Magnetic core, its manufacturing method, and coil component

A magnetic core with laminated soft magnetic layers and controlled crack intervals, featuring Fe-based nanocrystals or nanoheterostructures, addresses the issue of stress-induced deterioration during manufacturing, ensuring stable soft magnetic properties and efficient production.

JP7583093B2Active Publication Date: 2024-11-13TDK CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023060806
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-27
Filing Date
2023-04-04
Publication Date
2024-11-13
Estimated Expiration
2039-03-01

AI Technical Summary

Technical Problem

The challenge is to develop a magnetic core with stable soft magnetic properties that can be manufactured efficiently without deteriorating due to stress during punching, which is common when using laminated soft magnetic metals.

Method used

A magnetic core composed of laminated soft magnetic layers with cracks and a specific composition (Fe (1-( α + β )) X1αX2β) (1-(a+b+c+d+e+f)) M a B b P c Si d C e S f) containing Fe-based nanocrystals or nanoheterostructures, with controlled crack intervals and adhesive layers, allowing for easy processing and maintaining soft magnetic properties.

Benefits of technology

The solution results in a magnetic core with improved soft magnetic properties, reduced coercive force, and enhanced manufacturability, enabling efficient production and reduced eddy current losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583093000018
    Figure 0007583093000018
  • Figure 0007583093000019
    Figure 0007583093000019
  • Figure 0007583093000020
    Figure 0007583093000020
Patent Text Reader

Abstract

To provide a magnetic core having a stable soft magnetic property and a method of manufacturing the same and a coil component.SOLUTION: There is provided a magnetic core 10 in which a plurality of soft magnetic layers 12 and an adhesive layer 14 are alternately laminated in which a structure including a nanoheterostructure or an Fe-group nanocrystal is observed, and a crack is formed in the soft magnetic layers. The soft magnetic layers include Fe as a principal component. The soft magnetic layers include a composition formula: (Fe(1-(α+β))X1αX2β)(1-(a+b+c+d+e+f))MaBbPcSidCeSf, wherein: X1 is one or more selected from the group consisting of Co and Ni, X2 is one or more selected from the group consisting of Al, Mn, Ag, Zn, Sn, As, Sb, Cu, Cr, Bi, N, and O and rare-earth elements, M is one or more selected from the group consisting of Nb, Hf, Zr, Ta, Mo, V, and W; and a to f and α and β are in predetermined ranges.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic core, a manufacturing method thereof, and a coil component. [Background technology]

[0002] With the miniaturization of power devices in recent years, there is a demand for further miniaturization of transformers and coils, which occupy a large amount of space in the power devices. Patent Document 1 shows the use of soft magnetic metal as the material for the magnetic cores of transformers and coils. Research is also being conducted on forming magnetic cores by lamination.

[0003] However, when the magnetic core is formed by laminating and a soft magnetic metal is used as the magnetic material, the soft magnetic metal itself is hard, making it difficult to punch out, and there is a problem that the stress applied during punching causes a deterioration of the soft magnetic properties (especially an increase in coercive force). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-74108 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in view of the above circumstances, and has an object to provide a magnetic core etc. having stable soft magnetic characteristics. [Means for solving the problem]

[0006] In order to achieve the above object, a magnetic core according to a first aspect of the present invention comprises: A magnetic core comprising a plurality of soft magnetic layers laminated together, the soft magnetic layers each having a crack formed therein, The soft magnetic layer is mainly composed of Fe, The soft magnetic layer has the composition formula (Fe (1-( α + β )) X1αX2β) (1-(a+b+c+d+e+f)) M a B b P c S d C e S f It consists of: X1 is at least one selected from the group consisting of Co and Ni; X2 is one or more selected from the group consisting of Al, Mn, Ag, Zn, Sn, As, Sb, Cu, Cr, Bi, N, O and rare earth elements; M is one or more selected from the group consisting of Nb, Hf, Zr, Ta, Mo, V and W; 0≦a≦0.140 0.020 <b≦0.200 0≦c≦0.150 0≦d≦0.180 0≦e<0.040 0≦f≦0.030 α ≧ 0 β ≧ 0 0≦α+β≦0.50 and At least one of a, c, and d is greater than 0, The soft magnetic layer is characterized in that a nano-heterostructure consisting of amorphous and microcrystalline materials, the microcrystalline materials being present in the amorphous material, is observed.

[0007] The microcrystals may have an average particle size of 0.3 to 5 nm.

[0008] Also, the magnetic core of the present invention according to a second aspect comprises: A magnetic core comprising a plurality of soft magnetic layers laminated together, the soft magnetic layers each having a crack formed therein, The soft magnetic layer is mainly composed of Fe, The soft magnetic layer has the composition formula (Fe (1-( α + β )) X1αX2β) (1-(a+b+c+d+e+f)) M a B b P c Sd C e S f It consists of: X1 is at least one selected from the group consisting of Co and Ni; X2 is one or more selected from the group consisting of Al, Mn, Ag, Zn, Sn, As, Sb, Cu, Cr, Bi, N, O and rare earth elements; M is one or more selected from the group consisting of Nb, Hf, Zr, Ta, Mo, V and W; 0≦a≦0.140 0.020 <b≦0.200 0≦c≦0.150 0≦d≦0.180 0≦e<0.040 0≦f≦0.030 α ≧ 0 β ≧ 0 0≦α+β≦0.50 and At least one of a, c, and d is greater than 0, and a structure made of Fe-based nanocrystals is observed in the soft magnetic layer.

[0009] The Fe-based nanocrystals may have an average particle size of 5 to 30 nm.

[0010] By using the magnetic core of the present invention, it is possible to provide a magnetic core having stable soft magnetic properties.

[0011] In the magnetic core of the present invention, the soft magnetic layer may be divided into small pieces so that the average crack spacing is 0.015 mm or more and 1.0 mm or less.

