Manufacturing method for electronic component mounting board

The use of an oxidation prevention film and temporary fixing film with controlled softening points addresses the issue of solder precoat oxidation in miniaturized components, enhancing soldering reliability by reducing defects.

JP7584114B2Active Publication Date: 2024-11-15PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023525391
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-03
Filing Date
2022-02-21
Publication Date
2024-11-15
Estimated Expiration
2042-02-21

AI Technical Summary

Technical Problem

The increased miniaturization of electronic components leads to larger surface area per unit volume, making solder precoats more susceptible to oxidation, which results in higher soldering defects.

Method used

A method involving the use of an oxidation prevention film composed of a first thermoplastic resin and a temporary fixing film with a lower softening point, applied to cover solder precoats, allowing electronic components to be placed and securely fixed before soldering, where the films soften in a controlled manner to prevent oxidation and ensure proper alignment during the reflow process.

Benefits of technology

This method significantly reduces soldering defects by preventing oxidation of solder precoats and ensuring stable, defect-free mounting of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584114000002
    Figure 0007584114000002
  • Figure 0007584114000003
    Figure 0007584114000003
  • Figure 0007584114000004
    Figure 0007584114000004
Patent Text Reader

Abstract

Disclosed is an electronic-component-mounting-substrate manufacturing method that includes: a step (i) for forming a temporary fixing film 13 so as to cover a plurality of solder precoats (11) that are formed on a plurality of lands (10b) on a substrate and antioxidant films (12) that are formed so as to cover the solder precoats; a step (ii) for disposing a plurality of electronic components (30) on the plurality of solder precoats (11) via the antioxidant films (12) and the temporary fixing film (13); and a step (iii) for soldering the plurality of electronic components (30) to the plurality of lands (10b) by melting the plurality of solder precoats (11). The antioxidant films (12) contain a first thermoplastic resin. The temporary fixing film (13) contains an activator and a second thermoplastic resin. The softening point of the second thermoplastic resin is equal to or lower than the softening point of the first thermoplastic resin.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a board having electronic components mounted thereon. [Background technology]

[0002] A reflow method is known as a method for soldering a plurality of electronic components to a substrate, in which the electronic components are soldered using a solder precoat that has been formed on the substrate in advance.

[0003] Patent Document 1 (JP Patent Publication 6-90079A) describes a method for producing a printed circuit board (1) having a fine pitch pad section (5) with a pad arrangement pitch of less than 0.5 mm and a rough pitch pad section (4) with a pad arrangement pitch of 0.5 mm or more, in which a solder paste (8) is printed on the pads (3) of the rough pitch pad section (4), a solder deposition composition (12) mainly composed of an organic acid lead salt and tin powder is then solidly applied to the fine pitch pad section (5), and the printed circuit board (1) is then heated to melt the solder paste (8) and form a solder layer (13) on the pads (3) of the rough pitch pad section (4). and forming a solder layer (13) by precipitating solder from the solder deposition composition (12) on the pads (3) of the fine-pitch pad portion (5), then applying a flux (15) onto the printed circuit board (1), mounting an electronic component (16) thereon, temporarily fixing the lead (17) to the solder layer (13) on the pad (3) by the adhesive force of the flux (15), heating the printed circuit board (1) on which the electronic component (16) is mounted to melt the solder layer (13), and soldering the lead (17) of the electronic component (16) to the pad (3). Paragraph 0026 of Patent Document 1 states that "It is preferable to clean the precoated substrate 14 with an alternative cleaning agent such as a surfactant, a higher alcohol solvent, or a terpene solvent, water, an alternative freon, or the like, to remove paste residues, solder balls, and the like." [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-90079 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, electronic components have become smaller, and solder precoats have become smaller accordingly. As the solder precoat becomes smaller, its surface area per unit volume increases, making the surface of the solder precoat more susceptible to oxidation. When the surface of the solder precoat becomes oxidized, soldering defects are more likely to occur.

