Hydrometallurgical process for nickel oxide ore

By blending nickel-cobalt mixed sulfide with nickel oxide ore to control carbon and sulfur grades and ORP, the method addresses zinc concentration issues in the dezincing process, resulting in high-quality nickel-cobalt mixed sulfide with reduced zinc content and improved operational efficiency.

JP7585894B2Active Publication Date: 2024-11-19SUMITOMO METAL MINING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021039457
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-11
Publication Date
2024-11-19
Estimated Expiration
2041-03-11

AI Technical Summary

Technical Problem

The existing hydrometallurgical methods for nickel oxide ore face challenges in controlling the zinc concentration during the dezincing process, leading to increased zinc quality in the final reaction solution, which affects the quality of the nickel-cobalt mixed sulfide product, and this is exacerbated by low carbon grades in the ore and varying redox conditions.

Method used

A hydrometallurgical method that involves blending nickel-cobalt mixed sulfide with nickel oxide ore to create an ore slurry with specific carbon and sulfur grades, controlling the oxidation-reduction potential (ORP) within a range, and using high-pressure air as an oxidizing agent to suppress the re-dissolution of zinc, thereby adjusting the Fe2+ concentration in the leachate.

Benefits of technology

This method effectively reduces the zinc concentration in the final reaction solution, producing high-quality nickel-cobalt mixed sulfide with reduced zinc grade, enhancing operational efficiency and quality while minimizing nickel loss and chemical costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585894000005
    Figure 0007585894000005
  • Figure 0007585894000001
    Figure 0007585894000001
  • Figure 0007585894000002
    Figure 0007585894000002
Patent Text Reader

Abstract

To provide a method of preventing remelting of zinc in processing at a dezincification step and acquiring nickel cobalt mixed sulfide of high quality with reduced zinc grade.SOLUTION: A wet type smelting method for nickel oxide ore that generates sulfide including nickel from an exudate obtained by exudating nickel oxide ore, comprises: a preparing step of preparing ore slurry from the nickel oxide ore; an exudating step of adding a sulfuric acid to the ore slurry and performing exudation processing to obtain an exudate containing nickel and cobalt; a dezincification step of sulfidating the zinc contained in the exudate to remove the zinc; and a nickel collecting step of adding a sulfating agent to a reaction termination solution resulting from the processing in the dezincification step to acquire a nickel and cobalt mixed sulfide. In the preparing step, nickel and cobalt mixed sulfide is added to and blended with the nickel oxide ore, and preparation is performed so that a total sum of carbon grade and sulfur grade in the ore slurry is 0.28 mass% or greater and 0.63 mass% or smaller.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for hydrometallurgy of nickel oxide ore using a high-pressure acid leaching method in which nickel is leached from nickel oxide ore using sulfuric acid under high temperature and pressure. [Background technology]

[0002] One method for hydrometallurgy of nickel oxide ore is the high pressure acid leaching (HPAL) method using sulfuric acid. Unlike the conventional pyrometallurgy, which is a typical method for smelting nickel oxide ore, this method does not include reduction and drying processes and is a continuous hydrometallurgy process, which is advantageous in terms of energy and cost. In addition, it has the advantage of being able to obtain a sulfide containing nickel and cobalt with a nickel content of about 50 mass% (hereinafter also referred to as "nickel-cobalt mixed sulfide").

[0003] Specifically, the hydrometallurgical method for nickel oxide ore by high pressure acid leaching includes the following steps: (a) A leaching process in which sulfuric acid is added to a nickel oxide ore slurry and leaching is performed under high temperature and pressure to obtain a leachate containing nickel and cobalt as well as impurity elements. (b) A neutralizing step in which a neutralizing agent is added to the leachate to adjust the pH to obtain a neutralized slurry. (c) A liquid purification process in which the neutralized slurry is subjected to multiple washing steps and pH adjustment by adding a neutralizing agent, while separating the neutralized liquid containing nickel, cobalt, and impurities from the residue. (d) a dezincing step in which hydrogen sulfide gas is added to the neutralization end liquor containing nickel and cobalt to form a dezincing residue mainly containing zinc sulfide, and the dezincing residue is separated from a mother liquor for nickel recovery containing nickel and cobalt. (e) A nickel recovery process in which hydrogen sulfide gas is added to a nickel recovery mother liquor containing nickel and cobalt to form a nickel-cobalt mixed sulfide and separate and recover it.

[0004] In the above-mentioned hydrometallurgical method for nickel oxide ore, the dezincification step is carried out to remove divalent iron (Fe 2+ It is known that when the zinc concentration in the mother liquor for nickel recovery is low, the zinc concentration in the mother liquor for nickel recovery increases. This is thought to be because the fixation of zinc by sulfurization (reaction formula [1] below) is inhibited, and the effect of redissolution of zinc by oxidation of zinc sulfide in the dezincification residue (reaction formulas [2] and [3] below) becomes relatively large. Zinc 2+ +FeS → ZnS+Fe 2+ [1] 2Fe(OH)3+ZnS+6H + = Zn 2+ +2Fe 2+ +S0+6H2O [2] Fe(OH)3+ZnS+H2O = Zn 2+ +Fe 2+ +SO4 2- +5H + +7e [3]

[0005] If the zinc concentration in the reaction end solution in the dezincing process increases, the zinc grade in the nickel and cobalt mixed sulfide (hereinafter sometimes abbreviated as "MS") obtained in the nickel recovery process increases, causing poor quality. For this reason, in order to further reduce the zinc concentration in the reaction end solution obtained through the dezincing process, it is necessary to increase the amount of sulfurizing agent such as hydrogen sulfide gas added and to strengthen the sulfurization reaction. However, increasing the amount of sulfurizing agent such as hydrogen sulfide gas added and strengthening the sulfurization reaction not only increases the cost of chemicals, but also causes nickel coprecipitation in the zinc sulfide residue, leading to an increase in nickel loss, which is an economic obstacle to operation.

[0006] For this reason, in order to suppress the increase in zinc concentration in the final reaction solution in the dezincification process, the Fe concentration in the final neutralization solution used in the dezincification process is 2+ Concentration control is required.

