Hot stamped compact

A hot-stamped molded article with a controlled chemical composition and microstructure addresses the need for high bendability, achieving improved strength and collision resistance through a specific manufacturing process.

JP7583303B2Active Publication Date: 2024-11-14NIPPON STEEL CORPORATION
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022580677
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-10
Filing Date
2022-02-10
Publication Date
2024-11-14
Estimated Expiration
2042-02-10

AI Technical Summary

Technical Problem

Conventional hot-stamped molded bodies do not meet the demands for high bendability required by recent automobile safety standards, particularly in collision scenarios.

Method used

A hot-stamped molded article with a specific chemical composition and microstructure, comprising 85% martensite and less than 15% retained austenite, a standard deviation of nanohardness frequency distribution of 0.70 GPa or less, and an average crystal grain size of 4.0 μm or less, achieved by controlling the forming temperature and strain amount during hot stamping.

Benefits of technology

The solution provides a hot-stamped molded article with high strength and excellent bendability, enhancing collision resistance in automobiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583303000001
    Figure 0007583303000001
  • Figure 0007583303000002
    Figure 0007583303000002
  • Figure 0007583303000003
    Figure 0007583303000003
Patent Text Reader

Abstract

A hot-stamped molded body having: a chemical composition which contains, in mass%, C in the amount of 0.15-0.50%, inclusive, Si in the amount of 0.10-3.00%, inclusive, Mn in the amount of 0.10-3.00%, inclusive, P in an amount less than 0.10%, S in an amount less than 0.10%, N in an amount less than 0.10%, Ti in the amount of 0.020-0.150%, inclusive, and B in the amount of 0.002-0.010%, inclusive, and optionally contains Al, Cr, Mo, Co, Ni, Cu, V, W, Ca, Mg and rare earth metals, with the remainder being Fe and impurities; a microstructure which has martensite in an amount no less than 85% and residual austenite in an amount less than 15% as a volume percentage; and a standard deviation in the frequency distribution of nanohardness in the microstructure of no more than 0.70 GPa and an average crystalline particle diameter in said microstructure of no more than 4.0μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hot stamped product. This application claims priority based on Japanese Patent Application No. 2021-019911, filed on February 10, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] In recent years, in order to protect the environment and prevent global warming, there has been a demand to reduce the consumption of chemical fuels. For example, automobiles, which are indispensable in daily life and activities as a means of transportation, are no exception to this demand. In response to this demand, improvements in fuel efficiency, such as by reducing the weight of the automobile body, have been considered for automobiles. Since most automobile structures are formed of iron, particularly steel plates, reducing the weight of the steel plates by making them thinner is highly effective in reducing the weight of the automobile body. However, there is a concern that simply reducing the thickness of the steel plates to reduce the weight of the steel plates will reduce the strength of the structure and reduce safety. Therefore, in order to reduce the thickness of the steel plates, it is necessary to increase the mechanical strength of the steel plates used so as not to reduce the strength of the structure. Therefore, research and development is being conducted on steel sheets that can maintain or increase their mechanical strength even when made thinner than previously used steel sheets by increasing their mechanical strength. Such steel sheets are required not only in the automobile manufacturing industry but also in various other manufacturing industries.

[0003] Generally, materials with high mechanical strength tend to have low shape fixability in forming processes such as bending, and when they are processed into complex shapes, the processing itself becomes difficult. One of the means for solving the problem of formability is the so-called "hot stamping method." In this hot stamping method, the material to be formed is once heated to a high temperature, and the material softened by heating is pressed to form it, and then, or simultaneously with forming, the material is rapidly cooled by utilizing heat extraction by contact with a press die.

[0004] According to the hot stamping method, the material is first heated to a high temperature to soften it, and then pressed in the softened state, so that the material can be easily pressed. Therefore, this hot press processing can produce a press-formed product (hot stamped product) that has both good shape fixability and high mechanical strength. In particular, when the material is steel, the mechanical strength of the press-formed product can be increased by the quenching effect caused by cooling after forming.

[0005] For example, Patent Document 1 describes that a member having a tensile strength of 1400 MPa or more can be obtained by hot stamping a steel sheet having a tensile strength of 500 to 600 MPa.

[0006] Patent Document 2 discloses a high-strength, high-toughness steel plate member in which the grain size of martensite is refined by controlling the Mn content or the total content of Mn and at least one of Cr, Mo, Cu, and Ni, and performing press working to form the steel plate member into a predetermined shape one or more times during the cooling process before the Ms point is reached.

[0007] Because the members described in Patent Documents 1 and 2 have high strength, they are often used as deformation prevention members for protecting occupants in the event of a collision, such as door impact beams and center pillar uppers in automobiles. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Publication No. 2002-102980 [Patent Document 2] Japanese Patent Publication No. 2010-070806 Summary of the Invention [Problem to be solved by the invention]

[0009] However, in recent years, with the increasing demand for automobile safety, there is a demand for materials used in automobile parts to have better crashworthiness (shock absorption properties). Specifically, from the viewpoint of preventing cracking of components during a collision, there is a demand for components to have excellent bendability. As a result of investigations carried out by the present inventors, it has been found that conventional hot stamped steel sheets (members) may not be able to meet the recent demand for higher bendability.