[0006] In light of the above, an object of the present invention is to provide a method for manufacturing a substrate having electronic components mounted thereon, which can reduce soldering defects. [Means for solving the problem]

[0007] One aspect of the present invention relates to a method for manufacturing an electronic component mounting board, the method including the steps of: (i) forming a temporary fixing film so as to cover a plurality of solder precoats formed on a plurality of lands of a board and an oxidation prevention film formed so as to cover each of the plurality of solder precoats; (ii) arranging a plurality of electronic components on the plurality of solder precoats via the oxidation prevention film and the temporary fixing film; and (iii) soldering the plurality of electronic components to the plurality of lands by melting the plurality of solder precoats, the oxidation prevention film including a first thermoplastic resin, the temporary fixing film including an activator and a second thermoplastic resin, and the softening point of the second thermoplastic resin being equal to or lower than the softening point of the first thermoplastic resin. Effect of the Invention

[0008] According to the method for manufacturing an electronic component mounting board of the present invention, defects occurring when soldering electronic components can be reduced. The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings. [Brief description of the drawings]

[0009] [Figure 1A] 1A to 1C are cross-sectional views illustrating a process of an example of a manufacturing method according to the present invention. [Figure 1B] 1B is a cross-sectional view showing a schematic diagram of a step following the step in FIG. 1A. [Figure 1C] FIG. 2 is a cross-sectional view illustrating a step following the step in FIG. 1B. [Figure 1D] FIG. 1D is a cross-sectional view illustrating a step following the step in FIG. 1C. [Figure 1E] FIG. 1E is a cross-sectional view illustrating a step following the step in FIG. 1D. [Figure 1F] FIG. 1F is a cross-sectional view illustrating a step following the step in FIG. 1E. [Diagram 2] FIG. 4 is a diagram illustrating an example of a temperature profile of the substrate surface in step (iii). [Figure 3A] 4A to 4C are cross-sectional views each showing a schematic diagram of a part of an example of a process for forming a solder precoat. [Figure 3B] FIG. 3B is a cross-sectional view illustrating a step following the step in FIG. 3A. [Figure 3C] FIG. 3C is a cross-sectional view illustrating a step following the step in FIG. 3B. [Figure 3D] FIG. 3D is a cross-sectional view illustrating a step following the step in FIG. 3C. [Figure 3E] FIG. 3E is a cross-sectional view illustrating a step following the step in FIG. 3D. [Figure 4A] 5A to 5C are cross-sectional views illustrating a process of another example of a manufacturing method according to the present invention. [Figure 4B] FIG. 4B is a cross-sectional view illustrating a step following the step in FIG. 4A. [Figure 4C] FIG. 4C is a cross-sectional view illustrating a step following the step in FIG. 4B. [Figure 4D]FIG. 4D is a cross-sectional view illustrating a step following the step in FIG. 4C. [Figure 4E] FIG. 4E is a cross-sectional view illustrating a step following the step in FIG. 4D. [Figure 4F] FIG. 4F is a cross-sectional view illustrating a step following the step in FIG. 4E. [Figure 4G] FIG. 4C is a cross-sectional view illustrating a step following the step in FIG. 4F. [Figure 4H] FIG. 4C is a cross-sectional view illustrating a step following the step in FIG. 4G. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In the following, the embodiment of the present invention will be described with examples, but the present invention is not limited to the examples described below. In this specification, the description "numeric value A to numerical value B" includes numerical value A and numerical value B, and can be read as "numerical value A or more and numerical value B or less." In the following description, when a lower limit and an upper limit are exemplified for numerical values ​​of specific physical properties or conditions, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit.

[0011] (Method of manufacturing electronic component mounting board) The manufacturing method according to the present embodiment is a method for manufacturing an electronic component mounting board. This manufacturing method may be referred to as "manufacturing method (M)" below. The manufacturing method (M) includes steps (i), (ii), and (iii) in this order.

[0012] (Step (i)) Step (i) is a step of forming a temporary fixing film so as to cover the multiple solder precoats formed on the multiple lands of the substrate and the oxidation prevention film formed so as to cover each of the multiple solder precoats. The oxidation prevention film includes a first thermoplastic resin. The temporary fixing film includes an activator and a second thermoplastic resin. The softening point of the second thermoplastic resin is equal to or lower than the softening point of the first thermoplastic resin. Since both the oxidation prevention film and the temporary fixing film include a thermoplastic resin, they are softened by heating.

[0013] The oxidation-preventing film is formed so as to cover the surface of the solder precoat. Therefore, the oxidation-preventing film suppresses oxidation of the surface of the solder precoat. In other words, the oxidation-preventing film suppresses solder defects caused by oxidation of the surface of the solder precoat. The substrate on which the solder precoat is formed may be a commercially available substrate on which the solder precoat is formed. Alternatively, the solder precoat may be formed on the land of the substrate by a method to be described later.