[0007] Fe in the final neutralization solution 2+The concentration depends heavily on the redox atmosphere in the leaching process. The main component of nickel oxide ore, Fe (mainly present as FeOOH (goethite)), is oxidized and decomposed by acid leaching, and is dissolved in the solution (reaction formula [4] below). It is then fixed as hematite by hydrolysis at high temperatures (reaction formula [5] below). However, the plant-derived carbon contained in nickel oxide ore acts as a reducing agent under high temperature and pressure, lowering the oxidation-reduction potential (ORP), and the Fe dissolved in the solution is dissolved in the solution. 3+ The sulfate is reduced to Fe 2+ This is to produce sulfate (reaction formula [6] below). 2FeOOH+3H2SO4→ Fe2(SO4)3+4H2O ···[4] Fe2(SO4)3+3H2O → Fe2O3+3H2SO4...[5] 2Fe2(SO4)3+C+2H2O → 4FeSO4+CO2+2H2SO4 [6]

[0008] Therefore, the Fe in the final neutralization solution 2+ To control the concentration, it is necessary to adjust the ORP of the leachate, but the carbon content in the ore varies greatly depending on the mining site conditions. Therefore, when treating nickel oxide ore with a low carbon content, the Fe content of the final neutralization solution is 2+ As a result, the zinc concentration in the final reaction liquid (mother liquor for nickel recovery) obtained after the dezincing process increased, resulting in the problem of MS being produced with a zinc content exceeding the standard value.

[0009] For example, Patent Document 1 describes a method for controlling the carbon content of the ore and the oxygen concentration of the autoclave in the leaching process, which is an upstream process, to reduce the Fe content in the leaching solution obtained. 2+ However, there is no disclosure or suggestion as to how to suppress the increase in ORP during the processing of low carbon grade ores.

[0010] Furthermore, Patent Document 2 discloses that, in order to redissolve zinc in the dezincification step, the pH of the final neutralization solution is adjusted to 3.1 to 3.2 in the neutralization step, which is the preceding step. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2014-205901 A [Patent Document 2] JP 2010-37626 A Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention has been made in view of the above circumstances, and has an object to provide a method for obtaining high-quality nickel-cobalt mixed sulfides with reduced zinc content by preventing redissolution of zinc in the dezincing step in a hydrometallurgical method for nickel oxide ore. [Means for solving the problem]

[0013] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, it has been discovered that by blending nickel-cobalt mixed sulfide (MS) with nickel oxide ore to be leached and preparing an ore slurry with specific carbon and sulfur content, the Fe content in the leachate obtained by leaching the ore slurry can be reduced. 2+ It was found that the decrease in the zinc concentration can be suppressed. As a result, it was found that the re-dissolution of zinc in the treatment in the dezincing step can be prevented, and high-quality nickel sulfide with a reduced zinc content can be obtained, which led to the completion of the present invention.

[0014] (1) A first aspect of the present invention is a hydrometallurgical method for producing nickel oxide ore by leaching a raw material nickel oxide ore to produce a leachate containing nickel, the method comprising: a preparation step of preparing an ore slurry from the nickel oxide ore; a leaching step of charging the ore slurry into a reaction vessel, adding sulfuric acid thereto, and subjecting the ore slurry to a leaching treatment under high temperature and high pressure to obtain a leachate containing nickel and cobalt; a dezincification step of sulfurizing and removing zinc contained in the leachate; and a nickel recovery step of adding a sulfurizing agent to a reaction end liquid obtained through the treatment in the dezincification step to obtain a mixed sulfide of nickel and cobalt, wherein in the preparation step, the mixed sulfide of nickel and cobalt is blended with the nickel oxide ore to prepare the ore slurry so that the sum of the carbon content and the sulfur content in the ore slurry is 0.28% by mass or more and 0.63% by mass or less.

[0015] (2) A second aspect of the present invention is a method for hydrometallurgy of nickel oxide ore according to the first aspect of the present invention, wherein the leachate obtained by the leaching treatment and subjected to the dezincification step has a divalent iron concentration of 1.0 g / L or more.

[0016] (3) A third aspect of the present invention is the method for hydrometallurgy of nickel oxide ore according to the first or second aspect of the present invention, wherein the carbon content of the nickel oxide ore as a raw material ore is 0.05% by mass or more and 0.20% by mass or less.

[0017] (4) A fourth aspect of the present invention is a method for hydrometallurgy of nickel oxide ore according to any one of the first to third aspects of the present invention, wherein the leaching step is performed while controlling the oxidation-reduction potential (based on a silver / silver chloride electrode) to 350 mV or more and 520 mV or less.

[0018] (5) The fifth aspect of the present invention is the method according to any one of the first to fourth aspects of the present invention, wherein in the leaching step, high-pressure air is supplied as an oxidizing agent, and the supply amount of the high-pressure air is set to 100 to 1000 [Nm3] per ton of the total amount of carbon and sulfur contained in the ore slurry. 3 -Air / t] is a hydrometallurgical method for the refining of nickel oxide ore.

[0019] (6) A sixth aspect of the present invention is a method for hydrometallurgy of nickel oxide ore according to any one of the first to fifth aspects of the present invention, wherein a part of the mixed sulfide of nickel and cobalt obtained in the nickel recovery step is repeatedly used as the mixed sulfide of nickel and cobalt to be added to the nickel oxide ore in the preparation step. Effect of the Invention

[0020] According to the present invention, it is possible to prevent redissolution of zinc in the treatment in the dezincing step, and obtain a high-quality nickel-cobalt mixed sulfide with a reduced zinc content. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a process diagram showing an example of the flow of a hydrometallurgical method for producing nickel oxide ore. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Specific embodiments of the present invention will be described in detail below. The present invention is not limited to the following embodiments, and various modifications are possible without departing from the gist of the present invention. In this specification, the expression "X to Y" (X and Y are arbitrary numbers) means "X or more and Y or less."