[0010] The present invention has been made in view of the above. An object of the present invention is to provide a hot stamped steel sheet having high strength and excellent bendability. [Means for solving the problem]

[0011] The present inventors have investigated a method for improving the bendability of a high-strength hot stamped steel, and have found that high strength and excellent bendability can be obtained by making the microstructure of the hot stamped steel mainly martensite, reducing the hardness variation in the microstructure, and reducing the grain size. They also found that in order to obtain the above structure, the forming temperature during hot stamping and the amount of strain introduced are important.

[0012] The present invention has been made in view of the above findings. [1] A hot stamped steel according to one embodiment of the present invention has a chemical composition, in mass%, of C: 0.15% or more and 0.50% or less, Si: 0.10% or more and 3.00% or less, Mn: 0.10% or more and 3.00% or less, P: less than 0.10%, S: less than 0.10%, N: less than 0.10%, Ti: 0.020% or more and 0.150% or less, B: 0.002% or more and 0.010% or less, Al: 0% or more and 2.0% or less, Nb: 0% or more and 0.150% or less, Cr: 0% or more and 1.0% or less, Mo: 0% or more and 1.0% or less, Co: 0% or more and 2.0% or less, and Ni: 0% or less. a microstructure having, by volume fraction, 85% or more of martensite and less than 15% of retained austenite, and a standard deviation of a frequency distribution of nano-hardness in the microstructure is 0.70 GPa or less and an average crystal grain size is 4.0 μm or less. [2] The hot stamped steel according to [1] above may have a chemical composition, in mass%, of one or more selected from the group consisting of Al: 0.0002% or more and 2.0% or less, Nb: 0.010% or more and 0.150% or less, Cr: 0.1% or more and 1.0% or less, Mo: 0.1% or more and 1.0% or less, Co: 0.1% or more and 2.0% or less, Ni: 0.1% or more and 3.0% or less, Cu: 0.1% or more and 1.0% or less, V: 0.1% or more and 1.0% or less, W: 0.1% or more and 1.0% or less, Ca: 0.0010% or more and 0.0100% or less, Mg: 0.0010% or more and 0.0100% or less, and REM: 0.0010% or more and 0.0100% or less. [3] The hot stamped steel according to the above item [1] or [2] may have an alloy layer on its surface. Effect of the Invention

[0013] According to the above-described aspect of the present invention, it is possible to provide a hot stamped steel sheet having high strength and excellent bendability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, a hot-stamped steel according to one embodiment of the present invention (a hot-stamped steel according to this embodiment) will be described. The hot stamped body according to this embodiment has a predetermined chemical composition and a microstructure having, by volume fraction, 85% or more of martensite and less than 15% of retained austenite, in which the standard deviation of the frequency distribution of nano-hardness is 0.70 GPa or less and the average crystal grain size is 4.0 μm or less.

[0015] <Chemical composition> The chemical composition of the hot stamped steel according to this embodiment will be described. Unless otherwise specified, "%" indicating the content of each element in the chemical composition is mass%.

[0016] C: 0.15% or more, 0.50% or less C is an important element for obtaining the tensile strength required for automobile parts and the like in hot stamped bodies. If the C content is less than 0.15%, the martensite is soft and it is difficult to obtain sufficient tensile strength. Therefore, the C content is set to 0.15% or more. The C content is preferably 0.30% or more, more preferably 0.40% or more. On the other hand, if the C content exceeds 0.50%, coarse carbides are formed in the steel, and the toughness of the hot stamped body decreases. Therefore, the C content is set to 0.50% or less. The C content is preferably 0.48% or less.

[0017] Si: 0.10% or more, 3.00% or less Silicon is an element that is effective in improving the hardenability of steel and in stably ensuring strength after hardening. To obtain this effect, the silicon content must be 0.10% or more. The silicon content is preferably 0.35% or more. On the other hand, if the Si content exceeds 3.00%, the heating temperature required for austenite transformation during hot stamping becomes significantly high. This may lead to an increase in the cost required for heat treatment. Furthermore, if the Si content exceeds 3.00%, the toughness of the quenched part deteriorates. Therefore, the Si content is set to 3.00% or less. The Si content is preferably 2.60% or less.

[0018] Mn: 0.10% or more, 3.00% or less Mn is an extremely effective element for improving the hardenability of steel and stably ensuring strength after hardening. Mn also lowers the Ac3 point and promotes lowering the hardening temperature. If the Mn content is less than 0.10%, these effects are insufficient, so the Mn content is set to 0.10% or more. The Mn content is preferably 0.30% or more. On the other hand, if the Mn content exceeds 3.00%, the above effects are saturated and the toughness and bendability of the hardened portion deteriorate. Therefore, the Mn content is set to 3.00% or less. The Mn content is preferably 2.80% or less, and more preferably 2.50% or less.

[0019] P: Less than 0.10% P is an element that segregates at grain boundaries and reduces the strength of the grain boundaries. If the P content is 0.10% or more, the strength of the grain boundaries is significantly reduced, and the bendability of the hot stamped body is reduced. Therefore, the P content is less than 0.10%. The P content is preferably 0.05% or less. There is no particular lower limit for the P content, but if it is reduced to less than 0.0001%, the de-P cost increases significantly, which is economically undesirable. Therefore, for practical steel sheets, 0.0001% is the substantial lower limit.