[0014] The first thermoplastic resin contained in the oxidation-resistant film is, for example, rosin or modified rosin. Hereinafter, rosin and modified rosin may be collectively referred to as "rosins". Examples of modified rosins include modified rosins shown in the examples, but other modified rosins may be used, for example, natural rosins such as gum rosin and wood rosin, and derivatives thereof (polymerized rosin, hydrogenated rosin, disproportionated rosin, acid-modified rosin, rosin ester, etc.). The softening point of rosin can be changed by modifying it. The oxidation-resistant film may be a residue (flux residue) formed on the surface of the solder precoat when the solder precoat is formed. In that case, a part of the flux of the solder paste used to form the solder precoat forms the oxidation-resistant film. In that case, the thermoplastic resin contained in the flux becomes the first thermoplastic resin contained in the oxidation-resistant film. That is, when the residue of the solder paste is used as the oxidation-resistant film, a solder paste containing the first thermoplastic resin is used.

[0015] The temporary fixing film stably fixes the electronic components placed on the solder precoat until reflow is performed. By using the temporary fixing film, it is possible to prevent the electronic components from being misaligned and being improperly mounted.

[0016] The temporary bonding film can be formed by applying a temporary bonding agent (material for the temporary bonding film) so as to cover the solder precoat and the oxidation prevention film. After applying the temporary bonding agent, a process of drying and / or heat treating the temporary bonding agent may be performed as necessary. There is no limitation on the method of applying the temporary bonding agent, and it may be applied by screen printing using a mask or by using a dispenser.

[0017] The temporary fixing film includes an activator and a second thermoplastic resin, and further includes other components as necessary. The second thermoplastic resin may be a rosin. Examples of the other components include a component that increases viscosity and a liquid component (solvent or dispersion medium). The activator is a substance that facilitates soldering. The activator may be an activator used in a known solder flux. Examples of the activator include abietic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dimer acid, propionic acid, 2,2-bishydroxymethylpropionic acid, tartaric acid, malic acid, glycolic acid, diglycolic acid, thioglycolic acid, dithioglycolic acid, stearic acid, 12-hydroxystearic acid, palmitic acid, oleic acid, and modified versions thereof. Other activators having a reducing action include, for example, amines and halides. Examples of components that increase viscosity include known components used as thickeners (or thixotropic agents), such as castor wax, amide-based thixotropic agents, sorbitol-based thixotropic agents, etc. By using a temporary fixing film containing an activator, it becomes possible to remove the oxide film on the terminals of electronic components during the reflow process, thereby suppressing the occurrence of solder defects.

[0018] An example of the liquid component contained in the temporary fixing film includes hexyl diglycol (boiling point: about 260°C). The liquid component may have a boiling point higher than the melting point of the solder in the solder precoat. For example, the liquid component may be alcohol, polyol, glycol ether, or other organic compounds (e.g., glycol, ketone, hydrocarbon, ester, lupineol, etc.) having a boiling point in the range of 230 to 320°C. Among these, a substance with a relatively high viscosity is preferable.

[0019] Examples of modified rosins that can be used as the second thermoplastic resin include the modified rosins exemplified as the modified rosins that can be used in the oxidation prevention film. The softening point of the rosin can be changed by modifying the rosin. The temporary fixing film may be formed using a solder flux having a relatively high viscosity.

[0020] The viscosity of the temporary fixing film may be in the range of 20 to 200 Pa·s (for example, in the range of 50 to 180 Pa·s). By making the viscosity of the temporary fixing film 20 Pa·s or more, the electronic components can be stably fixed temporarily. In order to fix the electronic components more stably, the viscosity of the temporary fixing film is preferably 50 Pa·s or more. ·s It is particularly preferable that the viscosity is equal to or higher than this. The viscosity can be measured using a rheometer manufactured by Anton Paar and a 1.993° cone. The above viscosity values ​​are values ​​measured at 25°C.

[0021] The softening point T2 (°C) of the second thermoplastic resin is equal to or lower than the softening point T1 (°C) of the first thermoplastic resin, and may be lower than T1. The oxidation prevention film can be considered to start softening at the softening point T1 of the first thermoplastic resin. Similarly, the temporary fixing film can be considered to start softening at the softening point T2 of the second thermoplastic resin. Therefore, hereinafter, the softening point T1 and the softening point T2 may be described as the softening temperatures of the oxidation prevention film and the temporary fixing film. In this specification, the softening point of rosins means a value measured by the method described in JIS K 5902. Since various rosins with different softening points are commercially available, the softening points T1 and T2 can be easily adjusted by using them.