[0023] ≪1. Overview of the hydrometallurgical process for nickel oxide ore≫ The hydrometallurgical method for producing nickel oxide ore according to the present embodiment (hereinafter also simply referred to as the "hydrometallurgical method") is a smelting method for producing nickel and cobalt mixed sulfide (MS) from a leachate obtained by subjecting nickel oxide ore, which is a raw material ore, to a leaching treatment.

[0024] Specifically, this hydrometallurgical method includes a preparation step of preparing an ore slurry from nickel oxide ore, a leaching step of adding sulfuric acid to the ore slurry and performing a leaching treatment under high temperature and high pressure to obtain a leachate containing nickel and cobalt, a dezincification step of sulfurizing and removing zinc contained in the leachate, and a nickel recovery step of adding a sulfiding agent to the reaction end liquid (nickel recovery mother liquor) obtained through the treatment in the dezincification step to obtain a mixed sulfide of nickel and cobalt. In addition, a neutralization step can be provided in which the leachate is subjected to a neutralization treatment to remove impurities.

[0025] Here, the amount of divalent iron (Fe) in the leachate obtained through the leaching process (the final neutralized solution after the neutralization of the leachate) is 2+ It is known that when the zinc concentration is low, the zinc concentration in the final reaction solution obtained through the dezincification process increases. This is because fixation of zinc by sulfurization is inhibited, and zinc redissolves in the dezincification residue. If the zinc concentration in the final reaction solution, which is the mother liquor for nickel recovery, increases, the zinc grade in the resulting nickel and cobalt mixed sulfide increases, causing poor quality.

[0026] Therefore, in order to suppress the increase in zinc concentration in the mother liquor for nickel recovery obtained through the dezincification process, it is necessary to reduce the Fe concentration in the leachate used for the dezincification treatment. 2+ As mentioned above, the concentration of Fe in the leachate must be controlled. 2+ The concentration of Fe depends greatly on the redox atmosphere in the leaching process. 2+ To control the concentration, it is necessary to adjust the oxidation-reduction potential (ORP) of the leachate.

[0027] As a result of extensive research by the present inventors, it was found that in the leaching process, the oxidation-reduction potential (based on a silver / silver chloride electrode) of the leachate changes significantly depending on the composition, carbon content, sulfur content, etc. of the ore slurry to be treated, as shown in the test results in Table 1 below. When the oxidation-reduction potential of the leachate increases, there is no deterioration in the corrosion resistance of the corrosion-resistant materials used in pressurized reaction vessels such as autoclaves and mixers, and the fixation of iron to hematite is also promoted. However, when the ORP reaches approximately 530 mV or more, the Fe in the leachate2+ The concentration drops to less than 1.0 g / L, and redissolution of zinc occurs during the dezincification process.

[0028] The test results shown in Table 1 were carried out by adding nickel and cobalt mixed sulfide (MS: Mix Sulfide) to 350 g of nickel oxide ore to prepare an ore slurry with the carbon and sulfur grades shown in Table 1 below, charging the ore slurry into an autoclave, and adding sulfuric acid at a ratio of 250 g per 100 g of ore. The operating temperature of the autoclave was set to 250°C, the residence time to 200 minutes, and the operating pressure to 4.0 MPa.

[0029] The "zinc removal rate" in Table 1 is expressed as a percentage of "(1-B)÷A," where "A" is the zinc concentration in the final reaction liquid after separation into the dezincification residue and the final reaction liquid (mother liquor for nickel recovery) in the dezincification process, and "B" is the zinc concentration in the starting liquid in the nickel recovery process. For example, a negative value for the zinc removal rate indicates that zinc sulfide has been redissolved.

[0030] [Table 1]

[0031] Therefore, in the hydrometallurgical smelting method according to the present embodiment, nickel and cobalt mixed sulfide (MS) is added to and mixed with nickel oxide ore in the preparation step of preparing an ore slurry, thereby preparing an ore slurry in which the carbon content and sulfur content of the solid content are within specific ranges.

[0032] More specifically, the total content of carbon and sulfur in the ore slurry is set to 0.28% by mass or more and 0.63% by mass or less, and preferably, the total content is set to 0.30% by mass or more and 0.50% by mass or less.

[0033] The carbon content in the ore slurry can be adjusted by the carbon component contained in the raw nickel oxide ore. The carbon content may be adjusted by adding a carbon component such as a carbonaceous reducing agent as necessary. The sulfur content in the ore slurry can be adjusted by the sulfur component added to the nickel and cobalt mixed sulfide.

[0034] The nickel and cobalt mixed sulfide added in adjusting the composition of the ore slurry, particularly in adjusting the sulfur grade, can be a sulfide recovered through a nickel recovery step in the hydrometallurgical process of the nickel oxide ore. The nickel and cobalt mixed sulfide is suitable for adjusting the sulfur grade because it is a sulfide, and is also a compound containing nickel and cobalt, so it does not become an impurity component even if it enters the process, and can also increase the recovery rate of nickel and cobalt.

[0035] In addition, by repeatedly using a portion of the nickel and cobalt mixed sulfide recovered through the nickel recovery step of the hydrometallurgical process, not only can the sulfur grade of the ore slurry be appropriately adjusted, but also economically efficient operation can be realized. The nickel and cobalt mixed sulfide to be reused can be effectively used as long as it is obtained through a hydrometallurgical process, and may be, for example, a so-called off-standard product that does not meet a predetermined standard, or may be scale made of sulfides attached to the wall surface of the sulfurization reaction tank.

[0036] In this way, by mixing nickel and cobalt mixed sulfide (MS) with the raw nickel oxide ore to prepare an ore slurry with a carbon content and sulfur content of 0.28% by mass or more and 0.63% by mass or less, and then subjecting the ore slurry to a leaching treatment, the ORP (based on a silver / silver chloride electrode) of the leachate can be controlled to a range of 350 mV or more and 520 mV or less.

[0037] By controlling the ORP of the leachate to a range of 350 mV to 520 mV, the Fe in the leachate can be reduced. 2+The concentration can be appropriately controlled to 1.0 g / L or more. This makes it possible to suppress re-dissolution of zinc sulfide in the final reaction solution obtained through dezincification treatment using the leachate, and to obtain a high-quality mixed sulfide of nickel and cobalt with a reduced zinc content.

