Hydrometallurgical process for nickel oxide ore
By integrating the leaching residue slurry into the leachate for neutralization and processing neutralized precipitates in multiple stages of solid-liquid separation, the method effectively reduces nickel recovery loss and precipitate load, improving the efficiency and quality of nickel sulfide production in nickel oxide ore processing.
Patent Information
- Application Number
- JP2021050601
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-03-24
AI Technical Summary
Existing hydrometallurgical methods for nickel oxide ore suffer from high recovery loss and precipitate load in the solid-liquid separation process, particularly due to the inefficiencies in the neutralization and solid-liquid separation steps, which are not effectively addressed by conventional techniques.
The method involves adding the slurry of leaching residue to the leachate for neutralization and repeatedly processing the neutralized precipitate slurry in multiple stages of solid-liquid separation, specifically starting at the first-stage thickener, using a multi-stage thickener system, and adjusting flocculant use based on turbidity and viscosity measurements.
This approach reduces nickel recovery loss and precipitate load, enhancing the efficiency of the solid-liquid separation process and improving the quality of nickel sulfide production by minimizing the amount of liquid in the slurry.
Smart Images

Figure 0007585921000001 
Figure 0007585921000002 
Figure 0007585921000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for hydrometallurgy of nickel oxide ore, and to a method capable of effectively reducing nickel recovery loss. [Background technology]
[0002] Nickel is widely used as a raw material for stainless steel, and as the resource of the nickel sulfide ore used as the raw material tends to become depleted, technology for refining low-grade oxide ore has been developed and put into practical use.
[0003] Specifically, a manufacturing process known as "High Pressure Acid Leach (HPAL)" has been put into practical use, in which nickel oxide ores such as limonite or saprolite are placed in a pressurized device such as an autoclave together with a sulfuric acid solution, and nickel is leached under high temperatures and pressures of around 240°C to 260°C.
[0004] Specifically, in the hydrometallurgical process of nickel oxide ore by the HPAL method, first, several kinds of low-grade nickel oxide ores are mixed to have a predetermined nickel grade and impurity grade, and then mixed with water to form a slurry, which is sieved, and only the ore of a predetermined undersize (undersize) is used (ore slurry preparation step S11). Next, the ore slurry is charged into a pressurized reaction device such as an autoclave, and sulfuric acid is added under high temperature and pressure to leach nickel (leaching step S12). Next, residual free acid contained in the leaching slurry is removed by neutralization treatment (pre-neutralization step S13). The slurry after the pre-neutralization treatment is transferred to a solid-liquid separation device such as a thickener, and separated into a leachate and a leach residue while being washed in multiple stages (solid-liquid separation step S14). The leach residue after solid-liquid separation is transferred to a tailings dam (residue dam) after removing heavy metals to a predetermined concentration in the final neutralization step S17.
[0005] Next, a neutralizing agent is added to the leachate (pregnant liquor) obtained by solid-liquid separation to perform neutralization treatment to remove impurities (neutralization step S15), and a sulfurizing agent such as hydrogen sulfide gas is supplied to the final neutralization liquor, which is the mother liquor for nickel recovery, to generate and recover a mixed sulfide of nickel and cobalt (hereinafter also referred to as "nickel sulfide") (sulfurization step S16). The barren liquor after the nickel sulfide is separated and recovered in the sulfurization step is transferred to the final neutralization step S17 and made harmless. Note that a part of the barren liquor is reused in the treatment in the solid-liquid separation step S14 after the preliminary neutralization step S13.
[0006] Here, for example, in the treatment in the neutralization step S15, a slurry of limestone, slaked lime, or the like is added as a neutralizing agent to the leachate to perform neutralization treatment, thereby generating a precipitate (neutralized precipitate) mainly composed of hydroxides and gypsum as impurity metal elements. The slurry containing the neutralized precipitate is transferred to a solid-liquid separator such as a thickener and subjected to solid-liquid separation. In addition, a part of the neutralized precipitate slurry is repeatedly sent to the solid-liquid separation step S14 and subjected to solid-liquid separation together with the leach slurry in order to reduce the recovery loss of nickel in the precipitate (see, for example, Patent Document 1).
[0007] In the slurry containing such precipitates, nickel is contained in the liquid at a high concentration, which causes deterioration of washing in the solid-liquid separation process, so it is desirable to reduce the amount of liquid in the slurry containing precipitates as much as possible.
[0008] Conventionally, for example, improvements have been made to solid-liquid separation in the neutralization step (see, for example, Patent Documents 2 to 4). However, these conventional techniques are mainly aimed at improving the clarity of the supernatant liquid, and are not very effective in reducing the amount of liquid in the slurry that is repeated in the process. In addition, there is a limit to reducing the amount of liquid in the slurry that is repeated, that is, to increasing the solid concentration of the slurry, so there is a need to develop a method for further reducing nickel loss.
[0009] For example, Patent Document 5 discloses that in order to reduce nickel recovery loss, a part of the neutralized precipitate slurry after the neutralization step is repeatedly sent to the solid-liquid separation step S14. In this case, it is preferable to transfer the neutralized precipitate slurry to a thickener at the latter stage of the multi-stage washing in order to suppress an increase in the precipitate load in the thickener.
[0010] However, this method is not sufficient for reducing nickel recovery loss while reducing the sediment load in the solid-liquid separation process, and there is a need to develop a more effective method for reducing nickel loss. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2005-350766 A [Patent Document 2] JP 2004-225120 A [Patent Document 3] JP 2017-145454 A [Patent Document 4] JP 2017-201056 A [Patent Document 5] JP 2019-049020 A Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention has been made in view of the above circumstances, and has an object to provide a method for hydrometallurgy of nickel oxide ore, which can reduce the load of sediment in the solid-liquid separation step and effectively reduce nickel recovery loss. [Means for solving the problem]
[0013] As a result of extensive research, the inventors have found that the above-mentioned problems can be solved by adding a slurry of the leaching residue separated in the solid-liquid separation step to the leachate to be subjected to neutralization treatment in the neutralization step, and by repeatedly subjecting the slurry of neutralized precipitate produced by the neutralization treatment to the solid-liquid separation step, and by transferring the slurry of neutralized precipitate to the first-stage thickener, which is located at the most upstream of the multiple thickener stages provided in the solid-liquid separation device, when repeating the process, thereby completing the present invention.
