Positive electrode material, its manufacturing method, and lithium ion battery
A dual-coated positive electrode material with phosphoric acid layers on primary and secondary particles addresses the cracking issue in high-nickel cathodes, enhancing lithium ion conductivity and stability in lithium ion batteries.
Patent Information
- Application Number
- JP2022516738
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-16
- Filing Date
- 2022-02-22
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2042-02-22
AI Technical Summary
Conventional high-nickel cathode materials in lithium ion batteries are prone to particle cracking during long-term cycling, which compromises their long-term cycling stability and rate characteristics.
A positive electrode material with a dual coating layer structure, comprising a first coating layer on primary particles and a second coating layer on secondary particles, both made of phosphoric acid compounds, is developed. This structure enhances lithium ion conductivity, thermal stability, and reduces electrical resistance.
The dual coating method improves structural stability, thermal stability, safety, and long-term cycle performance of lithium ion batteries by reducing resistance and protecting the surface from electrolyte corrosion.
Smart Images

Figure 0007583797000002 
Figure 0007583797000003 
Figure 0007583797000004
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of cathode materials, specifically to cathode materials, their manufacturing methods, and lithium ion batteries. [Background technology]
[0002] Lithium-ion batteries have the advantages of high energy density, high power output, long cycle life, and less environmental pollution, and are therefore widely used in electric vehicles and consumer electronic products. How to improve the rate characteristics, thermal stability, and cycle stability of lithium batteries has always been the research direction of developers. After long-term cycles, traditional high-nickel positive electrode materials are prone to particle cracking, directly exposing the internal structure, which impairs the long-term cycle stability of the positive electrode material and impairs the rate characteristics of lithium batteries.
[0003] Therefore, there is an urgent need to provide a positive electrode material and a manufacturing method thereof that can improve the coating uniformity, and further improve the rate characteristics, thermal stability and cycle stability of lithium batteries, and reduce manufacturing costs. Summary of the Invention [Problem to be solved by the invention]
[0004] In view of the above circumstances, the present invention provides a positive electrode material that can improve coating uniformity, accurately control the coating amount, improve the rate characteristics, thermal stability, and cycle stability of a lithium battery, and reduce production costs, a method for producing the positive electrode material, and a lithium ion battery. [Means for solving the problem]
[0005] According to a first aspect of the present invention, General formula: Li b Ni x Co y M z R wO2 (where 0.95 ≦ b ≦ 1.10, 0.8 ≦ x < 1, 0 < y + z + w ≦ 0.2, x + y + z + w = 1, 0.0001 ≦ w ≦ 0.003, M is at least one of Mn and Al, and R is a doping metal.) including a plurality of secondary particles including primary particles containing the active material represented by A coating layer including a first coating layer formed on the surface of the primary particles and a second coating layer formed on the surface of the secondary particles, wherein both the first coating layer and the second coating layer are coating layers containing a phosphate compound, and a positive electrode material including the same is provided. For the positive electrode material, the single-point phosphorus content a' at any point on the surface and the surface average phosphorus content a satisfy the following relationship. 0.9a ≦ a' ≦ 1.1a (However, the a' and a are measured by the following method. When observing the positive electrode material using a scanning electron microscope (SEM), for any one point on the surface of the positive electrode material, point analysis is performed by EDS to measure the phosphorus content to obtain the value of a', and also, in the field of view of the scanning electron microscope (SEM), a 100 μm × 100 μm square region is randomly selected for surface analysis by EDS to measure the phosphorus content to obtain the value of a.)
[0006] In a first aspect, in one embodiment, the Li b Ni x Co y M z R w R in O2 contains at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn.
[0007] In a first aspect, in one embodiment, the positive electrode material satisfies at least one of the following conditions a to k. a. The secondary particles are spherical or substantially spherical; b. The average particle size of the primary particles is 200 nm to 1000 nm, and the average particle size of the secondary particles is 3 μm to 20 μm; c. The phosphate compound is Li3PO4 and LiR k (PO4) r(where 0 < k ≤ 2, 0 < r ≤ 2, and R contains at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn); including at least one of them; d. The raw materials for producing the phosphate compound in the first coating layer include a metal phosphate and a lithium compound, and the raw materials for producing the phosphate compound in the second coating layer include at least one of phosphoric acid, metaphosphoric acid, phosphorous acid, metaphosphorous acid, pyrophosphoric acid, hypophosphorous acid, soluble phosphate, soluble metaphosphate, soluble phosphite, soluble metaphosphite, soluble pyrophosphate, and soluble hypophosphite; e. The phosphate ion content in the phosphate compound in the first coating layer is 0.03 wt% to 0.3 wt% of the total mass of the secondary particles; f. The phosphate ion content of the phosphate compound in the second coating layer is 0.1 wt% to 0.7 wt% of the total mass of the secondary particles and the first coating layer; g. The crystalline phosphate ion content in the phosphate compound in the first coating layer or the second coating layer is 5 wt% to 50 wt% of the total mass of the phosphate ions; h. The thickness of the first coating layer is 0.005 μm to 0.05 μm; i. The thickness of the second coating layer is 0.02 μm to 0.2 μm; j. The 4 kN / cm 2 powder conductivity of the positive electrode material under pressure is more than 0.02 S / cm; k. The specific surface area of the positive electrode material is 0.2 m 2 / g to 2.0 m 2 / g. The "crystalline phosphate ion" described in the present invention refers to the phosphate ion in a crystalline phosphate ion-containing compound.
[0008] According to the second aspect of the present invention, Ni a Co b M c O or Ni a Co b M c(OH)2 (wherein a + b + c = 1, 0.8 ≦ a < 1, 0 < b + c ≦ 0.2, and M is at least one of Mn and Al), a lithium compound, and a metal phosphate are mixed, and the resulting mixture is sintered to obtain a sintered product. The sintered product includes a plurality of primary particles and a first coating layer that forms the surface of the primary particles and contains a phosphate compound, and the average particle diameter of the metal phosphate is less than 0.5 μm. The sintered product is washed with a solvent at 50°C or lower and dried to obtain the positive electrode material. The positive electrode material includes secondary particles that are aggregates of primary particles and a second coating layer that forms the surface of the secondary particles and contains a phosphate compound. A method for manufacturing a positive electrode material is provided, including this step.
[0009] In a second aspect, in one embodiment, the method satisfies at least one of the following conditions a to f. a. The addition amount of the lithium compound is such that the ratio of the total molar content of the metal elements in Ni, Co, M, and the metal phosphate to the molar content of Li is 1:(0.95 - 1.10); b. The lithium compound includes at least one of lithium carbonate, lithium hydroxide, lithium acetate, lithium nitrate, and lithium oxalate; c. The metal element of the metal phosphate is at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn; d. The phosphate ion content in the metal phosphate is 0.03 wt% - 0.3 wt% of the total mass of the mixture; e. As the mixing conditions for obtaining the mixture, solid-phase mixing is performed at 10°C - 50°C for 0.3 h - 2 h; f. As the sintering conditions for obtaining the sintered product, sintering is performed at 650°C - 850°C for 6 h - 20 h in an oxygen-containing atmosphere.
[0010] In a second aspect, in one embodiment, the method satisfies at least one of the following conditions a to b. a. the solvent comprises water and a non-aqueous material, the non-aqueous material comprising at least one of phosphoric acid, metaphosphoric acid, phosphorous acid, metaphosphorous acid, pyrophosphoric acid, hypophosphorous acid, a soluble phosphate, a soluble metaphosphate, a soluble phosphite, a soluble metaphosphite, a soluble pyrophosphate, and a soluble hypophosphite; b. The content of phosphate ions in the solvent is 0.1 wt % to 0.7 wt % of the total mass of the sintered body.
[0011] In the second aspect, in one embodiment, the method satisfies at least one of the following conditions a to f: a. The washing temperature is 10°C to 50°C; b. The concentration of the slurry consisting of the sinter and the solvent (sinter (g) / solvent (L)) is 500 g / L to 2000 g / L; c. the cleaning time is 10 min to 120 min; d. the drying is performed under a nitrogen atmosphere; e. the drying temperature is 80°C to 200°C; f. The drying time is 5 hours to 48 hours.
