Powder composition for coating thick film resistors and glass paste for coating thick film resistors

A lead-free glass powder composition with aluminum hydroxide for thick film resistors, fired at 650°C or lower, addresses resistance fluctuations and environmental concerns, ensuring chemical resistance and crack suppression, thereby improving yield and reliability.

JP7585612B2Active Publication Date: 2024-11-19SUMITOMO METAL MINING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020040466
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-10
Publication Date
2024-11-19
Estimated Expiration
2040-03-10

AI Technical Summary

Technical Problem

Existing thick film resistors face issues with high resistance value distribution and low yield due to large resistance fluctuations during firing, necessitating laser trimming, and require lead-free compositions to address environmental concerns.

Method used

A powder composition for thick film resistors using lead-free glass powder and aluminum hydroxide powder, with specific compositions of SiO2, B2O3, Al2O3, and Bi2O3, allowing firing at 650°C or lower, and a glass paste formulation that includes these components with a solvent and resin, ensuring chemical resistance and crack suppression.

Benefits of technology

The solution provides a lead-free, chemically resistant protective glass layer that maintains resistance stability during firing, preventing cracks and exposure to the external environment, thus enhancing yield and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585612000003
    Figure 0007585612000003
  • Figure 0007585612000004
    Figure 0007585612000004
  • Figure 0007585612000005
    Figure 0007585612000005
Patent Text Reader

Abstract

To provide a powder composition for coating a thick film resistor and a glass paste for coating the thick film resistor, which can be fired at a temperature of 650°C or lower, and even at a lower temperature, have chemical resistance and are substantially lead-free.SOLUTION: There are provided a powder composition for coating a thick film resistor, including lead-free glass powder and aluminum hydroxide powder, and there is also provided a glass paste for coating a thick film resistor, including a lead-free glass powder, an aluminum hydroxide powder, a resin, and a solvent.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powder composition for coating a thick-film resistor and a glass paste for coating a thick-film resistor, and more particularly to a powder composition for coating a thick-film resistor and a glass paste for coating a thick-film resistor that can be used as a material for a protective glass layer that protects a thick-film resistor or the like in the manufacture of electronic components such as chip resistors, hybrid ICs, or resistor networks. [Background technology]

[0002] In the manufacturing process of general chip resistors, hybrid ICs, resistor networks, etc., a thick-film resistor is formed by printing and firing a thick-film conductor paste mainly composed of Ag or Au on an alumina substrate to form a pair of electrodes with a certain distance between them, and then printing and firing a resistor paste between the electrodes to connect the pair of electrodes obtained. The thick-film resistor printed and fired in this way has a large distribution of resistance values, so there is a problem that the yield is low in order to achieve a resistance value in the desired range.

[0003] To solve such yield problems, the resistance value of the thick-film resistor is generally increased by laser trimming to adjust it to a desired range. Furthermore, in order to improve the accuracy of laser trimming and to improve the reliability of the resulting electronic component, which is a product using the thick-film resistor, a protective glass paste may be printed and baked on the thick-film resistor before laser trimming. This forms a protective glass layer (pre-coat), and then laser trimming is performed through the resulting protective glass layer.

[0004] For example, Patent Document 1 discloses a method for manufacturing a resistor. The precoat glass paste and the like that is fired at 590° C. disclosed in Patent Document 1 is generally composed of glass powder containing lead. However, in recent years, the lead component is undesirable in terms of its effect on the human body and pollution, and there is a strong demand for the development of a lead-free composition for coating a thick-film resistor.

[0005] As an example of a chip resistor, Fig. 1 shows a schematic cross-sectional side view of a chip resistor 100. The chip resistor 100 includes electrodes 20 made mainly of silver formed on the surface of an alumina substrate 10 with an inter-electrode distance, a thick-film resistor 30 provided so as to straddle the electrodes 20, and a protective glass layer 41 covering the thick-film resistor 30. The electrodes 20 are covered with a plating layer 60 of nickel or the like.