[0020] S: Less than 0.10% S is an element that forms inclusions in steel. If the S content is 0.10% or more, inclusions are formed in the steel, and the bendability of the hot stamped body is reduced. Therefore, the S content is less than 0.10%. The S content is preferably 0.02% or less, and more preferably 0.01% or less. There is no particular lower limit for the S content, but if it is reduced to less than 0.0010%, the cost of desulfurization increases significantly, which is economically undesirable. Therefore, for practical steel sheets, 0.0010% is the substantial lower limit.

[0021] N: Less than 0.10% N is an element that forms nitrides and reduces the bendability of hot stamped steel. If the N content is 0.10% or more, coarse nitrides are formed in the steel, and the bendability of the hot stamped steel is significantly reduced. Therefore, the N content is less than 0.10%. The N content is preferably 0.01% or less, 0.0075% or less, or 0.0030% or less. There is no particular lower limit for the N content, but if it is reduced to less than 0.0001%, the cost of denitrification increases significantly, which is economically undesirable. Therefore, 0.0001% is the substantial lower limit for practical steel sheets.

[0022] Ti: 0.020% or more, 0.150% or less Ti is an element that improves the strength of hot stamped steel by solid solution strengthening. Ti also improves the toughness of hot stamped steel by suppressing the coarsening of austenite grains during the heating process. If the Ti content is less than 0.020%, these effects are insufficient. Therefore, the Ti content is set to 0.020% or more. On the other hand, if the Ti content exceeds 0.150%, TiN, which becomes the starting point of bending cracks, is formed, and the bendability of the hot stamped steel deteriorates. Therefore, the Ti content is set to 0.150% or less. The Ti content is preferably 0.120% or less.

[0023] B: 0.002% or more, 0.010% or less B is an element that segregates at grain boundaries to improve the strength of the grain boundaries. B is also an extremely effective element for improving the hardenability of steel and stably ensuring the strength after hardening. If the B content is less than 0.002%, these effects are insufficient. Therefore, the B content is set to 0.002% or more. On the other hand, if the B content exceeds 0.010%, coarse BN, which becomes the starting point of bending cracks, is formed, and the bendability of the hot stamped steel deteriorates. Therefore, the B content is set to 0.010% or less. The B content is preferably 0.008% or less.

[0024] In the chemical composition of the hot stamped steel according to the present embodiment, other than the above elements, that is, the balance may be Fe and impurities. Alternatively, in order to improve various properties, one or more elements selected from the group consisting of Al, Nb, Cr, Mo, Co, Ni, Cu, V, W, Ca, Mg, and REM may be further contained within the ranges shown below. These elements are optional elements and do not necessarily need to be contained, so the lower limit is 0%. Here, the term "impurities" refers to components that are mixed in from raw materials such as ores and scraps or due to various factors in the manufacturing process when industrially producing a steel sheet, and that are permissible within a range that does not adversely affect the characteristics of the hot stamped steel according to the present embodiment.

[0025] Al: 0% or more, 2.0% or less Al is an element that has the effect of deoxidizing molten steel and improving the quality of the steel (suppressing the occurrence of defects such as blowholes in the steel). When Al is contained, in order to obtain a sufficient effect, the Al content is preferably 0.0002% or more. The Al content is more preferably 0.001% or more, and further preferably 0.010% or more. On the other hand, if the Al content exceeds 2.0%, coarse oxides are generated and the toughness of the hot stamped steel is impaired, so the Al content is set to 2.0% or less.

[0026] Nb: 0% or more, 0.150% or less Nb is an element that contributes to improving the strength of the hot stamped body by solid solution strengthening, and may be contained as necessary. When Nb is contained, in order to obtain a sufficient effect, the Nb content is preferably 0.010% or more. The Nb content is more preferably 0.030% or more. On the other hand, if the Nb content exceeds 0.150%, the above effect saturates. Therefore, the Nb content is set to 0.150% or less. The Nb content is preferably 0.120% or less.

[0027] Cr: 0% or more, 1.0% or less Cr is an element that contributes to improving the strength of the hot stamped body by solid solution strengthening, and may be contained as necessary. When Cr is contained, in order to obtain a sufficient effect, the Cr content is preferably 0.1% or more. The Cr content is more preferably 0.2% or more. On the other hand, if the Cr content exceeds 1.0%, the above effects are saturated and the economic efficiency decreases. Therefore, the Cr content is set to 1.0% or less. The Cr content is preferably 0.8% or less.

[0028] Mo: 0% or more, 1.0% or less Mo is an element that contributes to improving the strength of hot stamped steel by solid solution strengthening. Therefore, it may be contained as necessary. When Mo is contained, in order to obtain a sufficient effect, the Mo content is preferably 0.1% or more. The Mo content is more preferably 0.2% or more. On the other hand, if the Mo content exceeds 1.0%, the above effects are saturated and the economic efficiency decreases. Therefore, the Mo content is set to 1.0% or less. The Mo content is preferably 0.8% or less.

[0029] Co: 0% or more, 2.0% or less Co is an element effective for improving the hardenability of steel and stably ensuring the strength of the steel after hardening, and may be contained as necessary. When Co is contained, in order to obtain a sufficient effect, the Co content is preferably 0.1% or more. The Co content is more preferably 0.2% or more. On the other hand, if the Co content exceeds 2.0%, the above effects become saturated and the economic efficiency decreases. Therefore, the Co content is set to 2.0% or less.