[0014] (1) A first aspect of the present invention is a hydrometallurgical method for nickel oxide ore, which comprises adding an acid to nickel oxide ore to perform a leaching treatment, and obtaining nickel and cobalt sulfides from the obtained leachate, the method comprising the steps of: performing a solid-liquid separation treatment on the leach slurry obtained by the leaching treatment while performing multi-stage washing using a solid-liquid separation device having multiple thickeners to obtain a leachate and a leach residue; and adding a neutralizing agent to the leachate to perform a neutralization treatment, thereby obtaining a neutralized precipitate containing impurities and a neutralized final liquid containing nickel and cobalt. and a neutralization step of obtaining a leachate having a pH of 10 or more and a neutralization step of obtaining a leachate having a pH of 10 or more, the neutralization step including a step of adding a slurry of the leachate separated in the solid-liquid separation step to the leachate to be subjected to a neutralization treatment, and a step of repeating the neutralization precipitate slurry produced by the neutralization treatment to the solid-liquid separation step, the neutralization precipitate slurry being transferred to a first-stage thickener located at the most upstream of multiple thickener stages provided in the solid-liquid separation device.
[0015] (2) A second aspect of the present invention is a method for hydrometallurgy of nickel oxide ore, wherein in the solid-liquid separation step, a solid-liquid separator having 4 to 7 thickeners in multiple stages is used.
[0016] (3) A third aspect of the present invention is a method for hydrometallurgy of nickel oxide ore according to the first or second aspect of the present invention, wherein in the solid-liquid separation step, the turbidity and viscosity of the supernatant liquid in the first-stage thickener are periodically measured and monitored, and the amount of flocculant added in the solid-liquid separation treatment is adjusted.
[0017] (4) A fourth aspect of the present invention is a method for hydrometallurgy of nickel oxide ore according to the third aspect of the present invention, wherein in the solid-liquid separation step, the turbidity of the supernatant liquid in the first-stage thickener is adjusted to 200 NTU or less. Effect of the Invention
[0018] According to the present invention, it is possible to provide a method for hydrometallurgy of nickel oxide ore, which can reduce the sediment load in the treatment in the solid-liquid separation step and can effectively reduce nickel recovery loss. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a process diagram showing an example of a flow of a hydrometallurgical process for nickel oxide ore. [Diagram 2] FIG. 1 is a diagram showing an example of the configuration of a solid-liquid separation device in which thickeners are connected in multiple stages to perform a CCD method. [Diagram 3] FIG. 2 is a diagram showing an example of the configuration of a thickener (only one stage) constituting each stage of a solid-liquid separator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] A specific embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail below. Note that the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention. In this specification, when it is expressed as "X to Y" (X and Y are arbitrary numerical values), it means "X or more and Y or less" unless otherwise specified.
[0021] ≪1. Overview≫ The hydrometallurgical method for nickel oxide ore according to the present embodiment is a method for adding an acid to nickel oxide ore to perform a leaching treatment, and obtaining a nickel-containing sulfide from the obtained leachate. Note that in the hydrometallurgical process for nickel oxide ore, a nickel-cobalt mixed sulfide containing nickel and cobalt leached into the leachate is obtained by performing a sulfidation treatment based on the leachate, and the term "nickel-containing sulfide (nickel sulfide)" includes the meaning of the nickel-cobalt mixed sulfide.
[0022] Specifically, this method includes a solid-liquid separation step in which the leaching slurry obtained by the leaching treatment is subjected to a solid-liquid separation treatment while being washed in multiple stages using a solid-liquid separation device provided with multiple thickeners to obtain a leachate and a leachate residue, and a neutralization step in which a neutralizing agent is added to the leachate to perform a neutralization treatment to obtain a neutralized precipitate containing impurities and a neutralized final solution containing nickel and cobalt. In the neutralization step, the slurry of the leachate separated in the solid-liquid separation step is added to the leachate to be subjected to the neutralization treatment, thereby performing the neutralization treatment.
[0023] In addition, in this method, the neutralization step includes a process in which the neutralized precipitate slurry produced by the neutralization treatment is repeatedly subjected to a solid-liquid separation step, and when the neutralized precipitate slurry is repeatedly subjected to the solid-liquid separation step, the slurry is transferred to a first-stage thickener located at the most upstream of the thickeners provided in multiple stages in the solid-liquid separation device.
[0024] According to such a method, it is possible to effectively reduce nickel recovery loss without increasing the sediment load in the solid-liquid separation process.
[0025] ≪2. Nickel Ore Hydrometallurgy Process≫ First, each step of the hydrometallurgical process for nickel oxide ore will be described in detail.
[0026] Fig. 1 is a process diagram showing an example of the flow of a hydrometallurgical process for nickel oxide ore. As shown in Fig. 1, the hydrometallurgical process for nickel oxide ore includes a leaching step S1 in which sulfuric acid is added to a slurry of raw nickel oxide ore and leaching is performed under high temperature and high pressure, a solid-liquid separation step S2 in which a leach residue is separated from the leach slurry to obtain a leachate containing nickel, a neutralization step S3 in which the pH of the leachate is adjusted to separate impurities in the leachate as a neutralization precipitate to obtain a neutralization end solution, and a sulfurization step S4 in which a sulfurizing agent is added to the neutralization end solution to generate nickel sulfides.