[0012] In the second aspect, in one embodiment, the method further comprises washing the sintered body with a solvent, drying the sintered body, and then The method includes a step of subjecting the sintered product after washing and drying to a heat treatment at 150° C. to 600° C. for 4 hours to 10 hours in an oxygen-containing atmosphere to obtain the positive electrode material.
[0013] In the second aspect, in one embodiment, the method satisfies at least one of the following conditions a to f: a. the metal phosphate reacts with the lithium compound at an elevated temperature to form a first coating layer on the primary particles; b. phosphate ions in the solvent react with residual lithium on the surface of the sinter to form a second coating layer of the secondary particles; c. The phosphate compound is Li3PO4 and LiR k (PO4) r(where 0 < k ≤ 2, 0 < r ≤ 2, and R is at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn). It contains at least one of them; d. The content of crystalline phosphate ions in the phosphate compound in the first coating layer or the second coating layer is 5 wt% to 50 wt% of the total mass of phosphate ions; e. The average particle size of the primary particles is 200 nm to 1000 nm, and the thickness of the first coating layer is 0.005 μm to 0.05 μm; f. The average particle size of the secondary particles is 3 μm to 20 μm, and the thickness of the second coating layer is 0.02 to 0.2 μm.
[0014] According to a third aspect of the present invention, there is provided a lithium-ion battery including the positive electrode material according to the first aspect or the positive electrode material manufactured by the method for manufacturing a positive electrode material according to the second aspect.
Advantages of the Invention
[0015] The present invention can achieve at least the following beneficial effects.
[0016] First, the positive electrode material according to the present invention includes secondary particles formed by tightly bonding a plurality of primary particles, the primary particles having a first coating layer, the secondary particles having a second coating layer, and both the first coating layer and the second coating layer being made of a phosphate compound. This coating method in which the inside and the surface are simultaneously coated (also called "double coating") synergistically improves the structural stability, safety, rate characteristics, long-term cycle stability, and processability of the positive electrode material, contributes to the formation of a network having high lithium ion conductivity, improves the lithium ion conductivity of the material, and reduces the resistance of the battery. The second coating layer on the surface of the secondary particles not only protects the surface of the secondary particles from corrosion by the electrolyte and improves thermal stability, but also improves the lithium ion diffusion rate, and the positive electrode material obtained thereby can achieve both high rate characteristics and high thermal stability. In addition to having the same characteristics as above, the first coating layer forms a phosphate compound coating layer with high ion conductivity at the crystal grain boundaries between the primary particles, thereby reducing the electrical resistance at the crystal grain boundaries and contributing to improving the rate characteristics of the positive electrode material. In addition, since the single-point phosphorus content a' at any point on the surface of the positive electrode material and the surface average phosphorus content a thereof satisfy 0.9a≦a'≦1.1a, the phosphorus content at each point on the surface of the positive electrode material is close to the surface average phosphorus content, and the phosphorus content in the coating layer is uniformly distributed, which can suppress the loss of lattice lithium (i.e., lithium ions in the crystal lattice) on the surface of the positive electrode material and reduce the amount of free lithium on the material surface, thereby improving the rate characteristics and suppressing side reactions between the material and the electrolyte, improving the cycle stability of the material, and imparting excellent processability and safety to the positive electrode material.
[0017] Next, the method for producing the positive electrode material according to the present invention can achieve metal cation doping while coating the primary particles of the positive electrode material by uniformly diffusing the phosphate over the surface of the material through a single-step sintering process at high temperature. In addition, the phosphate can be uniformly deposited on the surface of the secondary particles of the positive electrode material by washing the sintered material at 50° C. or less using a solvent containing a non-aqueous substance, thereby forming a uniform phosphoric acid compound coating layer. This can improve the structural stability, thermal stability, safety, rate characteristics, long-term cycle performance and processability of the positive electrode material. [Brief description of the drawings]
[0018] [Figure 1] 1 is a schematic structural diagram of a positive electrode material according to the present invention. [Diagram 2] 1 is a flow chart of a method for producing a cathode material according to the present invention. [Figure 3a] and [Figure 3b] 1A-1C are scanning electron micrographs of the positive electrode material of Example 1 at different magnifications. [Figure 4a] and [Figure 4b] 1A-1C are scanning electron microscope photographs of the positive electrode material of Comparative Example 1 at different magnifications. [Diagram 5] FIG. 2 is a graph showing the rate characteristics of the positive electrode materials of Example 1 and Comparative Example 1. [Figure 6] 1 shows differential scanning calorimetry (DSC) curves of the positive electrode materials of Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] A preferred embodiment of the present invention will be described below. However, a person skilled in the art can make various improvements and modifications without departing from the principles and spirit of the present invention, and it should be understood that these improvements and modifications also fall within the scope of the present invention.
[0020] Conventional high-nickel cathode materials, after undergoing long-term cycling, are prone to particle cracking and direct exposure of the internal structure, which impairs the long-term cycle stability of the cathode material and the rate performance of lithium batteries. To improve the rate performance, thermal stability, and cycle stability of lithium-ion batteries, the present invention provides a cathode material.
[0021] The cathode material is General formula: Li b Ni x Co y M z R w O2 (where 0.95 ≤ b ≤ 1.10, 0.8 ≤ x < 1, 0 < y + z + w ≤ 0.2, x + y + z + w = 1, 0.0001 ≤ w ≤ 0.003, M is at least one of Mn and Al, and R is a doping metal 112.) including a plurality of secondary particles 10 containing primary particles 11 including an active material represented by A first coating layer 111 formed on the surface of the primary particles 11 and a second coating layer 101 formed on the surface of the secondary particles 10, and both the first coating layer 111 and the second coating layer 101 are coating layers containing a phosphate compound. The cathode material satisfies the following relationship between the single-point phosphorus content a' at any point on the surface and its surface average phosphorus content a. 0.9a ≤ a' ≤ 1.1a (However, the a' and a are measured by the following method. When observing the cathode material using a scanning electron microscope (SEM), for any one point on the surface of the cathode material, point analysis is performed by EDS to measure the phosphorus content to obtain the value of a', and also, a 100 μm × 100 μm square region is randomly selected in the field of view of the scanning electron microscope (SEM) for surface analysis by EDS to measure the phosphorus content to obtain the value of a.)
[0022] The positive electrode material according to the present invention includes secondary particles formed by tightly bonding a plurality of primary particles together, the primary particles having a first coating layer, the secondary particles having a second coating layer, and both the first coating layer and the second coating layer being made of a phosphate compound, and the phosphorus content a' at any single point on the surface of the positive electrode material and the surface average phosphorus content a satisfy 0.9a≦a'≦1.1a, so that it can be seen that the distribution of the phosphorus content at each point on the surface of the positive electrode material is small in variation and the coating layer is uniformly distributed. This coating method in which the inside and the surface are simultaneously coated contributes to the formation of a network with high lithium ion conductivity, improves the lithium ion conductivity of the material, and reduces the resistance of the battery. The second coating layer on the surface of the secondary particles not only protects the surface of the secondary particles from corrosion by the electrolyte and improves thermal stability, but also improves the lithium ion diffusion rate, and the positive electrode material obtained thereby can achieve both high rate characteristics and high thermal stability. In addition to having the above-mentioned characteristics, the first coating layer is formed with a phosphate compound coating layer having high ionic conductivity on the grain boundaries between the primary particles, which reduces the electrical resistance at the grain boundaries and contributes to improving the rate characteristics of the positive electrode material. Therefore, this internal / surface double coating method can synergistically improve the structural stability, thermal stability, safety, rate characteristics, long-term cycle characteristics, and processability of the positive electrode material.