[0012] In the magnetic core of the present invention, the space factor of the magnetic material in the magnetic core may be 70.0% or more and 99.5% or less.

[0013] The magnetic core of the present invention may satisfy the condition 0.020≦a≦0.100.

[0014] The magnetic core of the present invention may satisfy the condition: 0.730≦1−(a+b+c+d+e+f)≦0.950.

[0015] In the magnetic core of the present invention, α may be 0.

[0016] In the magnetic core of the present invention, β may be 0.

[0017] A coil component of the present invention includes any one of the magnetic cores described above and a coil.

[0018] The method for manufacturing a magnetic core of the present invention includes a step of subjecting a plurality of soft magnetic ribbons to small fragmentation processing, and a step of stacking the plurality of small fragmented soft magnetic ribbons in a thickness direction. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a schematic plan view of a magnetic core according to an embodiment of the present invention. [Diagram 2] 2 is a schematic cross-sectional view of a magnetic core according to an embodiment of the present invention. FIG. [Diagram 3] 2 is a schematic cross-sectional view of a soft magnetic layer included in a magnetic core according to one embodiment of the present invention. [Figure 4] This is a chart obtained by X-ray crystal structure analysis. [Diagram 5] This is a pattern obtained by profile fitting the chart in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, the present invention will be described based on the embodiments shown in the drawings.

[0021] The configuration of the magnetic core 10 according to this embodiment will be described. Fig. 1 is a schematic plan view of the cylindrical magnetic core 10 as viewed from one side of an extended central plane A. Fig. 2 is a schematic cross-sectional view of the magnetic core 10 of Fig. 1 taken along line II-II. Fig. 3 is a schematic cross-sectional view of the soft magnetic layer 12 of Fig. 2 taken along line III-III. The observation range of Fig. 3 is 4 mm x 4 mm.

[0022] As shown in Fig. 2, the magnetic core 10 according to this embodiment is formed by alternately laminating a plurality of soft magnetic layers 12 and adhesive layers 14. Fig. 2 illustrates an example in which the magnetic core 10 has a plurality of soft magnetic layers 12, but the number of layers may be changed as desired. When the magnetic core according to this embodiment has a plurality of soft magnetic layers 12 (for example, 2 layers or more and 10,000 layers or less), it is most preferable that all of the soft magnetic layers 12 have a plurality of cracks, which will be described later, formed therein.

[0023] The magnetic core 10 of this embodiment has as its main components a soft magnetic layer 12 and an adhesive layer 14. However, it may contain other components as long as they do not impair the effects of the present invention. Conversely, the soft magnetic layer 12 may be laminated without using the adhesive layer 14.

[0024] Moreover, the volume ratio (space factor) of the magnetic material in the magnetic core 10 is preferably 70% or more and 99.5% or less. When the space factor of the magnetic material is 70% or more, the saturation magnetic flux density can be sufficiently increased, and the magnetic core can be effectively used. When the space factor of the magnetic material is 99.5% or less, the magnetic core 10 becomes less likely to be damaged, and can be easily handled as a magnetic core. The space factor of the magnetic material may be 72% or more and 96% or less. In this embodiment, the volume of the magnetic material is substantially the same as the volume of the soft magnetic layer 12.

[0025] 3, a plurality of cracks C are formed in the soft magnetic layer 12 included in the magnetic core 10 according to this embodiment. The soft magnetic layer 12 is divided into a plurality of small pieces by the plurality of cracks C. The width of the cracks C may be, for example, 10 nm or more and 1000 nm or less.

[0026] In the magnetic core 10 of this embodiment, multiple cracks C are formed in the soft magnetic layer 12 and the soft magnetic layer 12 is divided into multiple small pieces, thereby suppressing changes in the soft magnetic properties due to stress during manufacturing, particularly an increase in coercive force, and making it possible to provide a good magnetic core 10.

[0027] Here, in this embodiment, when a virtual line B is drawn in an area divided and fragmented by a crack C, the average crack spacing is defined as the number of intersections D where the virtual line B and the crack C intersect, divided by the total length of the virtual line B.

[0028] Hereinafter, the method for calculating the average crack interval will be described with reference to a specific case shown in Fig. 3. A square observation area is shown in Fig. 3. In Fig. 3, crack C is shown by a solid line, and virtual line B is shown by a dotted line.

[0029] Virtual line B extends in one direction within the observation range (the horizontal direction in the figure), and 10 virtual lines B extend parallel to the vertical direction in the figure at equal intervals. In this case, the number of intersections D where virtual line B intersects with cracks C is measured. The number of intersections D is the total number of cracks C that intersect with virtual line B. The average crack spacing is calculated by dividing the total length of virtual line B by the total number of cracks C that intersect with virtual line B (the number of intersections D). Expressed as a calculation formula, this is shown in Equation (1). Average crack spacing (mm) = (total length of virtual line B) / (number of intersections D) Equation (1)

[0030] In the example shown in Figure 3, if the observation range is a square with sides of 4 mm, the total length of virtual line B is 40 mm and the number of intersections D is 43, so the average crack spacing is 40 / 43 [mm], or approximately 0.93 mm.

[0031] Since the average crack spacing varies depending on the selected observation range, it is preferable to calculate the average over multiple observation ranges. It is preferable to calculate the average over three or more different observation ranges. It is also preferable to determine how to select the observation range. For example, when using a ring-shaped magnetic core 10 as in this embodiment, the central surface A can be selected as the observation range to be selected when calculating the average crack spacing. The method for measuring the average crack spacing is arbitrary. For example, a SEM can be used.

