Conductive oligomer, conductive composition, conductive assistant, and capacitor electrode, transparent electrode, battery electrode, or capacitor electrode formed using the conductive composition
A conductive oligomer with controlled molecular weight and dopant introduction addresses solubility and conductivity issues in electrode materials, enabling efficient production of high-performance electrodes for in-vehicle electronic devices.
Patent Information
- Application Number
- JP2021527680
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-28
- Filing Date
- 2020-06-24
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-06-24
AI Technical Summary
Existing electrode materials for in-vehicle electronic devices face challenges in achieving high heat resistance, conductivity, and efficient production, particularly due to solubility issues with PEDOT/PSS.
Development of a conductive oligomer represented by specific general formulas with controlled molecular weight and structure, allowing for the introduction of dopants to enhance conductivity and solubility, resulting in a conductive composition with improved handling properties and productivity.
The conductive oligomer and composition exhibit excellent solubility, conductivity, and production efficiency, suitable for applications in electrodes requiring high conductivity and heat resistance, such as capacitor and battery electrodes.
Smart Images

Figure 0007583412000001 
Figure 0007583412000002 
Figure 0007583412000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive oligomer, a conductive composition, and the like. [Background technology]
[0002] In recent years, the shift to hybrid and electric vehicles and the associated progress in energy conservation have led to an increased demand for high heat resistance in on-board electronic devices. In particular, high heat resistance is required for drive system electrical components in order to reduce the load on the cooling systems around the engine and inverter. Many power storage devices are used in these drive system electrical components, so the electrode materials used in these components also require high heat resistance. Therefore, there is a need for electrode materials that are heat resistant and highly conductive, and can be efficiently produced, in order to meet these recent demands.
[0003] Conventionally, "PEDOT / PSS", in which poly(3,4-ethylenedioxythiophene) (also called PEDOT) is doped with polystyrene sulfonic acid (also called PSS) as a dopant, has been widely used in capacitor electrodes etc. Patent Document 1 discloses a fuel cell electrode containing a conductive polymer gel mainly composed of water and containing a conductive conjugated polymer, a surfactant and / or an alcohol, and PEDOT / PSS is used as the conductive conjugated polymer.
[0004] However, PEDOT / PSS may have poor solubility due to the use of PSS, and there are still issues in terms of production efficiency, etc. With recent technological advances, there is a strong demand for electrode materials that have excellent heat resistance and conductivity as well as being efficiently producible. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2005-166502 A Summary of the Invention
[0006] An object of the present invention is to provide a novel conductive oligomer, in particular a conductive oligomer which has excellent solubility and therefore excellent handleability and productivity, and which can be used to efficiently prepare conductive compositions and the like which also have excellent conductivity; to provide a conductive composition and a conductive assistant which are efficiently produced using the conductive oligomer and have excellent conductivity; and to provide a capacitor electrode, a transparent electrode, a battery electrode, and a capacitor electrode which are formed using the conductive composition and have excellent conductivity.
[0007] According to the present invention, the following conductive oligomers and the like are provided. 1. A conductive oligomer represented by the following general formula (1) or (1A): [ka] [In general formula (1) and (1A), R 1 and R 6 are each independently an alkyl group or an aryl group having 1 to 12 carbon atoms. n is an integer from 2 to 30. R 2 , R 3 , R 4 and R 5 are each independently a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. Multiple R 4 may be the same or different. Multiple R 5 may be the same or different. m is 1 or 2. X is S (sulfur atom), Se (selenium atom) or O (oxygen atom). A plurality of X's may be the same or different. Y is S (sulfur atom), Se (selenium atom), O (oxygen atom) or CR 7 R 8 where Y is CR 7 R 8 If R 1 and R6 are each independently a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. A plurality of Y's may be the same or different. R 7 and R 8 are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group. Z is H (hydrogen atom), F (fluorine atom), Cl (chlorine atom), Br (bromine atom), or I (iodine atom). Multiple Z's may be the same or different. 2. A conductive composition comprising the conductive oligomer according to 1, wherein a dopant is introduced into the conductive oligomer. 3. The dopant is BF4 - , ClO4 - , PF6 - , HSO4 - 3. The conductive composition according to claim 2, wherein the anion species is one or more selected from the group consisting of monovalent anion species of TCNQ or FxTCNQ (x is 2 or 4). 4. The conductive composition according to 2 or 3, wherein in said general formulas (1) and (1A), n is any single integer of 2 to 30. 5. The conductive composition according to any one of 2 to 4, containing 7 mol % or more (calculated as oligomer units) of a conductive oligomer. 6. Electrical conductivity is 1 x 10 -5 6. The conductive composition according to any one of 2 to 5, wherein the conductive composition has a viscosity of 1.5 S / cm or more. 7. A conductive assistant comprising the conductive composition according to any one of 2 to 6. 8. A capacitor electrode, a transparent electrode, a battery electrode, or a capacitor electrode formed using at least one of the conductive composition according to any one of 2 to 6 and the conductive assistant according to 7.