[0023] Specifically, the value of b may be, for example, 0.95, 0.98, 1.01, 1.03, 1.05, or 1.10, etc. The value of x may be, for example, 0.8, 0.83, 0.88, 0.91, 0.94, 0.98, or 0.99, etc. The value of y+z+w may be, for example, 0.02, 0.06, 0.09, 0.12, 0.17, or 0.2, etc., and the value of w may be, for example, 0.0001, 0.0005, 0.0010, 0.0015, 0.0020, 0.0025, or 0.0030, etc., but is not limited thereto.
[0024] Preferably, the Li b Ni x Co y M zR w R in O2 includes at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn.
[0025] In addition, the active material Li b Ni x Co y M z R w The content of each element in O2 can be measured by known instruments for performing qualitative and / or quantitative analysis of each element, such as ICP, ICP-MS, etc.
[0026] Each of the primary particles is an independent fine crystal grain, and the secondary particles are particles formed by agglomerating the primary particles. Preferably, the secondary particles are aggregates of the primary particles, have a dense interior, and are spherical or nearly spherical.
[0027] In the positive electrode material according to the present invention, the average particle size D50 of the primary particles of the active material is 200 nm to 1000 nm, for example, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, or 1000 nm, as measured jointly by a scanning electron microscope (SEM) and a particle size test.
[0028] The average particle size of the secondary particles is 3 μm to 20 μm, and may be, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 15 μm, or 20 μm, and is preferably 10 μm to 13 μm. The inventors conducted repeated tests and found that when the average particle size of the secondary particles is controlled within the range of 3 μm to 20 μm, the problem of cracking of the secondary particles during the cycle process can be avoided, and this is advantageous in improving the structural stability, thermal stability, and long-term cycle stability of the secondary particles.
[0029] In some embodiments, the thickness of the first coating layer is from 0.005 μm to 0.05 μm, and for example, it may be 0.005 μm, 0.01 μm, 0.015 μm, 0.02 μm, 0.025 μm, 0.03 μm, 0.035 μm, 0.04 μm, 0.045 μm or 0.05 μm. The thickness of the first coating layer may be other values as long as it is within the above range, and is not limited herein.
[0030] In some embodiments, the thickness of the second coating layer is from 0.02 μm to 0.2 μm, and for example, it may be 0.02 μm, 0.03 μm, 0.05 μm, 0.08 μm, 0.1 μm, 0.13 μm, 0.15 μm, 0.18 μm or 0.2 μm. The thickness of the first coating layer may be other values as long as it is within the above range, and is not limited herein.
[0031] In some embodiments, the phosphate compound includes at least one of Li3PO4 and LiR k (PO4) r (where 0 < k ≤ 2, 0 < r ≤ 2, and R is at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn).
[0032] The phosphate compound not only has a high lithium ion conductivity but also can reduce the residual alkali on the surface of the cathode material. Such a coating method that coats both the inside and the surface is advantageous for forming a coating layer that has a high lithium ion conductivity and isolates the active material from the electrolyte in all directions.
[0033] Specifically, the phosphate compound in the first coating layer is a phosphate compound formed by using a production raw material containing a metal phosphate salt and a lithium compound, and reacting the metal phosphate salt and the lithium compound at a high temperature, and aims to simultaneously perform phosphate compound coating and metal cation doping on the primary particles of the cathode material during the roasting process.
[0034] The raw materials for producing the phosphate compound in the second coating layer include at least one of phosphoric acid, metaphosphoric acid, phosphorous acid, metaphosphorous acid, pyrophosphoric acid, hypophosphorous acid, soluble phosphate, soluble metaphosphate, soluble phosphite, soluble metaphosphite, soluble pyrophosphate, and soluble hypophosphite. The second coating layer is a phosphate compound formed by a reaction between a non-aqueous substance added during the cleaning process and residual lithium on the surface of the sinter, and the phosphate compound contains at least Li ions having a high lithium ion conductivity. m PO n (1≦m≦3, 1≦n≦4).
[0035] The content of phosphate ions in the first coating layer is 0.03 wt% to 0.3 wt% of the total mass of the secondary particles, preferably 0.075 wt% to 0.175 wt%, and may be, for example, 0.075 wt%, 0.1 wt%, 0.125 wt%, 0.15 wt%, or 0.175 wt%.
[0036] The content of phosphate ions in the second coating layer is 0.1 wt% to 0.7 wt% of the total mass of the secondary particles and the first coating layer, and preferably 0.3 wt% to 0.5 wt%, for example, 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt%, or 0.5 wt%. Through repeated testing, the inventors have found that by controlling the content of phosphate ions within the above range, a good coating effect of the primary particles or secondary particles can be obtained without reducing the capacity of the positive electrode material.
[0037] In this specification, the term "primary coating" refers to the first coating treatment applied to the positive electrode material, and the term "secondary coating" refers to the second coating treatment applied to the positive electrode material.
[0038] The second coating layer on the surface of the secondary particles not only protects the surface of the secondary particles from corrosion by the electrolyte and improves thermal stability, but also improves the lithium ion diffusion rate and reduces residual alkali on the surface, enabling the obtained positive electrode material to combine high rate characteristics, high thermal stability, good processability, and safety.
[0039] In addition to having the same characteristics as above, the first coating layer on the surface of the primary particles can prevent the primary particles inside the positive electrode material from directly contacting the electrolyte during secondary particle cracking, suppressing side reactions and being advantageous for improving the structural stability, thermal stability and long-term cycle stability of the secondary particles. Furthermore, since a phosphate compound coating layer with high ionic conductivity is formed on the crystal grain boundaries between the primary particles, the electrical resistance at the crystal grain boundaries is reduced, which is advantageous for improving the rate characteristics of the positive electrode material. The internal / surface double coating method can synergistically improve the structural stability, thermal stability, safety, rate characteristics, long-term cycle characteristics and processability of the positive electrode material.
[0040] In the positive electrode material according to the present invention, the content of crystalline phosphate ions in the phosphate compound coating layer is 5 wt% to 50 wt% of the total mass of phosphate ions, and may be, for example, 5 wt%, 10 wt%, 20 wt%, 30 wt%, 40 wt%, or 50 wt%.
[0041] The positive electrode material is a ternary positive electrode material with a resistance of 4kN / cm 2 The powder conductivity under pressure is more than 0.02 S / cm, which can effectively improve the high-rate discharge capacity.
[0042] The specific surface area of the positive electrode material is 0.2 m 2 / g~2.0m 2 Preferably, the specific surface area of the positive electrode material is 0.3 m 2 / g~0.8m 2 / g, for example, 0.3m 2 / g, 0.4m 2 / g, 0.5m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, etc. As a result of repeated testing by the inventors, it was found that the specific surface area of the positive electrode material was 0.2 m 2 / g~2.0m 2 / g, it has been found that this is advantageous in improving the cycle characteristics of a lithium battery produced using the positive electrode material.
[0043] The present invention further provides a method for manufacturing a positive electrode material. As shown in FIG. 2, the manufacturing method includes the following steps S100 to S200.
[0044] <Step S100> In this step, Ni a Co b M c O or Ni a Co b M c (OH)2 (where a + b + c = 1, 0.8 ≦ a < 1, 0 < b + c ≦ 0.2, and M is at least one of Mn and Al), a lithium compound, and a metal phosphate are mixed, and the resulting mixture is sintered to obtain a sintered product. The sintered product includes a plurality of primary particles and a first coating layer that forms on the surface of the primary particles and contains a phosphate compound. The average particle size of the metal phosphate is less than 0.5 μm
[0045] By adding a metal phosphate component, phosphate compound coating and metal cation doping are simultaneously performed on the primary particles of the positive electrode material during the roasting process. The primary particle coating can prevent the primary particles inside the positive electrode material from directly contacting the electrolytic solution during secondary particle cracking, suppress side reactions, and is advantageous for improving the structural stability, thermal stability, and long-term cycle stability of the secondary particles. In addition, since a phosphate compound coating layer with high ionic conductivity is formed at the grain boundaries between the primary particles, the electrical resistance at the grain boundaries is reduced, which is advantageous for improving the rate performance of the positive electrode material.