[0022] The first thermoplastic resin is usually the main component of the oxidation prevention film. The second thermoplastic resin is usually the main component of the temporary fixing film. Here, the main component means the component with the highest content rate among the components excluding the liquid component (solvent or dispersion medium). The main component usually accounts for 50 mass % or more of the components excluding the liquid component. Note that each of the first and second thermoplastic resins may be composed of multiple thermoplastic resins.

[0023] The softening point T1 of the first thermoplastic resin may be in the range of 50 to 220°C (for example, in the range of 70 to 180°C). The softening point T2 of the second thermoplastic resin may be in the range of 50 to 220°C (for example, in the range of 70 to 180°C). The softening points T1 and T2 may satisfy 0≦(T1-T2)≦65. The value of (T1-T2) may be in the range of 0 to 110(°C). In these ranges, (T1-T2) may be greater than 0. It should be noted that the softening point T1 of the oxidation prevention film is naturally lower than the melting point of the solder precoat.

[0024] When the temporary fixing film contains a liquid component, it is preferable that both the first thermoplastic resin and the second thermoplastic resin dissolve in the liquid component of the temporary fixing film. According to this configuration, when both the oxidation prevention film and the temporary fixing film are softened, both films become compatible with each other. For example, it is preferable to use rosins as the first and second thermoplastic resins, and use a liquid component (such as hexyl diglycol) in which they dissolve as the liquid component of the temporary fixing film.

[0025] (Step (ii)) Step (ii) is a step of arranging a plurality of electronic components on a plurality of solder precoats via an oxidation prevention film and a temporary fixing film. There is no particular limitation on the method of arranging the electronic components, and a known method and a known device may be used. The plurality of electronic components may include electronic components of a size equal to or smaller than the JIS standard 0402 size. The present invention is particularly effective when mounting such electronic components of a very small size. Since the electronic components are fixed by the temporary fixing film, they are stably fixed to the substrate until step (iii) is performed.

[0026] (Step (iii)) Step (iii) is a step of melting the multiple solder precoats to solder the multiple electronic components to the multiple lands. Step (iii) can be performed by a step generally called a reflow step. In the reflow step, a substrate or the like (a substrate on which electronic components are arranged) is heated until the solder precoats melt, and then the substrate or the like is cooled to solidify the molten solder. Step (iii) results in a substrate on which electronic components are mounted. If necessary, soldering inspection or the like may be performed after step (iii).

[0027] In step (iii), when the substrate on which the electronic components are arranged is heated, the temporary fixing film and the oxidation preventing film soften simultaneously, or the temporary fixing film softens first, and then the oxidation preventing film softens. According to this configuration, the softened temporary fixing film comes into contact with the electrodes of the electronic components, and the oxidation film of the contacting portion is reliably cleaned. The oxidation preventing film softens simultaneously with or after the softening of the temporary fixing film, thereby enabling self-alignment and allowing the electronic components to be mounted well. When the softened temporary fixing film and the softened oxidation preventing film are compatible with each other, the electronic components can be mounted particularly well. On the other hand, when the oxidation preventing film softens before the temporary fixing film, the components of the activator are consumed in removing the oxidation film of the solder precoat, and the removal of the oxidation film of the electrodes of the electronic components is likely to be insufficient, which makes it easy for poor solder connection to occur.

[0028] The step (iii) is not particularly limited as long as it can solder a plurality of electronic components to the substrate, and a known reflow process may be used. For example, the heating process of the substrate may include a preheating process. Alternatively, the heating process of the substrate may not include a preheating process. In this case, the substrate may be heated so that the heating rate of the substrate during the heating from 50° C. to the melting point of the solder precoat is higher than 2° C. / sec. That is, in this case, the heating rate of the substrate during the heating from 50° C. to the melting point of the solder precoat is not 2° C. / sec or lower. The heating rate may be 3° C. / sec or higher, or 4° C. / sec or higher. The heating rate may be 10° C. / sec or lower (e.g., 8° C. / sec or lower). By setting the heating rate to 10° C. / sec or lower, it is possible to suppress the wiring and the land from peeling off from the substrate. The upper surface of the substrate is the surface on which the lands on which the electronic components are arranged are formed. By omitting the preheating step and adopting a high heating rate (eg, 4° C. / sec or higher), the time required for step (iii) can be significantly reduced.

