913:2010 "Testing methods for general nonwoven fabrics", section 6.4 "Tear strength", a) trapezoid method, as follows: (i) Three samples measuring 25 cm x 5.0 cm are taken from the nonwoven fabric at equal intervals in the MD direction. (ii) Make an isosceles trapezoid mark on the test piece and make a 1.0 cm cut at right angles to the short side at the centre of the short side of this mark. (iii) The test piece is attached to the grips of a constant-rate extension tensile testing machine with a gripping distance of 10 cm, with the short sides of the trapezoid taut and the long sides loose, along the marks. (iv) The maximum load required to tear the sample at a tensile speed of 100±10 mm / min is taken as the tear strength (N), and the average of three points is calculated to obtain the tear strength (N) of the spunbond nonwoven fabric. (v) The tear strength per unit area of ​​the spunbond nonwoven fabric (N / (g / m 2 )) and round off to the third decimal place. Tear strength per unit area of ​​spunbond nonwoven fabric (N / (g / m 2 )) = [Tear strength of spunbond nonwoven fabric (N)] / basis weight (g / m 2 ).

[0036] [Manufacturing method of spunbond nonwoven fabric] The spunbonded nonwoven fabric of the present invention can be preferably produced by the method for producing the spunbonded nonwoven fabric of the present invention, which is a method for producing the spunbonded nonwoven fabric of the present invention and includes the following steps (a) to (c) in this order:

[0037] [Step (a): Fiber spinning step] In step (a), a core-sheath type composite fiber is spun in which a low-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less and having an intrinsic viscosity (IV) lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin by 0.05 to 0.25, is disposed around a high-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less.

[0038] That is, in the sheath-core composite fiber, it is preferable that the high-viscosity polyethylene terephthalate resin is the core component and the low-viscosity polyethylene terephthalate resin is the sheath component. By making the difference between the intrinsic viscosity of the core component and the intrinsic viscosity of the sheath component 0.05 or more, more preferably 0.10 or more, spinning stress is concentrated on the core component during spinning, promoting the orientation of the core component and suppressing the orientation of the sheath component. On the other hand, by making the difference between the intrinsic viscosity of the core component and the intrinsic viscosity of the sheath component 0.25 or less, preferably 0.20 or less, the strength of the single fiber of the sheath-core composite fiber can be improved, and rapid softening during heat bonding can be suppressed, thereby suppressing sticking to a heated roll during production.

[0039] The core-sheath type composite fiber is preferably melted at a temperature not lower than its melting point but not higher than 70°C above the melting point, and is preferably melt-extruded from a spinneret having a temperature not lower than its melting point but not higher than 70°C above the melting point.

[0040] The shape of the outlet hole of the spinneret from which the core-sheath type composite fiber is extruded may be circular, elliptical, polygonal, multi-lobed, or a combination of these shapes in accordance with the cross-sectional shape of the fiber. Among these, a circular shape is more preferred from the viewpoints of efficiently obtaining bonding points between the fibers and firmly bonding the fibers together by thermocompression bonding.

[0041] [Step (b): Step of forming a fiber web] In step (b), the spun core-sheath type composite fiber is pulled and stretched by an ejector, and deposited on a moving net conveyor to form a fiber web.

[0042] In step (b), the spun fibers are preferably pulled and stretched by an ejector, and the fibers are deposited on a moving net conveyor to form a fiber web. In this case, the spinning speed for pulling the fibers is preferably 3000 m / min or more and 6000 m / min or less.

[0043] [Step (c): Step of thermocompressing the fiber web] In the step (c), the fiber web is heat-pressurized to an embossing rate of 5 area % or more and 30 area % or less.

[0044] The fiber web can be heat-pressed to obtain the intended spunbonded nonwoven fabric.

[0045] Examples of the method for thermocompression bonding the fiber web include a method of thermocompression bonding using various rolls, such as a heat embossing roll in which each of a pair of upper and lower rolls has an engraving (uneven portion) on its surface, and a heat embossing roll consisting of a combination of a roll with one roll having a flat (smooth) surface and a roll with the other roll having an engraving (uneven portion) on its surface. Among them, it is preferable to use a heat embossing roll in which each of a pair of upper and lower rolls has an engraving (uneven portion) on its surface, or a heat embossing roll consisting of a combination of a roll with one roll having a flat (smooth) surface and a roll with the other roll having an engraving (uneven portion) on its surface, because it is highly productive, provides strength in the partially thermocompressed parts, and can retain the texture unique to nonwoven fabrics in the non-compressed parts.