[0032] In this embodiment, the average crack interval is arbitrary, but it is preferable that the soft magnetic layer 12 has cracks formed such that the average crack interval is 0.015 mm or more and 1.0 mm or less. If the average crack interval is smaller than 0.015 mm, the magnetic permeability of the soft magnetic layer 12 is likely to decrease, the inductance Ls of the magnetic core 10 is likely to decrease, and the performance of the magnetic core 10 is likely to decrease. In addition, if the average crack interval is more than 1.0 mm, it becomes difficult to punch with a weak force in the punching process of the manufacturing method of the magnetic core 10 described later. As a result, the range of the stress generated on the cut surface during punching becomes wider, and the effect of forming multiple cracks and dividing into multiple small pieces is weakened. Preferably, the average crack interval is 0.015 mm or more and 0.75 mm or less. More preferably, the average crack interval is 0.075 mm or more and 0.75 mm or less.

[0033] In addition, the magnetic core 10 according to the present embodiment has an adhesive layer 14, which can prevent small pieces from falling off. A known adhesive layer 14 can be used as the adhesive layer 14. For example, an adhesive layer coated with an acrylic adhesive, a silicone resin, a butadiene resin, or a hot melt, etc., on the surface of the substrate can be used. A typical material for the substrate is a PET film. However, other than the PET film, resin films such as polyimide film, polyester film, polyphenylene sulfide (PPS) film, polypropylene (PP) film, and fluororesin film such as polytetrafluoroethylene (PTFE), can be used. An acrylic resin can be directly applied to the main surface of the soft magnetic ribbon after the heat treatment described later, and the applied layer can be used as the adhesive layer 14.

[0034] The magnetic core 10 may also have a protective film 13 on each of one end side and the other end side in the lamination direction (z-axis direction in Figs. 1 and 2). A known material can be used as the protective film 13. Examples include a PET film, a polyimide film, and an aramid film.

[0035] The soft magnetic layer 12 has a plurality of cracks which divide it into a plurality of small pieces.

[0036] The soft magnetic layer 12 is mainly composed of Fe. The soft magnetic layer has the composition formula (Fe (1-( α + β )) X1αX2β) (1-(a+b+c+d+e+f)) M a B b P c S d C e S f It consists of: X1 is at least one selected from the group consisting of Co and Ni; X2 is one or more selected from the group consisting of Al, Mn, Ag, Zn, Sn, As, Sb, Cu, Cr, Bi, N, O and rare earth elements; M is one or more selected from the group consisting of Nb, Hf, Zr, Ta, Mo, V and W; 0≦a≦0.140 0.020 <b≦0.200 0≦c≦0.150 0≦d≦0.180 0≦e<0.040 0≦f≦0.030 α ≧ 0 β ≧ 0 0≦α+β≦0.50 and It is characterized in that one or more of a, c, and d is greater than 0.

[0037] In the soft magnetic layer 12 of this embodiment, a nanoheterostructure (the above first aspect) or a structure made of Fe-based nanocrystals (the above second aspect) is further observed.

[0038] The nanoheterostructure refers to a structure consisting of amorphous and microcrystals, and the microcrystals are present in the amorphous. The term "consisting of amorphous and microcrystals" refers to the microcrystals being scattered in the amorphous. The term "microcrystals being scattered in the amorphous" refers to the amorphization rate X measured by normal X-ray diffraction measurement (XRD) being 85% or more, and the crystal phase being confirmed in the electron diffraction image and high-resolution image in a transmission electron microscope. The term "microcrystals" refers to crystals having a particle size of 30 nm or less. The average particle size of the microcrystals may be in the range of 0.3 to 5 nm.

[0039] The Fe-based nanocrystals are crystals having a nano-order particle size (specifically, an average particle size of about 30 nm or less) and an Fe crystal structure of bcc (body-centered cubic lattice structure). In this embodiment, it is preferable to precipitate Fe-based nanocrystals having an average particle size of 5 to 30 nm. In addition, the structure made of Fe-based nanocrystals is a structure that includes Fe-based nanocrystals and has the above-mentioned amorphization rate X of less than 85%.

[0040] The soft magnetic layer 12 of this embodiment has a composition within the above-mentioned specific range, and furthermore, a nano-hetero structure or a structure made of Fe-based nanocrystals is observed, so that cracks are easily generated during the fragmentation process during the manufacture of the magnetic core 10 described below. Furthermore, the presence of cracks C makes it possible to punch out with a weak force. Furthermore, changes in the soft magnetic properties due to stress during manufacture, particularly increases in coercive force, are suppressed, and a magnetic core 10 having good soft magnetic properties can be manufactured.

[0041] Furthermore, when the soft magnetic layer has a structure made of Fe-based nanocrystals, the saturation magnetic flux density tends to be high and the coercive force tends to be low.

[0042] The composition of the soft magnetic layer 12 of this embodiment will be described in more detail below.

[0043] M is one or more selected from the group consisting of Nb, Hf, Zr, Ta, Ti, Mo, V and W. M is preferably Nb.

[0044] The content (a) of M satisfies 0 ≦ a ≦ 0.140. That is, M may not be contained. However, when M is not contained, the magnetostriction constant tends to be high and the coercive force tends to be high. The content (a) of M is preferably 0.020 ≦ a ≦ 0.100, more preferably 0.040 ≦ a ≦ 0.100, and even more preferably 0.050 ≦ a ≦ 0.080. When a is large, the coercive force tends to increase during the production of the magnetic core 10.

[0045] The content (b) of B satisfies 0.020 < b ≦ 0.200. Also, it is preferably 0.025 ≦ b ≦ 0.200, more preferably 0.025 ≦ b ≦ 0.120, and most preferably 0.060 ≦ b ≦ 0.120. When b is small, a crystal phase composed of crystals larger than 30 nm in particle size tends to occur during the production of the soft magnetic thin strip described later, and it is difficult to form a nanoheterostructure or a structure composed of Fe-based nanocrystals. When b is large, the coercive force tends to increase during the production of the magnetic core 10.

