Nonaqueous electrolyte for lithium secondary battery and lithium secondary battery containing same
The use of a sulfonylpyridine additive in the non-aqueous electrolyte of lithium secondary batteries addresses the degradation issues under high temperatures by forming a stable film, enhancing thermal stability and extending battery life.
Patent Information
- Application Number
- JP2023526649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-16
- Filing Date
- 2022-03-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-03-16
AI Technical Summary
Lithium secondary batteries degrade under high-temperature conditions due to the thermal decomposition of LiPF6 in the electrolyte, leading to the formation of Lewis acids like HF, which can destroy electrode films and cause metal elution, resulting in increased resistance and reduced performance.
Incorporation of a sulfonylpyridine additive in the non-aqueous electrolyte, represented by a specific chemical formula, to form a stable film on the electrodes, reducing electrolyte decomposition and metal elution, thereby enhancing high-temperature stability and battery life.
The sulfonylpyridine additive stabilizes the electrolyte, suppresses HF generation, and forms a robust film, improving high-temperature performance and extending battery life by maintaining capacity and reducing gas generation.
Smart Images

Figure 0007584648000001 
Figure 0007584648000002 
Figure 0007584648000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2021-0034084, filed with the Korean Intellectual Property Office on March 16, 2021, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a non-aqueous electrolyte for a lithium secondary battery and a lithium secondary battery containing the same. [Background technology]
[0003] Lithium secondary batteries are generally manufactured by forming an electrode assembly by interposing a separator between a positive electrode including a positive electrode active material made of a lithium-containing transition metal oxide and a negative electrode including a negative electrode active material capable of storing lithium ions, inserting the electrode assembly into a battery case, injecting a non-aqueous electrolyte solution that serves as a medium for transferring lithium ions, and then sealing the battery case.
[0004] Lithium secondary batteries can be miniaturized and have high energy density and operating voltage, and therefore are applied in various fields such as mobile devices, electronic products, electric vehicles, etc. As the fields of application of lithium secondary batteries become more diverse, the required physical property conditions are also becoming more stringent, and in particular, there is a demand for the development of lithium secondary batteries that can be stably operated even under high temperature conditions.
[0005] On the other hand, when a lithium secondary battery is operated under high temperature conditions, the lithium salts such as LiPF6 contained in the electrolyte are converted to PF6 - The anions may be thermally decomposed to generate Lewis acids such as PF5, which react with moisture to generate HF. The decomposition products of PF5, HF, etc. may not only destroy the coating formed on the surface of the electrode, but may also cause a decomposition reaction of the organic solvent. They may also react with the decomposition products of the positive electrode active material to dissolve transition metal ions, which may be electrodeposited on the negative electrode and destroy the coating formed on the surface of the negative electrode.
[0006] If the electrolyte decomposition reaction continues on such a destroyed coating, the battery performance will further deteriorate, so there is a demand for the development of a secondary battery that can maintain excellent performance even under high temperature conditions. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention is intended to solve the above problems, and has an object to provide a nonaqueous electrolyte solution that contains a sulfonylpyridine-based additive and contributes to the formation of a positive electrode coating, and a lithium secondary battery containing the same. [Means for solving the problem]
[0008] According to one embodiment, the present invention provides a non-aqueous electrolyte for a lithium secondary battery, comprising a lithium salt, an organic solvent, and an additive comprising a compound represented by Chemical Formula 1 below:
[0009] [ka]
[0010] In the above Chemical Formula 1, R1 is fluorine; or an alkyl group having 1 to 10 carbon atoms substituted with one or more fluorine atoms; R2 is an alkyl group having 1 to 10 carbon atoms, m is an integer of 0 to 4.
[0011] According to another embodiment, the present invention provides a lithium secondary battery including: a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; and the non-aqueous electrolyte for the lithium secondary battery. Effect of the Invention
[0012] The present invention is intended to solve the above-mentioned problems, and can provide a nonaqueous electrolyte for lithium secondary batteries that can suppress the decomposition reaction of the electrolyte and reduce elution of the positive electrode by forming a strong coating on the surface of the positive electrode.
[0013] Moreover, the present invention can provide a lithium secondary battery containing the nonaqueous electrolyte for a lithium secondary battery, thereby improving the high-temperature storage characteristics and life characteristics of the battery. BEST MODE FOR CARRYING OUT THEINVENTION
[0014] The present invention will now be described in more detail.
[0015] In general, anions contained in lithium salts such as LiPF6, which are widely used in electrolytes for lithium secondary batteries, form decomposition products such as hydrogen fluoride (HF) and PF5 due to thermal decomposition or moisture. Such decomposition products have acid properties and deteriorate the coating or electrode surface in the battery.