[0046] As for the surface material of the hot embossing roll, a preferred embodiment is a pair of metal rolls in order to obtain a sufficient thermocompression effect and to prevent the engraving (convex and concave portions) of one embossing roll from being transferred to the surface of the other roll.

[0047] The embossing rate by the hot embossing roll is 5% by area or more and 30% by area or less. By setting the embossing rate to 5% by area or more, preferably 8% by area or more, more preferably 10% by area or more, it is possible to obtain a strength sufficient for practical use as a spunbonded nonwoven fabric. On the other hand, by setting the embossing rate to 30% by area or less, preferably 25% by area or less, more preferably 20% by area or less, it is possible to reduce the unevenness of the nonwoven fabric surface and obtain sufficient adhesion when used as a tape.

[0048] The shape of the part compressed by the hot embossing roll may be, for example, a circle, an ellipse, a square, a rectangle, a parallelogram, a rhombus, a regular hexagon, or a regular octagon.

[0049] It is also preferable that the compressed portions are uniformly spaced at regular intervals in the longitudinal direction (transport direction) and width direction of the spunbonded nonwoven fabric, thereby reducing variation in strength of the spunbonded nonwoven fabric.

[0050] The surface temperature of the hot embossing roll during thermocompression bonding is preferably 10°C to 100°C lower than the melting point (hereinafter sometimes referred to as Tm (°C)) of the polyethylene terephthalate resin used (i.e., (Tm-100)°C to (Tm-10)°C). By setting the surface temperature of the hot roll to (Tm-100)°C or higher, more preferably (Tm-90)°C or higher, it is possible to obtain a spunbonded nonwoven fabric having a strength that can be used for practical purposes by moderate thermocompression bonding. In addition, by setting the surface temperature of the hot embossing roll to (Tm-10)°C or lower, more preferably (Tm-15)°C or lower, it is possible to prevent excessive thermocompression bonding and prevent the spunbonded nonwoven fabric from partially becoming a sheet-like film.

[0051] The line pressure of the heat embossing roll during heat bonding is preferably 90 N / cm or more and 1000 N / cm or less. By setting the line pressure for heat bonding to 90 N / cm or more, a spunbonded nonwoven fabric having excellent mechanical strength can be obtained. By setting the line pressure for heat bonding to 1000 N / cm or less, excessive fusion between fibers can be prevented.

[0052] [tape] The tape of the present invention contains the nonwoven fabric. This makes it possible to obtain a tape that is excellent in mechanical strength and easy to tear by hand. The tape referred to here refers to a tape having an adhesive layer on at least one side of a nonwoven fabric substrate and a width of 150 mm or less.

[0053] The tape of the present invention can be used in various fields, such as building material applications, vehicle applications, and medical applications. In particular, it can be suitably used in building material applications that require hand tearability. Specific examples of the tape of the present invention include adhesive tapes, curing tapes, masking tapes, and sealing tapes. EXAMPLES

[0054] Next, the nonwoven fabric of the present invention will be specifically described based on examples, although the present invention is not limited to these examples.

[0055] [Measurement method] The evaluation methods and measurement conditions used in the examples are described below. Unless otherwise specified, the measurements of each physical property were performed according to the above-mentioned methods.

[0056] (1) Melting point of polyethylene terephthalate resin (℃) Measurement was performed using a differential scanning calorimeter (PerkinElmer, DSC-2) at a temperature rise rate of 16° C. / min, and the temperature giving an extreme value in the obtained melting endothermic curve was taken as the melting point.

[0057] (2) Intrinsic viscosity (IV) of polyethylene terephthalate resin The intrinsic viscosity (IV) of the polyethylene terephthalate resin was measured by the following method.

[0058] Dissolve 8 g of sample in 100 mL of orthochlorophenol, and measure the relative viscosity η using an Ostwald viscometer at 25°C. r was calculated by the following formula. η r =η / η0=(t×d) / (t0×d0) where η is the viscosity of the polymer solution, η0 is the viscosity of orthochlorophenol, t is the time the solution took to fall (sec), and d is the density of the solution (g / cm 3 ), t0 is the fall time of orthochlorophenol (sec), and d0 is the density of orthochlorophenol (g / cm 3 ) respectively. Next, the relative viscosity η r The intrinsic viscosity (IV) was calculated from the following formula. Intrinsic viscosity (IV)=0.0242η r +0.2634.