[0006] The protective glass layer 41 prevents debris generated by laser trimming from adhering to the thick-film resistor 30, and also prevents the laser light used in laser trimming from directly hitting the thick-film resistor 30. In this way, the protective glass layer 41 serves to reduce damage to the thick-film resistor 30 caused by the laser light during laser trimming.

[0007] After the laser trimming, a protective glass paste, either the same as that of the protective glass layer 41 or a different protective glass paste from that of the protective glass layer 41, is printed and baked as an overcoat to cover the surfaces of the thick film resistor 30 and the protective glass layer 41, thereby forming a surface protective glass layer 42 for protecting the thick film resistor 30 from the external environment. Alternatively, instead of the surface protective glass layer 42, a thermosetting protective resin paste is printed and thermoset after the laser trimming to form a surface protective resin layer 42 for protecting the thick film resistor 30 from the external environment.

[0008] After the surface protective glass layer 42 or the surface protective resin layer 42 is formed, the surface of the electrode 20 is coated with nickel plating or tin plating by, for example, a wet plating method. The surface protective glass layer 42 or the surface protective resin layer 42 has chemical resistance that prevents it from being corroded by a plating solution. However, even if the surface protective glass layer 42 or the surface protective resin layer 42 can protect the thick-film resistor 30 from the external environment, the surface protective glass layer 42 or the protective glass layer 41 between the surface protective resin layer 42 and the thick-film resistor 30 is also required to have similar chemical resistance so as to prevent it from being corroded by a plating solution.

[0009] Patent Document 2 discloses a technology of a glass paste for a precoat layer that is substantially free of lead, can be fired at 700° C. or less, has chemical durability, and is chemically durable. Patent Document 2 also discloses the results of forming a precoat layer by firing at 650° C. The firing temperature for forming the precoat layer in Patent Document 2 is higher than the firing temperature disclosed in Patent Document 1.

[0010] When protective glass layer 41 is formed by firing, if the firing temperature is high, the resistance value of thick film resistor 30 fluctuates greatly, and in particular, if the firing temperature exceeds 650° C., the resistance value of thick film resistor 30 may fluctuate significantly. Therefore, in order to avoid a decrease in product yield, it is important to form protective glass layer 41 at a firing temperature of 650° C. or less. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Japanese Patent Application Publication No. 11-224809 [Patent Document 2] JP 2007-176785 A Summary of the Invention [Problem to be solved by the invention]

[0012] In view of the above circumstances, an object of the present invention is to provide a powder composition for coating a thick-film resistor, which can be fired at 650° C. or less, or even lower, has chemical resistance, and is substantially free of lead, and a glass paste for coating a thick-film resistor. [Means for solving the problem]

[0013] In order to solve the above problems, the powder composition for coating a thick-film resistor of the present invention contains a lead-free glass powder and an aluminum hydroxide powder.

[0014] The aluminum hydroxide powder may be contained in an amount of 1.4 parts by mass to 5.6 parts by mass with respect to 100 parts by mass of the lead-free glass powder.

[0015] The lead-free glass powder may contain 5 mass % to 25 mass % of SiO2, 1 mass % to 5 mass % of B2O3, 2 mass % to 5 mass % of Al2O3, and 40 mass % to 80 mass % of Bi2O3.

[0016] In order to achieve the above object, the glass paste for covering a thick-film resistor of the present invention contains a lead-free glass powder, an aluminum hydroxide powder, a resin, and a solvent.

[0017] The aluminum hydroxide powder may be contained in an amount of 1.4 parts by mass to 5.6 parts by mass with respect to 100 parts by mass of the lead-free glass powder.

[0018] The lead-free glass powder may contain 5 mass % to 25 mass % of SiO2, 1 mass % to 5 mass % of B2O3, 2 mass % to 5 mass % of Al2O3, and 40 mass % to 80 mass % of Bi2O3. Effect of the Invention

[0019] According to the present invention, it is possible to provide a powder composition for coating a thick-film resistor and a glass paste for coating a thick-film resistor which can be fired at a temperature of 650° C. or less or even lower, have chemical resistance, and are substantially free of lead. [Brief description of the drawings]