[0008] According to the present invention, there are provided a conductive oligomer that has excellent solubility and therefore excellent handleability and productivity, and that can efficiently produce a conductive composition and the like that has excellent conductivity; a conductive composition that is efficiently produced using the conductive oligomer and has excellent conductivity; a conductive assistant; and a capacitor electrode, a transparent electrode, a battery electrode, and a capacitor electrode that are formed using the conductive composition and have excellent conductivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The conductive oligomer of the present invention will now be described. In this specification, the term "oligomer" refers to a polymer having a relatively low molecular weight and containing 2 to about 30 molecules of the same type. [Conductive oligomer] In one embodiment of the present invention, the conductive oligomer is represented by the following general formula (1) or (1A).
[0010] [ka]
[0011] In the general formulas (1) and (1A), R 1 and R 6 are each independently an alkyl group or an aryl group having 1 to 12 carbon atoms. n is an integer from 2 to 30. R 2 , R 3 , R 4 and R 5 are each independently a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. Multiple R 4 may be the same or different. Multiple R 5 may be the same or different. m is 1 or 2. X is S (sulfur atom), Se (selenium atom), or O (oxygen atom). In one embodiment of the present invention, from the viewpoint of stability, X is preferably S (sulfur atom). A plurality of X's may be the same or different. Y is S (sulfur atom), Se (selenium atom), O (oxygen atom) or CR 7 R 8 where Y is CR 7 R 8 If R 1 and R 6 are each independently a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. A plurality of Y's may be the same or different. R 7 and R 8 are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group. Z is H (hydrogen atom), F (fluorine atom), Cl (chlorine atom), Br (bromine atom), or I (iodine atom). A plurality of Z's may be the same or different.
[0012] In the general formulas (1) and (1A), R 1 , R 6 , R 7 and R 8 When R is an alkyl group, for example, an alkyl group having 1 to 12 carbon atoms can be mentioned. Among these, from the viewpoints of solubility and electrical conductivity, an alkyl group having 1 to 10 carbon atoms is preferred. The alkyl group may be linear or branched, but from the viewpoint of electrical conductivity, a linear group is preferred, and from the viewpoint of solubility, a branched group is preferred. From the viewpoint of heat resistance, an alkyl group having 1 to 5 carbon atoms can be mentioned. Among these, an alkyl group having 1 to 3 carbon atoms is preferred, in particular from the viewpoint of excellent heat resistance. In addition, in the general formulae (1) and (1A), R 1 , R 6 , R 7 and R 8 When is an alkyl group, the alkyl group may be substituted with a halogen to form a halogenated alkyl group.
[0013] In the general formulas (1) and (1A), R 1 , R 6 , R 7 and R 8When R is an aryl group, for example, an aryl group having 6 to 22 carbon atoms can be mentioned. Among these, an aryl group having 6 to 14 carbon atoms is preferable from the viewpoint of good solubility and electrical conductivity, and particularly excellent heat resistance. In the general formulas (1) and (1A), R 1 , R 6 , R 7 and R 8 In one embodiment of the present invention, R 1 and R 6 are preferably both methyl groups (Me).
[0014] In one embodiment of the present invention, the conductive oligomer has a terminal YR as represented by general formula (1). 1 and Y.R. 6 Since it has a structure having the above structure, it has high thermal stability and excellent electrical conductivity.
[0015] In the general formulas (1) and (1A), R 2 , R 3 , R 4 and R 5 When R is an alkyl group, for example, an alkyl group having 1 to 12 carbon atoms can be mentioned. Among these, from the viewpoint of improving electrical conductivity, an alkyl group having 1 to 10 carbon atoms is preferable. The alkyl group may be linear or branched, but from the viewpoint of improving electrical conductivity, a linear alkyl group is preferable, and from the viewpoint of improving solubility, a branched alkyl group is preferable. In one embodiment of the present invention, R 2 , R 3 , R 4 and R 5 are preferably all hydrogen atoms.
[0016] In the general formulas (1) and (1A), R 1 ~R 8 Each of may further have a substituent. In this case, it is possible to form a bulkier conductive oligomer, which is advantageous in terms of solubility.
[0017] In the general formulas (1) and (1A), n is, for example, 2 to 30, and from the viewpoint of good electrical conductivity, it is preferably 2 to 12, and may be, for example, 2 to 10, 2 to 8, 2 to 6, or 2 to 4. n is preferably a single integer. That is, in one aspect of the present invention, it is very preferable that the degree of polymerization of the monomer constituting the conductive oligomer is not distributed and the oligomer has a uniform molecular weight. In this way, if the degree of polymerization of the monomer constituting the conductive oligomer is not distributed and the conductive oligomer has a uniform molecular weight, it is easy to arrange the monomers in an orderly manner, and therefore it is possible to efficiently design a conductive composition with excellent electrical conductivity.