[0029] When the solder precoat is exposed to high temperatures for a long time, its surface is oxidized, and solder defects are likely to occur. By setting the heating rate at 4°C / sec or more, the oxidation of the surface of the solder precoat can be suppressed, and solder defects can be reduced. This effect is particularly significant when the multiple electronic components include minute electronic components. Here, minute electronic components are, for example, electronic components with a planar shape of one side of 0.4 mm or less. The electronic components include electronic components of the same size or smaller than electronic components of JIS standard 0402 size. In this specification, the "planar shape" refers to the shape of the electronic component when viewed from above the board when the electronic component is mounted on the board.

[0030] Step (iii) can be performed using a reflow device having the same or similar configuration as a known reflow device. In order to suppress oxidation of the surface of the solder precoat, step (iii) may be performed in a nitrogen gas atmosphere inside the reflow device. However, when the above-mentioned temperature rise rate is 4°C / sec or more, oxidation of the surface of the solder precoat can be suppressed even if step (iii) is performed in an air atmosphere inside the reflow device. Therefore, when the above-mentioned temperature rise rate is 4°C / sec or more, step (iii) may be performed in an air atmosphere.

[0031] The melting point of the solder precoat varies depending on the solder used. In the case of commonly used lead-free solder (solder that does not contain lead), the melting point is, for example, 200°C or higher. Therefore, when lead-free solder is used, the temperature of the upper surface of the substrate is raised to 200°C or higher (for example, 220°C or higher or 230°C or higher) in step (iii). The upper limit of the temperature of the upper surface of the substrate may be set to 250°C or lower (for example, 240°C or lower or 230°C or lower) in consideration of the effect on electronic components.

[0032] The manufacturing method (M) may include a step (x) of forming a plurality of solder precoats and an oxidation prevention film on the plurality of lands before the step (i). There is no limitation on the method of forming the plurality of solder precoats, and a known method may be used.

[0033] The manufacturing method (M) may further include, after step (x) and before step (i), a step (y) of pressing the multiple solder precoats and the anti-oxidation film from above the substrate to create cracks in the anti-oxidation film and flatten the upper surfaces of the multiple solder precoats.

[0034] Manufacturing method (M) is a process (x) In the case where at least one solder precoat is improperly formed so as to short-circuit two adjacent lands, the method may further include, after step (x) and before step (i), a step (z) of forming a notch in a portion of the improperly formed solder precoat that is above and between the two lands.

[0035] The manufacturing method (M) may include only one of the steps (y) and (z), or may include both. When the manufacturing method (M) includes both, the step (z) may be performed before or after the step (y).

[0036] In the following, examples of the embodiments according to the present invention will be specifically described with reference to the drawings. The embodiments described below can be modified based on the above description. The matters described below may be applied to the above embodiment. Matters that are not essential to the embodiments according to the present invention can be omitted. In addition, in order to facilitate understanding, the following figures may show components at a different scale. In addition, in the following figures, hatching of some components may be omitted. In addition, in the following figures, only one electronic component is shown as an electronic component mounted on a board, but in reality, multiple electronic components are mounted on a board.

[0037] (Embodiment 1) An example of the manufacturing method (M) will be described in embodiment 1. The steps in the manufacturing method of embodiment 1 are shown diagrammatically in the cross-sectional views of Figures 1A to 1F.

[0038] 1A, a temporary fixing film 13 is formed so as to cover each of the multiple solder pre-coats 11 and the oxidation prevention film 12 (step (i)). The solder pre-coats 11 are formed on lands 10b of a printed circuit board (substrate) 10. The printed circuit board 10 includes a plate-shaped substrate portion 10a and lands 10b formed on the surface of the substrate portion 10a.

[0039] 1B, a plurality of electronic components 30 are placed on the plurality of solder precoats 11 via the antioxidant film 12 and the temporary fixing film 13 (step (ii)). This results in a substrate 10X on which a plurality of electronic components 30 are arranged. The illustrated example of electronic component 30 includes two terminal portions 30a and an element portion 30b arranged therebetween.

[0040] Next, the substrate 10X is introduced into a reflow device, and heating of the substrate 10X is started. The temporary fixing film 13 softens before the oxidation-resistant film 12. FIG. 1C shows a state in which the temporary fixing film 13 is softened and the oxidation-resistant film 12 is not softened. At this time, a part of the softened temporary fixing film 13 spreads onto the surface of the terminal portion 30a of the electronic component 30, as shown in FIG. 1C. Since the temporary fixing film 13 contains an activator, the oxide film is removed from a wide area of ​​the terminal portion 30a.