[0030] Ni: 0% or more, 3.0% or less Ni is an element effective for improving the hardenability of steel and stably ensuring the strength of the steel after hardening, and may be contained as necessary. When Ni is contained, in order to obtain a sufficient effect, the Ni content is preferably 0.1% or more. The Ni content is more preferably 0.2% or more. On the other hand, if the Ni content exceeds 3.0%, the above effects become saturated and the economic efficiency decreases. Therefore, the Ni content is set to 3.0% or less.

[0031] Cu: 0% or more, 1.0% or less Cu is an element that contributes to improving the strength of the hot stamped body by solid solution strengthening, and may be contained as necessary. When Cu is contained, in order to obtain a sufficient effect, the Cu content is preferably 0.1% or more. The Cu content is more preferably 0.2% or more. On the other hand, if the Cu content exceeds 1.0%, the above effects are saturated and the economic efficiency decreases. Therefore, the Cu content is set to 1.0% or less. The Cu content is preferably 0.8% or less.

[0032] V: 0% or more, 1.0% or less V is an element that contributes to improving the strength of the hot stamped body by solid solution strengthening, and may be contained as necessary. When V is contained, in order to obtain a sufficient effect, the V content is preferably 0.1% or more. The V content is more preferably 0.2% or more. On the other hand, if the V content exceeds 1.0%, the above effects are saturated and the economic efficiency decreases. Therefore, the V content is set to 1.0% or less. The V content is preferably 0.8% or less.

[0033] W: 0% or more, 1.0% or less W is an element that has the effect of deoxidizing molten steel and improving the soundness of the steel, and may be contained as necessary. When W is contained, the W content is preferably 0.1% or more in order to obtain a sufficient effect. On the other hand, if the W content exceeds 1.0%, the above effects become saturated and the economic efficiency decreases. Therefore, the W content is set to 1.0% or less.

[0034] Ca: 0% or more, 0.0100% or less Ca is an element that has the effect of deoxidizing molten steel to improve the soundness of the steel, and may be added as necessary to improve the bendability of the hot stamped steel. In order to obtain the above effect, the Ca content is preferably 0.0010% or more. On the other hand, if the Ca content exceeds 0.0100%, the above effects are saturated and the cost increases. Therefore, the Ca content is set to 0.0100% or less. The Ca content is preferably 0.0080% or less.

[0035] Mg: 0% or more, 0.0100% or less Mg is an element that has the effect of deoxidizing molten steel to improve the soundness of the steel, and may be added as necessary to improve the bendability of the hot stamped steel. In order to obtain the above effect, the Mg content is preferably 0.0010% or more. On the other hand, if the Mg content exceeds 0.0100%, the above effects are saturated and the cost increases, so the Mg content is set to 0.0100% or less, and preferably 0.0080% or less.

[0036] REM: 0% or more, 0.0100% or less REM is an element that has the effect of deoxidizing molten steel to improve the soundness of the steel, and may be added as necessary to improve the bendability of the hot stamped steel. In order to obtain the above effect, the REM content is preferably 0.0010% or more. On the other hand, if the REM content exceeds 0.0100%, the above effects are saturated and the cost increases, so the REM content is set to 0.0100% or less, preferably 0.0080% or less. In this embodiment, REM refers to a total of 17 elements consisting of Sc, Y, and lanthanoids. In this embodiment, the content of REM refers to the total content of these elements. In the case of lanthanoids, they are industrially added in the form of misch metal.

[0037] The chemical composition of the hot stamped body may be measured by a general analytical method. For example, it may be measured by ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). C and S may be measured by a combustion-infrared absorption method, and N may be measured by an inert gas fusion-thermal conductivity method.

[0038] Next, the metal structure of the hot stamped steel according to this embodiment will be described. <Microstructure (metal structure)> [Contains 85% or more martensite and less than 15% retained austenite by volume fraction] Martensite is an important structure for increasing the tensile strength of a hot stamped body (steel sheet after hot stamping). If the volume fraction of martensite is less than 85%, sufficient strength (tensile strength) cannot be obtained. Therefore, the volume fraction of martensite is set to 85% or more. The preferred volume fraction of martensite is 90% or more, or 95% or more. The upper limit of the volume fraction of martensite does not need to be particularly set and may be 100%, but in order to greatly increase the volume fraction of martensite, it is necessary to increase the heating temperature of the steel sheet or the cooling rate in the hot stamping process, which may impair the productivity of hot stamped products. Therefore, the volume fraction of martensite may be 99% or less, or 98% or less. In this embodiment, martensite includes tempered martensite and fresh martensite. The remainder other than the martensite may contain less than 15% retained austenite. The retained austenite has the effect of improving the ductility of the hot stamped body. Therefore, the volume fraction of the retained austenite may be 1% or more, or 2% or more. In addition to the martensite and the retained austenite, bainite may be contained as long as its volume fraction is 10% or less. It is preferable that ferrite and pearlite are not contained.