[0018] In the general formulas (1) and (1A), m is 1 or 2. When m is 1, it is preferable in terms of electrical conductivity. When m is 2, it is preferable in terms of solubility because it is possible to design a relatively bulky conductive oligomer. In the general formulas (1) and (1A), X is S (sulfur atom), Se (selenium atom), or O (oxygen atom). When X is S (sulfur atom), it is preferable from the viewpoint of solubility. When X is O (oxygen atom), it is preferable from the viewpoint of electrical conductivity. It is preferable that the two X's are the same type of atom in the same compound. In the general formula (1), Y is S (sulfur atom), Se (selenium atom), O (oxygen atom), or CR 7 R 8 where Y is CR 7 R 8 If R 1 and R 6 are each independently a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. It is preferable that two Y's are the same in the same compound.
[0019] Suitable examples of the conductive oligomer of the present invention represented by general formula (1) include compounds 1 to 4 represented by the following formulas (2) to (5).
[0020] compound 1 [ka]
[0021] In the formula (2), Me represents a methyl group. n is an integer of 2 to 30, and preferably a single integer of 2 to 30. In one embodiment of the present invention, the use of a conductive oligomer having the skeleton of compound 1 is advantageous in terms of conductivity.
[0022] compound 2 [ka]
[0023] In the formula (3), Me represents a methyl group. n is an integer of 2 to 30, and preferably a single integer of 2 to 30. In one embodiment of the present invention, the use of a conductive oligomer having a skeleton represented by (3) is advantageous in terms of conductivity.
[0024] compound 3 [ka] In the formula (4), n is an integer of 2 to 30, and preferably a single integer of 2 to 30. In one embodiment of the present invention, the use of a conductive oligomer having a skeleton represented by (4) is advantageous in terms of conductivity.
[0025] compound 4 [ka]
[0026] In the formula (5), n is an integer of 2 to 30, and preferably a single integer of 2 to 30. In one embodiment of the present invention, the use of a conductive oligomer having a skeleton represented by formula (5) is advantageous in terms of solubility.
[0027] In one embodiment of the present invention, the conductive oligomer having the skeleton of general formula (1) and (1A) is a low molecular weight compound. By changing the substituent or structure, the intermolecular distance can be changed, and the solvent molecules can be easily inserted between the molecules. In other words, it is possible to design the conductive oligomer to be easily solvated efficiently. Therefore, the conductive oligomer has excellent solubility. Here, an example of a method for evaluating the "solubility" of the conductive oligomer is the evaluation described in the Examples. It can also be evaluated by measuring absorbance.
[0028] (Manufacturing method) The conductive oligomer according to one embodiment of the present invention can be efficiently produced, for example, by the method described in the Examples.
[0029] (Application) The conductive oligomer according to one embodiment of the present invention is a novel compound, and as described above, it has excellent electrical conductivity and heat resistance, and further has excellent solubility, and therefore has good production efficiency, and is therefore very useful in various applications requiring high electrical conductivity and heat resistance, for example, as an electrode for a capacitor, a transparent electrode, an electrode for a battery, an electrode for a capacitor, etc., and as a conductive assistant for electrodes, etc. In particular, by introducing an appropriate dopant into the conductive oligomer as described below, it is possible to provide a conductive composition having very excellent electrical conductivity.
[0030] The conductive composition of the present invention will now be described. [Conductive composition] In one embodiment of the present invention, the conductive composition is a conductive composition in which a dopant is introduced into the conductive oligomer described above as one embodiment of the present invention. When a dopant is introduced into the conductive oligomer, the stacking state of the conductive oligomer molecules can be changed. As a result, the conductivity of the conductive oligomer can be changed. Therefore, by adjusting the type of dopant to be introduced, the content of the dopant, and other conditions when introducing the dopant, it is possible to obtain a conductive composition having a desired conductivity. In particular, when a dopant is introduced into a conductive oligomer having a uniform molecular weight as described above, a conductive composition having excellent conductivity can be efficiently obtained.
[0031] The conductive oligomers that can be used in the conductive composition of the present invention are as described above. The dopant that can be used in the conductive composition of the present invention is not particularly limited as long as it can be introduced into the conductive oligomer that is one embodiment of the present invention described above, and any known dopant can be used. Preferred examples of the anion include monovalent anion species such as TCNQ or FxTCNQ (x is 2 or 4), halide ions such as chloride ion, bromide ion, and iodide ion; polyhalide ions such as triiodide ion; perchlorate ion; tetrafluoroborate ion; hexafluoroarsenate ion; sulfate ion; nitrate ion; thiocyanate ion; hexafluorosilicate ion; phosphate ions such as hexafluorophosphorus ion, phosphate ion, phenylphosphate ion, and hexafluorophosphate ion; trifluoroacetate ion; alkylbenzenesulfonate ions such as tosylate ion, ethylbenzenesulfonate ion, and dodecylbenzenesulfonate ion; alkylsulfonate ions such as methylsulfonate ion, ethylsulfonate ion, and diisooctylsulfosuccinate ion; and polymer ions such as polyacrylic acid ion, polyvinylsulfonate ion, polystyrenesulfonate ion, and poly(2-acrylamido-2-methylpropanesulfonate) ion. These may be used alone or in combination of two or more.