[0016] Due to the decomposition products of the electrolyte and the structural changes of the positive electrode caused by repeated charging and discharging, the transition metals in the positive electrode are easily dissolved into the electrolyte, and the dissolved transition metals are further re-deposited on the positive electrode, increasing the resistance of the positive electrode. Furthermore, if the dissolved transition metals move to the negative electrode through the electrolyte, they are electrodeposited on the negative electrode, causing destruction of the solid electrolyte interphase (SEI) film and further electrolyte decomposition reactions, which causes problems such as increased consumption of lithium ions and resistance.
[0017] In addition, during initial activation of the battery, a protective coating is formed on the positive and negative electrodes due to electrolyte reaction. If the coating becomes unstable for the reasons described above, further decomposition of the electrolyte will occur during charging / discharging or exposure to high temperatures, accelerating battery degradation and generating gas.
[0018] In order to solve such problems, the inventors have found that a sulfonylpyridine-based compound represented by the following chemical formula 1 can be used as an additive to a non-aqueous electrolyte to reduce the decomposition reaction of the electrolyte and suppress the elution of transition metals and the generation of gas. They have also confirmed that the S-based and F-based components have the effect of efficiently forming a protective film on the positive electrode in the positive / negative electrodes.
[0019] Specifically, as described above, lithium secondary batteries using an electrolyte containing LiPF6 have a problem in that the battery deteriorates due to HF, which is a decomposition product of LiPF6, but the pyridine group contained in the compound represented by Chemical Formula 1 acts as a Lewis base and has the effect of stabilizing PF5, which is an intermediate derivative and Lewis acid before HF is generated. In particular, the pyridine group is effective in reducing the generation of HF because it has a higher bond energy with PF5 than other N-containing structures such as an imidazole group.
[0020] In addition, the -SO2-R1 functional group contained in the compound represented by Chemical Formula 1 is decomposed at the positive / negative electrodes to form a coating film on the electrodes, which contributes to the formation of a stable interface between the electrodes and the electrolyte. In this case, if R1 containing fluorine is substituted with a pyridine group instead of a sulfonyl group, the structure of the pyridine group may be broken during oxidation / reduction decomposition due to the action of R1, but if it is substituted with a sulfonyl group as in the present invention, the structure of the pyridine group is not affected, so that a coating can be formed more smoothly. Furthermore, the -SO2-R1 functional group of Chemical Formula 1 of the present application is advantageous in that it can further contain fluorine, which is a functional group useful for the components of the coating, compared to -SO3, and by containing F instead of O, the coating can contain LiF components, which is advantageous in forming a coating with improved thermal stability and high voltage characteristics.
[0021] Each component of the present invention will be described in more detail below.
[0022] Non-aqueous electrolyte (1) Additives The non-aqueous electrolyte of the present invention contains an additive containing a compound represented by the following chemical formula 1.
[0023] [ka]
[0024] In the above Chemical Formula 1, R1 is fluorine; or an alkyl group having 1 to 10 carbon atoms substituted with one or more fluorine atoms; R2 is an alkyl group having 1 to 10 carbon atoms, m is an integer of 0 to 4.
[0025] In one embodiment of the present invention, the compound represented by Chemical Formula 1 may be represented by Chemical Formula 1-1 below.
[0026] [ka]
[0027] In the above Chemical Formula 1-1, R1, R2, and m are as defined in Chemical Formula 1 above.
[0028] In one embodiment of the present invention, R1 may be an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorines, specifically, a methyl group substituted with one or more fluorines, more specifically, a difluoromethyl group. The more fluorines are substituted, the more LiF is produced and the coating film can be strengthened, but if too much fluorine is substituted, the resistance may increase. That is, taking into consideration the amount of LiF formed on the surface of the positive / negative electrodes, a difluoromethyl group is most preferred.
[0029] In one embodiment of the present invention, R2 may be a linear or branched alkyl group having 1 to 5 carbon atoms.
[0030] In one embodiment of the present invention, m may be 0 or 1, specifically 0.
[0031] In one embodiment of the present invention, the compound represented by Chemical Formula 1 may be represented by Chemical Formula 1a below.
[0032] [ka]
[0033] In one embodiment of the present invention, the content of the compound represented by Chemical Formula 1 may be 0.1 wt % to 5 wt %, preferably 0.1 wt % to 3 wt %, and more preferably 0.5 wt % to 1 wt %, based on the total weight of the non-aqueous electrolyte solution.
[0034] When the content of the compound represented by Chemical Formula 1 is within the above range, an effect of improving performance can be obtained by forming a suitable level of positive / negative electrode coating.
[0035] Specifically, when the content of the compound represented by Formula 1 is less than 0.1 wt %, the content is too small to form a sufficient coating on the positive / negative electrodes, and when it exceeds 5 wt %, the content is too excessive, which may cause an increase in resistance and may deteriorate the battery performance.