[0020] [Figure 1] 1 is a schematic cross-sectional side view of a chip resistor 100. FIG. [Diagram 2] 3 is an SEM image of the protective glass layer according to Example 1 before immersion in sulfuric acid. [Diagram 3] 4 is an SEM image of the protective glass layer according to Example 1 after immersion treatment in sulfuric acid. [Figure 4] 4 is an SEM image of the protective glass layer according to Example 2 after immersion treatment in sulfuric acid. [Diagram 5]1 is an SEM image of the protective glass layer according to Example 3 after immersion treatment in sulfuric acid. [Figure 6] 4 is an SEM image of the protective glass layer according to Comparative Example 1 after immersion treatment in sulfuric acid. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Specific embodiments of the present invention will be described in detail below, however, the present invention is not limited to the following embodiments.

[0022] [Powder composition for coating thick film resistors] The powder composition for coating a thick-film resistor according to the present embodiment is characterized by containing a lead-free glass powder and an aluminum hydroxide powder.

[0023] Lead-free glass powder In the powder composition for covering thick-film resistors, it is necessary that the glass powder is sufficiently melted during firing so that each particle of the glass powder is fused. If each particle of the glass powder is not fused in this way, the strength of the protective glass layer is insufficient, and the chemical resistance against nickel plating, tin plating, etc. is not satisfied. In addition, when a defect occurs in the surface protective glass layer or the surface protective resin layer, if the protective glass layer also has a defect, there is a problem that the thick-film resistor itself is directly exposed to the external environment.

[0024] In addition, when a glass paste for covering a thick-film resistor is printed on a thick-film resistor and fired to form a protective glass layer, if the firing temperature TC (°C) is high, the resistance value of the thick-film resistor fluctuates greatly. For a normal thick-film resistor, firing the glass paste for covering a thick-film resistor at a firing temperature TC (°C) exceeding 650°C results in excessive fluctuation in the resistance value of the thick-film resistor. For this reason, the firing temperature TC (°C) of the thick-film protective glass paste is preferably 650°C or lower, more preferably 640°C or lower, and even more preferably 620°C or lower. The lower limit of the firing temperature (°C) is 400°C, since it must be higher than the decomposition temperature of the organic binder contained in the glass paste for covering a thick-film resistor.

[0025] In order to achieve such a firing temperature and to bring the individual particles of the glass powder into a fused state, the softening point of the lead-free glass powder is desirably a temperature 10° C. to 50° C. lower than the firing temperature for forming the protective glass layer. The softening point can be measured by differential thermal analysis (TG-DTA), and is the temperature at which the next differential thermal curve on the higher side decreases after heating the lead-free glass at a temperature increase of 10° C. / min in air, which is higher than the temperature at which the differential thermal curve on the lowest side decreases.

[0026] If the softening point is not within the range of 10°C to 50°C lower than the firing temperature, the particles of the glass powder will not be sufficiently fused even after firing, causing defects in the protective glass layer, which may result in direct exposure of the thick-film resistor itself to the external environment. Also, the glass powder may melt and flow out to areas other than between the electrodes of the chip resistor, causing defects in the shape of the protective glass layer.

[0027] In this embodiment, the lead-free glass powder has a composition of 5% to 25% by mass of SiO2, 1% to 5% by mass of B2O3, 2% to 5% by mass of Al2O3, and 40% to 80% by mass of Bi2O3. Glass containing Bi is widely known as a lead-free glass with a low softening point, and Bi2O3 has attracted attention as a low softening point glass as a component to replace PbO.

[0028] Here, lead-free means that it does not substantially contain lead, and this accepts cases including cases that do not contain lead and cases that contain 100 ppm by mass or less of lead as an unavoidable impurity due to lead being mixed in raw material powders such as conductive powders and oxide powders that contain lead or during the manufacturing process.

[0029] The lead-free glass powder preferably contains 5% to 25% by mass of SiO2, and more preferably 5% to 23% by mass of SiO2. If the SiO2 content is less than 5.0% by mass, the water resistance and acid resistance of the resulting protective glass layer may be reduced. If the SiO2 content is more than 25.0% by mass, the softening point SPa (°C) may be too high.