[0046] The content (c) of P satisfies 0 ≦ c ≦ 0.150. That is, P may not be contained. By containing P, the coercive force tends to decrease. From the viewpoint of reducing the coercive force and improving the inductance Ls of the magnetic core 10, it is preferably 0.050 ≦ c ≦ 0.150, and more preferably 0.050 ≦ c ≦ 0.080. Also, from the viewpoint of making it difficult to increase the coercive force during the production of the magnetic core 10, it is preferably 0 ≦ c ≦ 0.030. When c is large, the coercive force tends to increase during the production of the magnetic core 10.

[0047] The content (d) of Si satisfies 0 ≦ d ≦ 0.180. That is, Si may not be contained. 0 ≦ d ≦ 0.175 is also possible. It is preferably 0 ≦ d ≦ 0.060. Also, when 0.070 ≦ d ≦ 0.180, it tends to be easier to obtain the soft magnetic layer 12 and the magnetic core 10 having suitable soft magnetic properties by reducing the content (a) of M and the content (c) of P.

[0048] The C content (e) satisfies 0≦e<0.040. In other words, C does not need to be contained. From the viewpoint of reducing the coercive force, it is preferable that 0≦e≦0.030, and more preferably 0.001≦e≦0.010. When e is large, the coercive force is likely to increase during the manufacture of the magnetic core 10.

[0049] The S content (f) satisfies 0≦f≦0.030. In other words, S does not have to be contained. From the viewpoint of decreasing the coercive force, it is preferable that 0≦f≦0.001. If f is large, a crystalline phase consisting of crystals with a grain size larger than 30 nm is likely to occur during the production of the soft magnetic ribbon described later, making it difficult to form a nanoheterostructure or a structure consisting of Fe-based nanocrystals.

[0050] Moreover, at least one of a, c, and d is greater than 0. At least one of a, c, and d may be 0.001 or greater, or may be 0.010 or greater. That is, the soft magnetic layer 12 according to this embodiment contains at least one of M, P, and Si. This makes it easy to form a nanoheterostructure or a structure made of Fe-based nanocrystals.

[0051] The Fe content {1-(a+b+c+d+e+f)} is arbitrary. It is preferable to satisfy 0.730≦1-(a+b+c+d+e+f)≦0.950. It is preferable to satisfy 0.730≦1-(a+b+c+d+e+f)≦0.900. When 0.730≦1-(a+b+c+d+e+f), it is easy to improve the saturation magnetic flux density. Also, when 1-(a+b+c+d+e+f)≦0.950, it is easy to form a nanoheterostructure or a structure made of Fe-based nanocrystals.

[0052] In the soft magnetic alloy according to this embodiment, a portion of Fe may be substituted with X1 and / or X2.

[0053] X1 is at least one selected from the group consisting of Co and Ni. The content (α) of X1 may be α=0. That is, X1 may not be contained. The number of atoms of X1 is preferably 40 at% or less, where the number of atoms in the entire composition is 100 at%. That is, it is preferable to satisfy 0≦α{1-(a+b+c+d+e+f)}≦0.40.

[0054] X2 is one or more selected from the group consisting of Al, Mn, Ag, Zn, Sn, As, Sb, Cu, Cr, Bi, N, O, and rare earth elements. The content (β) of X2 may be β=0. That is, X2 may not be contained. In addition, the number of atoms of X2 is preferably 3.0 at% or less, with the number of atoms in the entire composition being 100 at%. That is, it is preferable to satisfy 0≦β{1-(a+b+c+d+e+f)}≦0.030.

[0055] The range of substitution amount of Fe with X1 and / or X2 is half or less of Fe on an atomic number basis. In other words, 0≦α+β≦0.50. If α+β>0.50, it becomes difficult to form a nanoheterostructure or a structure made of Fe-based nanocrystals.

[0056] The soft magnetic layer 12 according to the present embodiment may contain elements other than those mentioned above as inevitable impurities to the extent that they do not significantly affect the characteristics. For example, the soft magnetic layer 12 may contain 1% by weight or less when the soft magnetic layer 12 is taken as 100% by weight.

[0057] A method for manufacturing the magnetic core 10 according to this embodiment will now be described.

[0058] First, there will be described a method for manufacturing a soft magnetic ribbon which, when laminated, becomes the soft magnetic layer 12 included in the magnetic core 10. Hereinafter, the soft magnetic ribbon may be simply referred to as a ribbon.

[0059] There is no particular limitation on the method for producing the soft magnetic ribbon. For example, the soft magnetic ribbon according to the present embodiment may be produced by a single roll method. The ribbon may also be a continuous ribbon.

[0060] In the single roll method, first, the pure metals of each metal element contained in the soft magnetic alloy to be finally obtained are prepared and weighed so as to have the same composition as the soft magnetic alloy to be finally obtained. Then, the pure metals of each metal element are melted and mixed to prepare a master alloy. There is no particular limitation on the method of melting the pure metals, but for example, a method of melting by high-frequency heating after evacuating in a chamber is available. Note that the master alloy and the soft magnetic alloy made of Fe-based nanocrystals to be finally obtained usually have the same composition.

[0061] Next, the produced master alloy is heated and melted to obtain a molten metal (molten metal). There is no particular limit to the temperature of the molten metal, but it can be set to 1100 to 1350°C, for example.

[0062] In the single roll method, the thickness of the ribbon obtained can be adjusted mainly by adjusting the rotation speed of the roll, but the thickness can also be adjusted by adjusting the distance between the nozzle and the roll, the temperature of the molten metal, etc. The ribbon thickness is not particularly limited, but can be, for example, 14 to 30 μm. The ribbon thickness and the thickness of the soft magnetic layer 12 included in the finally obtained magnetic core 10 are approximately the same.