[0032] More specifically, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, LiCl, LiBr, LiB(C2H5)4, LiCH3SO3, LiC4F9SO3, Li(CF3SO2)2N, and Li[(CO2)2]2B are included. Among these, BF 4- , ClO4 - , HSO4 - , and those having a monovalent anion species of TCNQ or FxTCNQ (x is 2 or 4) are preferred from the viewpoint of electrical conductivity. These may be used alone or in combination of two or more. In this specification, "TCNQ" means tetracyanoquinodimethane.
[0033] The dopant concentration in the conductive oligomer means the concentration of the dopant (counter anion) relative to the monomer unit constituting the conductive oligomer. For example, if the conductive oligomer has a thiophene ring and the counter anion has sulfonic acid, the dopant concentration is defined as 100% when the thiophene ring:sulfonic acid is 1:1 (molar ratio). Since the conductive oligomer contains at least one thiophene ring as a constituent unit, the content ratio of the conductive oligomer and the dopant (dopant concentration) is preferably expressed as "dopant / thiophene unit (mol / mol) x 100 (%)". From the viewpoint of conductivity, the dopant concentration is preferably 6 to 120%, more preferably 10 to 100%.
[0034] The content of the conductive oligomer in the conductive composition is not particularly limited and depends on the application of the conductive composition. From the viewpoint of improving the conductivity of the conductive composition, however, the content is, for example, 7 mol % or more, preferably 30 mol % or more, and more preferably 30 to 200 mol %, calculated on an oligomer basis in the conductive composition.
[0035] The conductive composition may contain various components other than the conductive oligomer and dopant depending on the purpose and application.
[0036] The conductivity of the conductive composition is 1×10 -5 S / cm or more is preferable, and 2×10 -5 S / cm~1×10 3 S / cm is more preferred.
[0037] (Manufacturing method) The method for producing the conductive composition includes a step of adding a dopant to a conductive oligomer, and may include other steps as necessary. The conductive composition according to one embodiment of the present invention is efficiently produced by the method described in the Examples, as an example.
[0038] (Application) In one embodiment of the present invention, the conductive composition has good production efficiency and excellent conductivity and heat resistance as described above, and is therefore very useful for various applications requiring high conductivity and heat resistance, such as electrodes for capacitors, transparent electrodes, battery electrodes, and capacitor electrodes. For example, an electrode having excellent conductivity and heat resistance can be suitably obtained by coating the conductive composition on an electrode as described below to prepare a cured film. In addition, an electrode having high conductivity can be obtained by adding the conductive composition as a conductive assistant when forming an electrode. EXAMPLES
[0039] The present invention will be described in more detail below by way of examples, but the present invention is not limited to the following examples in any way.
[0040] The measurement methods carried out in the following examples are outlined below. Flash silica gel column chromatography was carried out using silica gel 60N (spherical and neutral gel, 40-50 μm, Kanto Chemical) (Still, WC; Kahn, M.; Mitra, A., J. Org. Chem., 1978, 43, 2923-2925). Gel permeation chromatography (GPC) was performed using a preparative HPLC (LC-908, Japan Analytical Industry Co., Ltd.) equipped with a high-speed preparative GPC column (polystyrene column, 20 mmφ×(600+600) mm) (JAIGEL-1HR, -2HR, Japan Analytical Industry Co., Ltd.). proton( 1 H) and carbon ( 13 C) Nuclear magnetic resonance (NMR) spectra were obtained using a JEOL JNM-AL300 ( 1 H:300MHz; 13 The measurements were performed using a 75 MHz (C: 75 MHz) spectrometer. 1 H NMR spectrum and 13 C NMR spectra were corrected for solvent absorption. Mass spectrometry was measured using a JEOL JMS-AX500 (FD probe, positive mode) mass spectrometer.
[0041] Example 1 Synthesis of conductive oligomer (2MeS-2EDOT) A stirrer was placed in a 100 mL Schlenk flask (reaction vessel), the ball stopper was attached, and the wall was heated with a heat gun for about 1 minute while reducing the pressure with a vacuum pump to remove moisture. After cooling to room temperature, the flask was connected to an argon line and reduced the pressure with a vacuum pump twice, and finally connected to the argon line once more to replace the atmosphere inside the reaction vessel with an argon atmosphere. All subsequent operations were performed while blocking light by wrapping the reaction vessel with aluminum foil, etc. With argon flowing, the ball stopper was opened, 341 mg of bis(3,4-ethylenedioxythiophene) (bisEDOT) was added to the Schlenk flask (reaction vessel), and the flask was plugged with a septum. 80 mL of tetrahydrofuran (THF) (Wako, ultra-dehydrated, stabilizer-containing) was added to the reaction vessel with a syringe, and the reaction vessel was cooled to -80°C while stirring with a magnetic stirrer. 2.3mL of n-butyl lithium (n-BuLi) (1.6M in n-hexane) (Kanto Chemical Co., Ltd.) was dropped little by little into the reaction solution using a syringe. Stirring was continued at -80°C for 2 hours, and the temperature was raised to -20°C and stirred for another 15 minutes. After that, it was cooled again to -80°C, and then 0.66mL of dimethyl disulfide (Wako, Wako first grade) was dropped into the reaction vessel. The temperature was then raised to room temperature and stirring was continued for 15 hours. The reaction solution was concentrated using a rotary evaporator, and the resulting brown solid was dissolved in diethyl ether (Wako, special grade reagent), and 1M NH4Cl (aqueous solution) was added to the organic layer to separate the liquids.