[0030] Next, the lead-free glass powder preferably contains 1% to 5% by mass of B2O3. If the content of B2O3 is less than 1.0% by mass, the softening point (°C) increases, and the mechanical strength of the resulting thick protective glass layer may decrease. If the content of B2O3 exceeds 5.0% by mass, the water resistance and acid resistance of the resulting thick protective glass layer may decrease.

[0031] The lead-free glass powder preferably contains 2% to 5% by mass of Al2O3. If the content of Al2O3 is less than 2.0% by mass, the thick protective glass layer obtained is likely to crystallize, and the water resistance and acid resistance of the thick protective glass layer obtained may decrease. If the content of Al2O3 exceeds 5.0% by mass, the softening point (°C) may become too high.

[0032] The lead-free glass powder preferably contains 40% to 80% by mass of Bi2O3. If the Bi2O3 content is less than 40.0% by mass, the softening point (°C) may be too high. If the Bi2O3 content exceeds 80.0% by mass, the water resistance and acid resistance of the resulting thick protective glass layer may be reduced.

[0033] (Other ingredients) The lead-free glass powder may contain components other than SiO2, B2O3, and Bi2O3. Examples of the other components include Al2O3, BaO, CaO, SrO, TiO2, ZrO2, ZnO, SnO2, MgO, and alkali metal oxides such as Li2O, Na2O, and K2O. Although alkali metal oxides have a large effect of lowering the softening point SPa (°C), if they are contained in large amounts, there is a risk of increasing the resistance value fluctuation due to the voltage load of the thick-film resistor. Therefore, the content of these other components as a whole is preferably 1.0 mass% or less.

[0034] The particle size of the lead-free glass powder is preferably such that the 50% cumulative volume particle size (median diameter) is 10 μm or less. If the median diameter is greater than 10 μm, it may be difficult to form a dense protective glass layer. Furthermore, with the miniaturization of electronic components in recent years, the thickness of the protective glass layer also tends to become thinner. Considering this trend, it is desirable to further reduce the 50% cumulative volume particle size of the lead-free glass powder, which is the raw material for the protective glass layer, so that the median diameter is 5 μm or less. The 50% cumulative volume particle size can be measured using a particle size distribution analyzer that uses laser diffraction.

[0035] <Aluminum hydroxide powder> The protective glass layer obtained by firing the powder composition for covering a thick-film resistor of the present embodiment, which contains a lead-free glass powder and an aluminum hydroxide powder, may develop cracks on its surface when immersed in sulfuric acid having the same pH as a nickel plating solution, a tin plating solution, etc., but the cracks do not grow to a width of more than 2 μm. In other words, this protective glass layer can satisfy chemical resistance in that it can prevent defects from occurring by suppressing the growth of cracks and can prevent the thick-film resistor itself from being directly exposed to the external environment.

[0036] The aluminum hydroxide powder used in combination with the lead-free glass powder changes to aluminum oxide during the firing process. The presence of aluminum oxide in the protective glass layer due to the aluminum hydroxide powder satisfies the chemical resistance and suppresses the growth of cracks during acid immersion. The growth of cracks during acid immersion can also be suppressed by using aluminum oxide powder instead of aluminum hydroxide. However, the effect of suppressing cracks when using aluminum oxide powder is inferior to that of aluminum hydroxide powder.

[0037] In the powder composition for covering a thick-film resistor, the aluminum hydroxide powder is preferably contained in an amount of 1.4 to 5.6 parts by mass relative to 100 parts by mass of the lead-free glass powder, and more preferably contained in an amount of 2.4 to 4.6 parts by mass in consideration of the chemical resistance of the protective glass layer, the manufacturing cost, the raw material cost, etc. If the aluminum hydroxide powder is contained in an amount of less than 1.4 parts by mass relative to 100 parts by mass of the lead-free glass powder, the growth of cracks generated in the protective glass layer may not be suppressed. In addition, if the aluminum hydroxide powder is contained in an amount of more than 5.6 parts by mass relative to 100 parts by mass of the lead-free glass powder, it may be difficult to ensure the transparency of the protective glass layer to a degree that does not interfere with laser trimming.