[0063] There are no particular limitations on the temperature of the rolls, the rotation speed, and the atmosphere inside the chamber. The temperature of the rolls is generally from room temperature to 80°C. The lower the temperature of the rolls, the smaller the average particle size of the microcrystals tends to be. The faster the rotation speed of the rolls, the smaller the average particle size of the microcrystals tends to be. For example, 10 to 30 m / sec. Considering costs, it is preferable that the atmosphere inside the chamber be air.

[0064] Before the heat treatment described later, the ribbon has an amorphous structure. That is, the ribbon has a structure consisting of only amorphous materials or a nanoheterostructure. By subjecting the ribbon to the heat treatment described later, a ribbon having a structure consisting of Fe-based nanocrystals can be obtained. Alternatively, a ribbon having a nanoheterostructure may be obtained by the heat treatment.

[0065] Whether the soft magnetic alloy ribbon has an amorphous structure or a crystalline structure can be confirmed by ordinary X-ray diffraction measurement (XRD).

[0066] Specifically, X-ray structural analysis is performed by XRD to calculate the amorphization rate X (%) shown in the following formula (1). If the amorphization rate X (%) is 85% or more, the structure is considered to be made of amorphous material, and if it is less than 85%, the structure is considered to be made of crystal material. X(%)=100-(Ic / (Ic+Ia)×100)…(1) Ic: Crystalline scattering integrated intensity Ia: Amorphous scattering integrated intensity

[0067] In order to calculate the amorphous ratio X, first, an X-ray crystal structure analysis is performed by XRD on the soft magnetic alloy according to this embodiment to obtain the chart shown in Fig. 4. Profile fitting is performed on the chart using the Lorentz function shown in the following formula (2).

number

[0068] As a result of profile fitting, the crystalline component pattern α showing the crystalline scattering integrated intensity shown in Figure 5 was obtained. c , amorphous component pattern α showing amorphous scattering integral intensity a , and the combined pattern α c+a From each pattern obtained, the crystalline scattering integrated intensity Ic and the amorphous scattering integrated intensity Ia are obtained. From Ic and Ia, the amorphization rate X is obtained by the above formula (1). The measurement range is the range of diffraction angle 2θ where an amorphous-derived halo can be confirmed. Specifically, the range is 2θ=30° to 60°. Within this range, the error between the integrated intensity actually measured by XRD and the integrated intensity calculated using the Lorentz function is set to within 1%.

[0069] In this embodiment, when the soft magnetic alloy is obtained in the form of a ribbon by the single roll method described later, the amorphous ratio (X A) and the amorphization rate on the surface not in contact with the roll surface (X B ) may differ. In this case, X A and X B The average of these is defined as the amorphous ratio X.

[0070] The ribbon before the heat treatment may have an amorphous structure, but preferably has a nanoheterostructure. The grain size of the microcrystals in the nanoheterostructure is not particularly limited, but the average grain size is preferably within a range of 0.3 to 5 nm.

[0071] In addition, in the case of a nanoheterostructure, the presence or absence of microcrystals and the average grain size can be observed, for example, by obtaining an electron diffraction image and a high-resolution image using a transmission electron microscope on a sample sliced ​​by ion milling. When using an electron diffraction image, a ring-shaped diffraction pattern is formed in the case of a structure consisting only of amorphous matter, whereas a structure containing microcrystals forms diffraction spots due to the microcrystals. Furthermore, when using a high-resolution image, a magnification of 1.00×10 5 ~3.00×10 5 The presence or absence of microcrystals and their average particle size can be observed by visual inspection at 100x magnification.

[0072] In addition, there is no particular restriction on the heat treatment conditions for manufacturing a ribbon having a structure made of Fe-based nanocrystals or a ribbon having a nanoheterostructure. The preferred heat treatment conditions vary depending on the composition of the soft magnetic ribbon. Usually, the preferred heat treatment temperature is about 400 to 700°C, and the preferred heat treatment time is about 0.1 to 6 hours. However, depending on the composition, the preferred heat treatment temperature and heat treatment time may be outside the above range. In addition, there is no particular restriction on the atmosphere during the heat treatment. The heat treatment may be performed in an active atmosphere such as air, or in an inert atmosphere such as Ar gas or N2 gas. This heat treatment embrittles the soft magnetic ribbon, making it easier to perform the fragmentation process. Furthermore, residual strain in the soft magnetic ribbon is removed.

[0073] If the ribbon has a nanoheterostructure at the stage of manufacturing the ribbon, the heat treatment can be omitted. However, for the above reasons, it is preferable to perform the heat treatment. The heat treatment may also be performed after manufacturing the magnetic core 10 described later.

[0074] There is no particular limit to the method for calculating the average grain size of the crystals contained in the obtained soft magnetic ribbon. For example, it can be calculated by observing with a transmission electron microscope. There is no particular limit to the method for confirming that the crystal structure is a bcc (body-centered cubic lattice structure). For example, it can be confirmed by X-ray diffraction measurement.

[0075] The manufacturing method of the magnetic core 10 according to this embodiment mainly includes an adhesive layer forming step, a crack forming step (fragmentation step), a punching step, and a lamination step. An overview of each step will be described below.

[0076] (Adhesive layer formation process) An adhesive layer is formed on each of the soft magnetic ribbons after the heat treatment. The adhesive layer can be formed by using a known method. For example, the adhesive layer may be formed by thinly applying a solution containing a resin to the soft magnetic ribbon and drying the solvent. Also, a double-sided tape may be attached to the soft magnetic ribbon, and the attached double-sided tape may be used as the adhesive layer. In this case, for example, a double-sided tape in which an adhesive is applied to both sides of a PET (polyethylene terephthalate) film may be used.

[0077] (Crack formation process (fragmentation process)) Cracks are generated in the soft magnetic ribbons on which the adhesive layer is formed, and the ribbons are divided into small pieces. A known method can be used to generate cracks. For example, an external force may be applied to the soft magnetic ribbon to generate cracks. Known methods for generating cracks by applying an external force include, for example, a method of pressing and breaking the ribbon with a die, and a method of passing the ribbon through a rolling roll to bend the ribbon. Furthermore, a predetermined uneven pattern may be provided on the die or rolling roll.