[0042] Pure water was added to the washed organic layer (upper layer) and separation was performed once more. Na2SO4 was added to the organic layer (upper layer) and stirred for about 10 minutes to remove water, after which the solids were filtered off and the resulting solution was concentrated using a rotary evaporator to obtain a crude product. The crude product was purified by flash silica gel column chromatography (4.0 cmφ×1810 cm, developing solvent n-hexane:CH2CH2=1:1) to obtain 290 mg (yield 64%) of a white powder, a conductive oligomer (2MeS-2EDOT) represented by the following formula. Physical properties: 1H NMR(CDCl3,300MHz)δ2.38(s,6H),4.29-4.35(m,8H); 13 C NMR(CDCl3,75MHz)δ21.4,64.8,65.0,107.0,111.7,136.8,142.7;MS(FD)calcd for C 14 H 14 O4S4[M + ]374.0,found 374.0.
[0043] [ka]
[0044] (Evaluation of solubility) The obtained conductive oligomer (2MeS-2EDOT) was added to each solvent shown in Table 1 so as to have a concentration of 1% by weight, and stirred at room temperature for 1 hour. Thereafter, the presence or absence of insoluble matter was visually judged according to the following evaluation criteria to evaluate the solubility. The results are shown in Table 1.
[0045] Evaluation criteria ⊚: No insoluble matter was found at all as a result of visual observation. ◯: No insoluble matter was observed by visual observation. Δ: As a result of visual observation, some insoluble matter was observed. ×: A large amount of insoluble matter was observed by visual inspection.
[0046] Example 2 Synthesis of conductive oligomer (2MeS-2EDTT) A stirrer was placed in a 100mL two-necked eggplant flask (reaction vessel), and the wall was heated with a heat gun for about 1 minute while reducing the pressure with a vacuum pump after closing a septum, to remove moisture. After cooling to room temperature, the vessel was connected to an argon line and reduced the pressure with a vacuum pump twice, and finally connected to the argon line once more to replace the atmosphere inside the vessel with argon. All subsequent operations were performed while blocking light by wrapping the vessel with aluminum foil, etc. With argon flowing, the septum was opened, and 645mg of 2,5-dibromo-3,4-ethylenedithiothiophene was added to the Schlenk flask (reaction vessel), and the flask was plugged with a septum. 10mL of THF (Wako, ultra-dehydrated, stabilizer-containing) was added to the reaction vessel with a syringe, and the vessel was cooled to -78℃ while stirring with a magnetic stirrer. 1.34mL of n-BuLi (1.6M in n-hexane) (Kanto Chemical Co., Ltd.) was dropped little by little into the reaction solution over 5 minutes using a syringe. Stirring was continued at -78°C for 2 hours, and then 1.21mL of dimethyl disulfide (Wako, Wako first grade) was dropped into the reaction vessel. Stirring was then continued at -78°C for 30 minutes, and saturated aqueous sodium bicarbonate solution (10mL) was added. The temperature was raised to room temperature while stirring, and the organic matter was extracted three times using 20mL of dichloromethane (Wako, special grade reagent). Magnesium sulfate was added to the mixed organic layer, and the mixture was stirred for 1 minute to remove moisture, after which the solid was filtered off and the resulting solution was concentrated using a rotary evaporator to obtain a crude product (459mg). This crude product was used as it was in the subsequent reaction without further purification.
[0047] A stirrer was placed in a 100mL two-necked eggplant flask (reaction vessel), and the wall was heated with a heat gun for about 1 minute while reducing the pressure with a vacuum pump after closing a septum. The water was removed. After cooling to room temperature, the reaction vessel was connected to an argon line and reduced the pressure with a vacuum pump twice, and finally connected to the argon line once more to replace the atmosphere in the reaction vessel with argon. The septum was opened while argon was flowing, and the crude product (459mg) obtained earlier was added to the Schlenk flask (reaction vessel), and the flask was plugged with a septum. 10mL of THF (Wako, ultra-dehydrated, stabilizer-containing) was added to the reaction vessel with a syringe, and the reaction vessel was cooled to -78℃ while stirring with a magnetic stirrer. 1.15mL of n-BuLi (1.6M in n-hexane) (Kanto Chemical Co., Ltd.) was gradually added dropwise to the reaction solution with a syringe over 5 minutes. Stirring was continued for 2 hours at -78°C, then the septum was opened while argon was flowing, and 247mg of anhydrous copper(II) chloride (Wako, Wako Grade 1) was added to the reaction vessel. Stirring was then continued for 2.5 hours at -78°C, and saturated aqueous sodium bicarbonate solution (50mL) was added. The temperature was raised to room temperature while stirring, and the organic matter was extracted five times using 100mL of dichloromethane (Wako, Special Grade Reagent). The mixed organic layer was washed with saturated aqueous ammonium chloride solution (250mL), magnesium sulfate was added, and the mixture was stirred for 1 minute to remove moisture, after which the solid was filtered off and the resulting solution was concentrated with a rotary evaporator to obtain a crude product.