[0036] The nonaqueous electrolyte of the present invention may selectively contain other additives as required in order to prevent the electrolyte from being decomposed in a high voltage environment, which may cause the electrode to collapse, or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and the effects of suppressing battery expansion at high temperatures.
[0037] The other additives may be one or more selected from cyclic carbonate compounds, halogen-substituted carbonate compounds, sultone compounds, sulfate compounds, phosphate or phosphite compounds, borate compounds, nitrile compounds, amine compounds, silane compounds, benzene compounds, and lithium salt compounds.
[0038] The cyclic carbonate compound may be at least one selected from vinylene carbonate (VC) and vinyl ethylene carbonate (VEC), and specifically may be vinylene carbonate.
[0039] The halogen-substituted carbonate compound may be fluoroethylene carbonate (FEC).
[0040] The sultone-based compound is a material capable of forming a stable SEI film on the surface of the negative electrode through a reduction reaction, and may be one or more compounds selected from 1,3-propane sultone (PS), 1,4-butane sultone, ethene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone, and specifically, may be 1,3-propane sultone (PS).
[0041] The sulfate-based compound is a material that can be electrically decomposed on the surface of the negative electrode to form a stable SEI film that does not crack even when stored at high temperatures, and may be at least one selected from ethylene sulfate (Esa), trimethylene sulfate (TMS), and methyl trimethylene sulfate (MTMS).
[0042] The phosphate or phosphite compound may be one or more selected from lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite.
[0043] The borate-based compound may be lithium tetraphenylborate.
[0044] The nitrile compound may be one or more selected from succinonitrile (SN), adiponitrile (ADN), acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, 4-fluorophenylacetonitrile, ethylene glycol bis(2-cyanoethyl)ether (ASA3), 1,3,6-hexanetricarbonitrile (HTCN), 1,4-dicyano-2-butene (DCB), and 1,2,3-tris(2-cyanoethyl)propane (TCEP).
[0045] The amine compound may be one or more selected from triethanolamine and ethylenediamine, and the silane compound may be tetravinylsilane.
[0046] The benzene-based compound may be one or more selected from monofluorobenzene, difluorobenzene, trifluorobenzene, and tetrafluorobenzene.
[0047] The lithium salt-based compound is a compound different from the lithium salt contained in the electrolyte, and may be one or more compounds selected from lithium difluorophosphate (LiDFP; LiPO2F2), lithium bis(oxalato)borate (LiBOB; LiB(C2O4)2), lithium tetrafluoroborate (LiBF4), and lithium difluoro(bis(oxalato)phosphate) (LiDFOP).
[0048] Preferably, the additive of the non-aqueous electrolyte according to one embodiment of the present invention may further include one or more selected from vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), 1,3-propane sultone (PS), 1,3-propene sultone (PRS), ethylene sulfate (ESa), succinonitrile (SN), adiponitrile (ADN), ethylene glycol bis(2-cyanoethyl)ether (ASA3), 1,3,6-hexanetricarbonitrile (HTCN), 1,4-dicyano-2-butene (DCB), 1,2,3-tris(2-cyanoethyl)propane (TCEP), lithium difluorooxalatoborate (LiODFB), lithium tetrafluoroborate (LiBF4), lithium difluoro(bisoxalato)phosphate (LiDFOP), and lithium difluorophosphate (LiDFP) as other additives.
[0049] More preferably, the additive of the non-aqueous electrolyte according to an embodiment of the present invention may further include one or more selected from vinylene carbonate (VC), 1,3-propane sultone (PS), ethylene sulfate (ESa), and lithium difluorophosphate (LiDFP) as other additives. In this case, a polymeric coating can be formed in addition to the coating components of the positive and negative electrodes mainly formed by the compound represented by Chemical Formula 1, which has the effect of further improving high temperature performance.
[0050] Meanwhile, the content of the other additives may be 0.1 wt% to 10 wt% based on the total weight of the nonaqueous electrolyte, and preferably 0.3 wt% to 5 wt%. If the content of the other additives is less than 0.1 wt%, the effect of forming an additional stable film is small, so there is no improvement in terms of high-temperature capacity and gas generation, and if it exceeds 10 wt%, side reactions in the electrolyte may occur excessively during charging and discharging of the battery. In particular, when the additives for forming the SEI film are added in excess, they may not be sufficiently decomposed at high temperatures and may remain unreacted or precipitated in the electrolyte at room temperature. This may cause side reactions that reduce the life or resistance characteristics of the battery.
[0051] (2) Organic Solvent The non-aqueous electrolyte of the present invention contains an organic solvent.