[0038] The particle size of the aluminum hydroxide powder is preferably 0.5 μm to 1.5 μm in terms of 50% cumulative volume particle size (median diameter), and more preferably 0.7 μm to 1.3 μm from the viewpoint of the chemical resistance of the protective glass layer and ease of sintering treatment. If the average particle size of the aluminum hydroxide powder exceeds 1.5 μm, it is likely to cause problems in laser trimming. The 50% cumulative volume particle size can be measured by a particle size distribution analyzer that uses laser diffraction.

[0039] (Other ingredients) In addition to the lead-free glass powder and aluminum hydroxide powder, the powder composition for coating thick-film resistors of the present invention may contain additives and other components as necessary. Examples of additives include pigments or dyes for coloring, and inorganic powders for adjusting the thermal expansion coefficient. Representative examples of pigments for coloring include black pigments such as Cu-Cr-Mn, Fe-Cr-Mn, and Co-Fe-Cr, and green pigments such as Cr2O3. In particular, green pigments are generally used to reduce damage to thick-film resistors caused by laser light, as they are said to absorb a large amount of laser light during laser trimming. In addition, dyes can be contained for the purpose of improving visibility when the glass paste for coating thick-film resistors is printed, and a representative example of a dye that does not remain colored after firing the glass paste for coating thick-film resistors is blue phthalocyanine blue.

[0040] [Glass paste for covering thick film resistors] The powder composition for coating a thick-film resistor of the present invention can be mixed and dispersed with an organic vehicle or a solvent to form a paste, thereby making it possible to prepare a glass paste for coating a thick-film resistor. In place of the powder composition for coating a thick-film resistor, or in combination with the powder composition for coating a thick-film resistor, the above-mentioned lead-free glass powder and aluminum hydroxide powder may be used.

[0041] For the reasons mentioned above, the aluminum hydroxide powder is preferably contained in an amount of 1.4 parts by mass to 5.6 parts by mass per 100 parts by mass of the lead-free glass powder.

[0042] Furthermore, for the reasons mentioned above, the lead-free glass powder preferably contains 5 mass% to 25 mass% SiO2, 1 mass% to 5 mass% B2O3, 2 mass% to 5 mass% Al2O3, and 40 mass% to 80 mass% Bi2O3.

[0043] <resin> Examples of resins that can be used include resins that are generally used in pastes such as glass pastes for covering thick-film resistors, etc. For example, ethyl cellulose, alkyd resins, acrylic resins, etc. can be used.

[0044] <solvent> Examples of the solvent that can be used include solvents that are generally used in pastes such as glass pastes for coating thick-film resistors, such as terpineol and butyl carbitol.

[0045] The resin and the solvent are mixed in advance to prepare an organic vehicle, which can be used to manufacture a paste for forming a thick-film conductor. For example, from the viewpoint of cost and ease of handling, a solution of ethyl cellulose in terpineol can be used as the organic vehicle. The ratio of the resin to the solvent in the organic vehicle is appropriately selected depending on the printability and application method of the final glass paste composition for covering a thick-film resistor. For example, the resin content in the organic vehicle can be 2 to 50 mass %.

[0046] The content of the organic vehicle in the glass paste for covering a thick-film resistor can be appropriately selected in consideration of the viscosity of the paste, the amount of oil to be supplied to the powder, the ease of application, etc. If the viscosity of the glass paste for covering a thick-film resistor is too high, the application of the paste may be substantially impossible. If the content of the organic vehicle is too high, the particles of the lead-free glass or the particles of the aluminum hydroxide powder may settle or separate, or the density of the protective glass layer after firing may be significantly reduced, resulting in an insufficient chemical resistance.

[0047] For example, the content of the organic vehicle can be 15 parts by mass to 100 parts by mass relative to 100 parts by mass of the total mass of the lead-free glass powder and the aluminum hydroxide powder. In consideration of printability, ease of application, settling of particles as a paste, separation, chemical resistance, raw material costs, etc., the content is preferably 20 parts by mass to 80 parts by mass.

