Hydrometallurgical process for nickel oxide ore

Using nickel-cobalt mixed hydroxide as a neutralizing agent in the preliminary neutralization step with multi-stage tanks stabilizes pH and reduces turbidity, improving the efficiency and yield of nickel-cobalt mixed sulfide production in nickel oxide ore processing.

JP7585928B2Active Publication Date: 2024-11-19SUMITOMO METAL MINING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021053440
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-26
Publication Date
2024-11-19
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

The existing hydrometallurgical methods for processing nickel oxide ore face challenges in maintaining stable pH levels during the preliminary neutralization step, leading to variations that increase the turbidity of the overflow liquid and reduce the yield of nickel-cobalt mixed sulfide.

Method used

The use of nickel-cobalt mixed hydroxide as a neutralizing agent in the preliminary neutralization step, combined with multi-stage neutralization in series reaction tanks, effectively stabilizes pH levels and promotes iron precipitation, reducing turbidity and improving the efficiency of the process.

Benefits of technology

This approach stabilizes the pH, suppresses variations, enhances iron precipitation, and maintains the quality of the nickel-cobalt mixed sulfide production by reducing turbidity and increasing the actual yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585928000003
    Figure 0007585928000003
  • Figure 0007585928000004
    Figure 0007585928000004
  • Figure 0007585928000001
    Figure 0007585928000001
Patent Text Reader

Abstract

To provide a method capable of conducting a stable treatment by suppressing scattering of pH in a preliminary neutralization treatment of a wet-type smelting method of a nickel oxide ore.SOLUTION: A wet-type smelting method of a nickel oxide ore for producing a nickel cobalt mixed sulfide from an exudation slurry obtained by exuding a nickel oxide ore includes: an exudation process of subjecting to exudation treatment by adding a sulfuric acid to the nickel oxide ore; and a preliminary neutralization process of subjecting neutralization treatment by adding a neutralizer to the exudation slurry obtained by the exudation treatment to remove a free acid contained in the exudation slurry, where a nickel cobalt mixed hydroxide is used as a neutralizer in the preliminary neutralization process.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a process for hydrometallurgy of nickel oxide ores to produce nickel-cobalt mixed sulfides. [Background technology]

[0002] Nickel is widely used as a raw material for stainless steel, and as the resource of the nickel sulfide ore used as the raw material tends to become depleted, technology for refining low-grade oxide ore has been developed and put into practical use.

[0003] Specifically, a manufacturing process known as "High Pressure Acid Leach (HPAL)" has been put into practical use, in which nickel oxide ores such as limonite or saprolite are placed in a pressurized device such as an autoclave together with a sulfuric acid solution, and nickel is leached under high temperatures and pressures of around 240°C to 260°C.

[0004] In a manufacturing process based on the HPAL method, nickel is leached into a sulfuric acid solution, and then excess acid is neutralized by adding a neutralizing agent, and the nickel is separated from the leaching residue by solid-liquid separation. After that, the nickel in the leachate is separated from impurities and recovered as intermediate raw materials in the form of hydroxides, sulfides, etc. The intermediate raw materials are then further refined to produce nickel metal, nickel salt compounds, etc. (see, for example, Patent Document 1).

[0005] For example, nickel-cobalt mixed hydroxide (MHP) is recovered as an intermediate raw material. Nickel-cobalt mixed hydroxide is used as a raw material for manufacturing nickel salts, especially nickel sulfate. Nickel salts are used in general electrolytic plating, as well as in electroless plating for hard disks, as a plating raw material, catalyst, battery material, etc., but in recent years, there has been a demand from the market for nickel salts with higher purity.

[0006] Nickel-cobalt mixed sulfide (MS) as an intermediate raw material is used as a raw material for refining into high-purity electrolytic nickel and nickel sulfate. Here, "high purity" refers to a quality in which the content of impurities, including zinc, is controlled below a specified level. Therefore, there is a demand for nickel-cobalt mixed sulfide with a low zinc content, that is, a quality guaranteed within the range of a specified standard (zinc content ≦ 250 ppm by weight).

[0007] However, when the supply and demand balance of the above-mentioned intermediate raw materials, nickel-cobalt mixed hydroxide and nickel-cobalt mixed sulfide, is disrupted due to fluctuations in demand in the final product market, this results in a surplus of intermediate raw materials, which causes an increase in production costs.

[0008] In the manufacturing process based on the HPAL method, the leaching slurry obtained by leaching nickel oxide ore is subjected to a subsequent pre-neutralization step in which the pH is adjusted to remove free acid in the slurry. In this case, the pH of the leaching slurry is kept as high as possible in the neutralization step in order to promote the precipitation of iron, which is an impurity. Depending on the pH of the leaching slurry that is adjusted, the turbidity of the overflow liquid (leachate) obtained from a solid-liquid separation device such as a thickener in the solid-liquid separation step that follows the pre-neutralization step may increase.