[0027] (1) Leaching process In the leaching step S1, a high-temperature pressurized reaction vessel such as an autoclave is used to add sulfuric acid to a slurry of nickel oxide ore (hereinafter also referred to as "ore slurry") and perform leaching treatment by stirring under conditions of, for example, a temperature of about 230°C to 270°C and a pressure of about 3 MPa to 5 MPa. This produces a leaching slurry consisting of a leachate and a leach residue.
[0028] The raw nickel oxide ore mainly includes so-called laterite ores such as limonite ore and saprolite ore. The nickel content of the laterite ore is usually 0.8% by weight to 2.5% by weight, and is contained as hydroxide or magnesium silicate mineral. The iron content is 10% by weight to 50% by weight, and is mainly in the form of trivalent hydroxide, with some divalent iron being contained in the magnesia siliceous mineral. In addition to such laterite ore, the leaching step S1 can also use oxide ores containing valuable metals such as nickel, cobalt, manganese, and copper, such as manganese nodules present on the deep seabed.
[0029] In the leaching process, for example, the leaching reactions represented by the following formulas [1] to [5] and high-temperature hydrolysis reactions occur, resulting in the leaching of nickel, cobalt, and the like as sulfates and the immobilization of the leached iron sulfate as hematite. However, since the immobilization of iron ions does not proceed completely, the liquid portion of the resulting leaching slurry usually contains divalent and trivalent iron ions in addition to nickel, cobalt, and the like. In the leaching process, it is preferable to adjust the pH of the resulting leaching solution to 0.1 to 1.0 from the viewpoint of the filterability of the leaching residue containing hematite separated in the next solid-liquid separation step S2.
[0030] Leaching reaction MO+H2SO4 → MSO4+H2O [1] (In the formula, M represents Ni, Co, Fe, Zn, Cu, Mg, Cr, Mn, etc.) 2Fe(OH)3+3H2SO4→Fe2(SO4)3+6H2O ···[2] FeO+H2SO4 →FeSO4+H2O [3] High-temperature hydrolysis reaction 2FeSO4+H2SO4+1 / 2O2→Fe2(SO4)3+H2O ···[4] Fe2(SO4)3+3H2O→Fe2O3+3H2SO4··[5]
[0031] The amount of sulfuric acid added to the autoclave containing the ore slurry is not particularly limited, but an excess amount is used so that the iron in the ore is leached out, for example, 300 kg to 400 kg per ton of ore.
[0032] (2) Solid-liquid separation process In the solid-liquid separation step S2, the leaching slurry produced in the leaching step S1 is washed in multiple stages while a solid-liquid separation treatment is carried out to separate the leachate containing valuable metals such as nickel from the leach residue.
[0033] In the solid-liquid separation step S2, a solid-liquid separation device having thickeners connected in multiple stages is used to mix the leaching slurry with a washing liquid, and then a solid-liquid separation process is performed to separate the leaching liquid and the leaching residue. Specifically, the leaching slurry is first diluted with the washing liquid, and then the leaching residue in the leaching slurry is concentrated as a sediment in the thickener. This makes it possible to reduce the nickel content adhering to the leaching residue according to the degree of dilution. In addition, by using thickeners connected in multiple stages in this way to perform solid-liquid separation while performing multi-stage washing, it is possible to improve the nickel recovery rate in the washing liquid, i.e., the leaching liquid.
[0034] In the solid-liquid separation step S2, at least a part of the slurry of the neutralized precipitate obtained in the subsequent neutralization step S3 is transferred and subjected to solid-liquid separation together with the leaching slurry, thereby reducing nickel recovery loss.
[0035] As a multi-stage washing method in the solid-liquid separation treatment, for example, a continuous countercurrent washing method (CCD method) is used in which a washing solution not containing nickel is used to contact the solid-liquid separation treatment with a countercurrent. The washing solution is not particularly limited, but any solution that does not contain nickel and does not affect the process can be used. Among them, it is preferable to use an aqueous solution with a pH of 1 to 3. If the pH of the washing solution is high, bulky aluminum hydroxide is generated when aluminum is contained in the leaching solution, which causes poor settling of the leaching residue in the thickener. In addition, as the washing solution, it is preferable to repeatedly use a low pH (pH of about 1 to 3) barren solution obtained in the subsequent sulfurization step S4. This makes it possible to reduce the amount of washing solution newly introduced into the system and to increase the recovery rate of nickel and cobalt.
[0036] The solid-liquid separation device may, for example, have a thickener equipped with a settling tank having an overflow section at the periphery for discharging supernatant liquid and a cylindrical feedwell disposed vertically in the center, and a stirring tank. In the solid-liquid separation device, the thickeners are connected in multiple stages, and the leach slurry to be treated is washed in multiple stages while separating and removing the leach residue, which is the solid content.
[0037] The leachate separated by such solid-liquid separation is subjected to neutralization in the subsequent neutralization step S3. On the other hand, a part of the separated leachate slurry is added to the leachate to be neutralized in the subsequent neutralization step S3, and the remainder is appropriately treated with wastewater.
[0038] The solid-liquid separation apparatus and the specific operation of treating while performing multi-stage washing using the apparatus will be described in detail later.
[0039] (3) Neutralization process In the neutralization step S3, a neutralizing agent is added to the obtained leachate while suppressing oxidation of the leachate to adjust the pH to a predetermined range, and a neutralized precipitate containing impurity elements and a neutralized end liquid that serves as a mother liquor for nickel recovery are generated. By carrying out such neutralization treatment, the impurity content in the obtained neutralized end liquid can be reduced, and the quality of the nickel sulfide (product) obtained by carrying out a sulfurization treatment (sulfurization step S4) on the neutralized end liquid can be improved.
[0040] Specifically, in the neutralization step S3, a neutralizing agent is added to the leachate to adjust the pH, thereby producing a neutralized end solution and a neutralized precipitate slurry containing, for example, trivalent iron as an impurity element. By subjecting the leachate to neutralization in this manner, the excess acid used in the leaching treatment in the leaching step S1 is neutralized to produce a neutralized end solution, and impurity elements such as iron ions and aluminum ions remaining in the solution are removed as neutralized precipitate.