[0048] The crude product was purified by flash silica gel column chromatography (4.0 cmφ×20 cm, developing solvent n-hexane:ethyl acetate=1:1) to obtain 155 mg of a mixture. Of this, 112 mg was dissolved in 50 mL of chloroform (Wako, special grade reagent), washed with 50 mL of saturated aqueous sodium bicarbonate solution, and then washed with 50 mL of aqueous sodium thiosulfate solution (0.2 M). Magnesium sulfate was added, stirred for 1 minute to remove moisture, and the solid was filtered off. The resulting solution was concentrated with a rotary evaporator to obtain a crude product (104 mg). The product was purified by GPC (eluent: chloroform (Wako, special grade reagent)), and a conductive oligomer (2MeS-2EDTT) represented by the following formula was obtained in a total yield of 4.9% from the raw material 2,5-dibromo-3,4-ethylenedithiothiophene over four steps. Physical properties: 1 H NMR(CDCl3,300MHz)δ2.44(s,6H),3.18(dd,J=2.7,5.1Hz,2H),3.20(dd,J=2.7,4.5Hz,2H),3.27(dd,J=2.7,4.5Hz,2H),3.30(dd,J=2.7,5.1Hz,2H); 13 C NMR(CDCl3,75MHz)δ20.1,27.6,27.7,126.7,126.7,128.0,130.7;MS(FD)calcd for C 14 H 14 S8[M + ]437.9,found 437.9.
[0049] [ka]
[0050] Example 3 Synthesis of conductive oligomer (2Br-2EDTT) A stirrer was placed in a 100mL two-necked eggplant flask (reaction vessel), and the wall was heated with a heat gun for about 1 minute while reducing the pressure with a vacuum pump after closing a septum, to remove moisture. After cooling to room temperature, the reaction vessel was connected to an argon line and reduced the pressure with a vacuum pump twice, and finally connected to the argon line once more to replace the inside of the reaction vessel with an argon atmosphere. All subsequent operations were performed while blocking light by wrapping the reaction vessel with aluminum foil, etc. With argon flowing, the septum was opened, 574mg of 3,4-ethylenedithiothiophene was added to the Schlenk flask (reaction vessel), and the flask was plugged with a septum. 20mL of THF (Wako, ultra-dehydrated, stabilizer-containing) was added to the reaction vessel with a syringe, and the reaction vessel was cooled to 0°C while stirring with a magnetic stirrer. With argon flowing, the septum was opened, and 586mg of N-bromosuccinimide (NBS) was added. After the mixture was plugged with a septum and stirred at 0°C for 2 hours, the septum was opened and 120 mL of aqueous sodium bicarbonate solution was added, and the organic matter was extracted three times with 100 mL of diethyl ether. The insoluble matter was also dissolved in 50 mL of dichloromethane and mixed, and magnesium sulfate was added to this and stirred for 1 minute to remove moisture. The solid was then filtered off, and the resulting solution was concentrated with a rotary evaporator to obtain a crude product (776 mg). This crude product was 1 H NMR analysis confirmed that the raw material was a mixture of 3,4-ethylenedithiothiophene:2-bromo-3,4-ethylenedithiothiophene:2,5-dibromo-3,4-ethylenedithiothiophene in a ratio of 1:5:5.
[0051] Of this crude product, 333 mg was added to a 100 mL two-necked eggplant flask (including a reaction vessel and a stirrer) that had been dried in the same manner as above, with the septum opened while flowing argon, and the flask was plugged with a septum. 8 mL of THF (Wako, ultra-dehydrated, containing stabilizers) was added to the reaction vessel with a syringe, and the flask was cooled to 0°C while stirring with a magnetic stirrer. 502 mg of NBS was added while flowing argon. The flask was plugged with a septum and stirred at 0°C for 1 hour. This solution was added to 50 mL of aqueous sodium bicarbonate solution, and the precipitated dark green solid was filtered off with a membrane filter (Omnipore, 5.0 μm PTFE membrane). The solid was washed with 20 mL of water, 20 mL of methanol, 20 mL of dichloromethane, and 20 mL of chloroform, and then 20 mL of aqueous sodium thiosulfate solution (0.2 M), 5 mL of methanol, and 20 mL of chloroform were added and mixed.