[0038] The ORP of the leaching solution is preferably 380 mV or more, and more preferably 400 mV or more. In particular, an ORP of 400 mV or more can prevent deterioration of the corrosion-resistant material of the autoclave used in the leaching treatment, and can promote fixation of iron as hematite, thereby suppressing an increase in the impurity content.

[0039] This hydrometallurgical method is particularly suitable for nickel oxide ore, which is a raw material, having a low carbon content. The carbon content of nickel oxide ore varies greatly depending on, for example, the conditions of the mining site. Therefore, when treating nickel oxide ore with a low carbon content, the Fe content of the leachate is preferably 0.01 to 0.01. 2+ In this regard, according to the hydrometallurgical refining method of the present embodiment, even when a nickel oxide ore with a low carbon grade is used as the raw material ore, the ore slurry is prepared so that the total of the carbon grade and the sulfur grade falls within a specific range, so that the oxidation-reduction atmosphere in the leaching treatment can be appropriately controlled, and high-quality nickel sulfide with a reduced zinc grade can be satisfactorily obtained.

[0040] ≪2. Each step of the hydrometallurgical process≫ Each step of the hydrometallurgical method according to the present embodiment will be described in detail below more specifically. Fig. 1 is a process diagram showing an example of the flow of the hydrometallurgical method for nickel oxide ore.

[0041] As shown in FIG. 1, the hydrometallurgical smelting method of nickel oxide ore according to the present embodiment includes a preparation step S1 of preparing an ore slurry, a leaching step S2 of adding sulfuric acid to the ore slurry to perform a leaching treatment, a neutralization step S3 of performing a neutralization treatment on the leachate to remove impurities, a liquid purification step (solid-liquid separation step) S4 of performing solid-liquid separation from the neutralized slurry into a neutralization end liquid and a residue, a dezincification step S5 of sulfurizing and removing zinc contained in the neutralization end liquid, and a nickel recovery step S6 of sulfurizing nickel and cobalt contained in a nickel recovery mother liquor (dezincification end liquid) obtained after dezincification to obtain a nickel and cobalt mixed sulfide (MS).

[0042] (1) Ore slurry preparation process [Overview of the processing steps] The preparation step S1 is a pretreatment step for the leaching step S2 in which leaching is performed, and is a step of slurrying the raw material ore, nickel oxide ore, to prepare an ore slurry to be used for the leaching treatment. Specifically, in the preparation step S1, the nickel oxide ore is crushed to a predetermined size, classified at a predetermined classification point to remove oversized ore particles, and then only the undersized ore is used and mixed with water to obtain a slurry.

[0043] The nickel oxide ore, which is the raw material powder, is mainly so-called laterite ore such as limonite ore and saprolite ore. The nickel content of the laterite ore is usually 0.8% by weight to 2.5% by weight, and is contained as hydroxide or magnesium silicate mineral. The iron content is 10% by weight to 50% by weight, and is mainly in the form of trivalent hydroxide (goethite), but some divalent iron is contained in the magnesium silicate mineral.

[0044] In particular, in the hydrometallurgical method according to the present embodiment, nickel oxide ore having a so-called low carbon content, which contains only a small amount of organic components with a carbon content of 0.05 mass % or more and 0.20 mass % or less, can be used as a raw material, as described in detail below. The carbon content of nickel oxide ore can be measured, for example, by an infrared absorption method using a known carbon / sulfur analyzer, in which high-frequency combustion is performed in an oxygen stream.

[0045] As the nickel oxide ore, one type may be used, or multiple types having different nickel grades depending on the place of origin, etc. may be mixed and used. When multiple types of nickel oxide ores are used, they are mixed so as to have a predetermined nickel grade and impurity grade.

[0046] The slurry concentration (solid content concentration) of the ore slurry prepared in the preparation step S1 is not particularly limited, but is generally prepared to be about 25% by mass to 45% by mass. If the slurry concentration is less than 25% by mass, a large facility is required to obtain the same residence time during the leaching treatment in the next leaching step S2, and the amount of acid added also increases. In addition, the nickel concentration of the leachate may also be reduced. If the slurry concentration exceeds 45% by mass, the scale of the facility can be reduced, but the viscosity (yield stress) of the slurry itself increases, causing problems such as difficulty in transportation (frequent clogging of the pipes, energy required, etc.).

[0047] [Addition of nickel and cobalt mixed sulfides] In the hydrometallurgical method according to the present embodiment, in the preparation step S1, nickel and cobalt mixed sulfide is added to and mixed with nickel oxide ore to prepare an ore slurry such that the carbon grade and sulfur grade of the solid content in the obtained ore slurry are within specific ranges. Specifically, the ore slurry is prepared such that the total carbon grade and sulfur grade of the solid content is within a range of 0.28 mass% or more and 0.63 mass% or less.

[0048] By carrying out such a preparation process, it is possible to appropriately control the treatment atmosphere while suppressing an increase in the redox potential in the leaching process in the next leaching step S2, and the Fe content in the leachate obtained from the leaching process can be reduced. 2+ This makes it possible to suppress the re-dissolution of zinc in the treatment in the dezincing step S5, thereby making it possible to obtain a high-quality mixed sulfide of nickel and cobalt with a reduced zinc content.

[0049] In addition, the carbon content of nickel oxide ore varies greatly depending on the conditions of the mining site. For example, when processing nickel oxide ore with a low carbon content, the Fe content in the leachate is high. 2+ In this regard, by carrying out the preparation process in the preparation step S1, even when a nickel oxide ore with a low carbon content (for example, a carbon content of 0.05 mass% or more and 0.20 mass% or less) is used as the raw material ore, the increase in the redox potential during the leaching process is suppressed, and the Fe concentration in the resulting leachate is reduced. 2+ The decrease in concentration can be suppressed.