[0048] The glass paste for covering a thick-film resistor of the present invention can be produced by mixing and dispersing the powder composition for covering a thick-film resistor with an organic vehicle. The mixing and dispersing methods are not particularly limited, but for example, a three-roll mill or a ball mill is generally used. Even when a lead-free glass powder and an aluminum hydroxide powder are used instead of the powder composition for covering a thick-film resistor or when they are used in combination, a glass paste for covering a thick-film resistor can be produced in the same manner as described above. In addition, the viscosity of the obtained glass paste for covering a thick-film resistor is appropriately selected depending on the film thickness of the intended protective glass layer and the type of the thick-film resistor to be coated with the paste.

[0049] (Other ingredients) In addition to the lead-free glass powder and aluminum hydroxide powder, the glass paste for covering a thick-film resistor of the present invention may contain additives and other components as necessary. Examples of additives include pigments or dyes for coloring, and inorganic powders for adjusting the thermal expansion coefficient. Representative examples of pigments for coloring include black pigments such as Cu-Cr-Mn, Fe-Cr-Mn, and Co-Fe-Cr, and green pigments such as Cr2O3. In particular, green pigments are generally used to reduce damage to thick-film resistors caused by laser light, since they are said to absorb a large amount of laser light during laser trimming. In addition, dyes can be contained for the purpose of improving visibility when the glass paste for covering a thick-film resistor is printed, and a representative example of a dye that does not remain colored after firing the glass paste for covering a thick-film resistor is blue phthalocyanine blue.

[0050] [Method of forming protective glass layer] The protective glass layer can be formed by printing the glass paste for covering a thick film resistor of the present invention so as to cover the thick film resistor, drying it, and then firing it. Considering the chemical resistance and processability such as laser trimming, it is desirable to form the protective glass layer so that the thickness of the layer obtained after firing is 3 μm to 10 μm.

[0051] A method for forming a protective glass layer can include, for example, a coating step of applying the glass paste for covering thick film resistors of the present invention to the surface of a thick film resistor of a chip resistor, a drying step of drying the chip resistor to which the paste has been applied, and then a firing step of firing at a temperature of 650°C or less.

[0052] (Coating process) The application method is not particularly limited, and any known technique can be used, such as a printing method such as screen printing, letterpress printing, or gravure printing, or a drawing method using a dispenser. From the viewpoint of mass production with an appropriate film thickness, application by screen printing is preferable.

[0053] (drying process) After the thick-film resistor coating glass paste is applied to the thick-film resistor, the applied film is preferably dried for 2 to 15 minutes together with the chip resistor at a temperature of 80°C to 200°C. In this way, by providing a drying step between the application step and the firing step, it is possible to prevent the volatilization and combustion of the solvent due to the volatile components such as the solvent remaining even during firing, and therefore, when a firing furnace is used in the firing step, it is possible to obtain the effect of preventing contamination of the firing furnace. In this step, the drying method is not particularly limited, and known means such as an oven or a belt-type drying furnace can be used, but from the viewpoint of mass production, it is preferable to dry using a belt-type drying furnace. In addition, if the drying temperature is less than 80°C, the time required for drying is long, which may deteriorate productivity, and this may not be preferable. In addition, if the drying temperature exceeds 200°C, the resin may be oxidized and the film after drying may become brittle.

[0054] (Firing process) In the firing process after the drying process, the dried film is heated together with the chip resistor to fire the film. A belt furnace is preferably used as the firing method. In this case, the peak temperature in firing is set to 650°C or less so that the resistance value of the thick film resistor does not fluctuate significantly. In addition, taking into consideration the fusion of lead-free glass particles and the conditions for generating aluminum oxide from aluminum hydroxide powder, it is preferable to fire at a temperature of 400°C or more.

[0055] It is necessary to hold the above peak temperature for 2 to 20 minutes, preferably 5 to 13 minutes. If the holding time of the peak temperature exceeds 20 minutes, the protective glass layer may be over-sintered, and if the holding time is less than 2 minutes, the sintering may be insufficient. In addition, the total time of the firing process including heating to the peak temperature, holding the peak temperature, and cooling from the peak temperature must be 20 to 90 minutes, preferably 30 to 60 minutes. If the total time is less than 20 minutes, the heating rate and cooling rate may become too large, and the protective glass layer may crack due to a sudden temperature change. In addition, if the total time exceeds 90 minutes, the problem of reduced productivity may occur.