[0052] After the mixture was stirred vigorously at room temperature for 30 minutes, the organic matter was extracted three times with 20 mL of dichloromethane. The extracted organic layers were mixed and washed with 50 mL of saturated aqueous sodium bicarbonate solution, after which magnesium sulfate was added and stirred for 1 minute to remove moisture. The solid was then filtered off, and the resulting solution was concentrated with a rotary evaporator to obtain a crude product (2.9 mg). This crude product was purified using a medium pressure column chromatography with an automatic purification system (Biotage, Isorela One) under the conditions of 25 g of Biotage (registered trademark) KP-Sil as a chromatography cartridge and methanol:dichloromethane = 0:10 to 1:9 as a developing solvent, and 1.7 mg of an orange powder of a conductive oligomer (2Br-2EDOT) represented by the following formula was obtained with a yield of 0.24% based on the raw material 3,4-ethylenedioxythiophene. Physical properties: 1 H NMR(CDCl3)δ3.15-3.24(m,4H),3.25-3.34(m,4H); 13 C NMR(CDCl3)27.6,27.6,107.0,124.2,127.0,127.0;FD MS(positive mode)calcd for C 12 H8Br2S6calc[M+ ]501.7,found 501.7.
[0053] [ka]
[0054] Example 4 Synthesis of conductive oligomer (2MeS-3EDOT) A stirrer was placed in a 6 mL screw-capped vial (reaction vessel), 61 mg of 5-(methylthio)-(3,4-ethylenedioxythiophene) (MeS-EDOT-H), 69 mg of 2,5-dibromo-(3,4-ethylenedioxythiophene) (2Br-EDOT), 6 mg of palladium acetate (Pd(OAc)2), and 380 mg of potassium carbonate (K2CO3) were added, and the vessel was placed in a nitrogen-substituted glove box. After adding 16 mg of pivalic acid to the screw-capped vial (reaction vessel) in the glove box, 3 mL of dimethylformamide (DMF) (Wako, ultra-dehydrated) was added to the reaction vessel, and the screw cap was closed. The reaction vessel was heated to 90 °C on a stage-type hot plate while stirring with a magnetic stirrer, and stirring was continued at that temperature for 2 hours. Thereafter, the reaction solution was cooled to room temperature, diluted with 50 mL of dichloromethane (manufactured by Wako, special grade reagent), and the organic layer was separated three times in total using 50 mL of water.
[0055] Na2SO4 was added to the organic layer (lower layer) washed by separation, and the mixture was stirred for about 10 minutes to remove moisture. The solid was then filtered off, and the resulting solution was concentrated with a rotary evaporator to obtain a crude product. The crude product was purified using a medium pressure column chromatography with an automatic purification system (Biotage, Isorela One) under the conditions of 50 g of Biotage (registered trademark) SNAP Ultra as a chromatography cartridge and n-hexane:CH2CH2 = 1:1 to 0:10 as a developing solvent, and 21 mg of a yellow powder of the conductive oligomer (2MeS-3EDOT) represented by the following formula was obtained in a yield of 26% based on the raw material 2,5-dibromo-(3,4-ethylenedioxythiophene). Physical properties: 1 H NMR(CDCl3,300MHz)δ2.38(s,6H),4.29-4.52(m,12H);MS(FD)calcd for C 20 H 18 O6S5[M + ]514.0,found 514.0.
[0056] [ka]
[0057] Example 5 Preparation of conductive composition (chemical oxidation method) A conductive composition was prepared by the diffusion method as follows. 3.97 mg of 2MeS-2EDOT was added as a conductive oligomer to one side of a liquid-liquid diffusion H-type cell, and 2.54 mg of F2TCNQ (Tokyo Chemical Industry Co., Ltd.) was added as a dopant source to the other side. 10 mL of CHCl3 (Wako, special grade reagent) was added slowly along the wall. After mixing, the mixture was left to stand for 48 hours, and then the precipitated glossy rod-shaped black crystals were separated from the solution by filtration to obtain a conductive composition (composition 1). In the same manner as above, conductive compositions (compositions 2 to 3, 9) were prepared using the solvents shown in Table 2 and the conductive oligomers and dopants (dopant supply sources) shown in Table 2.
[0058] Example 6 Preparation of conductive composition (electrolytic oxidation method) 3.7 mg of 2MeS-2EDOT was added as a conductive oligomer to the oxidation side of the H-type electrolytic oxidation cell, 10 mg of n-Bu4NBF4 (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as a dopant supply source to both sides, and 10 mL of acetone (manufactured by Wako, special grade reagent) was slowly added along the wall. In a thermostatic chamber at 25°C, a current of 0.3 μA was applied to the platinum electrode, and the mixture was left to stand for 3 days. The precipitated glossy rod-shaped black crystals were then separated from the solution by filtration to obtain a conductive composition (composition 4). In the same manner as above, conductive compositions (compositions 5 to 8, 10, and 11) were prepared using the solvents shown in Table 2 and the conductive oligomers and dopants shown in Table 2.