[0050] The mixed sulfide of nickel and cobalt to be blended is not particularly limited, but a part of the mixed sulfide obtained through the hydrometallurgical process of the nickel oxide ore (mixed sulfide recovered from the nickel recovery process) can be repeatedly used. In this way, by reusing a part of the mixed sulfide of nickel and cobalt recovered through the hydrometallurgical process, economically efficient operation can be performed. In addition, the mixed sulfide to be reused may be, for example, a so-called off-standard product that does not meet a predetermined standard, or may be scale made of sulfides attached to the wall surface of the sulfurization reaction tank.

[0051] In addition to blending the nickel and cobalt mixed sulfide, a carbonaceous reducing agent may be added separately to adjust the carbon content. Examples of the carbonaceous reducing agent include coal, coke, charcoal, organic matter (wood chips, straw chips, etc.), alcohol, oils and fats, etc., and coal is particularly preferred because of its ease of availability and handling.

[0052] Regarding the carbon content and sulfur content in the prepared ore slurry, the oxidation-reduction potential (ORP: silver / silver chloride electrode standard) can be controlled within an appropriate range during the leaching treatment by adjusting the total carbon content and sulfur content to within a range of 0.28% by mass or more and 0.63% by mass or less. If the carbon content falls below 0.28% by mass, the ORP during the leaching treatment increases, and the Fe content in the resulting leachate increases. 2+ The concentration of carbon and sulfur in the leaching process will decrease, causing re-dissolution of zinc in the subsequent dezincing process S5. If the total of the carbon and sulfur content exceeds 0.63 mass%, the ORP will decrease, causing deterioration of the oxide film (corrosion-resistant material) of the Ti lining of the autoclave used in the leaching process, which may cause damage to the equipment. In addition, the fixation of iron as hematite in the leaching process will not progress, and the impurity content may increase.

[0053] Furthermore, it is more preferable to compound the nickel and cobalt mixed sulfide so that the total content of carbon and sulfur falls within the range of 0.30 mass % or more and 0.50 mass % or less.

[0054] The amount of the nickel and cobalt mixed sulfide to be added is preferably determined according to the analysis value of the carbon grade and sulfur grade of the solid content in the ore slurry in advance. For example, when the total of the carbon grade and sulfur grade (mainly carbon grade because it is ore before preparation) in the prepared ore slurry is 0.15 mass%, the appropriate amount of the nickel and cobalt mixed sulfide to be added can be calculated by multiplying the ore slurry weight (dry-t) to be supplied to the autoclave by the difference between the control value of the carbon grade and sulfur grade of 0.28 mass% and the analysis value of 0.15 mass%.

[0055] [Regarding sieving during the preparation process] In the preparation step S1, the ore slurry to be subjected to the leaching treatment is prepared as described above. From the viewpoint of increasing the efficiency of the leaching treatment, it is preferable that the nickel oxide ore constituting the ore slurry has a particle size equal to or smaller than a predetermined particle size. Therefore, in the preparation step S1, the nickel oxide ore as the raw material ore is crushed, and only the ore particles that are undersized at a predetermined classification point are classified by a classification device (sieve) and used. "Undersized" refers to ore particles that have a size smaller than the sieve opening of the classification device and are undersized particles that have passed through the sieve. "Oversized" refers to ore particles that have a size larger than the sieve opening of the classification device and are oversized particles that have not passed through the sieve and remain on the sieve.

[0056] In the classification process, the crushed nickel oxide ore is first loaded into a first sieve and sieved, for example, with a sieve opening of 150 mm, to recover undersized ore particles with a particle size of 150 mm or less. The recovered undersized ore particles are then loaded into a drum washer or the like, mixed with water supplied into the drum, and subjected to a wet crushing process.

[0057] Specifically, a drum washer is a wet grinding device that mixes nickel oxide ore, which is a raw ore, with water and grinds the ore particles. In a drum washer, nickel oxide ore (undersized ore particles that have passed through a sieve) is fed from a processing target inlet, and a predetermined amount of water is supplied from a water supply inlet. In the drum washer, the nickel oxide ore and the supply water are mixed and stirred in the drum as the drum rotates, thereby grinding the nickel oxide ore. This mixing and stirring also simultaneously breaks down lumps (agglomerates) formed by the aggregation and solidification of multiple ore particles. The degree of grinding can be adjusted by the rotation speed of the drum.

[0058] The nickel oxide ore thus crushed by the drum washer is then charged into a second sieve and sieved, for example, through a sieve opening of 25 mm, to recover undersized ore particles having a particle size of 25 mm or less.

[0059] Next, the undersized ore particles recovered from the second sieve are subsequently loaded into a third sieve, where they are sieved, for example, with a sieve opening of 1.4 mm, and undersized ore particles with a particle size of 1.4 mm or less are recovered. The undersized ore particles (1.4 mm or less) thus recovered are used as the ore that constitutes the ore slurry. In other words, the undersized ore particles are mixed with, for example, industrial water to form a slurry, which is then loaded into an autoclave to be used for the treatment in the next leaching step S2.

[0060] In addition, the opening of the third sieve, that is, the opening of the sieve for sieving and recovering the ore particles constituting the prepared ore slurry, is exemplified as 1.4 mm in the above description, but is not limited thereto. The opening of the third sieve is preferably about 0.5 mm to 2.0 mm, more preferably 0.8 mm to 1.6 mm, and particularly preferably about 1.4 mm. If the opening of the sieve is less than 0.5 mm, it takes time and cost to crush the particles using a drum washer or the like. In addition, if the opening of the sieve exceeds 2.0 mm, the reaction rate in the autoclave used for the treatment in the leaching step S2 becomes slow, which is not preferable. In addition, it is particularly preferable and effective to use a vibrating sieve as the sieve.

[0061] [Timing of adding nickel and cobalt mixed sulfides] In the preparation step S1, as described above, nickel and cobalt mixed sulfide (hereinafter also simply referred to as "mixed sulfide") is added to the nickel oxide ore, which is the raw ore, and mixed so that the total carbon content and sulfur content of the solid content in the prepared ore slurry is in the range of 0.28 mass% to 0.63 mass%. At this time, the nickel and cobalt mixed sulfide is not particularly limited, but can be directly charged together with the nickel oxide ore into the first sieve used in the above-mentioned sieving process, for example. Then, the undersize material (undersize) obtained from the first sieve, that is, the undersize material containing nickel and cobalt mixed sulfide, is subsequently charged into a drum washer, and the nickel oxide ore particles and the mixed sulfide are brought into contact with each other in the drum washer to finely crush the mixed sulfide.