[0039] The volume fraction of each phase is determined by the following method. First, a sample is taken from a position that avoids the end of the hot stamped product (for example, a position 50 mm or more away from the end face) so that the plate thickness cross section can be observed. The area of ​​the observation surface of the sample that is 1 / 4 of the plate thickness (1 / 4 thickness) from the surface of the steel plate is measured with a 4.0×10 -4 m 2 The above area is chemically polished. The polished surface is then subjected to an X-ray diffraction (XRD) to calculate the retained austenite fraction. For the measurement, a Co tube is used as the X-ray source, and the (100), (200), and (211) peaks of the bcc phase and the (111), (200), and (220) peaks of the fcc phase are used as the plane indices. In addition, samples were taken from a position that avoided the end of the hot stamped product (for example, a position 50 mm or more away from the end face) so that the plate thickness cross section could be observed. The observation surface of the sample was mechanically polished to a mirror finish, and then subjected to nital etching. A total of 2.0 × 10 -9 m 2A scanning electron microscope is used to observe secondary electron images of the above areas. As a result of the observation, areas that have a substructure within the grains and where cementite precipitates with multiple variants are judged to be tempered martensite. Areas that are bright and where the substructure is not revealed by etching are judged to be fresh martensite or retained austenite. The martensite fraction (the sum of the tempered martensite fraction and the fresh martensite fraction) is measured by subtracting the retained austenite fraction obtained by XRD measurement from the fractions of the areas judged to be tempered martensite, fresh martensite, or retained austenite. In addition, as a result of observing secondary electron images, regions that have a substructure within the grains and in which cementite precipitates with the same variant are defined as bainite, and among the regions that do not have a substructure within the grains, regions that do not contain carbides are defined as ferrite, and regions that contain carbides are defined as pearlite.

[0040] [Standard deviation of nano hardness frequency distribution is 0.70 GPa or less] [Average grain size is 4.0 μm or less] The present inventors have investigated a method for improving the bendability of a high-strength hot stamped steel. In this embodiment, the strength-bend angle balance calculated by TS×α is used as an index of bendability, using the bend angle (α) and tensile strength (TS) obtained in a plate bending test (VDA test) for the purpose of evaluating the crack behavior when a component is crushed. As a result of the inventors' investigations, it was found that high strength and excellent bendability can be obtained by reducing the variation in hardness in the microstructure and by reducing the grain size. Specifically, it was found that an excellent balance between strength and bending angle can be obtained if the standard deviation of the frequency distribution of nanohardness obtained by performing a nanoindentation test in a region centered on a position 1 / 4 of the plate thickness (1 / 4 thickness) from the surface is 0.70 GPa or less and further the average crystal grain size is 4.0 μm or less. The reason why the strength-bending angle balance is improved by reducing the standard deviation of the nanohardness frequency distribution and the average crystal grain size is thought to be because reducing the variation in hardness within the microstructure makes it possible to suppress the generation of voids that are the starting point of ductile fracture, and by reducing the average crystal grain size, it is possible to suppress the progression of ductile fracture cracks. If the standard deviation of the frequency distribution of nano-hardness exceeds 0.70 GPa or the average crystal grain size exceeds 4.0 μm, a sufficient strength-bending angle balance cannot be obtained.

[0041] The grain size in this embodiment refers to the circle-equivalent diameter of a crystal grain when the boundary of the bcc phase, which has an orientation difference of 5° or more with the adjacent measurement area, is defined as a grain boundary, and the area surrounded by the grain boundary is defined as a crystal grain. The hot stamped steel according to this embodiment has a structure mainly composed of martensite. The martensite structure has a hierarchical structure in which one prior austenite grain is formed from a plurality of packets, one packet is formed from a plurality of blocks, and one block is formed from a plurality of laths. The orientation difference between adjacent laths is less than 5°, and the orientation difference between adjacent blocks is 5° or more. Therefore, the average grain size in this embodiment corresponds to measuring the average block diameter of martensite.

[0042] The standard deviation of the frequency distribution of nanohardness and the average grain size may be satisfied in at least a part of the hot stamped body. In particular, it is preferable that the standard deviation of the frequency distribution of nanohardness and the average grain size are within the above ranges in the microstructure of a region that is subjected to severe deformation upon collision when used as an automobile part.

[0043] The standard deviation of the frequency distribution of nanohardness is determined by conducting a nanoindentation test in the following manner. A sample is taken from the hot stamped body so that a cross section perpendicular to the plate width direction (L cross section) can be observed. An area of ​​this sample, centered at a position 1 / 4 of the plate thickness from the surface in the plate thickness direction (1 / 4 thickness part), and 150 μm in width in the plate thickness direction and 600 μm or more in width in the rolling direction, is electrolytically polished. Then, the area is indented with a Berkovich indenter at 30 μm intervals at a total of 100 points (5 points in the plate thickness direction × 20 points in the rolling direction) with an indentation load of 2000 μN to measure the nanohardness at each point. The frequency distribution of the obtained nanohardness is obtained, and the standard deviation is calculated.

[0044] In this embodiment, the nanohardness is the hardness of a microscopic region measured by indenting a Berkovich indenter with a load of 2000 μN, as described above. If measured by a normal Vickers hardness test (for example, a load of 1 kgf), the indentation becomes large and the hardness of the microscopic region cannot be evaluated. Therefore, even if a material has a small variation in hardness in a Vickers hardness test, it cannot be said that the standard deviation of the frequency distribution of the nanohardness evaluated in this embodiment is 0.70 GPa or less.