[0041] In the method according to the present embodiment, in the neutralization treatment, a slurry of the leaching residue obtained by subjecting the leaching slurry to solid-liquid separation in the solid-liquid separation step S2 is added to the leaching solution to be subjected to the neutralization treatment at a predetermined ratio. By adding the leaching residue slurry to the leaching solution in this manner, the turbidity of the resulting neutralization end solution can be effectively reduced, and the recovery loss of nickel can be reduced.
[0042] At least a part of the neutralized precipitate slurry obtained by the neutralization treatment is repeatedly subjected to the solid-liquid separation step S2, and is subjected to the solid-liquid separation treatment together with the leaching slurry. In this case, in the method according to the present embodiment, the leaching residue slurry is added at a predetermined ratio to the leachate subjected to the neutralization treatment, so that an excessive increase in the neutralized precipitate slurry can be prevented, and nickel recovery loss can be reduced while reducing the precipitate load in the treatment in the solid-liquid separation step S2.
[0043] (4) Sulfurization process In the sulfurization step (nickel recovery step) S4, the neutralization end liquid, which is the mother liquor for nickel recovery, is used as the starting liquid for the sulfurization reaction, and a sulfurization agent such as hydrogen sulfide gas is added to the starting liquid for the sulfurization reaction to cause a sulfurization reaction, thereby producing a sulfide (nickel sulfide) containing nickel with few impurity components and a sulfurization end liquid, which is a barren liquid in which the nickel concentration is stabilized at a low level.
[0044] In addition, when zinc is contained in the final neutralization solution, the zinc can be selectively separated as a sulfide prior to separating nickel as a sulfide.
[0045] The sulfurization treatment in the sulfurization step S4 can be carried out using a sulfurization reaction tank or the like, and for example, hydrogen sulfide gas is blown into the gas phase of the sulfurization reaction starting solution introduced into the sulfurization reaction tank, and the hydrogen sulfide gas that moves into the solution can cause a gentle sulfurization reaction. This sulfurization treatment fixes nickel as a sulfide.
[0046] After the sulfurization reaction is completed, the resulting slurry containing nickel sulfide is charged into a filter such as a filter press and filtered to collect the sulfide on a filter cloth. The aqueous solution component that has passed through the filter cloth is collected as a poor liquid. In order to reduce the amount of liquid passing through the filter, it is preferable to charge the slurry in advance into a sedimentation concentration device such as a thickener and remove the supernatant liquid as a poor liquid.
[0047] ≪3. Solid-liquid separation process≫ Here, the solid-liquid separation apparatus used in the treatment in the solid-liquid separation step S2 in the above-mentioned hydrometallurgical process and the specific treatment operation using the apparatus will be described in more detail.
[0048] As described above, in the solid-liquid separation step S2, a solid-liquid separation device configured by connecting thickeners in multiple stages is used to perform multi-stage washing by a continuous countercurrent washing method (CCD method) in which the leached slurry obtained by the leaching treatment in the leaching step S1 is brought into contact with a nickel-free washing solution in a countercurrent manner, while separating the solids (leaching residue) contained in the leached slurry, and a crude nickel sulfate aqueous solution (leachate) from which the solids have been removed is obtained.
[0049] <3-1. Structure of solid-liquid separator (thickener) and multi-stage cleaning> Fig. 2 is a configuration diagram showing an example of a solid-liquid separation apparatus in which thickeners are connected in multiple stages to perform the CCD method. The solid-liquid separation apparatus 1 shown in Fig. 2 shows an example of a configuration in which thickeners are connected in five stages, and although the number of connected stages is not limited to this, a solid-liquid separation apparatus provided with 4 to 7 thickener stages is preferable.
[0050] In the CCD method, a solid-liquid separator 1 is used in which a thickener consisting of a settling tank where solid-liquid separation treatment is performed and a stirring tank is connected in series in multiple stages, for example, 4 to 7 stages. In the solid-liquid separator 1, the leached slurry obtained in the leaching step S1 is charged into the first-stage thickener located at the most upstream side (side A in Fig. 2), and for example, wash water such as industrial water or smelting waste liquid (barren liquid) is charged into the final-stage (fifth-stage) thickener located at the most downstream side (side B in Fig. 2).
[0051] In the solid-liquid separation device 1, the leaching slurry and washing liquid charged are brought into contact with each other in a countercurrent manner within the device, and at the same time, a flocculant is added to the leaching slurry charged from the most upstream side (side A) to flocculate the solids in the slurry and promote solid-liquid separation.
[0052] (About each stage of thickener and mixing tank) Fig. 3 shows a configuration diagram of a thickener (only one stage) constituting each stage of the solid-liquid separation apparatus 1 shown in Fig. 2. As described above, the solid-liquid separation apparatus 1 has a plurality of thickeners connected in multiple stages, and the thickener 10 is composed of an agitation tank 11 and a sedimentation tank 12.
[0053] The stirring tank 11 is a tank equipped with stirring members such as a stirring shaft and stirring blades inside. In the stirring tank 11, the leaching slurry and the overflow liquid sent from the thickener in the subsequent stage are respectively charged and stirred and mixed. Note that the stirring tank 11 of the thickener in the final stage (the fifth stage in the example of Figure 2) is charged with smelting waste liquid (barren liquid) or new washing water, rather than the overflow liquid. In this stirring tank 11, the leaching slurry and the overflow liquid are stirred and mixed, whereby the leaching slurry is washed and the adhering liquid adhering to the solids is washed away.
[0054] The settling tank 12 is, for example, a cylindrical treatment tank into which the leaching slurry is charged and the solids in the leaching slurry are allowed to settle and separate. The settling tank 12 is provided therein with a vertically disposed cylindrical feedwell 13. For example, when the settling tank 12 is cylindrical, the feedwell 13 is provided approximately concentrically with the settling tank 12. The feedwell 13 serves as a passage for sending (feeding) the leaching slurry supplied from the stirring tank 11 into the settling tank 12.