[0078] Then, a plurality of cracks are formed in each soft magnetic ribbon to break it into small pieces so that the average crack spacing falls within the above-mentioned range. The method for controlling the average crack spacing is arbitrary. When the ribbon is pressed and broken using a die, the average crack spacing can be appropriately changed, for example, by changing the pressure applied during pressing. When the ribbon is passed through rolling rolls and folded, the average crack spacing can be appropriately changed, for example, by changing the number of times the ribbon is passed through the rolling rolls.

[0079] When an adhesive layer is formed in advance, it becomes easier to prevent the small pieces divided by the crack from scattering. That is, although the soft magnetic ribbon after the crack is formed is divided into a plurality of small pieces, the position of each small piece is fixed via the adhesive layer. As for the soft magnetic ribbon as a whole, the shape before the crack is formed is almost maintained even after the crack is formed. However, if the crack can be formed while maintaining the shape of the soft magnetic ribbon as a whole without using an adhesive layer, it is not necessarily necessary to form the adhesive layer before the crack is formed.

[0080] (Punching process) Next, the soft magnetic ribbons in which cracks are formed and which have been broken into small pieces are punched out into a predetermined shape. As shown in FIG. 1, in this embodiment, the center is punched out into a circular shape. A known method can be used for the punching process. For example, the soft magnetic ribbon is sandwiched between a die having a desired shape and a face plate, and pressure is applied from the face plate side to the die side, or from the die side to the face plate side. Note that, if an adhesive layer is formed on the soft magnetic ribbon before punching, the soft magnetic ribbon is punched out together with the adhesive layer.

[0081] The soft magnetic ribbon made of the soft magnetic material of this embodiment is hard. Therefore, it is difficult to punch it out with a weak force. When the soft magnetic ribbon is punched out, the punched part is cut from the remaining part, generating stress. The stronger the punching force, the greater the stress. This stress is transmitted to the remaining part of the soft magnetic ribbon, deteriorating the soft magnetic properties. In other words, the coercive force increases.

[0082] However, the soft magnetic ribbon of this embodiment has cracks and is fragmented. Therefore, it can be punched out with a weaker force than when it does not have cracks and is not fragmented. Therefore, the above-mentioned stress is smaller. Furthermore, the portion near the cut surface where stress occurs during punching is physically separated from the other portions. Therefore, the above-mentioned stress is not transmitted to most areas other than the vicinity of the cut surface. And, the deterioration of the soft magnetic properties due to stress can be minimized.

[0083] Therefore, the soft magnetic ribbon of this embodiment is less susceptible to deterioration of the soft magnetic properties (increase in coercive force) due to punching, improving the soft magnetic properties of the finally obtained magnetic core 10. Furthermore, the soft magnetic ribbon of this embodiment can be punched with a relatively weak force, so it is easy to process into a desired shape and has excellent productivity.

[0084] (Lamination process) The magnetic core 10 of this embodiment can be obtained by stacking a plurality of punched soft magnetic ribbons together in the thickness direction via an adhesive layer. A protective film 13 may be formed on each of one end side and the other end side in the stacking direction (z-axis direction in Figs. 1 and 2). The method for forming the protective film 13 is arbitrary.

[0085] Note that steps other than the crack forming step and the lamination step are not essential, and the order of each step may be appropriately rearranged.

[0086] The magnetic core 10 according to this embodiment has a structure in which a plurality of soft magnetic ribbons are laminated to increase the space factor of the magnetic material (soft magnetic layer 12), and is strong and easy to handle.

[0087] Since the magnetic core 10 of this embodiment is formed by laminating a plurality of soft magnetic ribbons, the current path is divided at a plurality of locations in the lamination direction. Furthermore, since each soft magnetic ribbon (soft magnetic layer 12) of the magnetic core 10 of this embodiment has cracks and is fragmented, the current path is also divided at a plurality of locations in the direction intersecting the lamination direction. Therefore, in the coil component having the magnetic core of this embodiment, the path of the eddy current accompanying the change in magnetic flux in the AC magnetic field is divided in all directions, and eddy current loss can be significantly reduced.

[0088] 1 shows a cylindrical magnetic core as an example, the shape of the magnetic core is not particularly limited and may be any known shape. For example, it may be a rectangular tube. In addition, a combination of multiple cores such as E-shaped cores may be used.

[0089] There is no particular limit to the application of the magnetic core 10, but it can be used, for example, in coil components including a conductor (transformers, choke coils, magnetic sensors, etc.). EXAMPLES

[0090] (Experimental Example 1) <Production of soft magnetic ribbon> Raw material metals were weighed out so as to obtain the alloy compositions of the examples and comparative examples shown in the table below, and were melted by high-frequency heating to prepare master alloys.

[0091] The mother alloy thus prepared was then heated and melted to produce a molten metal at 1250°C, after which the metal was sprayed onto a roll at 60°C in air at a rotation speed of 20 m / sec by a single roll method to produce a ribbon with a thickness of approximately 20 μm and a width of approximately 50 mm.

[0092] Next, whether the obtained ribbon has an amorphous structure (a structure consisting only of amorphous materials or a nanoheterostructure) or a crystalline structure was confirmed by a conventional X-ray diffraction measurement (XRD). The results are shown in Table 1.

[0093] Thereafter, heat treatment was performed on the ribbons of all the examples except for Sample 1 and Sample 12 in Tables 1 and 2. The heat treatment conditions were as follows: Samples 2 to 6 and 13 to 17 had a heat treatment temperature of 500°C, a holding time of 60 minutes, a heating rate of 1°C / min, and a cooling rate of 1°C / min, while Samples 7 to 11 and 18 to 22 had a heat treatment temperature of 570°C, a holding time of 60 minutes, a heating rate of 1°C / min, and a cooling rate of 1°C / min.