[0046] In one embodiment, the addition amount of the lithium compound is selected such that the ratio of the total molar content of Ni, Co, M, and the metal elements in the metal phosphate to the molar content of Li is 1: (0.95 to 1.10). Within the above range, not only can Li / Ni cation mixing be reduced, but it is also possible to prevent the processability and safety from being impaired due to too high an amount of residual lithium on the surface of the sintered product.
[0047] Specifically, the lithium compound includes at least one of lithium carbonate, lithium hydroxide, lithium acetate, lithium nitrate, and lithium oxalate. Preferably, the lithium compound is lithium hydroxide.
[0048] The metal phosphate may have an average particle size of less than 0.5 μm, for example, 0.001 μm, 0.01 μm, 0.05 μm, 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm or 0.45 μm.
[0049] The metal element of the metal phosphate is at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn. In the case of a combination of a plurality of elements, typical examples include, but are not limited to, a combination of SrHPO4 and Zr(HPO4)2, a combination of MgHPO4 and Al(H2PO4)3, etc.
[0050] The content of phosphate ions in the metal phosphate is 0.03 wt% to 0.3 wt% of the total mass of the mixture, and may be, for example, 0.03 wt%, 0.05 wt%, 0.1 wt%, 0.15 wt%, 0.2 wt%, or 0.3 wt%, etc. Preferably, the content of phosphate ions in the metal phosphate is 0.075 wt% to 0.175 wt% of the total mass of the mixture. Through repeated testing, the inventors have found that by controlling the content of phosphate ions within the above range, a good primary particle covering effect can be obtained without reducing the capacity of the positive electrode material.
[0051] Ni a Co b M c O or Ni a Co b M cDuring the mixing process of (OH)2, a lithium compound, and a metal phosphate, the mixing time is 0.3 h to 2.0 h. For example, it may be 0.3 h, 0.4 h, 0.5 h, 0.7 h, 0.8 h, 1.0 h, 1.2 h, 1.5 h, or 2.0 h, etc., but it is not limited to the values listed above. Other unlisted values within the above range are also applicable. The mixing temperature is 10°C to 50°C. For example, it is 10°C, 15°C, 25°C, 30°C, 35°C, 40°C, 45°C, or 50°C, etc. Preferably, the mixing temperature is 10°C to 40°C. Through repeated tests, the inventors found that under the above mixing conditions, not only can sufficient and uniform mixing be achieved, but also the occurrence of side reactions in the mixed raw materials due to too high a temperature can be prevented.
[0052] Note that the sintered product is an active material having a first coating layer, and the active material has the general formula: Li b Ni x Co y M z R w O2 (where 0.95 ≤ b ≤ 1.10, 0.8 ≤ x < 1, 0 < y + z + w ≤ 0.2, x + y + z + w = 1, 0.0001 ≤ w ≤ 0.003, M is at least one of Mn and Al, and R is at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn).
[0053] The first coating layer consists of a phosphate compound containing at least one of Li3PO4 and LiR k (PO4) r (where 0 < k ≤ 2, 0 < r ≤ 2, and R is at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn).
[0054] Preferably, the mixture is sintered at 650°C to 850°C for 6 h to 20 h in an oxygen-containing atmosphere, pulverized, and sieved to obtain a sintered product containing a plurality of primary particles having a first coating layer.
[0055] The average particle size D50 of the primary particles is from 200 nm to 1000 nm, and may be, for example, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, or 1000 nm.
[0056] In one embodiment, the metal phosphate reacts with the lithium compound at high temperature to form a first coating layer of the primary particles. The thickness of the first coating layer is 0.005 μm to 0.05 μm, and may be, for example, 0.005 μm, 0.01 μm, 0.015 μm, 0.02 μm, 0.025 μm, 0.03 μm, 0.035 μm, 0.04 μm, 0.045 μm, or 0.05 μm. The thickness of the first coating layer may be a value other than the above as long as it is within the above range, and is not limited here.
[0057] The content of crystalline phosphate ions in the first coating layer is 5 wt% to 50 wt% of the total mass of phosphate ions, and may be, for example, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 30 wt%, 40 wt%, or 50 wt%.
[0058] The oxygen content in the oxygen-containing atmosphere is ≧95%. The sintering temperature may be, for example, 650°C, 700°C, 720°C, 730°C, 750°C, 770°C, 780°C, 800°C, or 850°C, and preferably, the sintering temperature is 720°C to 800°C, but is not limited to the values listed above, and other values not listed may be applied as long as they are within the range of the sintering temperature. After repeated testing, the inventors found that sufficient oxygen can promote the oxidation of divalent nickel to trivalent nickel, reduce Li / Ni cation mixing, and improve the capacity of the positive electrode material, and that the above temperature range is advantageous for the formation of a layered structure without decomposing the material.
[0059] The sintering time may be, for example, 6h, 8h, 10h, 12h, 15h, 18h, or 20h, but is not limited to the values listed above, and other values not listed may be applied as long as they are within the range of the sintering time. After repeated testing, the inventors found that the above sintering time can effectively form a layered structure and a uniform primary particle coating layer, and can simultaneously satisfy various performance requirements of the positive electrode material.
[0060] During the sintering process, controlling the particle size of the metal phosphate is advantageous in forming a uniform first coating layer on the surface of the primary particles. In addition, controlling the content of crystalline phosphate ions in the first coating layer to 5 wt% to 50 wt% can further stabilize the bond between the coating layer and the surface of the positive electrode material. The primary particle coating can prevent the primary particles inside the positive electrode material from directly contacting the electrolyte during secondary particle cracking, suppressing side reactions, and is advantageous in improving the structural stability, thermal stability, and long-term cycle stability of the secondary particles. In addition, since a phosphate compound coating layer with high ionic conductivity is formed at the crystal grain boundaries between the primary particles, the electrical resistance at the crystal grain boundaries is reduced, which is advantageous in improving the rate characteristics of the positive electrode material.
[0061] <Process S200> In this step, the sintered product is washed with a solvent at 50° C. or less and dried to obtain the positive electrode material. The positive electrode material includes secondary particles that are aggregates of primary particles, and a second coating layer that forms the surface of the secondary particles and contains a phosphate compound.
[0062] The method for producing a positive electrode material according to the present invention realizes primary particle coating and metal cation doping on the active material during the sintering process, and further uses a solvent containing a non-aqueous substance to wash the sintered product, thereby realizing secondary particle coating on the positive electrode material during the washing process, and suppressing the loss of lattice lithium on the surface of the positive electrode material, thereby improving its rate characteristic, thermal stability, and cycle stability.
[0063] In some embodiments, the solvent comprises water and a non-aqueous substance, i.e., the solvent is obtained by dissolving a non-aqueous substance in an aqueous solution, the non-aqueous substance comprising at least one of phosphoric acid, metaphosphoric acid, phosphorous acid, metaphosphorous acid, pyrophosphoric acid, hypophosphorous acid, soluble phosphate, soluble metaphosphate, soluble phosphite, soluble metaphosphite, soluble pyrophosphate, and soluble hypophosphite, preferably at least one of H3PO4, NH4H2PO4, (NH4)2HPO4, (NH4)3PO4, NaH2PO4, Na2HPO4, and Na3PO4.
[0064] Preferably, the content of phosphate ions in the solvent is 0.1wt% to 0.7wt% of the total mass of the sintered material, and may be, for example, 0.1wt%, 0.15wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, or 0.7wt%. Preferably, the content of phosphate ions in the solvent is 0.3wt% to 0.5wt% of the total mass of the sintered material. After repeated testing, the inventors found that by controlling the content of phosphate ions within the above range, a good secondary particle covering effect can be obtained without reducing the capacity of the positive electrode material.
[0065] As can be seen, during the solvent cleaning process, the non-aqueous materials remaining on the surface of the sintered material can react with the lithium on the surface of the sintered material to form a coating layer, which has high lithium ion conductivity and can not only improve the rate performance of the material, but also effectively reduce the corrosion degree of the positive electrode material surface caused by the electrolyte, which is favorable for improving the cycle performance of the positive electrode material.