[0041] Fig. 1D shows the state of the substrate 10X when the temperature is further increased. In Fig. 1D, a part of the solder precoat 11 melts, and a molten nucleus 11b is formed on the land 10b. In addition, the oxidation prevention film 12 softens and dissolves with the temporary fixing film 13 to form a mixture 13a.

[0042] When the temperature of the substrate 10X is further increased, the entire solder precoat 11 becomes molten solder 11c as shown in FIG. 1E. Then, by cooling the substrate 10X, the molten solder solidifies to become solder 11d as shown in FIG. 1F. The electronic component 30 is soldered to the land 10b by the solder 11d. The temporary fixing film 13 becomes a residue 13g. In this manner, the substrate 10Y on which the electronic component 30 is mounted is obtained. The substrate 10Y is an electronic component mounting substrate.

[0043] As described above, the substrate 10X may be heated so that the temperature of the upper surface 10sa of the printed circuit board 10 is lower than the temperature of the lower surface 10sb of the printed circuit board 10. Also, as described above, when heating the substrate 10X, a preheating step may or may not be provided. In the case where the preheating step is not provided, the step (iii) FIG. 2 shows an example of a temperature profile of the upper surface 10sa and the lower surface 10sb of the printed circuit board 10 in the above-described embodiment.

[0044] 2 shows an example in which the temperature of the substrate surface is increased from room temperature (25° C.) to the maximum temperature at a constant rate. In the example shown in FIG. 2, the rate of increase in the surface temperature of the upper surface 10sa is 4° C. / sec or more. The rate of increase in the surface temperature of the lower surface 10sb is faster than the rate of increase in the surface temperature of the upper surface 10sa. expensive The softening point T2 (°C) of the second thermoplastic resin in the temporary fixing film 13 is No. 1 The softening temperature of the temporary fixing film 13 is equal to or lower than the softening point T1 (°C) of the thermoplastic resin. That is, the softening temperature of the temporary fixing film 13 is equal to or lower than the softening temperature of the antioxidant film 12. In the example shown in Fig. 2, after the reflow process in the heating zone is completed, a cooling process in the cooling zone is carried out.

[0045] The manufacturing method (M) of the present invention may include a step (x) of forming a plurality of solder precoats 11 and an oxidation prevention film 12 on a plurality of lands 10b. An example of such a step (x) is shown in Figs. 3A to 3E. First, a printed circuit board (substrate) 10 shown in Fig. 3A is prepared. The printed circuit board 10 includes a plate-shaped substrate portion 10a and lands 10b formed on the surface of the substrate portion 10a. The lands 10b are connected to wiring (not shown) on the substrate portion 10a as necessary.

[0046] Next, as shown in Fig. 3B, a mask 20 is placed on the printed circuit board (substrate) 10. The mask 20 has openings 20h at positions corresponding to the lands 10b to which the solder paste is to be applied. Next, as shown in Fig. 3C, solder paste 11p is applied to place the solder paste 11p on the lands 10b. The solder paste 11p contains solder particles 11a and flux 11f.

[0047] Next, as shown in FIG. 3D, the mask 20 is moved from above the printed circuit board 10. Next, the printed circuit board 10 on which the solder paste 11p is arranged is heated to melt the solder particles 11a, and then the printed circuit board 10 is cooled. As a result, the solder precoat 11 is formed on the lands 10b as shown in FIG. 3E. At this time, the residue of the flux 11f becomes the oxidation prevention film 12. The thermoplastic resin contained in the flux 11f becomes the first thermoplastic resin in the oxidation prevention film 12.

[0048] It has been believed in the past that leaving the flux 11f residue would cause solder defects in the reflow process. Therefore, in the past, the remaining flux residue has been removed by cleaning. However, in this embodiment, the flux residue is used as the oxidation prevention film 12 of the solder precoat 11. The oxidation prevention film 12 remains until just before the solder melts in the reflow process, so oxidation of the surface of the solder precoat 11 can be suppressed. Therefore, even if the action of the activator in the temporary fixing film 13 is low, solder defects can be suppressed. In other words, even if the temporary fixing film 13 softens before the oxidation prevention film 12, solder defects can be suppressed. Furthermore, by using the flux residue as the oxidation prevention film 12, the process of removing the flux residue can be omitted.

[0049] The manufacturing method (M) may include the above-mentioned step (y) and / or step (z) after step (x) and before step (i). Cross-sectional views of steps showing an example of carrying out step (y) and step (z) after step (x) are shown in Figures 4A to 4H.