[0094] <Evaluation of soft magnetic ribbons> The microstructure of each ribbon after heat treatment was confirmed by X-ray diffraction measurement (XRD) and observation using a transmission electron microscope (TEM). Specifically, it was observed whether each ribbon had a structure made of Fe-based nanocrystals, a nanoheterostructure, or a structure made only of amorphous matter. The structure made of Fe-based nanocrystals had a bcc crystal structure.

[0095] In addition, when the microstructure of each ribbon after the heat treatment was a nanoheterostructure, it was confirmed that the average grain size of the microcrystals was 0.3 to 5.0 nm in all examples, and when the microstructure of each ribbon after the heat treatment was a structure made of Fe-based nanocrystals, it was confirmed that the average grain size of the Fe-based nanocrystals was 5.0 nm or more and 30 nm or less in all examples.

[0096] Furthermore, the saturation magnetic flux density Bs and coercive force Hca of each ribbon after heat treatment were measured. The saturation magnetic flux density was measured using a vibrating sample magnetometer (VSM) in a magnetic field of 1000 kA / m. The coercive force was measured using a DC BH tracer in a magnetic field of 5 kA / m.

[0097] <Magnetic core production> First, a resin solution was applied to the obtained soft magnetic ribbon. After that, the solvent was dried and adhesive layers with a thickness of about 1 to 2 μm were formed on both sides of the soft magnetic ribbon, thereby producing a magnetic sheet equipped with adhesive layers.

[0098] Next, the produced magnetic sheet was subjected to a crack formation process so that the average crack interval of the soft magnetic ribbon became the value shown in Table 2, and a fragmented magnetic sheet was produced. Note that the magnetic sheets of Sample 1 and Sample 12, which used soft magnetic ribbons with an amorphous microstructure, were unable to form cracks and were unable to be fragmented.

[0099] Next, the resulting fragmented magnetic sheet was punched to form a ring shape (outer diameter 18 mm, inner diameter 10 mm). Specifically, this punching was performed by sandwiching the fragmented magnetic sheet between a punching die and a face plate, and applying pressure from the face plate side toward the punching die side. Note that the magnetic sheets of Samples 1 and 12, which could not be fragmented, could not be punched out with the same amount of force as the fragmented magnetic sheets of the other Examples.

[0100] Next, the punched magnetic sheets were laminated together to a height of about 5 mm to obtain a magnetic core. The soft magnetic layer of the obtained magnetic core had a space factor of about 85%. Furthermore, 30 magnetic cores were produced for each sample using the same procedure.

[0101] <Evaluation of magnetic cores> The coercive force Hcb of the magnetic core was measured in a magnetic field of 5 kA / m using a DC BH tracer in the same manner as the coercive force Hca of the ribbon. Note that the coercive force of each of the 30 magnetic cores was measured and then averaged to obtain Hcb.

[0102] Next, the coercive force change ΔHc (=Hcb-Hca) was calculated from the obtained Hca and Hcb. Furthermore, the coercive force change rate (%) was calculated. Specifically, it was calculated by substituting ΔHc and Hca into the formula (ΔHc / Hca)×100(%). A coercive force change rate of less than 100% was considered good.

[0103] Finally, a coil was wound around each of the obtained magnetic cores in the circumferential direction to form 30 coil components, and the inductance of each coil at 100 kHz was measured using an LCR meter, and the average was taken as Ls.

[0104] [Table 1]

[0105] [Table 2]

[0106] As shown in Tables 1 and 2, the soft magnetic ribbons of each Example could be cut into small pieces and punched out, and the magnetic cores of each Example had a good rate of coercive force change. The reason why the magnetic cores of each Example had a good rate of coercive force change will be described.

[0107] By breaking the soft magnetic ribbon into small pieces, the force required during punching can be reduced. Furthermore, by breaking the soft magnetic ribbon into small pieces, the stress generated near the cross section during punching is less likely to be transmitted to the inside. As a result, the deterioration of the soft magnetic properties (increase in coercive force and decrease in inductance) is suppressed. Furthermore, the inductance Ls became higher as the average crack spacing became larger and the size of each small piece became larger.

[0108] In contrast, the soft magnetic ribbons of the comparative examples, which had an amorphous microstructure, could not be cut into small pieces, and could not be punched out.

[0109] When the microstructure is a nanoheterostructure or a structure made of Fe-based nanocrystals, it is believed that fragmentation is possible because the grain boundaries become the starting points for fragmentation when an external force is applied. In contrast, when the microstructure is amorphous, fragmentation is not possible because there are no grain boundaries and therefore no starting points for fragmentation.

[0110] (Experimental Example 2) In Experimental Example 2, the soft magnetic ribbons were formed under the same conditions as Samples Nos. 7 to 11 in Experimental Example 1, except that the compositions of the soft magnetic ribbons were changed within the ranges shown in Tables 3 to 12.

[0111] [Table 3]

[0112]

Table 4

[0113]

Table 5

[0114]

Table 6

[0115]

Table 7

[0116]

Table 8

[0117]

Table 9

[0118]

Table 10

[0119]

Table 11

[0120]

Table 12

[0121] It was confirmed that the soft magnetic ribbons of all the above examples had a microstructure made of Fe-based nanocrystals, and the average grain size of the Fe-based nanocrystals was 5.0 nm or more and 30 nm or less. In addition, the soft magnetic ribbons of each example, whose composition was within a specific range, showed a better coercive force change rate than the comparative examples, whose soft magnetic ribbons had a composition outside the specific range. In addition, in sample 34, whose B content (b) was too small, and sample 59, whose S content (f) was too large, the soft magnetic ribbons before heat treatment had a microstructure made of crystals, and Fe-based nanocrystals could not be precipitated by heat treatment, resulting in a significantly high coercive force. In addition, the inductance Ls of the magnetic core was significantly reduced.