[0045] The average crystal grain size is measured by the following method using the EBSD method. A sample is taken from the hot stamped body so that a cross section (L cross section) perpendicular to the sheet width direction can be observed. A region of this sample, centered at a position (1 / 4 thickness part) of 1 / 4 of the sheet thickness from the surface in the sheet thickness direction, and 240 μm in the sheet thickness direction and 80 μm or more in the rolling direction, is electrolytically polished. Then, EBSD measurement is performed on the region at an acceleration voltage of 20 kV, an irradiation current of 18 mA, and a measurement pitch of 0.4 μm intervals, and analysis is performed using OIM Analysis (registered trademark). A boundary with an orientation difference of 5° or more with an adjacent measurement region is defined as a grain boundary, and the area surrounded by the grain boundary is defined as a crystal grain, and the circle equivalent diameter of the crystal grain is defined as the crystal grain size. The average crystal grain size is defined as the average crystal grain size. However, in this embodiment, the average crystal grain size is calculated only for grains having a bcc structure, and grains with an area of ​​less than 2 pixels are excluded from the grain size measurement.

[0046] [Mechanical properties] The hot stamped steel according to this embodiment has high strength and excellent bendability. For example, it is preferable that the tensile strength (TS) is 980 MPa or more and the strength-bending angle balance (TS×α) is 85,000 MPa·deg or more.

[0047] <Manufacturing method> The hot stamped steel according to the present embodiment can obtain the above-mentioned effects regardless of the manufacturing method. However, a manufacturing method including the steps described below is preferable because it can be stably manufactured. (I) a heating step of heating the steel sheet to the Ac3 point or higher; (II) A forming process in which the heated steel sheet is formed (processed) in a temperature range above the Ms point so that the amount of strain between the Ms point and Ms point + 100°C is 10% or more while preventing the precipitation of ferrite or pearlite. Each step will be described below. For steps or conditions that are not described, known conditions can be applied.

[0048] [Heating process] In the heating step, the steel sheet to be subjected to hot stamping is heated to a temperature of the Ac3 point or higher. If the heating temperature is lower than the Ac3 point, the microstructure does not transform into austenite, and a sufficient volume fraction of martensite cannot be obtained after hot stamping. After heating to the Ac3 point or higher, it is preferable to hold the temperature for 3 minutes or longer so that the structure is completely transformed into austenite. The Ac3 point (°C) can be calculated using the following formula. Ac3(℃)=910-203×[%C] 0.5 +66×[%Si]-25×[%Mn]+700×[%P]-11×[%Cr]+109×[%Al]+400×[%Ti]-15.2×[%Ni]+104×[%V]+31.5×[%Mo] Here, [% element] is the content (mass%) of each element. There is no need to limit the upper limit of the heating temperature, but it is preferable that the temperature be 1100° C. or lower.

[0049] Since the chemical composition does not substantially change due to hot stamping (heating process + forming process), the chemical composition of the steel sheet subjected to the heating process is made the same as the chemical composition of the hot stamped body to be obtained. The steel sheet is not limited in terms of structure, etc., other than the chemical composition. For example, the steel sheet may be a hot-rolled steel sheet as specified in JIS G3113:2018, a cold-rolled steel sheet as specified in JIS G3135:2018, or a steel sheet as specified in JIS G3135:2018. Hot-dip galvanized steel sheets described in JIS G3302:2019, hot-dip aluminum-plated steel sheets described in JIS G3314:2019, hot-dip zinc-5% aluminum alloy-plated steel sheets described in JIS G3317:2019, hot-dip 55% aluminum-zinc alloy-plated steel sheets described in JIS G3321:2019, and the like can be used.

[0050] [Molding process] In the forming process, the heated steel plate is cooled and formed as follows. In the manufacturing method of the hot stamped steel according to the present embodiment, in the cooling of the hot stamp, plastic deformation is performed in the supercooled austenite region, dislocations are introduced into the supercooled austenite, and the number of martensite nucleation sites is increased, so that the martensite finally obtained is homogenized (the standard deviation of nano-hardness is reduced) and refined (the average crystal grain size is reduced). In order to introduce dislocations into the supercooled austenite and obtain a sufficient number of martensite nucleation sites, the heated steel sheet is cooled and formed as in 1) or 2) below. 1) While cooling to a temperature range below the Mf point at a cooling rate equal to or higher than the upper critical cooling rate, forming is performed so that the amount of plastic strain between the Ms point and Ms point + 100°C is 10% or more. 2) Cool at a rate equal to or higher than the upper critical cooling rate, interrupt the cooling at least once, and form the material so that the plastic strain between the Ms point and Ms point + 100°C is 10% or more. Then, cool further at a rate equal to or higher than the upper critical cooling rate to a temperature range below the Mf point.

[0051] In either case of 1) or 2), the cooling rate is always equal to or higher than the upper critical cooling rate. The upper critical cooling rate is the minimum cooling rate at which ferrite and pearlite are not precipitated in the structure and austenite is supercooled to form martensite. If the material is cooled at a rate lower than the upper critical cooling rate, ferrite and pearlite are formed and the strength of the hot stamped body is insufficient. Cooling may be performed by water cooling or by sandwiching the material between dies and cooling by extracting heat from the dies. Furthermore, if the cooling stop temperature is higher than the Mf point, a sufficient volume fraction of martensite cannot be obtained, so the cooling stop temperature is set to the Mf point or lower.