[0059] (3) Average single fiber diameter of fibers (μm) The average single fiber diameter of the fibers was calculated by the above-mentioned method using a scanning electron microscope "VHX-D500" manufactured by Keyence Corporation.

[0060] (4) Crystallization peak temperature (Tc) of spunbond nonwoven fabric The crystallization peak temperature of the spunbond nonwoven fabric was calculated by the above-mentioned method using a PerkinElmer "DSC-2" differential scanning calorimeter.

[0061] (5) Melting peak temperature (Tm) of spunbond nonwoven fabric The melting peak temperature of the spunbond nonwoven fabric was calculated by the above-mentioned method using a differential scanning calorimeter "DSC-2" manufactured by PerkinElmer Co., Ltd.

[0062] (6) Fiber fraying rate (%) The fiber fraying rate of the spunbond nonwoven fabric was calculated by the above-mentioned method using a scanning electron microscope "VHX-D500" manufactured by Keyence Corporation.

[0063] (7) Tensile strength per unit area of ​​spunbond nonwoven fabric ((N / 5cm) / (g / m 2 )) The tensile strength per unit area of ​​the spunbond nonwoven fabric was measured by the above-mentioned method using a constant-speed extension tensile tester "RTG-1250" manufactured by Baldwin.

[0064] (8) Tear strength per unit area of ​​spunbond nonwoven fabric (N / (g / m 2 )) The tear strength per unit area of ​​the spunbonded nonwoven fabric was measured by the above-mentioned method using a constant-speed extension tensile tester "RTG-1250" manufactured by Baldwin.

[0065] [Resin used] The resins used in the examples and comparative examples are described in detail below. · Polyethylene terephthalate resin A (PET_A): Polyethylene terephthalate that has been dried to a moisture content of 50 mass ppm or less, has an intrinsic viscosity (IV) of 0.65, and a melting point of 255°C. · Polyethylene terephthalate resin B (PET_B): Polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, with an intrinsic viscosity (IV) of 0.51 and a melting point of 255°C. · Polyethylene terephthalate resin C (PET_C): Polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, with an intrinsic viscosity (IV) of 0.70 and a melting point of 255°C. · Polyethylene terephthalate resin D (PET_D): Polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, with an intrinsic viscosity (IV) of 0.56 and a melting point of 255°C. · Polyethylene terephthalate resin E (PET_E): Polyethylene terephthalate that has been dried to a moisture content of 50 mass ppm or less, has an intrinsic viscosity (IV) of 0.45, and a melting point of 255°C. · Polyethylene terephthalate resin F (PET_F): Polyethylene terephthalate that has been dried to a moisture content of 50 mass ppm or less, has an intrinsic viscosity (IV) of 0.62, and a melting point of 255°C. Polyethylene terephthalate resin G (CO-PET): Copolymerized polyethylene terephthalate that has been dried to a moisture content of 50 ppm by mass or less, has an intrinsic viscosity (IV) of 0.64, an isophthalic acid copolymerization rate of 11 mol%, and a melting point of 230°C.

[0066] [Example 1] (The process of spinning fibers) Polyethylene terephthalate resin A and polyethylene terephthalate resin B were each melted at a temperature of 295° C. Then, concentric core-sheath composite fibers were spun from a circular extrusion hole with polyethylene terephthalate resin A as a core component and polyethylene terephthalate resin B as a sheath component at a spinneret temperature of 295° C. and a core:sheath mass ratio of 80:20.

[0067] (Step of forming a fiber web) The fiber spun by the above process was drawn at a spinning speed of 5000 m / min, and the basis weight of the resulting nonwoven fabric was 80.0 g / m 2 A fiber web consisting of fibers with a fiber diameter of 12.1 μm was formed by depositing the mixture on a net conveyor whose moving speed was adjusted so that the diameter of the fibers was 12.1 μm.

[0068] (Process for thermocompression bonding of fiber web) Subsequently, the formed fiber web was thermally pressed using a pair of upper and lower thermal embossing rolls consisting of an upper roll and a lower roll under the conditions of a surface temperature of the thermal embossing roll: 170°C and a linear pressure of 686 N / cm to obtain a spunbond nonwoven fabric. Upper roll: Metal embossed roll with 16% adhesive area Bottom roll: metal flat roll.

[0069] The obtained spunbond nonwoven fabric was evaluated and the results are shown in Table 1.