[0052] As the organic solvent, various organic solvents that are generally used in lithium electrolytes can be used without limitation.For example, the organic solvent may be a cyclic carbonate solvent, a linear carbonate solvent, a linear ester solvent, a cyclic ester solvent, a nitrile solvent, or a mixture thereof, and preferably may include a mixture of two or more selected from a cyclic carbonate solvent, a linear carbonate solvent, and a linear ester solvent.
[0053] The cyclic carbonate solvent is a high-viscosity organic solvent that has a high dielectric constant and can effectively dissociate the lithium salt in the electrolyte. The cyclic carbonate solvent may be one or more selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate, and may specifically include ethylene carbonate (EC).
[0054] In addition, the linear carbonate solvent is an organic solvent having low viscosity and low dielectric constant, and may be one or more selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and may specifically include ethyl methyl carbonate (EMC).
[0055] In order to produce an electrolyte solution having high ionic conductivity, it is preferable to use a mixture of a cyclic carbonate solvent and a linear carbonate solvent as the organic solvent.
[0056] The linear ester solvent may be one or more selected from methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.
[0057] The cyclic ester solvent may be one or more selected from γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.
[0058] The nitrile solvent may be one or more selected from succinonitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile, and may be preferably succinonitrile.
[0059] In the total weight of the nonaqueous electrolyte, the remainder excluding the organic solvent, for example, the additive and the lithium salt, is the organic solvent unless otherwise specified.
[0060] (3) Lithium salt The non-aqueous electrolyte of the present invention contains a lithium salt. The lithium salt may be any one that is commonly used in electrolytes for lithium secondary batteries, and may be used without limitation. Specifically, the lithium salt may have a cation of Li + and as an anion, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , BF2C2O4CHF - , PF4C2O4 - , PF2C4O8 - , PO2F2 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO -, (CF3SO2)2CH - , CF3(CF2)7SO3 - , and SCN - may include any one or more selected from the following:
[0061] Specifically, the lithium salt may be LiPF6, LiClO4, LiBF4, LiN(FSO2)2 (LiFSI), LiTFSI, lithium bis(pentafluoroethanesulfonyl)imide (LiBETI), LiSO3CF3, LiPO2F2, lithium bis(oxalate)borate (LiBOB), lithium difluoro(oxalate)borate (LiFOB), lithium difluoro(bisoxalato)phosphate (LiDFOP), lithium tetrafluoro(oxalate)phosphate (LiTFOP), and lithium fluoromalonato(difluoro)borate (LiTFOP). borate, LiFMDFB), and preferably, one or more selected from LiPF6 and LiN(FSO2)2 (LiFSI).
[0062] In one embodiment of the present invention, the concentration of the lithium salt in the electrolyte may be 0.5 to 4.0 M, specifically 0.5 to 3.0 M, more specifically 0.8 to 2.0 M. When the concentration of the lithium salt is within the above range, the effect of improving low-temperature output and cycle characteristics is sufficiently ensured, while the viscosity and surface tension are prevented from becoming excessively high, and appropriate electrolyte impregnation is obtained.
[0063] Lithium secondary battery Next, the lithium secondary battery according to the present invention will be described.
[0064] The lithium secondary battery according to the present invention includes a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, a separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, the non-aqueous electrolyte being the non-aqueous electrolyte according to the present invention. The non-aqueous electrolyte is as described above, so a description thereof will be omitted, and other components will be described below.
[0065] (1) Positive electrode The positive electrode according to the present invention includes a positive electrode active material, and can be manufactured by coating a positive electrode slurry including a positive electrode active material, a binder, a conductive material, a solvent, etc., on a positive electrode current collector, followed by drying and rolling.
[0066] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel; aluminum; nickel; titanium; baked carbon; or aluminum or stainless steel whose surface has been surface-treated with carbon, nickel, titanium, silver, or the like may be used.
[0067] The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and may be one or more selected from LCO (LiCoO2); LNO (LiNiO2); LMO (LiMnO2); LiMn2O4; LiCoPO4; LFP (LiFePO4); and lithium composite transition metal oxides containing nickel (Ni), cobalt (Co), and manganese (Mn).
[0068] In one embodiment of the present invention, the lithium composite transition metal oxide is LiNiCoMnO2; LiNi 1-x-y-z Co x M 1 y M 2 z O2(M 1 and M. 2are each independently any one selected from the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg, and Mo, and x, y, and z are each independently atomic fractions of oxide composition elements, 0≦x<0.5, 0≦y<0.5, 0≦z<0.5, x+y+z=1); and may be one or more selected from compounds represented by the following chemical formula 2.