[0052] In both cases 1) and 2), forming may be performed in a temperature range above Ms point + 100°C, provided that the amount of plastic strain is 10% or more between Ms point and Ms point + 100°C. In other words, after forming in a temperature range above Ms point + 100°C, forming may be performed again in a temperature range from Ms to Ms point + 100°C so that the plastic strain is 10% or more. If forming is performed while cooling, cooling may be started from a temperature range above Ms + 100°C and forming may be completed so that the plastic strain is 10% or more in the temperature range from Ms to Ms + 100°C. However, the forming end temperature (for example, when the die reaches the bottom dead center in the case of press forming) (the final forming end temperature when performing multiple times) must be above Ms point. If forming is performed at a temperature below Ms point, forming will be performed on martensite that has been transformed, and the residual ductility of the hot stamped body will decrease, resulting in a decrease in bendability. If the plastic strain from the Ms point to Ms point + 100° C. is less than 10%, the martensite will not be homogenized or refined sufficiently. The amount of plastic strain between the Ms point and Ms point + 100°C is limited because, when forming is performed in a temperature range above Ms + 100°C, the dislocations introduced by forming are partially or completely recovered and disappear. If only some of the dislocations are recovered, the grain size distribution becomes non-uniform, and non-uniform deformation occurs during bending deformation, which may reduce bendability. Furthermore, if all of the dislocations are recovered, fine crystal grains cannot be obtained.

[0053] As described above, if the amount of plastic strain between the Ms point and Ms point + 100°C is 10% or more, the effect of homogenizing and refining martensite can be obtained even if forming is performed in a temperature range of Ms point + 100°C or higher. However, since forming in a temperature range of Ms point + 100°C or higher may cause the grain size to become non-uniform, from the viewpoint of bendability, it is preferable to only perform forming in the temperature range of Ms point to Ms point + 100°C. In this embodiment, the plastic strain is the strain on the bent outer surface, which can be calculated from the bending radius R and the plate thickness t by t / (2R+t)×100.

[0054] In the case of 2), the time for which cooling is interrupted (the time when cooling does not exceed the upper critical cooling rate) must be shorter than the time to reach the ferrite transformation start line Fs or the bainite transformation start line Bs on the time temperature transformation (TTT) curve. If the interruption time is long and exceeds Fs or Bs, ferrite, pearlite, etc. will be generated and the desired structure will not be obtained.

[0055] Applying surface pressure during molding increases the martensite transformation completion temperature (Mf point), resulting in an automatic tempering effect. In this case, the standard deviation of the nano-hardness distribution decreases, so applying surface pressure during molding is a more preferable manufacturing condition. When applying surface pressure, the surface pressure is preferably 10 MPa or more, more preferably 20 MPa or more, and even more preferably 30 MPa or more.

[0056] The upper critical cooling rate Vc (℃ / sec), Ms point (℃), and Mf point (℃) are calculated by the following formula. The following formula is used to calculate the Mf point when the surface pressure is 0 MPa, and when surface pressure is applied, the Mf point increases beyond the temperature calculated by the following formula. log10(Vc)=2.94-0.75(2.7×[%C]+0.4×[%Si]+1.0×[%Mn]+0.45×[%Ni]+0.8Cr+2×[%Mo]) In the hot stamped steel according to this embodiment, the B content is 0.002% or more. When the B content is less than 0.002%, the upper critical cooling rate Vc (° C. / sec) is calculated by the following formula. log10(Vc)=2.94-0.75(2.7×[%C]+0.4×[%Si]+1.0×[%Mn]+0.45×[%Ni]+0.8Cr+2×[%Mo]-1) Ms(℃)=560.5-407.3×[%C]-7.3×[%Si]-37.8×[%Mn]-19.5×[%Ni]-19.8×[%Cr]-4.5×[%Mo]-20.5×[%Cu] Mf(℃)=Ms-209 Here, [% element] in the formula is the content of the element in steel in mass %.

[0057] In the hot stamped steel according to this embodiment, an alloy layer may be formed on the surface (one side or both sides). The alloy layer is not limited, and may be, for example, an Fe-Al alloy layer or an Fe-Zn alloy layer. The Fe-Al alloy layer is an alloy layer containing Fe and Al in a total of 70 mass% or more, and the Fe-Zn alloy layer is an alloy layer containing Fe and Zn in a total of 70 mass% or more. The presence of the alloy layer improves corrosion resistance. The thickness of the alloy layer is preferably 10 to 100 μm. The alloy layer is formed by hot stamping a steel sheet having a plating layer (a Zn-based plating layer, an Al-based plating layer, or the like) so that the plating layer is alloyed with Fe in the steel sheet. EXAMPLES

[0058] Steel sheets having the chemical compositions shown in Tables 1A and 1B and a thickness of 0.8 to 4.0 mm were prepared. Some of the steel sheets were subjected to galvannealing. This steel sheet was subjected to hot stamping (heating, cooling, forming) under the conditions shown in Tables 2A to 2D to obtain a hot stamped product. The following patterns were adopted for hot stamping: 1) Cooling at a rate equal to or higher than the upper critical cooling rate to a temperature range below the Mf point, while forming so that the amount of plastic strain from the Ms point to Ms point + 100°C is 10% or more; or 2) Cooling at a rate equal to or higher than the upper critical cooling rate, interrupting the cooling once or more to form so that the amount of plastic strain from the Ms point to Ms point + 100°C is 10% or more, and then further cooling at a rate equal to or higher than the upper critical cooling rate to a temperature range below the Mf point. For example, in the table, compact No. 1 was heated to 910°C and then cooled at a rate of 60°C / sec or more. The graph shows that the molded product was cooled to 25°C, and molding was performed at 430°C during the process. In addition, for molded product No. 2, the molded product was heated to 910°C, then cooled to 430°C at a cooling rate of 60°C / sec or more, the cooling was once interrupted, molding was performed at that temperature, and after molding, the molded product was cooled to 25°C at a cooling rate of 60°C / sec or more. In addition, for molded product No. 3, the molded product was heated to 910°C, then cooled to 580°C at a cooling rate of 60°C / sec or more, the cooling was once interrupted, molding was performed at that temperature (first time), after molding, cooling was performed to 430°C at a cooling rate of 50°C / sec or more, the cooling was once interrupted, molding was performed at that temperature (second time), and after molding, cooling was performed to 25°C at a cooling rate of 50°C / sec or more. When cooling was interrupted, the interruption time was about 10 to 30 seconds in all cases.