[0056] In order to perform firing at the peak temperature and firing time described above, it is preferable that the heating rate to the peak temperature is 20°C / min or more and 150°C / min or less, and the cooling rate from the peak temperature is 20°C / min or more and 200°C / min or less. If the heating rate is less than 20°C / min or the cooling rate is less than 20°C / min, productivity may deteriorate, which is not preferable. In addition, if the heating rate exceeds 150°C / min or the cooling rate exceeds 200°C / min, it is not preferable because cracks may occur in the protective glass layer due to a sudden temperature change.

[0057] The atmosphere during firing is not particularly limited, but firing in an air atmosphere is preferred from the viewpoint of softening the lead-free glass.

[0058] The protective glass layer formed as described above can satisfy the chemical resistance. Specifically, when the protective glass layer is immersed in sulfuric acid having a pH equivalent to that of a nickel plating solution, the glass layer is not dissolved by the sulfuric acid, but cracks having a width of 5 μm or less may occur on the surface. However, the cracks that occur do not penetrate into the protective glass layer, and the protective glass layer can protect the thick-film resistor from the external environment.

[0059] If the thickness of the protective glass layer is extremely thin, for example, less than 2 μm, the thick-film resistor may not be protected if a crack with a width of 2 μm or more occurs. Therefore, the thickness of the protective glass layer is important, and it is desirable to form the protective glass layer so that the thickness after firing is 3 μm to 10 μm as described above. EXAMPLES

[0060] The present invention will be further described below with reference to examples, but the scope of the present invention is not limited to these examples.

[0061] [Production of Powder Composition for Coating Thick Film Resistor] As shown in Table 1, 100 parts by mass of lead-free glass powder having a composition of SiO2: 21.6 mass%, B2O3: 1.4 mass%, Al2O3: 3.3 mass%, and Bi2O3: 72.8 mass%, a softening point (℃) of 595℃, and a 50% cumulative volume particle size of 2.0μm, and 1.4 parts by mass, 2.8 parts by mass, and 5.6 parts by mass of aluminum hydroxide powder having a 50% cumulative volume particle size of 0.9μm were mixed in the mixing ratios shown in Table 2 to obtain a powder composition for covering a thick-film resistor. The 50% cumulative volume particle size was measured by a particle size distribution analyzer using laser diffraction.

[0062] [Table 1]

[0063] [Manufacture of glass paste for covering thick film resistors] To 100 parts by mass of the obtained powder composition for covering thick film resistors, 30 parts by mass of a terpineol solution containing 4% ethyl cellulose was added as an organic vehicle, and the mixture was mixed and dispersed using a three-roll mill to obtain glass pastes for covering thick film resistors of Examples 1 to 3.

[0064] In addition, without mixing aluminum hydroxide powder, 30 parts by mass of a terpineol solution containing 4% ethyl cellulose was added as an organic vehicle to 100 parts by mass of lead-free glass powder having the composition shown in Table 1, and the mixture was mixed and dispersed using a three-roll mill in the same manner as in Examples 1 to 3 to obtain a glass paste for covering thick-film resistors in Comparative Example 1.

[0065] The obtained glass paste for covering thick film resistors was screen printed in a square pattern of 20 mm long x 20 mm wide on a 96% alumina substrate (25.4 mm x 25.4 mm x 1 mm), dried, and then fired in a firing furnace under conditions of a peak temperature (°C) of 600°C and a peak time of 5 minutes, obtaining protective glass layers for Examples 1 to 3 and Comparative Example 1 with the film thicknesses shown in Table 2.

[0066] The protective glass layers according to Examples 1 to 3 and Comparative Example 1 were immersed together with the alumina substrate in 5% sulfuric acid at 25° C. for 120 minutes to evaluate the chemical resistance and crack growth of the protective glass layer. The chemical resistance was evaluated based on visual changes in the surface of the protective glass layer before and after immersion in sulfuric acid. The inhibition of crack growth was evaluated by observation with a scanning electron microscope (SEM) after immersion in sulfuric acid. The evaluation results are shown in Table 2.