[0055] The settling tank 12 is provided with an overflow section 14 at the periphery of the upper part of the tank for overflowing (OF) and discharging the leachate, which is the supernatant liquid obtained by settling and separating the solids in the leaching slurry. The overflow section 14 is shaped like a gutter, for example, and is connected to a flow path for sending the overflow liquid from the thickener in the downstream stage to the stirring tank 11.
[0056] In the settling tank 12, the overflowed solution (hereinafter also referred to as the "overflow liquid") is transferred to the upstream stirring tank 11 as described above, while the slurry including other solid contents is taken out from the bottom of the settling tank 12 and transferred to the downstream stirring tank 11 by the pump 15.
[0057] (Basic flow of multi-stage cleaning) Next, a basic flow of the leaching slurry during multi-stage washing using the solid-liquid separator 1 (Fig. 2) will be described. The arrows in Fig. 2 indicate the flow of the leaching slurry and the overflow liquid.
[0058] First, in the first-stage thickener, the leaching slurry obtained by the leaching treatment in the leaching step S1 and the overflow liquid from the settling tank 12 of the subsequent second-stage thickener are charged into the stirring tank 11, and they are stirred and mixed. In the stirring tank 11 of the first-stage thickener, the adhering liquid adhering to the solids in the leaching slurry is washed with the overflow liquid, and then the washed leaching slurry is charged from the stirring tank through the feed well 13 into the settling tank 12.
[0059] At this time, in the first-stage thickener, a flocculant for flocculating the solids in the slurry is added together with the leaching slurry via the feedwell 13. The leaching slurry and the flocculant are then mixed in the settling tank 12, and the solids in the slurry are flocculated and precipitated to be separated.
[0060] In addition, as will be described in detail later, in the method according to the present embodiment, the neutralized precipitate slurry generated by the neutralization treatment in the neutralization step S3 is transferred and added to the first-stage thickener via the feedwell 13. In this manner, in the method according to the present embodiment, the neutralized precipitate slurry is subjected to the solid-liquid separation step S2 repeatedly, and is particularly characterized in that it is added to the first-stage thickener in the solid-liquid separation apparatus 1 configured by connecting thickeners in multiple stages.
[0061] The slurry containing the separated solids is extracted from the bottom of the settling tank 12 and transferred via a pump to the stirring tank 11 of the second-stage thickener at the downstream. On the other hand, the supernatant liquid overflowing from the settling tank 12 via the overflow section 14 is supplied to the next neutralization step S3 in the hydrometallurgical process.
[0062] Next, in the second-stage thickener, the solids extracted from the lower part of the settling tank 12 of the first-stage thickener in the previous stage are charged into the stirring tank 11, and the overflow liquid from the settling tank 12 of the third-stage thickener in the subsequent stage is charged into the stirring tank 11, and the moisture adhering to the solids is washed away by the overflow liquid. Then, the slurry obtained by washing in the stirring tank 11 is charged into the settling tank 12 through the feed well 13, and the solids in the slurry are separated by coagulation and precipitation. The slurry containing the separated solids is discharged from the lower part of the settling tank 12 and transferred to the stirring tank 11 of the third-stage thickener in the subsequent stage via a pump. On the other hand, the overflow liquid overflowing from the settling tank 12 via the overflow section 14 is charged into the stirring tank 11 through piping or the like connected to the stirring tank 11 of the first-stage thickener in the previous stage.
[0063] Thereafter, in the third and fourth thickeners, the slurry containing solids is washed in multiple stages by coming into countercurrent contact with the overflow liquid in a similar manner.
[0064] In the fifth thickener, which is the final stage located at the most downstream side, the solids extracted from the lower part of the settling tank 12 of the preceding fourth thickener are charged into its stirring tank 11, and new washing water (for example, a process liquid with a low nickel concentration in a hydrometallurgical process) is charged to wash away the moisture adhering to the solids. The slurry obtained by washing in the stirring tank 11 is charged into the settling tank 12 via the feed well 13, and the solids in the slurry are coagulated and precipitated to be separated.
[0065] The slurry containing the separated solids is pumped out from the bottom of the settling tank 12 and treated as leaching residue (CCD residue). On the other hand, the overflow liquid that overflows from the settling tank 12 via the overflow section 14 is charged into the agitation tank 11 of the fourth-stage thickener in the previous stage via piping or the like connected to that tank.
[0066] By subjecting the leaching slurry to solid-liquid separation while washing in multiple stages in this manner, new wash water only needs to be charged to the thickener in the final stage, and new wash water is not required for the thickeners in the remaining stages, which makes it possible to significantly save on wash water.
[0067] <3-2. Specific operations for solid-liquid separation treatment> As for the overflow liquid from each thickener stage, the overflow liquid from the final thickener stage (the fifth stage in Fig. 2) has the lowest content of valuable metals such as nickel and cobalt. One reason for this is that the valuable metals have already been washed in the mixing tank 11 of the thickener two stages before (the third stage in Fig. 2). Another reason is that the slurry separated into solid and liquid in the previous thickener stage (the fourth stage in Fig. 2) and new washing water overflow, and the slurry is then charged into the mixing tank 11 of the previous stage (the fourth stage in Fig. 2), where it is stirred and washed, and then charged into the final thickener stage.
[0068] On the other hand, the overflow from the stage before the final stage (the fourth stage in Figure 2) has a higher content of valuable metals adhering to the solids than the final stage, and the more distant it is from the final stage, the more valuable metals there are, with the overflow from the first thickener having the highest valuable metal content. In general, operations are carried out to recover a crude nickel sulfate aqueous solution (leachate), which is the overflow liquid, with a nickel and cobalt recovery rate of 90% or more.