[0069] Specifically, the positive electrode active material may include a lithium composite transition metal oxide represented by the following Chemical Formula 2:
[0070] [Chemical formula 2] Li 1+x (Ni a Co b Mn c M d )O2
[0071] In the above Chemical Formula 2, M is W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, or Mo; 1+x, a, b, c, and d are the atomic fractions of each independent element, -0.2≦x≦0.2, 0.50≦a<1, 0 <b≦0.30、0<c≦0.30、0≦d≦0.10、a+b+c+d=1である。
[0072] The 1+x represents the molar ratio of lithium, and may be -0.1≦x≦0.2 or 0≦x≦0.2. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium composite transition metal oxide can be stably formed.
[0073] The a represents the molar ratio of nickel in all metals excluding lithium, and may be 0.60≦a<1, 0.70≦a<1, or 0.80≦a<1. When the nickel molar ratio satisfies the above range, a high energy density is exhibited and a high capacity can be realized.
[0074] Said b represents the molar ratio of cobalt in all metals excluding lithium, and may be 0 < b ≤ 0.25, 0 < b ≤ 0.20, or 0 < b ≤ 0.15. When the molar ratio of cobalt satisfies the above range, good resistance characteristics and output characteristics can be realized.
[0075] Said c represents the molar ratio of manganese in all metals excluding lithium, and may be 0 < c ≤ 0.25, 0 < c ≤ 0.20, or 0 < c ≤ 0.15. When the molar ratio of manganese satisfies the above range, it has excellent structural stability of the positive electrode active material.
[0076] Said d represents the molar ratio of the doping element in all metals excluding lithium, and may be 0 < d ≤ 0.08, 0 < d ≤ 0.05, or 0 < d ≤ 0.03.
[0077] More specifically, the lithium composite transition metal oxide may be one or more selected from Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2, and Li(Ni 0.8 Mn 0.1 Co 0.1 )O2.
[0078] The positive electrode active material may be contained in an amount of 80% by weight to 99% by weight, specifically 90% by weight to 99% by weight, based on the total weight of the solid content in the positive electrode slurry. At this time, when the content of the positive electrode active material is 80% by weight or less, the energy density may be low and the capacity may decrease.
[0079] The binder is a component that assists in binding the active material and conductive material, etc., and binding to the current collector, and may be added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content in the positive electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, or various copolymers thereof.
[0080] The conductive material is a substance that imparts conductivity to the battery without causing any chemical change, and may be added in an amount of 0.5% by weight to 20% by weight based on the total weight of the solid content in the positive electrode slurry.
[0081] Examples of the conductive material include carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite with a highly developed crystal structure, artificial graphite, carbon nanotubes, or graphite; conductive fibers such as carbon fibers or metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive materials such as polyphenylene derivatives.
[0082] The solvent for the positive electrode slurry may contain an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a suitable viscosity when containing the positive electrode active material, binder, conductive material, etc. For example, the positive electrode slurry containing the positive electrode active material, binder, and conductive material may be contained so that the solid content concentration is 40% by weight to 90% by weight, preferably 50% by weight to 80% by weight.
[0083] (2) Negative electrode The negative electrode according to the present invention includes a negative electrode active material, and can be manufactured by coating a negative electrode slurry including a negative electrode active material, a binder, a conductive material, a solvent, etc., on a negative electrode current collector, followed by drying and rolling.
[0084] The negative electrode current collector generally has a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and for example, copper; stainless steel; aluminum; nickel; titanium; baked carbon; copper or stainless steel surface treated with carbon, nickel, titanium, silver, or the like; or an aluminum-cadmium alloy may be used. In addition, as with the positive electrode current collector, the binding force of the negative electrode active material may be strengthened by forming fine irregularities on the surface, and the negative electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0085] The negative electrode active material may include one or more selected from a carbon material capable of reversibly intercalating / deintercalating lithium ions; a metal or an alloy of such a metal and lithium; a metal composite oxide; a material capable of doping and dedoping lithium; lithium metal; and a transition metal oxide.
[0086] The carbonaceous material capable of reversibly intercalating / deintercalating lithium ions may be any carbonaceous negative electrode active material commonly used in lithium ion secondary batteries, and representative examples thereof include crystalline carbon, amorphous carbon, or a combination of both. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, and calcined coke.
[0087] As the metal or an alloy of these metals and lithium, a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, or an alloy of these metals and lithium can be used.
[0088] Examples of the metal composite oxide include PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3 (0 ≦ x ≦ 1), Li x WO2 (0 ≦ x ≦ 1), and Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, elements of Group 1, Group 2, Group 3 of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8), and one or more selected from the group can be used.
[0089] Examples of the substance capable of doping and undoping lithium include Si, SiO x (0 < x < 2), Si-Y alloy (where Y is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, and a combination thereof, and is not Si), Sn, SnO2, Sn-Y (where Y is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, and a combination thereof, and is not Sn), etc. Also, at least one of these and SiO2 may be mixed and used. The element Y may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db (dubnium), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and a combination thereof.