[0050] Step (z) is performed when at least one solder precoat 11 is improperly formed so as to short-circuit two adjacent lands 10b, as shown in FIG. 4A. When step (z) is performed, an inspection step is performed after step (x) and before step (z) to check whether the solder precoat 11 is properly formed. The inspection step can be performed by a known method. For example, defects in the solder precoat 11 can be detected by photographing the printed circuit board 10 on which the solder precoat 11 is formed with a camera and processing the obtained image.

[0051] In step (y), as shown in FIG. 4B, a flattening tool 51 with a flat pressing surface is used to press the multiple solder precoats 11 and the oxidation prevention film 12 from above the printed circuit board 10 (flattening step). This causes cracks (not shown) in the oxidation prevention film 12, flattens the upper surface 11t of the solder precoat, and reduces the thickness of the solder precoat 11. When the size of the electronic component 30 becomes smaller, the size of the solder precoat 11 also becomes smaller. When the size of the solder precoat 11 becomes smaller, the upper surface 11t of the solder precoat 11 becomes hemispherical due to the influence of surface tension, which may make it difficult to stably arrange the electronic component 30. By flattening the upper surface of the solder precoat 11 in step (y), the electronic component 30 can be stably arranged. In addition, by forming cracks in the oxidation prevention film 12, the solvent contained in the temporary fixing film 13 and the solvent contained in the oxidation prevention film 12 become more compatible with each other. In addition, the oxidation-preventing film 12 peels off to reveal a new surface of the solder metal, which facilitates connection between the electrodes of the electronic component and the solder of the solder precoat. Since the oxidation-preventing film 12 is applied immediately after the flattening process, the new surface of the solder metal is hardly oxidized.

[0052] Next, step (z) is performed. First, as shown in FIG. 4C, a notch 11k is formed in the portion of the improperly formed solder precoat 11 that is located above the area between the two lands 10b. The notch 11k can be formed, for example, by poking the above-mentioned portion of the solder precoat 11 with a chisel-shaped tool 52 as shown in FIG. 4C.

[0053] 1A to 1F, electronic components 30 are mounted. Specifically, first, as shown in FIG 4D, a temporary fixing film 13 is formed so as to cover the solder precoat 11 and the oxidation prevention film 12 (step (i)).

[0054] 4E, a plurality of electronic components 30 are disposed on the plurality of solder precoats 11 via the antioxidant film 12 and the temporary fixing film 13 (step (ii)). This results in a substrate 10X on which a plurality of electronic components 30 are disposed.

[0055] Next, the board 10X is heated to melt the solder precoat 11 and then solidify it, and the electronic component 30 is mounted on the printed circuit board 10. The process at this time is shown in the cross-sectional views of FIG. 4F to FIG. 4H. In FIG. 4F, the temporary fixing film 13 softens and spreads. In FIG. 4G, the oxidation prevention film 12 softens and dissolves with the temporary fixing film 13 to form a mixture 13a. In addition, a part of the solder precoat 11 melts to form a molten core 11b. In FIG. 4H, the molten solder solidifies to become solder 11d. In addition, the mixture 13a becomes a residue 13g. In this way, the board 10Y on which the electronic component 30 is mounted is obtained. When the solder precoat 11 melts, the unmelted solder precoat 11 melts while being attracted to the previously melted molten core 11b. Therefore, as shown in FIG. 4H, the short circuit is finally eliminated. By forming the notch 11k, the solder precoat 11 present between the two lands 10b is easily attracted to the molten core 11b, which makes it easier to eliminate a short circuit between the two lands. EXAMPLES

[0056] The present invention will now be described in more detail with reference to examples. In these examples, electronic components were mounted on the substrate by changing the composition of the oxidation prevention film and the composition of the temporary fixing film.

[0057] (Experimental Example 1) In Experimental Example 1, a solder precoat was formed on the land of a printed circuit board using a solder paste. The film of flux residue formed on the surface of the solder precoat was used as an oxidation prevention film. For the solder paste, a mixture of solder particles (90 mass%), polymerized rosin (4.5 mass%, softening point 140°C), abietic acid (0.5 mass%), castor wax (0.5 mass%), and hexyl diglycol (4.5 mass%) was used. Hexyl diglycol is a liquid component (solvent), abietic acid is an activator, and castor wax is a thixotropic agent (the same applies to the following examples). For the solder particles, solder particles made of a SnAgCu alloy were used. The main component of the oxidation prevention film (film of flux residue) formed using this solder paste is polymerized rosin, and it can be considered that the oxidation prevention film begins to soften at 140°C.