[0069] In addition, the overflow from the first thickener is subjected to solid-liquid separation in each thickener stage, and the settling of fine particles is also progressing. Therefore, the overflow from the first thickener has the lowest turbidity (highest transparency). Specifically, the operation is performed so that the turbidity is 200 NTU or less.
[0070] In the method according to the present embodiment, the slurry of the leaching residue separated in the solid-liquid separation step S2 is added to the leachate to be subjected to the neutralization treatment in the next neutralization step S3, and the neutralized precipitate slurry generated by the neutralization treatment is returned to the solid-liquid separation step. When the neutralized precipitate slurry is returned to the solid-liquid separation step S2, the slurry is transferred to the first-stage thickener located at the most upstream position. This method can reduce the load of precipitate in the solid-liquid separation treatment and suppress the recovery loss of nickel.
[0071] In the solid-liquid separation process, an appropriate amount of flocculant is added to the thickener containing the leaching slurry. In the method according to the present embodiment, it is preferable to periodically measure and monitor the turbidity and viscosity of the supernatant liquid (overflow liquid, leachate) in the first-stage thickener located at the most upstream position, and adjust the amount of flocculant added in the solid-liquid separation process based on the monitoring results.
[0072] It is known that the recovery rate of nickel and cobalt recovered from the leachate (crude nickel sulfate aqueous solution) is correlated with the turbidity of the leachate. For this reason, the recovery rate of nickel and cobalt in actual operation can be controlled by the turbidity of the obtained leachate. Specifically, the value is 200 NTU or less as measured by a turbidimeter (e.g., HACH 2100P scattered light turbidimeter). This means that the higher the transparency of the leachate (the lower the turbidity), the more the solids are coagulated and the more thoroughly the adhering liquid is washed off, and a good correlation is established.
[0073] Therefore, by periodically measuring and monitoring the turbidity of the supernatant (overflow liquid) and adjusting the amount of flocculant added based on the change over time, the flocculant can be efficiently added to the solids in the leaching slurry, and solid-liquid separation can proceed more effectively. This effectively reduces the turbidity of the supernatant from the first-stage thickener and increases its clarity.
[0074] Specifically, if the turbidity of the supernatant is higher than a specified value (e.g., 200 NTU), the amount of flocculant added is increased to restore clarity. On the other hand, if the turbidity of the supernatant is lower than the specified value, the amount of flocculant added is decreased. This makes it possible to suppress the use of excessive flocculant and perform efficient treatment.
[0075] However, when the turbidity is low, the clarity may suddenly deteriorate after the amount of flocculant added is reduced, so it is preferable to control the amount of flocculant added by periodically measuring and monitoring the turbidity.
[0076] In order to prevent a sudden deterioration in clarity, it is preferable to periodically measure and monitor the viscosity of the supernatant (overflow liquid). The viscosity of the supernatant can be measured using the filtration time of a certain amount of the supernatant as a parameter. Specifically, the filtration time can be measured as the time required to aspirate and filter a predetermined amount of the supernatant from the first thickener through a membrane filter with a mesh size of 0.45 μm.
[0077] For example, when the concentration of the flocculant is reduced, the filtration time of the supernatant from the first thickener is reduced accordingly. This is presumably because the reduced concentration of the flocculant solution inhibits the flocculation of the flocculant components, lowering the viscosity of the supernatant. For this reason, by setting a lower limit for the viscosity of the supernatant and periodically monitoring the results of viscosity measurements, the amount of flocculant added can be controlled so that the viscosity of the supernatant does not fall below the set lower limit, thereby maintaining the clarity of the supernatant.
[0078] In this way, preferably, the turbidity and viscosity of the supernatant liquid (overflow liquid, leachate) in the first-stage thickener are periodically measured and monitored, and the amount of flocculant added in the solid-liquid separation treatment is adjusted, so that even when the neutralized precipitate slurry is repeatedly charged from the neutralization step S3 (in other words, when the treatment load due to the precipitate fluctuates), the precipitate load can be more effectively reduced. Furthermore, the effect of reducing nickel recovery loss by repeatedly charging the neutralized precipitate and subjecting it to solid-liquid separation treatment together with the leach slurry can be more effectively achieved.
[0079] It is also possible to prevent the addition of excessive flocculant, and as a result, the amount of flocculant used can be effectively reduced, enabling efficient treatment.
[0080] ≪4. Neutralization process in the neutralization process≫ In the hydrometallurgical smelting method for nickel oxide ore according to the present embodiment, in the neutralization treatment in the neutralization step S3, a neutralizing agent is added to the leachate to be treated to adjust the pH to a predetermined value. At this time, a slurry of the leachate residue obtained by solid-liquid separation of the leachate slurry is added at a predetermined ratio to the leachate to be subjected to the neutralization treatment.
[0081] (pH adjustment) In the neutralization process, it is preferable to adjust the pH of the resulting neutralized final solution to a range of 2.5 to 3.5 by adding a neutralizing agent to the leachate. If the pH of the neutralized final solution is adjusted to less than 2.5, impurity elements contained in the leachate may not be sufficiently converted into precipitates such as hydroxides. This increases the impurity content of the resulting neutralized final solution, and the amount of impurities in the nickel-containing sulfide generated in the sulfurization step S4 increases. On the other hand, if the pH of the neutralized final solution is adjusted to more than 3.5, fine particles with poor sedimentation properties are generated, which tends to increase the turbidity. In addition, when zinc is removed as sulfide in a subsequent step, part of the nickel and cobalt are also precipitated.
[0082] The neutralizing agent is not particularly limited, and may be, for example, an aqueous solution or slurry of an alkali metal hydroxide or an alkali metal carbonate, such as magnesium hydroxide or calcium carbonate. From an industrial perspective, it is preferable to use a slurry of inexpensive calcium carbonate.
[0083] (Addition of leach residue slurry) In the neutralization treatment, a neutralizing agent is added, and a slurry of the leaching residue obtained by solid-liquid separation of the leaching slurry is added. This effectively reduces the turbidity of the resulting neutralization end solution. This effectively reduces the impurity content in the nickel sulfide obtained by subjecting the neutralization end solution to a sulfurization treatment, thereby improving the quality of the nickel sulfide.