[0062] In this way, when the nickel and cobalt mixed sulfide is added to the nickel oxide ore and mixed, for example, it is put into a first sieve used in the sieving process, and then it is crushed by contact with the nickel oxide ore, so that the particle size can be made almost uniform. This makes it possible to effectively increase the reduction reaction rate in the treatment in the leaching step S2. In addition, it is possible to eliminate the need to separately crush the nickel and cobalt mixed sulfide to be added, and it becomes possible to perform efficient treatment.

[0063] The mixed powder of nickel oxide ore and mixed sulfide obtained from the drum washer is then fed successively into a second sieve and a third sieve, and ore particles (undersize) smaller than the sieve opening are collected to prepare an ore slurry. In this way, when preparing the ore slurry, the mixed powder of nickel oxide ore and mixed sulfide, which has a substantially uniform particle size and is uniformly mixed, can be used as the raw material for the ore slurry.

[0064] (2) Leaching process The leaching step S2 is a step in which a reaction vessel such as an autoclave is used to add sulfuric acid to the prepared ore slurry and perform leaching treatment under high temperature and pressure to obtain a leaching slurry consisting of a leachate containing nickel and a leach residue containing hematite (Fe2O3).

[0065] Specifically, in the leaching treatment in the leaching step S2, leaching reactions represented by the following formulas (i) to (iii) and high-temperature hydrolysis reactions represented by the following formulas (iv) and (v) occur, resulting in leaching of nickel, cobalt, and the like as sulfates and fixation of the leached iron sulfate as hematite.

[0066] "Leaching reaction" MO+H2SO4⇒MSO4+H2O (i) (In the formula, M represents Ni, Co, Fe, Zn, Cu, Mg, Cr, Mn, etc.) 2FeOOH+3H2SO4⇒Fe2(SO4)3+4H2O ···(ii) FeO+H2SO4⇒FeSO4+H2O ···(iii) "High-temperature hydrolysis reaction" 2FeSO4+H2SO4+1 / 2O2⇒Fe2(SO4)3+H2O ···(iv) Fe2(SO4)3+3H2O⇒Fe2O3+3H2SO4...(v)

[0067] Here, in the leaching treatment in the leaching step S2, high-pressure air is supplied as an oxidizing agent to control the oxidation-reduction potential (ORP: silver / silver chloride electrode standard) in the leaching treatment within a predetermined range. Specifically, the leaching treatment is performed by controlling the ORP within a range of 350 mV to 520 mV by supplying high-pressure air to the ore slurry. In particular, by supplying only high-pressure air as an oxidizing agent and not supplying other oxidizing agents, the ORP can be controlled more appropriately.

[0068] If the ORP is less than 350 mV, the oxide film on the metal lining of the equipment will decrease, which may cause damage to the equipment. In addition, the high-temperature hydrolysis reaction of iron will be suppressed, leaving a large amount of iron in the leaching solution, which will increase the amount of chemicals used in the next neutralization step S3 and the amount of co-precipitation of nickel and cobalt, resulting in a decrease in the leaching rate of nickel and cobalt. In addition, if the ORP exceeds 520 mV, the Fe content in the neutralization final solution obtained through the neutralization step S3 in the subsequent dezincification step S5 will be reduced. 2+ The zinc concentration in the nickel recovery mother liquor containing nickel and cobalt after separation decreases, and the zinc concentration increases.

[0069] As described above, in the hydrometallurgical smelting method according to the present embodiment, in the preparation step S1 for preparing an ore slurry, nickel and cobalt mixed sulfides are blended with nickel oxide ore as a raw ore to prepare the ore slurry so that the total carbon and sulfur content of the solid content in the ore slurry is 0.28 mass% or more and 0.63 mass% or less. By controlling the carbon and sulfur content of the ore slurry to be leached in this manner, it becomes possible to appropriately control the ORP of the leachate within the above range by supplying only high-pressure air as an oxidizing agent.

[0070] In addition, by controlling the carbon content and sulfur content of the ore slurry and controlling the ORP of the leachate within the above range, the Fe content in the leachate (in the final neutralization solution after neutralization treatment) used for the dezincification step S5 can be reduced. 2+ The decrease in the zinc concentration can be effectively suppressed, and the increase in the zinc concentration in the mother liquor for nickel recovery obtained through the dezincing step S5 can be prevented.

[0071] Specifically, by controlling the carbon content of the ore slurry and controlling the oxidation-reduction potential within the above range, the Fe content in the leachate (in the final neutralization solution after neutralization) used in the dezincification step S5 can be reduced. 2+ The concentration can be controlled to 1.0 g / L or more, preferably 1.1 g / L or more. 2+The upper limit of the concentration is not particularly limited, but is preferably 20 g / L or less, more preferably 10 g / L or less, and particularly preferably 3.5 g / L or less.

[0072] The amount of compressed air supplied as an oxidizing agent is not particularly limited, but is preferably 100 to 1000 [Nm3] per ton of the total amount of carbon and sulfur contained in the ore slurry. 3 -Air / t]. If the supply amount of high-pressure air is out of this range, it may be difficult to control the ORP in the leaching treatment to the desired range described above. In the leaching treatment, it is preferable to appropriately adjust the supply amount of high-pressure air while monitoring the ORP of the leaching solution so that the ORP is controlled to a range of 350 mV to 520 mV.

[0073] The temperature condition in the leaching treatment is not particularly limited, but is preferably about 220°C to 280°C, and more preferably about 240°C to 270°C. By carrying out the reaction in such a temperature range, iron can be more efficiently fixed as hematite. If the temperature is less than 220°C, the rate of the high-temperature hydrolysis reaction slows down, and iron remains dissolved in the leaching solution, and the processing load in the next neutralization step S3 to remove the iron increases, making it difficult to separate it from nickel. In addition, if the temperature exceeds 280°C, although the high-temperature hydrolysis reaction itself is accelerated, it becomes difficult to select the material of the container (autoclave, etc.) used for high-temperature, high-pressure leaching, and the cost of high-pressure steam required for increasing the temperature increases.