[0090] Examples of the transition metal oxide include lithium-containing titanium oxide (LTO), vanadium oxide, and lithium vanadium oxide.
[0091] The negative electrode active material may be included in an amount of 80% by weight to 99% by weight based on the total weight of solids in the negative electrode slurry.
[0092] The binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and may be added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content in the negative electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.
[0093] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 0.5% by weight to 20% by weight based on the total weight of the solid content in the negative electrode slurry. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and may be, for example, carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, carbon nanotube, or graphite with a highly developed crystal structure; conductive fiber such as carbon fiber or metal fiber; conductive powder such as carbon fluoride powder, aluminum powder, or nickel powder; conductive whisker such as zinc oxide or potassium titanate; conductive metal oxide such as titanium oxide; or conductive material such as polyphenylene derivative.
[0094] The solvent for the negative electrode slurry may include water or an organic solvent such as NMP or alcohol, and may be used in an amount that provides a suitable viscosity when containing the negative electrode active material, binder, conductive material, etc. For example, the solvent may be included so that the concentration of solids in the slurry containing the negative electrode active material, binder, and conductive material is 30% by weight to 80% by weight, preferably 40% by weight to 70% by weight.
[0095] (3) Separator The lithium secondary battery according to the present invention includes a separator between the positive electrode and the negative electrode.
[0096] The separator separates the negative electrode and the positive electrode and provides a path for lithium ion migration. Any separator that is typically used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to the migration of ions in the electrolyte and has excellent electrolyte impregnation ability and safety is preferred.
[0097] Specifically, the separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer; or a laminated structure of two or more layers thereof. In addition, a normal porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, or the like, may be used. In order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be used as a single layer or a multilayer structure.
[0098] The lithium secondary battery according to the present invention as described above can be usefully used in portable devices such as mobile phones, notebook computers, and digital cameras; and electric vehicles such as hybrid electric vehicles (HEVs).
[0099] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.
[0100] The battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, including power tools; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); and power storage systems.
[0101] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.
[0102] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for small devices, but also suitably as a unit battery in a medium- to large-sized battery module containing a large number of battery cells.
[0103] The present invention will now be described in more detail with reference to specific examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0104] Example 1. (Production of non-aqueous electrolyte) Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70, and LiPF6 was dissolved therein to a concentration of 1.0 M to prepare a non-aqueous organic solution. 0.5 wt% of the compound represented by the formula 1a, 0.5 wt% of vinylene carbonate (VC), and the remaining non-aqueous organic solution were mixed to prepare a 100 wt% non-aqueous electrolyte.
[0105] (manufacturing lithium secondary batteries) N-methyl-2-pyrrolidone (NMP) was used as the positive electrode active material, Li(Ni 0.8 Co0.1 Mn 0.1 A cathode slurry (solid content: 60 wt%) was prepared by adding 02, a conductive material (carbon black), and a binder (polyvinylidene fluoride) in a weight ratio of 97.5:1:1.5. The cathode slurry was applied to an aluminum (Al) thin film, which is a cathode current collector, having a thickness of 15 μm, and dried, followed by roll pressing to prepare a cathode.
[0106] Anode active material (graphite:SiO = 94.5:5.5 weight ratio), binder (SBR-CMC), and conductive material (carbon black) were added to water as a solvent in a weight ratio of 95:3.5:1.5 to prepare anode slurry (solid content: 60 wt%). The anode slurry was applied to a copper (Cu) thin film as anode current collector with a thickness of 6 μm, dried, and then roll pressed to prepare anode.
[0107] The positive electrode, a polyolefin-based porous separator coated with inorganic particles (Al2O3), and a negative electrode were sequentially stacked to prepare an electrode assembly.
[0108] The electrode assembly thus assembled was placed in a pouch-shaped battery case, and the non-aqueous electrolyte solution thus prepared was poured into the case to prepare a lithium secondary battery.
[0109] Example 2. A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound represented by Chemical Formula 1a was added in an amount of 1 wt % during the preparation of the non-aqueous electrolyte.
[0110] Example 3. A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound represented by Chemical Formula 1a was added in an amount of 2 wt % during the preparation of the non-aqueous electrolyte.
[0111] Comparative Example 1 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound represented by Formula 1a was not added during the preparation of the non-aqueous electrolyte.
[0112] Comparative Example 2 A lithium secondary battery was manufactured in the same manner as in Example 1, except that pyridine was added instead of the compound represented by Formula 1a when preparing the non-aqueous electrolyte.
[0113] Comparative Example 3. A lithium secondary battery was manufactured in the same manner as in Example 1, except that 2-fluoropyridine, in which fluorine is directly substituted on pyridine, was added instead of the compound represented by Formula 1a when preparing the non-aqueous electrolyte.