[0084] Here, the leaching residue slurry is a slurry of the leaching residue obtained by subjecting the leaching slurry generated in the leaching step S1 of the hydrometallurgical process to solid-liquid separation in the solid-liquid separation step S2. The leaching residue contains hematite (Fe2O3) as a main component (usually 50% by mass to 70% by mass) and has a high specific gravity. In addition, the leaching residue contains a trace amount of nickel that did not migrate into the leachate but became a precipitate during the leaching treatment in the leaching step S1.
[0085] In the neutralization treatment of the leachate, a slurry of the leach residue is added to the leachate to perform the neutralization treatment, and the neutralization precipitate is formed by flocculating the leach residue having a large specific gravity as a core, and as a result, the settling property of the neutralization precipitate can be increased and the turbidity of the resulting neutralization end liquid can be reduced. Then, by using the neutralization end liquid (nickel recovery mother liquor) with effectively reduced turbidity as the sulfurization reaction starting liquid in the sulfurization step S4, nickel sulfide with an extremely low impurity content can be produced.
[0086] In addition, as described above, since the leaching residue contains trace amounts of nickel, the recovery loss of nickel can be reduced by adding a slurry of the leaching residue to the leaching liquid and returning it to the process system.
[0087] The amount of the leaching residue slurry added to the leachate is not particularly limited, but is preferably added at a flow rate that is 5.0 volume % or more, more preferably 6.0 volume % or more, relative to the flow rate of the leachate used for the neutralization treatment. The leach residue slurry is also added at a flow rate that is preferably 8.0 volume % or less, more preferably 7.5 volume % or less, relative to the flow rate of the leachate. In this way, by adding the leach residue slurry to the leachate at a flow rate in the above-mentioned range, the turbidity of the resulting neutralization end solution can be reduced, for example, to less than 100 NTU, preferably less than 70 NTU. On the other hand, the neutralization precipitate slurry can be prevented from increasing excessively, and the decrease in the recovery rate of nickel obtained through the hydrometallurgical process can be effectively suppressed while suppressing the precipitate load.
[0088] Regarding the amount of leaching residue slurry added, if it is less than 5% by volume relative to the flow rate of the leachate, the nuclei on which the neutralized precipitate can precipitate are insufficient, which tends to increase turbidity, and the impurity content increases in the subsequent process. On the other hand, if it exceeds 8% by volume relative to the flow rate of the leachate, the amount of neutralized precipitate generated becomes excessive, resulting in a decrease in the nickel recovery rate. That is, as will be described in detail later, the generated neutralized precipitate is transferred to a treatment tank performing a solid-liquid separation step S2 and is subjected to a solid-liquid separation process together with the leach slurry. However, if the amount of neutralized precipitate slurry becomes excessive, the nickel in the neutralized precipitate is transferred to the leach residue separated by solid-liquid separation, which increases the load of the precipitate in the solid-liquid separation step S2 and reduces the nickel recovery rate obtained through the hydrometallurgical process of nickel oxide ore.
[0089] The slurry of the leaching residue is preferably obtained by solid-liquid separation by multi-stage washing in the solid-liquid separation step S2, and the leaching residue obtained by such multi-stage washing has little adhesion of acid or alkali. This can prevent the leaching residue from interfering with the pH control of the entire leaching solution in the neutralization treatment. In addition, the local pH in the vicinity of the added leaching residue also follows the change in the bulk pH, making it easy to control the precipitation rate and particle size of the neutralized precipitate. Furthermore, the leaching residue obtained by solid-liquid separation by multi-stage washing has excellent specific gravity separability and filtration separability with water, and by selecting and using a leaching residue with particularly strong such properties (for example, the bottom part of the thickener or initial precipitate), the neutralized precipitate can be separated even more easily, and the turbidity of the final neutralization solution can be more effectively reduced.
[0090] The slurry of leaching residue has a slurry concentration of 1.5t / m 3 ~1.7t / m 3 By using a leaching residue slurry having such a slurry concentration, the turbidity of the final neutralization solution can be more effectively reduced.
[0091] When adding the leaching residue slurry to the leachate to be subjected to neutralization treatment, it is preferable to add a coagulant as well. Generally, neutralized precipitates such as hydroxide precipitates are known to have poor settling properties, and by adding the leaching residue slurry, which serves as the base for flocculation, and a coagulant, the leaching residue slurry, which has a high specific gravity, and the neutralized precipitates such as hydroxide precipitates are coagulated, thereby promoting the settling properties. Examples of the coagulant that can be used include polyamine, polydadomac, polyethyleneimine, and polyacrylamide.
[0092] When the flow rate of the leachate used in the neutralization treatment is increased or decreased, it is preferable to increase or decrease the amount of the leachate slurry added accordingly. However, when increasing the flow rate of the leachate slurry added, it is desirable to increase it gradually. Since the leachate only becomes effective when it is coagulated with the neutralized precipitate, depending on the composition of the neutralized precipitate and the amount of coagulant added, increasing the amount of addition may not promote the settling of the neutralized precipitate, which may be disadvantageous in terms of the residence time.
[0093] ≪5. Repetition of the neutralization sediment slurry from the neutralization process to the solid-liquid separation process≫ As described above, the method according to the present embodiment includes a process of repeatedly sending at least a part of the neutralized precipitate slurry obtained in the neutralization step S3 to the solid-liquid separation step S2. In this manner, the neutralized precipitate slurry is repeatedly sent to the solid-liquid separation step S2, and the neutralized precipitate slurry is subjected to a solid-liquid separation process together with the leaching slurry in the solid-liquid separation step S2, whereby nickel can be recovered from the neutralized precipitate slurry and nickel recovery loss can be effectively reduced.