[0066] In a preferred embodiment of the present invention, the cleaning temperature is 10°C to 50°C, and specifically may be 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, or 50°C, but is not limited to the values listed above, and other values not listed above may also be applied as long as they are within the above temperature range.
[0067] In a preferred embodiment of the present invention, the cleaning time is 10 min to 120 min, and specifically may be 10 min, 20 min, 30 min, 60 min, 90 min, or 120 min, but is not limited to the values listed above, and other values not listed above may also be applied as long as they are within the above range.
[0068] In a preferred embodiment of the present invention, the concentration of the slurry consisting of the sinter and the solvent (sinter (g) / solvent (L)) is 500 g / L to 2000 g / L, and may be specifically 500 g / L, 800 g / L, 1000 g / L, 1250 g / L or 2000 g / L. If the concentration of the slurry is too high, the amount of solvent used is insufficient, which is disadvantageous for removing the lithium content on the material surface, and if the free lithium content on the positive electrode material surface is too high, it is likely to cause the generation of a large amount of gas and an increase in surface impedance. On the other hand, if the concentration of the slurry is too low, the cleaning time increases, which is likely to cause damage to the structure between the primary particles inside the material, the loss of lattice lithium in the primary particles near the surface of the secondary particles consisting of the primary particles, and the loss of M oxide or lithium-M composite compound on the surface.
[0069] The solubility of lithium in water on the surface of the positive electrode material varies with temperature, so controlling the cleaning temperature within an appropriate range can contribute to controlling the lithium content on the surface of the material, which is also advantageous for reducing gas generation and improving processability. The cleaning temperature, slurry concentration, and cleaning time affect each other, and controlling these three conditions together can protect the surface structure of the positive electrode material particles, improve the corrosion resistance of the particle surface, control the lithium content on the surface of the material, and reduce gas generation, which effectively combines discharge capacity, thermal stability, rate characteristics, safety, and cycle characteristics.
[0070] In one preferred embodiment of the invention, the drying is carried out under a nitrogen atmosphere, in other embodiments the drying may be carried out under other protective gases, for example argon atmosphere.
[0071] In a preferred embodiment of the present invention, the drying temperature is 80°C to 200°C, and specifically may be 80°C, 100°C, 120°C, 150°C, 180°C, or 200°C, but is not limited to the values listed above, and other values not listed above may also be applied as long as they are within the above temperature range.
[0072] In a preferred embodiment of the present invention, the drying time is 5 h to 48 h, and specifically may be 5 h, 10 h, 12 h, 15 h, 18 h, 20 h, 24 h, 28 h, 32 h, 36 h, 40 h, 44 h, 48 h, or the like, but is not limited to the values listed above, and other values not listed above may also be applied as long as they are within the above range of time.
[0073] The average particle size of the secondary particles is 3 μm to 20 μm, and may be, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 15 μm, or 20 μm, and preferably, the average particle size of the secondary particles is 10 μm to 13 μm. The inventors conducted repeated tests and found that when the average particle size of the secondary particles is controlled within the range of 3 μm to 20 μm, the problem of cracking of the secondary particles during cycling can be avoided, and this is advantageous in improving the structural stability, thermal stability, and long-term cycle stability of the secondary particles.
[0074] The thickness of the second coating layer is 0.02 μm to 0.2 μm, and may be, for example, 0.02 μm, 0.03 μm, 0.05 μm, 0.08 μm, 0.1 μm, 0.13 μm, 0.15 μm, 0.18 μm, or 0.2 μm. The thickness of the second coating layer may be a value other than the above as long as it is within the range of the above values, and is not limited here.
[0075] Specifically, the non-aqueous substance in the solvent reacts with the residual lithium on the surface of the sintered body to form the second coating layer. The content of crystalline phosphate ions in the second coating layer is 5 wt% to 50 wt% of the total mass of phosphate ions, and specifically may be 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, or 50 wt%.
[0076] Furthermore, after the sintered body is washed with a solvent and dried, the method further comprises: The method includes a step of subjecting the sintered product after washing and drying to a heat treatment at 150° C. to 600° C. for 4 hours to 10 hours in an oxygen-containing atmosphere to obtain the positive electrode material.
[0077] Preferably, the heat treatment temperature may be specifically 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 550°C, or 600°C, and the heat treatment time may be specifically 4h, 5h, 6h, 7h, 8h, 9h, or 10h, but is not limited to the values listed above, and other values not listed may also be applied as long as they are within the range of the above numerical values.
[0078] As can be seen, by heat treating the washed and dried sintered product, the phosphate compound can be coated more uniformly and firmly on the surface of the sintered product, and the non-aqueous substance reacts with the residual lithium on the surface of the sintered product to reduce the residual alkali, thereby forming a phosphate compound with high lithium ion conductivity, and contributing to control the content of crystalline phosphate ions in the secondary particle coating layer, thereby improving processability and rate characteristics without causing decomposition of the sintered product and lithium precipitation.
[0079] Preferably, the mixing method used in the present invention may be a mechanical mixing method, such as a high speed mixer or a VC mixer.
[0080] The method for preparing a positive electrode material according to the present invention realizes primary particle coating and metal cation doping on the positive electrode material during the sintering process, and secondary particle coating on the positive electrode material during the washing process, thereby forming a uniform coating layer on the surface of the positive electrode material and better suppressing the loss of lattice lithium on the surface of the positive electrode material, thereby improving its rate performance, thermal stability and cycle stability.
[0081] According to a third aspect of the present invention, there is further provided a lithium ion battery comprising the above-mentioned positive electrode material or a positive electrode material produced by the above-mentioned method for producing a positive electrode material. EXAMPLES
[0082] The present invention will be further described below with reference to several examples. The present invention is not limited to the following specific examples, and may be modified as appropriate without departing from the spirit and scope of the present invention.
[0083] <Example 1> In this example, a method for producing a positive electrode material was carried out, which included the following steps (1) to (4).
[0084] (1) Precursor Ni 0.88 Co 0.09 Al 0.03 (OH)2, lithium hydroxide, and SrHPO4 with an average particle size D50 of 0.2 μm were uniformly mixed in a high-speed mixer at a mixing temperature of 30°C for a mixing time of 1 hour to obtain a mixture, in which Li / (Ni+Co+Al)=1.05 and the phosphate ion content was 0.3 wt% of the total mass of the mixture. (2) The mixture is sintered at 750°C for 10h in an atmosphere with an oxygen content of ≥ 95%, then crushed and sieved to obtain the sintered Li that is coated with a phosphate compound and doped with Sr. 1.05 Ni 0.88 Co 0.09 Al 0.03 Sr 0.0026 Got O2. (3) The sinter Li was dissolved in a solvent (H2O + NH4H2PO4) in a ratio of 500 g of sinter to 1 L of solvent. 1.05 Ni 0.88 Co 0.09 Al 0.03 Sr 0.0026 The mixture was washed with O2 at 20°C for 10 min (in the mixture of the sinter and solvent, the phosphate ion content was 0.5 wt% of the total mass of the sinter), and the cake obtained by pressure filtration was dried at 80°C for 24 h to obtain a positive electrode material coated with secondary particles. (4) The positive electrode material is sintered at 200°C for 8 hours in an atmosphere with an oxygen content of ≥ 95%, then crushed and sieved to obtain the positive electrode material Li coated with a phosphate compound. 1.05 Ni 0.88 Co 0.09 Al 0.03 Sr0.0026 Got O2.
[0085] The positive electrode material obtained in this example contained a plurality of secondary particles, and the secondary particles were aggregates of a plurality of primary particles. A first coating layer was formed on the surface of the primary particles, and a second coating layer was formed on the surface of the secondary particles. The primary particles had an average particle size of 0.6 μm, and the secondary particles had an average particle size of 12 μm. The material of the primary particles was Li 1.05 Ni 0.88 Co 0.09 Al 0.03 Sr 0.0026 The primary particles were agglomerates of primary particles coated with the first coating layer, the thickness of the second coating layer was 0.06 μm, and the materials of the second coating layer were Li3PO4 and Li3Al(PO4)2. The surface average phosphorus content a of the positive electrode material was 0.231 wt%, and the single-point phosphorus content a' at any 10 points on the surface was measured to be a minimum of 0.209 wt% and a maximum of 0.245 wt%.