[0122] (Experimental Example 3) Experimental Example 3 was carried out under the same conditions as Sample No. 45 in Experimental Example 2, except that the temperature of the molten metal obtained by heating the prepared master alloy was changed, and further, the presence or absence of heat treatment, the heat treatment temperature, and the heat treatment time were changed. The results are shown in Tables 13 and 14. Note that, for the sake of convenience, Table 13 states that in the examples and comparative examples in which heat treatment was not performed, the average crystal grain size and microstructure before heat treatment are the same as those after heat treatment.

[0123] [Table 13]

[0124] [Table 14]

[0125] From Tables 13 and 14, even if the temperature of the molten metal obtained by heating the produced master alloy was changed, and further, the presence or absence of heat treatment, the heat treatment temperature, and the heat treatment time were changed, when the microstructure of the soft magnetic ribbon used in the end was a nanoheterostructure or a structure made of Fe-based nanocrystals, the soft magnetic ribbon could be cut into small pieces and punched out, and the coercive force change rate was good. In contrast, when the microstructure of the soft magnetic ribbon used in the end was an amorphous structure, the soft magnetic ribbon could not be cut into small pieces, and it could not be punched out.

[0126] (Experiment 4) Experiment 4 was carried out under the same conditions as sample number 7 in Experimental Example 1, except that the space factor of the magnetic material was changed. The results are shown in Tables 15 and 16.

[0127] [Table 15]

[0128] [Table 16]

[0129] As can be seen from Tables 15 and 16, even when the space factor was changed, the coercive force change rate was good in each example in which the space factor was 70% or more and 99.5% or less. Note that the higher the space factor, the higher the inductance Ls tended to be, and at the same time, the coercive force change rate tended to be larger. [Explanation of symbols]

[0130] 10. Magnetic core 12...Soft magnetic layer 13...Protective film 14...adhesive layer A Central plane B Virtual line C...Crack D...intersection

Claims

1. A magnetic core comprising a plurality of soft magnetic layers laminated together, the soft magnetic layers each having a crack formed therein, the soft magnetic layer is divided into small pieces so that the average crack spacing is 0.015 mm or more and 0.75 mm or less; The soft magnetic layer is mainly composed of Fe, The soft magnetic layer has a composition formula (Fe(1-(α+β))X1αX2β) (1-(a+b+c+d+e+f)) M a B b P c S d C e S f It consists of: X1 is at least one selected from the group consisting of Co and Ni; X2 is at least one selected from the group consisting of Al, Mn, Ag, Zn, Sn, As, Sb, Cu, Cr, Bi, N, O and rare earth elements; M is one or more selected from the group consisting of Nb, Hf, Zr, Ta, Mo, V and W; 0≦a≦0.140 0.020<b≦0.200 0≦c≦0.150 0≦d≦0.180 0≦e<0.040 0≦f≦0.030 α≧0 β≧0 0≦α+β≦0.50 and At least one of a, c, and d is greater than 0; A coil component having a magnetic core and a coil, characterized in that a nano-hetero structure consisting of an amorphous material and a microcrystal, the microcrystal being present in the amorphous material, is observed in the soft magnetic layer, A coil component, characterized in that the coil is wound around the magnetic core.

2. 2. The coil component according to claim 1, wherein the average grain size of the microcrystals is 0.3 to 5 nm.

3. A magnetic core comprising a plurality of soft magnetic layers laminated together, the soft magnetic layers each having a crack formed therein, the soft magnetic layer is divided into small pieces so that the average crack spacing is 0.015 mm or more and 0.75 mm or less; The soft magnetic layer is mainly composed of Fe, The soft magnetic layer has a composition formula (Fe(1-(α+β))X1αX2β) (1-(a+b+c+d+e+f)) M a B b P c S d C e S f It consists of: X1 is at least one selected from the group consisting of Co and Ni; X2 is at least one selected from the group consisting of Al, Mn, Ag, Zn, Sn, As, Sb, Cu, Cr, Bi, N, O and rare earth elements; M is one or more selected from the group consisting of Nb, Hf, Zr, Ta, Mo, V and W; 0≦a≦0.140 0.020<b≦0.200 0≦c≦0.150 0≦d≦0.180 0≦e<0.040 0≦f≦0.030 α≧0 β≧0 0≦α+β≦0.50 and At least one of a, c, and d is greater than 0; A coil component having a magnetic core and a coil, characterized in that a structure made of Fe-based nanocrystals is observed in the soft magnetic layer, A coil component, characterized in that the coil is wound around the magnetic core.

4. 4. The coil component according to claim 3, wherein the Fe-based nanocrystals have an average grain size of 5 to 30 nm.

5. 5. The coil component according to claim 1, wherein a space factor of the magnetic material in the magnetic core is 70.0% or more and 99.5% or less.

6. The coil component according to any one of claims 1 to 5, wherein 0.020≦a≦0.

100.

7. The coil component according to any one of claims 1 to 6, wherein 0.050≦a≦0.

080.

8. The coil component according to any one of claims 1 to 7, wherein 0.730≦1−(a+b+c+d+e+f)≦0.

950.

9. The coil component according to any one of claims 1 to 8, wherein α=0.

10. The coil component according to any one of claims 1 to 9, wherein β=0.

Citation Information

Patent Citations

  • Magnetic core and manufacture thereof

    JP1993335154A

  • Laminated magnetic core

    JP1999074108A

  • Method of manufacturing magnetic sheet

    JP2008112830A

  • Magnetic sheet

    JP2011134959A

  • Magnetic field shielding sheet for wireless chargers, method for manufacturing the same, and receiving device for wireless chargers using the same

    JP2015505166A