[0058] Next, a temporary adhesive film was formed to cover the solder pre-coat and the oxidation prevention film. The material of the temporary adhesive film was a mixture of hydrogenated rosin (45% by mass, softening point 75°C), abietic acid (5% by mass), castor wax (5% by mass), and hexyl diglycol (45% by mass). The main component of the temporary adhesive film is hydrogenated rosin, and it can be considered that the temporary adhesive film begins to soften at 75°C.

[0059] 20 electronic components were placed on the solder precoat of the obtained board via an oxidation prevention film and a temporary fixing film. The electronic components used were JIS standard 0201 size electronic components (planar size 0.25 mm x 0.125 mm). The solder precoat was melted in a reflow device to mount the electronic components on the printed board. In this way, the electronic component mounting board of Experimental Example 1 was produced.

[0060] (Experimental Examples 2 to 5) Except for changing the polymerized rosin in the solder paste and / or the hydrogenated rosin in the temporary fixing film to other rosins, the solder paste and the materials for the temporary fixing film were prepared in the same compounding ratio as in Experimental Example 1. Then, using these, electronic component mounting boards of Experimental Examples 2 to 5 were produced in the same manner as in Experimental Example 1.

[0061] The electronic component mounting boards of the above Experimental Examples 1 to 5 were inspected to see if 20 electronic components were properly soldered to the lands. Specifically, the presence or absence of defects (opens) where the lands and electronic components were not electrically connected was inspected. The rosins used in Experimental Examples 1 to 5, their softening points, and the inspection results are shown in Table 1. The defect rate in Table 1 indicates the percentage of electronic components that were not properly soldered to the lands out of the 20 electronic components.

[0062] [Table 1]

[0063] As shown in Table 1, no defects occurred in Experimental Examples 1, 2, and 5, in which the softening point T2 was equal to or lower than the softening point T1. On the other hand, defects occurred in Experimental Examples 3 and 4, in which the softening point T2 was higher than the softening point T1. [Industrial Applicability]

[0064] The present invention can be used in a method for manufacturing an electronic component mounting board. Although the present invention has been described with respect to the presently preferred embodiments, such disclosure should not be interpreted as limiting. Various variations and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. Accordingly, the appended claims should be interpreted to cover all variations and modifications without departing from the true spirit and scope of the present invention. [Explanation of symbols]

[0065] 10: Printed circuit board (substrate) 10X, 10Y: Substrate 10b: Land 10sa:Top surface 10sb: Bottom side 11: Solder precoat 11a: Solder particles 11c, 11d: solder 11f: Flux 11k: Notch 11p: Solder paste 11t:Top surface 12: Anti-oxidation film 13: Temporary fixing film 30: Electronic components

Claims

1. A method for manufacturing an electronic component mounting board, comprising: A step (i) of forming a temporary fixing film so as to cover a plurality of solder precoats formed on a plurality of lands of a substrate and an oxidation prevention film formed so as to cover each of the plurality of solder precoats; (ii) placing a plurality of electronic components on the plurality of solder precoats via the oxidation prevention film and the temporary fixing film; and (iii) soldering the electronic components to the lands by melting the solder precoats; the oxidation prevention film includes a first thermoplastic resin; The temporary coating includes an active agent and a second thermoplastic resin, the softening point of the second thermoplastic resin is equal to or lower than the softening point of the first thermoplastic resin; The method for manufacturing an electronic component mounting substrate, wherein the oxidation prevention film is a residue formed on a surface of the solder precoat when the solder precoat is formed.

2. The manufacturing method according to claim 1 , further comprising, before the step (i), a step (x) of forming the plurality of solder precoats and the oxidation prevention film on the plurality of lands.

3. The manufacturing method according to claim 2, further comprising a step (y) of pressing the plurality of solder precoats and the anti-oxidation film from above the substrate, after the step (x) and before the step (i), to create cracks in the anti-oxidation film and flatten upper surfaces of the plurality of solder precoats.

4. In the step (x), when at least one of the solder precoats is improperly formed so as to short-circuit two adjacent lands, The manufacturing method according to claim 2 or 3, further comprising a step (z) of forming a notch in a portion of the improperly formed solder precoat that is above and between two of the lands, after the step (x) and before the step (i).

Citation Information

Patent Citations

  • Temporary adhesive for soldering

    JP1986181883A

  • Temporary adhesive for soldering

    JP1989150493A

  • Method for mounting electronic parts on printed circuit board

    JP1994090079A

  • Mounting method for electronic part