[0074] The temperature in the leaching treatment can be controlled, for example, by supplying high-pressure steam into the reaction vessel. The pressure condition in the reaction vessel is preferably, for example, pressurized to about 3 MPaG to 6 MPaG. The pressure in the reaction vessel can be controlled by supplying the above-mentioned high-pressure steam together with high-pressure air. In the leaching treatment performed under such temperature and pressure conditions, a pressurized reaction vessel such as an autoclave is preferably used as the reaction vessel.

[0075] The amount of sulfuric acid added in the leaching process is not particularly limited, but is preferably about 200 to 250 [kg-H2SO4 / t-dry (solid)] per ton of dry ore. If the amount of sulfuric acid added per ton of dry ore is too large, the cost of using sulfuric acid will increase, and the amount of neutralizing agent used in the subsequent neutralization step S3 may increase.

[0076] The pH of the resulting leachate is preferably in the range of 0.1 to 1.0 from the viewpoint of filterability for separating the leach residue containing the generated hematite.

[0077] (3) Neutralization process The neutralization step S3 is a step of neutralizing the leachate obtained through the leaching step S2. Specifically, a neutralizing agent is added to the leachate to adjust the pH, and a neutralized slurry consisting of a neutralized precipitate containing impurity elements and a neutralization end solution is obtained. By such neutralization treatment, metals such as nickel and cobalt are contained in the neutralization end solution, and most of the impurities including aluminum become neutralized precipitates.

[0078] As the neutralizing agent used in the neutralization treatment, a known neutralizing agent can be used. For example, limestone, slaked lime, sodium hydroxide, etc. can be mentioned. In addition, in the neutralization treatment, it is preferable to adjust the pH to a range of 1 to 4 while suppressing the oxidation of the separated leachate, and it is more preferable to adjust the pH to a range of 1.5 to 2.5. If the pH is less than 1, the neutralization is insufficient, and it is possible that the neutralization end solution and the neutralized precipitate cannot be effectively separated. In addition, if the pH exceeds 4, not only impurities such as aluminum but also valuable metals such as nickel may be coprecipitated and included in the neutralized precipitate.

[0079] (4) Liquid purification process (solid-liquid separation process) The liquid purification step S4 is a step of washing the neutralized slurry obtained through the neutralization step S3 and separating the neutralized slurry into a neutralization end liquid and a neutralized sediment.

[0080] In the liquid purification step S4, the neutralized slurry is mixed with a washing liquid, and then a solid-liquid separation process is performed using a solid-liquid separation device such as a thickener. Specifically, the neutralized slurry is first diluted with the washing liquid, and then the neutralized precipitate in the neutralized slurry is concentrated as a sediment in the thickener. This allows the nickel content attached to the neutralized precipitate to be reduced according to the degree of dilution.

[0081] In addition, in the liquid purification process in the liquid purification step S4, it is preferable to use thickeners having the above-mentioned functions connected in multiple stages to perform multi-stage washing. Also, as the washing liquid, the sulfidation end liquid (barren liquid) obtained from the nickel recovery step S6 in the hydrometallurgical process may be circulated and used.

[0082] (5) Dezincification process The dezincification step S5 is a step in which a sulfiding agent is added to the leachate obtained through the leaching treatment in the above-mentioned leaching step S2, and the zinc contained in the leachate is separated and removed as a sulfide. Note that the leachate to be treated also means the neutralization end liquid obtained through the neutralization treatment in the neutralization step 3.

[0083] The leachate (neutralized final liquid obtained through the neutralization step S3) contains nickel and cobalt, which are the targets of recovery in the hydrometallurgical process, as well as zinc as an impurity. In the dezincification step S5, prior to recovering nickel from the leachate, a sulfide of zinc is generated by causing a sulfurization reaction under specified conditions, and this is separated and removed to obtain a mother liquor for nickel recovery, which contains nickel.

[0084] Specifically, in the dezincing step S5, for example, a leachate is supplied into a pressurized reaction vessel (sulfurization reaction tank), and a sulfurizing agent such as hydrogen sulfide gas, sodium sulfide, or sodium hydrosulfide is added to the leachate to selectively sulfurize zinc with respect to nickel, thereby generating a dezincing slurry consisting of zinc sulfide and a dezincing end liquid (nickel recovery mother liquid).Then, the obtained dezincing slurry is subjected to solid-liquid separation to obtain a nickel recovery mother liquid from which zinc has been separated.

[0085] In the next nickel recovery step S6, a sulfurizing agent such as hydrogen sulfide gas is added to cause a sulfurization reaction to generate sulfides containing nickel, but in the dezincification step S5, which is carried out prior to the sulfurization treatment of nickel, etc., the sulfurization reaction conditions are milder than the sulfurization reaction conditions for nickel, allowing the zinc contained in the leachate to be selectively sulfurized.

[0086] In the hydrometallurgical method according to the present embodiment, the total carbon content and sulfur content of the ore slurry to be subjected to the leaching treatment is adjusted to a specific range. According to this method, the ORP of the leachate can be appropriately controlled in the leaching treatment in the leaching step S2, and the Fe content in the leachate can be appropriately controlled. 2+ The decrease in the concentration of Fe is effectively suppressed. 2+ The concentration can be 1.0 g / L or more.

[0087] Therefore, by subjecting such a leachate to a dezincing treatment in the dezincing step S5, it is possible to effectively prevent the re-dissolution of the sulfidized zinc and reduce the amount of zinc contained in the mother liquor for nickel recovery.

[0088] (6) Nickel recovery process The nickel recovery step S6 is a step of adding a sulfurizing agent to the nickel recovery mother liquor from which zinc has been removed through the treatment in the dezincing step S5 to obtain a nickel sulfide and a sulfurization end liquid.