[0067] An SEM image of the surface of the protective glass layer according to Example 1 taken before immersion in sulfuric acid is shown in Fig. 2, and an SEM image of the surface of the protective glass layer according to Example 1 taken after immersion in sulfuric acid is shown in Fig. 3. In addition, an SEM image of the surface of the protective glass layer according to Example 2 taken after immersion in sulfuric acid is shown in Fig. 4, an SEM image of the surface of the protective glass layer according to Example 3 taken after immersion in sulfuric acid is shown in Fig. 5, and an SEM image of the surface of the protective glass layer according to Comparative Example 1 taken after immersion in sulfuric acid is shown in Fig. 6.

[0068] [Table 2]

[0069] The protective glass layer obtained using the powder composition for thick-film resistor coating of Examples 1 to 3 containing lead-free glass powder and aluminum hydroxide powder did not change in surface appearance when visually observed even when immersed in sulfuric acid. In addition, even when looking at SEM images, it was confirmed that there was no problem with chemical resistance because the occurrence of cracks exceeding 2 μm in width was suppressed. In addition, the fact that the appearance such as gloss did not change visually even when the protective glass layer was immersed in sulfuric acid means that the protective glass layer has chemical resistance, and since the visual appearance did not change in the protective glass layers in Examples 1 to 3, it was confirmed that there was no problem with chemical resistance even when visually observed.

[0070] On the other hand, the protective glass layer obtained using the powder composition for covering thick-film resistors of Comparative Example 1, which used the same lead-free glass powder as in Examples 1 to 3 but did not contain aluminum hydroxide powder, did not change in appearance such as gloss when visually observed after immersion in sulfuric acid, but SEM images confirmed that cracks exceeding 2 μm in width had occurred, indicating that the protective glass layer may not have sufficient chemical resistance.

[0071] [summary] From the above results, it was confirmed that, according to this embodiment, even a lead-free protective glass layer formed at a firing temperature of 600° C. has chemical resistance. Therefore, the thick-film resistor covering glass paste of the present invention, which is a molding material for a chemical-resistant protective glass layer, is a desirable material from the viewpoint of environmental protection since it does not contain lead, and can replace the thick-film resistor glass paste disclosed in Patent Document 1 and the like. [Explanation of symbols]

[0072] 10 Alumina substrate 20 electrodes 30 Thick film resistor 41 Protective Glass Layer 42 Surface protection glass layer (surface protection resin layer) 60 Plating layer 100 Chip Resistors

Claims

1. Contains lead-free glass powder and aluminum hydroxide powder, The lead-free glass powder contains 5% by mass to 25% by mass of SiO 2 and 1% by mass to 5% by mass of B 2 O 3 and 2% by weight to 5% by weight of Al 2 O 3 and 40% by mass to 80% by mass of Bi 2 O 3 A powder composition for coating a thick film resistor comprising:

2. 2. The powder composition for coating a thick film resistor according to claim 1, wherein the aluminum hydroxide powder is contained in an amount of 1.4 parts by mass to 5.6 parts by mass per 100 parts by mass of the lead-free glass powder.

3. Lead-free glass powder; Aluminum hydroxide powder; Resin and A solvent, The lead-free glass powder contains 5% by mass to 25% by mass of SiO 2 and 1% by mass to 5% by mass of B 2 O 3 and 2% by weight to 5% by weight of Al 2 O 3 and 40% by mass to 80% by mass of Bi 2 O 3 A glass paste for covering a thick film resistor comprising:

4. 4. The glass paste for covering a thick-film resistor according to claim 3, wherein the aluminum hydroxide powder is contained in an amount of 1.4 to 5.6 parts by mass per 100 parts by mass of the lead-free glass powder.

Citation Information

Patent Citations

  • Paste composition

    JP1990124744A

  • Manufacture of square plate type chip resistor

    JP1999224809A

  • Sealing composition

    JP2002241143A

  • Manufacturing method of electronic component

    JP2005286253A

  • Glass paste for over coat and thick film resistance element

    JP2007176785A