[0070] [Example 2] In the step of thermocompression bonding the fiber web, an embossing roll with a bonding area ratio of 8% was used as the upper roll. Except for this, a spunbonded nonwoven fabric was obtained under the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0071] [Example 3] In the step of thermocompression bonding the fiber web, an embossing roll with a bonding area ratio of 20% was used as the upper roll. Except for this, a spunbonded nonwoven fabric was obtained under the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0072] [Example 4] In the fiber spinning process, the polyethylene terephthalate resin A was changed to polyethylene terephthalate resin C. A spunbonded nonwoven fabric was obtained under the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0073] [Example 5] In the fiber spinning process, polyethylene terephthalate resin A was changed to polyethylene terephthalate resin D. A spunbonded nonwoven fabric was obtained under the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0074] [Example 6] In the fiber spinning process, polyethylene terephthalate resin A was changed to polyethylene terephthalate resin C, and polyethylene terephthalate resin B was changed to polyethylene terephthalate resin E. A spunbonded nonwoven fabric was obtained using the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0075] [Example 7] In the step of thermocompression bonding the fiber web, the surface temperature of the hot embossing roll was set to 180° C. Except for this, a spunbonded nonwoven fabric was obtained under the same procedure and conditions as in Example 6. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0076] [Example 8] In the step of thermocompression bonding the fiber web, the surface temperature of the hot embossing roll was set to 190° C. Except for this, a spunbonded nonwoven fabric was obtained under the same procedure and conditions as in Example 6. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0077] [Comparative Example 1] In the fiber spinning process, polyethylene terephthalate resin B was replaced with polyethylene terephthalate resin A to form a single component fiber. In addition, in the process of thermocompression bonding the fiber web, the surface temperature of the hot embossing roll was set to 250° C. Other than that, a spunbonded nonwoven fabric was obtained under the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0078] [Comparative Example 2] In the fiber spinning process, polyethylene terephthalate resin B was changed to polyethylene terephthalate resin G. A spunbonded nonwoven fabric was obtained using the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0079] [Comparative Example 3] In the fiber spinning process, polyethylene terephthalate resin B was changed to polyethylene terephthalate resin F. A spunbonded nonwoven fabric was obtained under the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0080] [Table 1]

[0081] The spunbond nonwoven fabrics of Examples 1 to 8 had high tensile strength and excellent mechanical strength, and also had low tear strength and excellent hand tearability, and thus exhibited favorable properties as a tape substrate.

[0082] On the other hand, the spunbond nonwoven fabrics of Comparative Examples 1 to 3 had high tear strength and poor hand-tearability (Comparative Examples 1 to 3), or had low tensile strength and insufficient mechanical strength (Comparative Example 1). [Explanation of symbols]

[0083] 1: Fibers with no fraying 2: Fibers with sores 3: Sore areas

Claims

1. A spunbond nonwoven fabric composed of fibers containing a polyethylene terephthalate resin as a main component, the spunbond nonwoven fabric having a crystallization peak in the range of 100°C or more and 150°C or less and a single melting peak in the range of 250°C or more and 270°C or less, as measured by differential scanning calorimetry, and an embossed compression ratio of 5 area % or more and 30 area % or less.

2. 2. The spunbond nonwoven fabric according to claim 1, wherein the fiber breakage rate per unit area in the non-pressure-bonded portion is 5.0% or more and 50.0% or less.

3. A tape comprising the spunbond nonwoven fabric according to claim 1 or 2.

4. A method for producing the spunbonded nonwoven fabric according to claim 1 or 2, comprising the following steps (a) to (c) in this order: Step (a): A step of spinning a core-sheath type composite fiber in which a low-viscosity polyethylene terephthalate-based resin having a melting point of 250° C. or more and 270° C. or less and having an intrinsic viscosity (IV) that is 0.05 or more and 0.25 or less lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate-based resin is disposed around the high-viscosity polyethylene terephthalate-based resin having a melting point of 250° C. or more and 270° C. or less. Step (b): A step of drawing and stretching the spun core-sheath type composite fiber by an ejector and depositing it on a moving net conveyor to form a fiber web. Step (c): A step of thermally compressing the fiber web to an embossing rate in the range of 5 area % to 30 area %.

Citation Information

Patent Citations

  • Filament nonwoven fabric and tape of holding and winding electric wire

    JP2007162186A

  • Composite nonwoven fabric for patch

    JP2008163538A

  • Area-bonded nonwoven fabric manufactured from a single polymer system

    JP2010537068A

  • Short-cut fiber for wet-laid nonwoven fabric

    JP2014037644A

  • Nonwoven fabric tape substrate

    JP2012180615A