[0059] (Evaluation of electrical conductivity) The electrical conductivity of the obtained conductive composition was measured and evaluated as follows. The results are shown in Table 2. A gold wire of 15 μm diameter was attached to the obtained conductive composition using a conductive carbon paste (XC-12, manufactured by DOTITE), and the electrical resistance was measured at room temperature using the two-terminal method or the four-terminal method to measure the electrical conductivity. In order to relieve distortion of the single crystal during bonding, the Au wire was cross-linked using Ag paste (DOTITE (D-500), manufactured by Kamakura Kasei Co., Ltd.) and connected to the substrate. The carbon paste and Ag paste were mixed with a small amount of butyl glycol acetate (manufactured by Tokyo Kasei Kogyo Co., Ltd.) to obtain an appropriate viscosity.
[0060] Comparative Example 1 Preparation of conductive polymer (PEDOT / PSS) The conductive polymer (PEDOT / PSS) was obtained by drying the aqueous solution manufactured by Aldrich.
[0061] (Evaluation of solubility) The solubility of the obtained conductive polymer (PEDOT / PSS) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0062] Preparation of conductive composition The obtained conductive polymer (PEDOT / PSS) was dispersed in a water solvent, and the aqueous solution was freeze-dried to remove water, thereby obtaining a solid powder (composition 12).
[0063] (Evaluation of electrical conductivity) The obtained conductive composition was evaluated for conductivity by measuring the electrical conductivity in the same manner as in Examples 4 and 5. The results are shown in Table 2. In Table 2, the oligomer concentration and dopant concentration are defined as already explained in this specification.
[0064] [Table 1]
[0065] [Table 2]
[0066] The conductive oligomer of Example 1 was dissolved in all of the solvents, diethyl ether, tetrahydrofuran, and methylene chloride, and no insoluble matter was observed. On the other hand, the PEDOT / PSS of Comparative Example 1 was not sufficiently soluble in any of the solvents, and many insoluble matters were observed.
[0067] Conductive compositions 1 to 11 obtained by combining a specific conductive oligomer with a specific dopant exhibited excellent electrical conductivity for practical use. Composition 12 (PEDOT / PSS) had high electrical conductivity, but was not soluble enough, and therefore did not achieve both solubility and electrical conductivity. [Industrial Applicability]
[0068] The novel conductive oligomer according to one embodiment of the present invention has excellent solubility, and therefore excellent handling properties and productivity, and can efficiently produce a conductive composition having excellent conductivity. By using the conductive oligomer according to one embodiment of the present invention, a conductive composition and a conductive assistant which are efficiently produced and have excellent conductivity can be provided, and further, a capacitor electrode, a transparent electrode, a battery electrode, and a capacitor electrode which are formed using the conductive composition and have excellent conductivity can be provided.
[0069] Although some embodiments and / or examples of the present invention have been described in detail above, those skilled in the art can easily make many modifications to these exemplary embodiments and / or examples without substantially departing from the novel teachings and advantages of the present invention, and therefore many such modifications are within the scope of the present invention. The contents of all documents cited in this specification and of the application from which this application claims priority under the Paris Convention are incorporated by reference in their entirety.
Claims
1. A conductive composition comprising a conductive oligomer represented by the following general formula (1), wherein a dopant is introduced into the conductive oligomer: 【Chemistry 1】 [In general formula (1), R 1 and R 6 are each independently an alkyl group having 1 to 5 carbon atoms. n is an integer from 2 to 30. R 2 , R 3 , R 4 and R 5 are each independently a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. Multiple R 4 may be the same or different. Multiple R 5 may be the same or different. m is 1. X is S (sulfur atom), Se (selenium atom) or O (oxygen atom). A plurality of X's may be the same or different. Y is S (sulfur atom), Se (selenium atom), or O (oxygen atom). The multiple Y's may be the same or different.
2. The dopant is BF 4 - , ClO 4 - , P.F. 6 - , H.S.O. 4 - 2. The conductive composition according to claim 1, wherein the anion species is one or more selected from the group consisting of monovalent anion species of TCNQ or FxTCNQ (x is 2 or 4).
3. 3. The conductive composition according to claim 1, wherein in the general formula (1), n is a single integer of 2 to 30.
4. 4. The conductive composition according to claim 1, comprising 7 mol % or more (calculated in oligomer units) of the conductive oligomer.
5. Conductivity is 1 x 10 -5 The conductive composition according to any one of claims 1 to 4, having a viscosity of 2.0 S / cm or more.
6. A conductive assistant comprising the conductive composition according to any one of claims 1 to 5.
7. A capacitor electrode, a transparent electrode, a battery electrode, or a capacitor electrode formed using at least one of the conductive composition according to any one of claims 1 to 5 and the conductive assistant according to claim 6.
Citation Information
Patent Citations
Conductive paste, electrical conduction functional member, and printed circuit member
JP2005166502A
High electronic conductivity polymer and high-capacity / high-power electrical energy storage device using the same
JP2009537061A
Photoelectric conversion element, method for producing photoelectric conversion element, and solar cell
JP2013077549A
Electron-conductive oligomer, method for manufacturing the same, coating material including the electron-conductive oligomer, antistatic coated object, electronic member, and electron-conductive composition
JP2014070066A