[0086] Scanning electron micrographs of the positive electrode material S1 prepared in this example are shown in Figures 3a and 3b.
[0087] The performance test results of the positive electrode material S1 prepared in this example are shown in Table 1.
[0088] <Example 2> In this example, a method for producing a positive electrode material was carried out, which included the following steps (1) to (4). (1) Precursor Ni 0.83 Co 0.11 Mn 0.06 (OH)2, lithium hydroxide, and Zr(HPO4)2 with an average particle size D50 of 0.4 μm were mixed uniformly using a high-speed mixer at a mixing temperature of 25°C for a mixing time of 2 hours to obtain a mixture, in which Li / (Ni+Co+Al)=1.03 and the phosphate ion content was 0.2 wt% of the total mass of the mixture. (2) The mixture is sintered at 800°C for 20h in an atmosphere with an oxygen content of ≥ 95%, then crushed and sieved to obtain the sintered Li that is coated with a phosphate compound and doped with Zr. 1.03 Ni 0.83 Co 0.11 Mn 0.06 Zr 0.0009 Got O2. (3) Solvent (HO+N a H2PO4) to the above sintered Li 1.03 Ni 0.83 Co 0.11 Mn 0.06 Zr 0.0009 The mixture was washed with O2 at 30°C for 20 min (in the mixture of the sinter and solvent, the phosphate ion content was 0.3 wt% of the total mass of the sinter), and the cake obtained by pressure filtration was dried at 120°C for 20 h to obtain a positive electrode material coated with secondary particles. (4) The positive electrode material is sintered at 300°C for 6 hours in an atmosphere with an oxygen content of ≥ 95%, then crushed and sieved to obtain the positive electrode material Li coated with a phosphate compound. 1.03 Ni 0.83 Co 0.11 Mn 0.06 Zr 0.0009 Got O2.
[0089] The positive electrode material obtained in this example contained a plurality of secondary particles, and the secondary particles were aggregates of a plurality of primary particles. A first coating layer was formed on the surface of the primary particles, and a second coating layer was formed on the surface of the secondary particles. The primary particles had an average particle size of 0.7 μm, and the secondary particles had an average particle size of 11.5 μm. The material of the primary particles was Li 1.03 Ni 0.83 Co 0.11 Mn 0.06 Zr 0.0009The primary particles were agglomerates of primary particles coated with the first coating layer, the thickness of the second coating layer was 0.10 μm, and the material of the second coating layer was Li3PO4. The positive electrode material had a surface average phosphorus content a of 0.135 wt%, and the single-point phosphorus content a' at any 10 points on the surface was measured to have a minimum value of 0.125 wt% and a maximum value of 0.142 wt%.
[0090] The performance test results of the positive electrode material S2 prepared in this example are shown in Table 1.
[0091] <Example 3> In this example, a method for producing a positive electrode material was carried out, which included the following steps (1) to (4). (1) Precursor Ni 0.88 Co 0.09 Al 0.03 (OH)2, lithium hydroxide, MgHPO4 with an average particle size D50 of 0.05 μm, and Zr(HPO4)2 with a median size of 0.4 μm were uniformly mixed in a high-speed mixer at a mixing temperature of 20°C for a mixing time of 1.5 hours to obtain a mixture, in which Li / (Ni+Co+Al)=1.00 and the phosphate ion content was 0.1 wt% of the total mass of the mixture. (2) The mixture is sintered at 650°C for 20h in an atmosphere with an oxygen content of ≥ 95%, then crushed and sieved to obtain the sintered LiNi 0.88 Co 0.09 Al 0.03 Mg 0.0009 Zr 0.0004 Got O2. (3) The sintered LiNi was dissolved in a solvent (H2O + H3PO4) in a ratio of 1000g of sintered material to 1L of solvent. 0.88 Co 0.09 Al 0.03 Mg 0.0009 Zr 0.0004The mixture was washed with O2 at 40°C for 30 min (the phosphate ion content in the mixture of the sinter and solvent was 0.15 wt% of the total mass of the sinter), and the cake obtained by pressure filtration was dried at 150°C for 12 h to obtain a positive electrode material coated with secondary particles. (4) The positive electrode material is sintered at 500°C for 10 hours in an atmosphere with an oxygen content of ≥ 95%, crushed, and sieved to obtain a positive electrode material LiNi 0.88 Co 0.09 Al 0.03 Mg 0.0009 Zr 0.0004 Got O2.
[0092] The positive electrode material obtained in this example contained a plurality of secondary particles, and the secondary particles were aggregates of a plurality of primary particles. A first coating layer was formed on the surface of the primary particles, and a second coating layer was formed on the surface of the secondary particles. The primary particles had an average particle size of 0.3 μm, and the secondary particles had an average particle size of 12 μm. The material of the primary particles was LiNi 0.88 Co 0.09 Al 0.03 Mg 0.0009 Zr 0.0004 The primary particles were agglomerates of primary particles coated with the first coating layer, the thickness of the second coating layer was 0.15 μm, and the material of the second coating layer was Li3PO4. The positive electrode material had a surface average phosphorus content a of 0.069 wt%, and the single-point phosphorus content a' at any 10 points on the surface was measured to have a minimum value of 0.063 wt% and a maximum value of 0.074 wt%.
[0093] The performance test results of the positive electrode material S3 prepared in this example are shown in Table 1.
[0094] <Example 4> In this example, a method for producing a positive electrode material was carried out, which included the following steps (1) to (4). (1) Precursor Ni 0.88 Co 0.09 Al 0.03(OH)2, lithium hydroxide, and SrHPO4 with an average particle size D50 of 0.2 μm were mixed uniformly in a high-speed mixer at a mixing temperature of 15°C for a mixing time of 2 hours to obtain a mixture, in which Li / (Ni+Co+Al)=0.95 and the phosphate ion content was 0.03 wt% of the total mass of the mixture. (2) The mixture is sintered at 730°C for 6h in an atmosphere with an oxygen content of ≥ 95%, then crushed and sieved to obtain the sintered LiNi 0.88 Co 0.09 Al 0.03 Sr 0.0003 Got O2. (3) The above sintered LiNi was dissolved in water in a ratio of 2000 g of sintered material to 1 L of solvent (H2O + NaH2PO4 + H3PO4, where the molar ratio of phosphate ions in NaH2PO4 and H3PO4 was 1:1). 0.88 Co 0.09 Al 0.03 Sr 0.0003 The mixture was washed with O2 at 50°C for 60 min (the phosphate ion content in the mixture of the sinter and solvent was 0.1 wt% of the total mass of the sinter), and the cake obtained by pressure filtration was dried at 200°C for 10 h to obtain a positive electrode material coated with secondary particles. (4) The positive electrode material is sintered at 500°C for 5h in an atmosphere with an oxygen content of ≥ 95%, crushed, and sieved to obtain the positive electrode material LiNi 0.88 Co 0.09 Al 0.03 Sr 0.0003 Got O2.
[0095] The positive electrode material obtained in this example contained a plurality of secondary particles, and the secondary particles were aggregates of a plurality of primary particles. A first coating layer was formed on the surface of the primary particles, and a second coating layer was formed on the surface of the secondary particles. The primary particles had an average particle size of 0.6 μm, and the secondary particles had an average particle size of 11 μm. The material of the primary particles was LiNi 0.88 Co 0.09 Al 0.03 Sr 0.0003The primary particles were agglomerates of primary particles coated with the first coating layer, the thickness of the second coating layer was 0.18 μm, and the materials of the second coating layer were Li3PO4 and Li2Zr(PO4)2. The surface average phosphorus content a of the positive electrode material was 0.039 wt%, and the single-point phosphorus content a' at any 10 points on the surface was measured to be a minimum of 0.036 wt% and a maximum of 0.041 wt%.