[0059] [Table 1A]

[0060] [Table 1B]

[0061] [Table 2A]

[0062] [Table 2B]

[0063]

Table 2C

[0064]

Table 2D

[0065] For this hot-stamped molded body, the volume fraction of each phase in the microstructure, the standard deviation of the frequency distribution of the nano-hardness, and the average crystal grain size were measured by the method described above. When there was an alloy layer (Fe-Zn alloy layer), the thickness of the alloy layer was measured. The results are shown in Table 3A and Table 3B.

[0066] Also, the tensile strength TS (MPa) and the bending angle α (°) were obtained in the following manner. The results are shown in Table 3C and Table 3D.

[0067] <Tensile test> For the tensile test, a test piece with a JIS No. 5 shape was taken from a flat part of the hot-stamped molded body such that the direction perpendicular to the rolling direction became the longitudinal direction of the tensile test piece, and the test was carried out in accordance with JIS Z2241:2011.

[0068] <VDA bending test> For the VDA bending test, a 60 mm square test piece was cut out from a flat part of the hot-stamped molded body such that the rolling direction became parallel to the bending ridge line, and the test was carried out in accordance with the VDA 238-100 standard.

[0069]

Table 3A

[0070]

Table 3B

[0071]

Table 3C

[0072] [Table 3D]

[0073] As can be seen from the results in Tables 1A to 3D, in the examples of the invention, the chemical composition and microstructure (volume fraction of each phase, standard deviation of the frequency distribution of nanohardness, and average crystal grain size) were within the range of the present invention, and as a result, high strength and excellent bendability were obtained. In contrast, in the comparative examples, the chemical composition was outside the range of the present invention or the manufacturing method was unfavorable, so that the desired microstructure was not obtained, and as a result, at least one of strength and bendability was inferior. [Industrial Applicability]

[0074] According to the present invention, a hot stamped steel having high strength and excellent bendability can be provided. This hot stamped steel contributes to improving the crashworthiness of automobiles, and therefore has high industrial applicability.

Claims

1. The chemical composition, in mass%, is C: 0.15% or more, 0.50% or less, Si: 0.10% or more, 3.00% or less, Mn: 0.10% or more, 3.00% or less, P: less than 0.10%; S: less than 0.10%, N: less than 0.10%; Ti: 0.020% or more, 0.150% or less, B: 0.002% or more, 0.010% or less, Al: 0% or more, 2.0% or less, Nb: 0% or more, 0.150% or less, Cr: 0% or more, 1.0% or less, Mo: 0% or more, 1.0% or less, Co: 0% or more, 2.0% or less, Ni: 0% or more, 3.0% or less, Cu: 0% or more, 1.0% or less, V: 0% or more, 1.0% or less, W: 0% or more, 1.0% or less, Ca: 0% or more, 0.0100% or less, Mg: 0% or more and 0.0100% or less, and REM: 0% or more and 0.0100% or less; The balance is Fe and impurities, The microstructure has, by volume fraction, 85% or more of martensite and less than 15% of retained austenite; In the microstructure, the standard deviation of the nano-hardness frequency distribution is 0.70 GPa or less, and the average crystal grain size is 4.0 μm or less. The hot stamped product is characterized by:

2. The chemical composition, in mass%, Al: 0.0002% or more, 2.0% or less, Nb: 0.010% or more, 0.150% or less, Cr: 0.1% or more, 1.0% or less, Mo: 0.1% or more, 1.0% or less, Co: 0.1% or more, 2.0% or less, Ni: 0.1% or more, 3.0% or less, Cu: 0.1% or more, 1.0% or less, V: 0.1% or more, 1.0% or less, W: 0.1% or more, 1.0% or less, Ca: 0.0010% or more, 0.0100% or less, Mg: 0.0010% or more and 0.0100% or less, and REM: 0.0010% or more, 0.0100% or less, Contains one or more selected from the group consisting of The hot stamped product according to claim 1 .

3. The hot stamped product according to claim 1 or 2, characterized in that the hot stamped product has an alloy layer on a surface thereof.

Citation Information

Patent Citations

  • Manufacturing method for collision reinforcing material for vehicle and collision reinforcing material

    JP2002102980A

  • Steel sheet member and production method therefor

    JP2010070806A

  • Hot press member having excellent ductility, steel sheet for the hot press member and method for producing the hot press member

    JP2010174281A

  • Hot press member and manufacturing method therefor

    JP2017179588A

  • Hot-pressed steel plate member and manufacturing method therefor

    WO2010032776A1