[0114] <Experimental Example 1: High-temperature life evaluation> The lithium secondary batteries manufactured in the examples and comparative examples were activated at 0.1 C CC and then degassed.
[0115] Next, the battery was charged at 0.33C CC to 4.20V under constant current-constant voltage (CC-CV) charging conditions at 25°C, and then a 0.05C current cut was performed, followed by discharging at 0.33C to 2.5V under CC conditions. The above charge / discharge cycle was counted as one cycle, and three cycles were performed. The initial discharge capacity was then measured using a PNE-0506 charger / discharger (manufacturer: PNE Solution Co., Ltd., 5V, 6A).
[0116] Next, the battery was charged at 0.33C CC to 4.20V under constant current-constant voltage (CC-CV) charging conditions at 45°C, and then a 0.05C current cut was performed, followed by discharging at 0.33C to 2.50V under CC conditions. The above charge / discharge cycle was counted as one cycle, and 200 charge / discharge cycles were performed. The discharge capacity after 200 cycles at 45°C was then measured using a PNE-0506 charger / discharger (manufacturer: PNE Solutions, Inc., 5V, 6A).
[0117] The discharge capacity retention rate after 200 cycles at high temperature (45° C.) was calculated using the following formula (1), and the results are shown in Table 1 below.
[0118] Formula (1): Discharge capacity retention rate after 200 cycles (%) = (discharge capacity after 200 cycles / initial discharge capacity) × 100
[0119] [Table 1]
[0120] From the results in Table 1 above, it can be seen that Examples 1 to 3, in which the compound represented by Chemical Formula 1a according to the present invention was used as an additive, had a higher capacity retention rate than Comparative Examples 1 to 3.
[0121] These characteristics are due to the fact that the sulfonylpyridine additive represented by formula 1a used in the examples stabilizes PF5 in high temperature environments, reducing the generation of HF, and forms a stable coating on the electrodes, improving thermal stability and high voltage characteristics.
[0122] On the other hand, the capacity retention rates of Examples 1 to 3 were significantly improved not only compared to Comparative Example 1, which did not contain a pyridine-based additive, but also compared to Comparative Example 2, which used an additive that did not contain a sulfonyl group or fluorine. From this, it can be seen that the battery life characteristics of Examples 1 to 3 were significantly improved not only due to the stabilizing effect of PF5 due to the pyridine structure, but also due to the effect of forming positive / negative electrode coatings due to the sulfonyl group and fluorine contained in Chemical Formula 1a.
[0123] It can also be seen that Examples 1 to 3 have improved capacity retention rates compared to Comparative Example 3, which uses an additive in which fluorine is directly substituted for pyridine without a sulfonyl group. This is because Comparative Example 3 not only loses the effect of film formation by the sulfonyl group, but also affects the pyridine ring structure during oxidation / reductive decomposition due to the action of fluorine as described above, making it difficult to form a smooth film. This confirms that when Chemical Formula 1a contains both a sulfonyl group and fluorine, there is an effect of improving high-temperature life due to the formation of a film.
[0124] That is, it can be seen that when a non-aqueous electrolyte solution containing the compound represented by Chemical Formula 1a according to the present invention is used, a lithium ion battery having excellent high-temperature life characteristics can be provided.
[0125] <Experimental Example 2: High-temperature storage evaluation> The lithium secondary batteries manufactured in the examples and comparative examples were activated at 0.1 C CC and then degassed.
[0126] Next, the battery was charged at 0.33C CC to 4.20V under constant current-constant voltage (CC-CV) charging conditions at 25°C, and then a 0.05C current cut was performed, and the battery was discharged at 0.33C to 2.5V under CC conditions. The above charge and discharge constitutes one cycle, and after three cycles, the battery was charged at 0.33C CC to 4.20V under constant current-constant voltage (CC-CV) charging conditions at 25°C, and then a 0.05C current cut was performed. The initial thickness of the battery was then measured using a plate measuring instrument weighing 300g. Specifically, the thickness was measured by placing the battery on the plate measuring instrument and placing a 300g weight on the battery to confirm the value that appeared.
[0127] The secondary batteries whose initial thickness had been measured were left in a 60°C oven (0F-02GW, manufactured by JEIO TECH) for 4 weeks, and after 4 weeks were removed from the oven and cooled at room temperature for 1 hour. The thickness after high-temperature storage was then measured using a 300g plate measuring instrument in the same manner as for the initial thickness.
[0128] The thickness increase rate of the battery after high-temperature storage was calculated using the following formula (2), and the results are shown in Table 2 below.
[0129] Equation (2): Thickness increase rate after 4 weeks of storage at 60°C (%) = (battery thickness after 4 weeks of storage at 60°C - initial battery thickness) / initial battery thickness x 100
[0130] [Table 2]
[0131] From the results in Table 2, it can be seen that Examples 1 to 3, in which the compound represented by Chemical Formula 1a according to the present invention is used as an additive, have a lower thickness increase rate after high temperature storage than Comparative Examples 1 to 3.