[0096] The performance test results of the positive electrode material S4 prepared in Example 4 are shown in Table 1.
[0097] <Comparative Example 1> The manufacturing method of Example 1 was carried out in the same manner, except that SrHPO4 was not added in step (1) and the solvent used in step (3) was pure water.
[0098] The performance test results of the positive electrode material D1 prepared in Comparative Example 1 are shown in Table 1.
[0099] Scanning electron microscope photographs of the positive electrode material D1 prepared in Comparative Example 1 are shown in FIG. 4a and FIG. 4b.
[0100] The surface average phosphorus content a of the positive electrode material D1 produced in the comparative example was measured to be 0 wt %, and the single-point phosphorus contents a' at any ten points on the surface were all measured to be 0 wt %.
[0101] <Comparative Example 2> The same production method as in Example 1 was carried out, except that the solvent used in step (3) was pure water.
[0102] The performance test results of the positive electrode material D2 prepared in Comparative Example 2 are shown in Table 1.
[0103] The surface average phosphorus content a of the positive electrode material D2 produced in the comparative example was 0.092 wt%, and the single-point phosphorus content a' at any 10 points on the surface was measured to be a minimum of 0.075 wt% and a maximum of 0.116 wt%.
[0104] <Comparative Example 3> The same production method as in Example 1 was carried out, except that SrHPO4 was not added in step (1).
[0105] The performance test results of the positive electrode material D3 prepared in Comparative Example 3 are shown in Table 1. The surface average phosphorus content a of the positive electrode material D3 produced in the comparative example was 0.154 wt%, and the single-point phosphorus content a' at any 10 points on the surface was measured to be a minimum of 0.135 wt% and a maximum of 0.173 wt%.
[0106] <Comparative Example 4> The manufacturing method of Example 1 was carried out in the same manner, except that the average particle size of SrHPO4 added in step (1) was 10 μm.
[0107] The performance test results of the positive electrode material D4 prepared in Comparative Example 4 are shown in Table 1. The surface average phosphorus content a of the positive electrode material D4 produced in the comparative example was 0.245 wt%, and the single-point phosphorus content a' at any 10 points on the surface was measured to be a minimum of 0.183 wt% and a maximum of 0.302 wt%.
[0108] <Comparative Example 5> The manufacturing method was the same as in Example 1, except that the solvent washing was performed at a washing temperature of 80° C. for a washing time of 60 minutes.
[0109] The performance test results of the positive electrode material D5 prepared in Comparative Example 5 are shown in Table 1. The surface average phosphorus content a of the positive electrode material D5 produced in the comparative example was 0.198 wt%, and the single-point phosphorus content a' at any 10 points on the surface was measured to be a minimum of 0.152 wt% and a maximum of 0.226 wt%.
[0110] (Testing Method) A morphological analysis was performed on the positive electrode material using a scanning electron microscope, and scanning electron micrographs thereof were obtained. Point analysis was performed using an energy dispersive X-ray analyzer (EDS) attached to a scanning electron microscope to measure the single-point phosphorus content a' at multiple points on the surface of the positive electrode material. In addition, an area analysis was carried out using an energy dispersive X-ray analyzer (EDS) attached to a scanning electron microscope to measure the surface average phosphorus content a of the positive electrode material.
[0111] The electrochemical performance evaluation was performed on the positive electrode material manufactured using the button half cell, and the specific method was as follows. The positive electrode material, conductive carbon black Super P, and polyvinylidene fluoride (PVDF) were weighed in a mass ratio of 96:2:2, N-methylpyrrolidone was added so that the solid content was 50%, and the mixture was made into a viscous slurry using a high-speed disperser. The mixture was uniformly applied to aluminum foil with a blade, and then dried in an oven at 80 °C. The product was then rolled and cut to form a positive electrode sheet with a diameter of 14 mm. A lithium sheet with a diameter of 16 mm was used as the negative electrode sheet, a Celgard polypropylene (PP) film was used as the separator, and a carbonate solution of LiPF6 with a concentration of 1 mol / L (volume ratio of diethyl carbonate (DEC) / ethylene carbonate (EC) = 1:1) was used as the electrolyte, and the button half cell was assembled in a glove box filled with argon gas.
[0112] Using a LAND battery test system, the capacity, initial coulombic efficiency, and rate performance were measured at 25° C. and 3.0 V to 4.3 V, with the reference capacity set to 200 mA / g and the current density corresponding to 1 C being 200 mA / g.
[0113] The total amount of lithium compounds on the surface of the positive electrode material was measured using a potentiometric titrator. Specifically, the amount was titrated with hydrochloric acid, and the amount of consumed hydrochloric acid was converted into the amount of lithium compounds.
[0114] An ion beam cutter was used to cut particles of the positive electrode material, and then a high-precision electron spectrometer was used to perform elemental line analysis on the cross section of the cut particles. Based on the element distribution curve obtained by the line analysis, the distribution position of the phosphate compound coating layer was calculated.
[0115] A thermal stability test was performed on the electrode material in a closed high-pressure crucible under nitrogen atmosphere at 5°C / min using a Netzsch differential scanning calorimeter to obtain the differential scanning calorimeter curves. The electrode material was the active material scraped off from the electrode sheet in a fully charged state after the button cell was cycled 2.5 times at 0.1C.
[0116] The structure and composition of the positive electrode material were identified using an X-ray diffractometer manufactured by BRUKER, and furthermore, Rietveld analysis was performed on the X-ray diffraction pattern to calculate the content of crystalline phosphate ions in the phosphate compound of the coating layer.
[0117] The results of the above performance tests are as follows (Table 1: Performance Comparison Results Table).
[0118] [Table 1]
[0119] As can be seen from Figures 3a and 3b, in the positive electrode material obtained in Example 1, a uniform coating layer is formed on the surface of the secondary particles, and the gaps between the primary particles are filled with a phosphate compound, resulting in very close contact at the grain boundaries and very close bonding between the coating layer and the positive electrode material.
[0120] As can be seen from Figures 4a and 4b, the positive electrode material obtained in Comparative Example 1 had relatively smooth surfaces of secondary particles, no coating layer, and large gaps between the primary particles, allowing the electrolyte to easily penetrate into the secondary particles.
[0121] As shown in FIG. 5, the positive electrode material obtained in Example 1 has better rate characteristics than that of Comparative Example 1, which indicates that the rate characteristics of the positive electrode material in which the primary particles were not coated with a phosphate compound were clearly inferior.
[0122] As shown in FIG. 6, the decomposition temperature and heat release amount of the positive electrode material obtained in Example 1 were superior to those of Comparative Example 1, which shows that coating the primary particles and secondary particles of the positive electrode material with a phosphate compound can contribute to improving the thermal stability of the positive electrode material.
[0123] As can be seen from Table 1, the positive electrode materials prepared in Examples 1 to 5 of the present invention all had excellent electrochemical performance, a discharge capacity of 209 mAh / g or more, an initial Coulombic efficiency of about 90%, good rate characteristics, excellent long-term cycle characteristics, and a low free lithium content on the surface.
[0124] Comparing the experimental data of Example 1 and Comparative Example 2 in Table 1, it was found that when the primary particles or secondary particles were not coated with a phosphate compound, the produced positive electrode material had a somewhat high residual alkali on the surface, and the rate characteristics, discharge capacity, and cycle characteristics were all significantly impaired. Furthermore, the above comparison further showed that when washing was performed without using a solvent containing a non-aqueous substance during secondary coating, the obtained positive electrode material had a very high residual alkali on the surface and did not pass the processability test.
[0125] In addition, by comparing the experimental data of Example 1 with those of Comparative Examples 3 and 4, it was found that if metal phosphate (SrHPO4) was not added during the primary coating or if the particle size of the added metal phosphate was too large, it was not favorable for the metal phosphate to form a uniform first coating layer on the surface of the primary particles, and the produced positive electrode material had a somewhat high residual alkali on the surface, and the rate characteristics, discharge capacity, and cycle characteristics were all significantly impaired.