[0094] Nickel loss to the neutralized precipitate is due to the adhesion of the neutralized precipitate liquid and the adhesion of nickel hydroxide due to local reactions on the surface of the neutralized precipitate, and both cannot be completely prevented. In contrast, by repeatedly passing the neutralized precipitate slurry through the solid-liquid separation step S2 operated at a low pH, it is possible to promote the dissolution of the locally reacted nickel hydroxide while simultaneously washing the leaching residue in the solid-liquid separation treatment by multi-stage washing.
[0095] The neutralized precipitate slurry from the neutralization step S3 is transferred to the solid-liquid separation step S2, where it is subjected to solid-liquid separation together with the leaching slurry. When transferring the neutralized precipitate slurry to the solid-liquid separation step, the slurry is transferred to the first-stage thickener located at the most upstream of the multiple thickener stages in the solid-liquid separation equipment 1 (see FIG. 2). This makes it possible to more effectively reduce nickel recovery losses.
[0096] Furthermore, as described above, it is preferable to periodically measure and monitor the turbidity and viscosity of the supernatant liquid in the first-stage thickener and adjust the amount of flocculant added in the solid-liquid separation process, thereby making it possible to more effectively reduce the sediment load even when the neutralized sediment slurry is transferred to the first-stage thickener in the solid-liquid separation process. EXAMPLES
[0097] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0098] [Example 1] In the hydrometallurgical smelting method of nickel oxide ore (see Fig. 1), the neutralization step involves adding the slurry of the leaching residue separated in the solid-liquid separation step to the leachate to be subjected to the neutralization treatment. In the neutralization step, the slurry of the neutralized precipitate generated by the neutralization treatment is repeatedly subjected to the solid-liquid separation step.
[0099] The solid-liquid separation process in the solid-liquid separation step uses a solid-liquid separation device (see Figure 2 for an overview) consisting of seven connected thickeners. Multi-stage washing is performed using the continuous countercurrent washing method (CCD method), in which nickel-free washing solution is brought into countercurrent contact with the leaching slurry to be treated, while separating the solid leachate residue and recovering the leachate from which the solids have been removed as the supernatant liquid (overflow liquid).
[0100] When the slurry of the neutralized precipitate generated by the neutralization treatment was transferred to the solid-liquid separation treatment in the solid-liquid separation step, the slurry was transferred to the first-stage thickener located at the most upstream position in the solid-liquid separation device. In the solid-liquid separation treatment, the turbidity and viscosity of the supernatant (overflow liquid) from the first-stage thickener were periodically measured and monitored to control the amount of flocculant added, thereby controlling the clarity of the supernatant while treatment was performed.
[0101] As a result of this treatment, the nickel loss rate in the solid-liquid separation process was 2.92%.
[0102] The nickel loss rate is expressed as a percentage of the amount of nickel contained in the slurry liquid discharged to the final neutralization step after solid-liquid separation treatment, relative to the amount of nickel contained in the ore slurry subjected to the hydrometallurgical process.
[0103] [Comparative Example 1] In Comparative Example 1, when the slurry of the neutralized precipitate generated by the neutralization treatment was transferred to the solid-liquid separation treatment in the solid-liquid separation step, the slurry was transferred to the second-stage thickener connected subsequent to the first stage in the solid-liquid separation device. In addition, the treatment was performed without controlling the clarity of the supernatant from the first-stage thickener located at the most upstream. The other conditions were the same as those in Example 1.
[0104] As a result of such treatment, the nickel loss rate in the solid-liquid separation process was 3.10%. Compared to Example 1, the nickel loss was increased.
Claims
1. A method for hydrometallurgy of nickel oxide ore, comprising adding an acid to nickel oxide ore to subject the nickel oxide ore to a leaching treatment, and obtaining nickel and cobalt sulfides from the resulting leachate, the method comprising the steps of: a solid-liquid separation step in which the leaching slurry obtained by the leaching treatment is subjected to a solid-liquid separation treatment while being washed in multiple stages using a solid-liquid separation device provided with multiple thickeners, thereby obtaining a leachate and a leaching residue; A neutralization step of adding a neutralizing agent to the leachate to perform a neutralization treatment, thereby obtaining a neutralized precipitate containing impurities and a neutralized final solution containing nickel and cobalt, In the neutralization step, neutralizing the leachate by adding the slurry of the leachate separated in the solid-liquid separation step to the leachate to be subjected to the neutralization treatment in an amount of 5.0 vol. % or more and 8.0 vol. % or less with respect to the flow rate of the leachate to be subjected to the neutralization treatment; The neutralization treatment includes repeating the neutralization precipitate slurry produced by the neutralization treatment to the solid-liquid separation step, When the neutralized precipitate slurry is subjected to the solid-liquid separation step again, the slurry is transferred to a first-stage thickener located at the most upstream of the thickeners provided in multiple stages in the solid-liquid separation device. A hydrometallurgical process for nickel oxide ores.
2. In the solid-liquid separation step, The treatment is carried out using a solid-liquid separation device having 4 to 7 thickeners in multiple stages.
2. The method for hydrometallurgy of nickel oxide ore according to claim 1.
3. In the solid-liquid separation step, The turbidity and viscosity of the supernatant in the first-stage thickener are periodically measured and monitored, and the amount of flocculant added in the solid-liquid separation treatment is adjusted.
3. The method for hydrometallurgy of nickel oxide ore according to claim 1 or 2.
4. In the solid-liquid separation step, Adjusting the turbidity of the supernatant in the first-stage thickener to less than 100 NTU. The method for hydrometallurgy of nickel oxide ore according to claim 3.
Citation Information
Patent Citations
Method for improving precipitation property of neutralized sediment
JP2004225120A
Hydrometallurgical process of nickel oxide ore
JP2005350766A
Zinc sulfide separation method
JP2010037626A
Solid-liquid separation treatment method and hydrometallurgical method of nickel oxide ore
JP2015061951A
Neutralization treatment method, and wet refining method for nickel oxide ore
JP2017145454A