[0089] Specifically, in the nickel recovery step S6, a sulfiding agent such as hydrogen sulfide gas, sodium sulfide, or sodium hydrosulfide is added to the mother liquor for nickel recovery to generate nickel sulfide with few impurity components and a sulfidation end liquid in which the concentration of nickel, etc. is stabilized at a low level. The resulting slurry containing nickel sulfide is subjected to solid-liquid separation treatment using a sedimentation device such as a thickener, and the nickel sulfide is separated and recovered from the bottom of the thickener, while the sulfidation end liquid, which is an aqueous solution component, is allowed to overflow and recovered.

[0090] As described above, the mother liquor for nickel recovery that is subjected to the sulfurization treatment in the nickel recovery step S6 is a solution that contains almost no zinc. Therefore, by carrying out the sulfurization treatment using such a mother liquor for nickel recovery, it is possible to obtain high-quality nickel sulfide in which the zinc content is effectively reduced. EXAMPLES

[0091] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0092] [Examples and Comparative Examples] A test was conducted in which nickel and cobalt mixed sulfide (MS: Mix Sulfide) was added to nickel oxide ore (raw ore) with a low carbon content to prepare an ore slurry, which was then subjected to leaching treatment, and the oxidation-reduction potential (ORP: silver / silver chloride electrode standard) value of the leachate was measured.

[0093] Specifically, first, 5 g (Example 1) and 1 g (Comparative Example 1) of MS were added to approximately 350 g of nickel oxide ore to prepare two ore slurries, which were then charged into a 3-liter stainless steel autoclave reaction vessel. Table 2 shows the composition of the ore slurries in each test example. Table 3 shows the composition of the nickel oxide ore and the composition of MS used. In Comparative Example 2, no MS was added to the nickel oxide ore, which was the raw material ore.

[0094] [Table 2]

[0095] [Table 3]

[0096] The test conditions for the leaching treatment were set as follows: autoclave operating temperature: 250°C, residence time: 200 minutes, and autoclave operating pressure: 4.0 MPa. Sulfuric acid was added to the ore slurry at a ratio of 250 g per 100 g of ore to perform the leaching treatment.

[0097] [result] Table 4 below shows the ORP value of the leachate and the Fe content of the leachate as a result of the leaching treatment. 2+ The measured values ​​of the concentrations are shown in Table 4. Table 4 also shows the carbon grade, sulfur grade, and the sum of the carbon grade and sulfur grade (total grade) of the ore slurry subjected to the leaching treatment.

[0098] [Table 4]

[0099] Based on the results shown in Table 4 and the results shown in Table 1 described above, nickel and cobalt mixed sulfide (MS) was added to the raw ore to prepare an ore slurry with a specific range of total carbon and sulfur content. This slurry was then subjected to leaching treatment, which made it possible to appropriately control the ORP during the leaching treatment, and the Fe content in the resulting leachate was reduced. 2+ It was found that the concentration could be increased to 1.0 g / L or more.

[0100] Thus, the Fe in the leachate 2+ Since the decrease in the concentration of zinc sulfide was effectively suppressed, it is predicted that the re-dissolution of zinc sulfide in the final dezincification solution obtained by subjecting the leachate to a dezincification process can be suppressed. Then, a high-quality mixed nickel and cobalt sulfide can be produced through a nickel recovery process.

[0101] On the other hand, in Comparative Example 1, in which MS was added to the nickel oxide ore but the total value of the carbon content and sulfur content was less than 0.28 mass%, the Fe content in the leachate was 0.1%. 2+ The concentration was reduced to 0.5 g / L. In Comparative Example 2, in which MS was not added, the Fe 2+The concentration was 0 g / L. In these comparative examples, referring to the results in Table 1, it is predicted that re-dissolution of zinc sulfide occurs in the final dezincification solution obtained through the dezincification step, and zinc cannot be sufficiently removed.

Claims

1. A method for hydrometallurgy of nickel oxide ore, which produces sulfides containing nickel and cobalt from a leachate obtained by leaching nickel oxide ore as a raw material ore, comprising the steps of: preparing an ore slurry from the nickel oxide ore; a leaching step of charging the ore slurry into a reaction vessel, adding sulfuric acid thereto, and subjecting the ore slurry to a leaching treatment under high temperature and high pressure to obtain a leachate containing nickel and cobalt; a dezincing step of removing zinc contained in the leachate by sulfurization; A nickel recovery step of adding a sulfurizing agent to the reaction end liquid obtained through the treatment in the dezincing step to obtain a mixed sulfide of nickel and cobalt, In the preparation step, a mixed sulfide of nickel and cobalt is added to the nickel oxide ore so that the total carbon content and sulfur content in the ore slurry is 0.28% by mass or more and 0.63% by mass or less; In the leaching step, the leaching treatment is performed while controlling the oxidation-reduction potential (based on a silver / silver chloride electrode) to 350 mV or more and 520 mV or less. The divalent iron concentration in the leachate obtained by the leaching treatment and subjected to the dezincing step is 1.0 g / L or more. A hydrometallurgical process for nickel oxide ores.

2. The carbon content of the nickel oxide ore as the raw material ore is 0.05% by mass or more and 0.20% by mass or less.

2. The method for hydrometallurgy of nickel oxide ore according to claim 1.

3. In the leaching step, compressed air is supplied as an oxidizing agent, and the supply amount of the compressed air is set to 100 to 1000 [Nm3] per ton of the total amount of carbon and sulfur contained in the ore slurry. 3 -Air / t], 3. The method for hydrometallurgy of nickel oxide ore according to claim 1 or 2.

4. A part of the mixed sulfide of nickel and cobalt obtained in the nickel recovery step is repeatedly used as the mixed sulfide of nickel and cobalt to be added to the nickel oxide ore in the preparation step.

4. The method for hydrometallurgy of nickel oxide ore according to claim 1.

Citation Information

Patent Citations

  • Nickel smelting process

    JP2005281733A

  • Wet-smelting method for nickel-oxide ore

    JP2009197298A

  • Zinc sulfide separation method

    JP2010037626A

  • Wet smelting method for nickel oxide ore

    JP2014205901A

  • Wet refining method for nickel oxide ore

    JP2018070918A