[0126] In addition, by comparing the experimental data of Example 1 and Comparative Example 5, it was found that if the cleaning temperature is too high, the free lithium content on the surface is likely to be high and the coating layer on the surface of the active material is likely to be non-uniform, resulting in the impairment of the rate characteristics, discharge capacity, and cycle characteristics of the battery.
[0127] The present invention has been disclosed above with reference to the preferred embodiments, but these should not be construed as limiting the scope of the claims. Those skilled in the art may make various possible modifications and variations without departing from the spirit of the present invention. Therefore, the scope of protection of the present invention should be in accordance with the scope defined in the claims.
Claims
1. General formula: Li b Ni x Co y M z R w O 2 (wherein 0.95≦b≦1.10, 0.8≦x<1, 0<y+z+w≦0.2, x+y+z+w=1, 0.0001≦w≦0.003, M is at least one of Mn and Al, and R is a doping metal), and A coating layer including a first coating layer formed on a surface of the primary particles and a second coating layer formed on a surface of the secondary particles, The first coating layer and the second coating layer each contain a phosphoric acid compound, The positive electrode material is characterized in that a single-point phosphorus content a' at any point on the surface and its surface average phosphorus content a satisfy the following relationship: 0.9a≦a'≦1.1a (Note that a' and a were measured by the following method. When observing the positive electrode material using a scanning electron microscope (SEM), a point analysis was performed by EDS on any one point on the surface of the positive electrode material to measure the phosphorus content and obtain the value of a'. Also, a square region of 100 μm×100 μm was randomly selected in the field of view of the scanning electron microscope (SEM) and an area analysis was performed by EDS to measure the phosphorus content and obtain the value of a.)
2. The Li b Ni x Co y M z R w O 2 2. The cathode material of claim 1, wherein R comprises at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn.
3. The positive electrode material according to claim 1 or 2, which satisfies at least one of the following conditions a to k: a. The secondary particles have a spherical or nearly spherical shape; b. The primary particles have an average particle size of 200 nm to 1000 nm, and the secondary particles have an average particle size of 3 μm to 20 μm; c. The phosphate compound is Li 3 P.O. 4 and LiR k (P.O. 4 ) r (wherein 0<k≦2, 0<r≦2, and R includes at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn); d) The raw materials for producing the phosphoric acid compound in the first coating layer include a metal phosphate and a lithium compound, and the raw materials for producing the phosphoric acid compound in the second coating layer include at least one of phosphoric acid, metaphosphoric acid, phosphorous acid, metaphosphorous acid, pyrophosphoric acid, hypophosphorous acid, soluble phosphate, soluble metaphosphate, soluble phosphite, soluble metaphosphite, soluble pyrophosphate, and soluble hypophosphite; e. The content of phosphate ions in the phosphate compound in the first coating layer is 0.03 wt % to 0.3 wt % of the total mass of the secondary particles; f. The content of phosphate ions in the phosphate compound in the second coating layer is 0.1 wt % to 0.7 wt % of the total mass of the secondary particles and the first coating layer; g. The content of crystalline phosphate ions in the phosphate compound in the first coating layer or the second coating layer is 5 wt % to 50 wt % of the total mass of phosphate ions; h. the thickness of the first coating layer is 0.005 μm to 0.05 μm; i. the thickness of the second coating layer is 0.02 μm to 0.2 μm; j. 4 kN / cm of the positive electrode material 2 The powder conductivity under pressure is greater than 0.02 S / cm; k. The specific surface area of the positive electrode material is 0.2 m 2 / g to 2.0 m 2 / g.
4. Ni a Co b M c O or Ni a Co b M c (OH) 2 (wherein a+b+c=1, 0.8≦a<1, 0<b+c≦0.2, and M is at least one of Mn and Al), a lithium compound, and a metal phosphate are mixed together, and the resulting mixture is sintered to obtain a sintered product, the sintered product comprising a plurality of primary particles and a first coating layer that forms the surface of the primary particles and contains a phosphate compound, and the metal phosphate has an average particle size of less than 0.5 μm; A step of washing the sintered product with a solvent at 50° C. or less and drying the product to obtain a positive electrode material, a concentration of a slurry consisting of the sinter and the solvent during washing (sinter (g) / solvent (L)) is 500 g / L to 2000 g / L, a phosphate ion content in the solvent is 0.1 wt % to 0.7 wt % of the total mass of the sinter, and the cathode material includes secondary particles which are aggregates of primary particles, and a second coating layer which forms a surface of the secondary particles and contains a phosphate compound.
5. The method according to claim 4, which satisfies at least one of the following conditions a to f: a. The amount of the lithium compound added is such that the ratio of the total molar content of Ni, Co, M, and the metal elements in the metal phosphate to the molar content of Li is 1:(0.95 to 1.10); b. the lithium compound includes at least one of lithium carbonate, lithium hydroxide, lithium acetate, lithium nitrate, and lithium oxalate; c) The metal element of the metal phosphate is at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn; d. the content of phosphate ions in the metal phosphate is 0.03 wt % to 0.3 wt % of the total mass of the mixture; e. The mixing conditions for obtaining the mixture are 10°C to 50°C and solid-state mixing for 0.3 h to 2 h; f) The sintering conditions for obtaining the sintered product are as follows: sintering in an oxygen-containing atmosphere at 650°C to 850°C for 6 hours to 20 hours.
6. The manufacturing method described in claim 4, wherein the solvent comprises water and a non-aqueous substance, and the non-aqueous substance comprises at least one of phosphoric acid, metaphosphoric acid, phosphorous acid, metaphosphorous acid, pyrophosphoric acid, hypophosphorous acid, soluble phosphates, soluble metaphosphates, soluble phosphites, soluble metaphosphites, soluble pyrophosphates, and soluble hypophosphites.
7. The method according to claim 4 or 6, which satisfies at least one of the following conditions b to f: b. the washing temperature is between 10°C and 50°C; c. The cleaning time is 10 min to 120 min; d. The drying is carried out under a nitrogen atmosphere; e. the drying temperature is 80°C to 200°C; f) The drying time is 5 hours to 48 hours.
8. The sintered product is washed with a solvent, dried, and then The method according to claim 4, further comprising a step of heat-treating the sintered product after washing and drying in an oxygen-containing atmosphere at 150° C. to 600° C. for 4 h to 10 h to obtain the positive electrode material.
9. The method according to claim 4, which satisfies at least one of the following conditions a to f: a. the metal phosphate reacts with the lithium compound at high temperature to form a first coating layer on the primary particles; b. The phosphate ions in the solvent react with the residual lithium on the surface of the sinter to form a second coating layer on the secondary particles; c. The phosphate compound is Li 3 P.O. 4 and LiR k (P.O. 4 ) r (wherein 0<k≦2, 0<r≦2, and R is at least one of Co, Mn, Al, Ti, Zr, Sr, Mg, Ca, Y, Ba, Cu, W, Nb, La, Ce, Mo, and Sn); d. The content of crystalline phosphate ions in the phosphate compound in the first coating layer or the second coating layer is 5 wt % to 50 wt % of the total mass of phosphate ions; e. the average particle size of the primary particles is 200 nm to 1000 nm, and the thickness of the first coating layer is 0.005 μm to 0.05 μm; f) The secondary particles have an average particle size of 3 μm to 20 μm, and the second coating layer has a thickness of 0.02 to 0.2 μm.
10. A lithium ion battery comprising the positive electrode material according to any one of claims 1 to 3.
Citation Information
Patent Citations
Method for removing lithium ion battery nickel-rich material surface lithium residues by liquid phase precipitation method
CN102881911A
Preparation method of lithium phosphate coated lithium-ion battery ternary positive electrode material
CN110190254A
High-nickel positive electrode material, preparation method thereof and lithium ion secondary battery
CN112382741A
Positive electrode active material, positive electrode plate and lithium ion secondary battery
CN112447966A
Positive electrode active material, preparation method thereof and lithium ion battery
CN114050255A