[0132] These characteristics are due to the fact that the sulfonylpyridine additive represented by formula 1a used in the examples stabilizes PF5 in high temperature environments, reduces the generation of HF, forms a stable coating on the electrode, improves thermal stability, and reduces gas generation due to side reactions in the coating.
[0133] On the other hand, in Examples 1 to 3, the thickness increase rate after high-temperature storage was significantly reduced compared to not only Comparative Example 1, which did not contain a pyridine-based additive, but also Comparative Example 2, which used an additive that did not contain a sulfonyl group and fluorine. From this, it can be seen that in Examples 1 to 3, side reactions at the electrode interface are suppressed not only due to the stabilizing effect of PF5 due to the pyridine structure, but also due to the effect of the formation of positive / negative electrode coatings due to the sulfonyl group and fluorine contained in Chemical Formula 1a.
[0134] In addition, the results of Comparative Example 3, which uses an additive in which fluorine is directly substituted with pyridine without a sulfonyl group, show that when only fluorine is substituted, the effect of forming a coating on the electrode is reduced compared to when both the sulfonyl group and fluorine are substituted, resulting in an increase in the amount of gas generated. In other words, it can be confirmed that when Chemical Formula 1a contains both a sulfonyl group and fluorine, there is an effect of reducing the amount of gas generated by forming a coating.
[0135] That is, it is found that when a non-aqueous electrolyte solution containing the compound represented by Chemical Formula 1a according to the present invention is used, a lithium ion battery having excellent characteristics of suppressing gas generation due to high-temperature storage can be provided.
Claims
1. A non-aqueous electrolyte for a lithium secondary battery, comprising a lithium salt, an organic solvent, and an additive containing a compound represented by the following chemical formula 1-1: [Formula 1] (In the above Chemical Formula 1-1, R1 is fluorine; or an alkyl group having 1 to 10 carbon atoms substituted with one or more fluorine atoms; R2 is an alkyl group having 1 to 10 carbon atoms, m is an integer of 0 to 4.
2. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein R1 is an alkyl group having 1 to 5 carbon atoms and substituted with one or more fluorine atoms.
3. 3. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein R1 is a methyl group substituted with one or more fluorine atoms.
4. The nonaqueous electrolyte for a lithium secondary battery according to claim 1 , wherein m is 0.
5. The non-aqueous electrolyte for a lithium secondary battery according to any one of claims 1 to 4, wherein the content of the compound represented by Chemical Formula 1-1 is 0.1 wt % to 5 wt % based on the total weight of the non-aqueous electrolyte.
6. The non-aqueous electrolyte for a lithium secondary battery according to any one of claims 1 to 5, wherein the content of the compound represented by Chemical Formula 1-1 is 0.1 wt % to 3 wt % based on the total weight of the non-aqueous electrolyte.
7. 7. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the additive further comprises at least one selected from the group consisting of vinylene carbonate, 1,3-propane sultone, ethylene sulfate, and lithium difluorophosphate.
8. The lithium salt is LiPF 6 and LiN(FSO 2 ) 2 The nonaqueous electrolyte solution for a lithium secondary battery according to claim 1 , comprising at least one selected from the group consisting of:
9. 9. The nonaqueous electrolyte solution for a lithium secondary battery according to claim 1, wherein the organic solvent comprises a mixture of two or more solvents selected from the group consisting of cyclic carbonate solvents, linear carbonate solvents, and linear ester solvents.
10. a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; A lithium secondary battery comprising the nonaqueous electrolyte solution according to claim 1 .
11. The lithium secondary battery according to claim 10 , wherein the positive electrode active material comprises a lithium composite transition metal oxide represented by the following Chemical Formula 2: [Chemical formula 2] Li 1+x (Ni a Co b Mn c M d ) O 2 (In the above Chemical Formula 2, M is W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, or Mo; 1+x, a, b, c, and d are each independently the atomic fraction of an element, -0.2≦x≦0.2, 0.50≦a<1, 0<b≦0.30, 0<c≦0.30, 0≦d≦0.10, a+b+c+d=1.)
12. The lithium secondary battery according to claim 11, wherein a satisfies 0.60≦a<1.
Citation Information
Patent Citations
High-voltage electrolyte with rapid charge function and preparation method and application thereof
CN107195970A
Electrolyte for lithium secondary battery
JP2002134168A
Electrolyte additive for lithium secondary batteries, non-aqueous electrolyte containing the said electrolyte additive, and lithium secondary battery
JP2015522209A
Pyridine sulfur trioxide complexes as electrolyte components for high voltage batteries.
JP2020504434A