[0009] Therefore, in the preliminary neutralization step, the pH of the leachate to be adjusted must be kept high in order to promote iron precipitation, and must be adjusted within a range that does not cause an increase in the turbidity of the thickener overflow liquid.

[0010] However, in the conventional neutralization process in the preliminary neutralization step, the pH may vary widely, which may result in an increase in the turbidity of the overflow liquid. The increase in turbidity of the overflow liquid also affects the recovery rate of the nickel-cobalt mixed sulfide that is finally obtained. Therefore, there was a demand for a method to suppress the pH variation in the neutralization process in the preliminary neutralization step and perform the process stably. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2016-6233 A [Patent Document 2] JP 2016-222989 A Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide a method for performing a stable treatment while suppressing the variation in pH in a preliminary neutralization treatment in a hydrometallurgical method for nickel oxide ore. [Means for solving the problem]

[0013] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by using nickel-cobalt mixed hydroxide (MHP) as a neutralizing agent in a preliminary neutralization step in a hydrometallurgical method for nickel oxide ore, and have completed the present invention.

[0014] (1) A first aspect of the present invention is a hydrometallurgical method for producing nickel-cobalt mixed sulfides from a leaching slurry obtained by leaching nickel oxide ore, the method including: a leaching step of adding sulfuric acid to the nickel oxide ore to perform a leaching treatment; and a pre-neutralization step of neutralizing the leached slurry obtained by the leaching treatment by adding a neutralizing agent to the leached slurry and removing free acid contained in the leached slurry, wherein a nickel-cobalt mixed hydroxide is used as the neutralizing agent in the pre-neutralization step.

[0015] (2) A second aspect of the present invention is a method for hydrometallurgy of nickel oxide ore according to the first aspect of the present invention, wherein the nickel-cobalt mixed hydroxide is produced through a production process using the leaching slurry as a raw material.

[0016] (3) A third aspect of the present invention is a method for hydrometallurgy of nickel oxide ore according to the first or second aspect of the present invention, wherein the preliminary neutralization step comprises continuously carrying out a multi-stage neutralization treatment using two or more reaction tanks arranged in series, and adding the nickel-cobalt mixed hydroxide as neutralizing agent A to at least a first reaction tank located at the most upstream side.

[0017] (4) A fourth aspect of the present invention is a method for hydrometallurgy of nickel oxide ore according to the third aspect of the present invention, wherein a neutralizing agent different from the nickel-cobalt mixed hydroxide is added as neutralizing agent B to a second or subsequent reaction tank provided adjacent to the first reaction tank.

[0018] (5) A fifth aspect of the present invention is the method for hydrometallurgy of nickel oxide ore according to the fourth aspect of the present invention, wherein the neutralizing agent B is a limestone slurry.

[0019] (6) A sixth aspect of the present invention is a method for hydrometallurgy of nickel oxide ore according to the fourth or fifth aspect of the present invention, wherein the neutralizing agent A is added to the first reaction tank so that the pH of the solution after neutralization is 2.0 or more and 2.5 or less, and the neutralizing agent B is added to the second or subsequent reaction tanks so that the pH of the solution after neutralization in the most downstream reaction tank is 2.8 or more and 3.2 or less.

[0020] (7) A seventh aspect of the present invention is the method for hydrometallurgy of nickel oxide ore according to any one of the first to sixth aspects, wherein the concentration of the free acid contained in the leaching slurry is 30 g / L to 60 g / L.

[0021] (8) An eighth aspect of the present invention is a method for hydrometallurgy of nickel oxide ore according to any one of the first to seventh aspects, wherein the leaching slurry has a nickel concentration of 5 g / L to 10 g / L and an iron concentration of 3 g / L to 10 g / L.

[0022] (9) A ninth aspect of the present invention is the method for hydrometallurgy of nickel oxide ore according to any one of the first to eighth aspects, wherein the leaching slurry has a slurry concentration of 30% by mass to 50% by mass. Effect of the Invention

[0023] According to the present invention, it is possible to provide a method for performing a stable pre-neutralization treatment with reduced pH variation in a hydrometallurgical method for nickel oxide ore. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a process diagram showing an example of a flow of a hydrometallurgical process for nickel oxide ore. [Diagram 2] FIG. 1 is a diagram showing an example of the configuration of free acid removal equipment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described below. Note that the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention.

[0026] ≪1. Overview≫ The hydrometallurgical method for nickel oxide ore according to the present embodiment involves subjecting nickel oxide ore to a leaching treatment using an acid such as sulfuric acid under high temperature and high pressure, and producing nickel-cobalt mixed sulfide (MS) from the resulting leached slurry.

[0027] Specifically, this method includes a leaching step in which sulfuric acid is added to nickel oxide ore to perform leaching treatment, and a preliminary neutralization step in which a neutralizing agent is added to the leached slurry obtained by the leaching treatment to perform neutralization treatment and remove free acid contained in the leached slurry, and is characterized in that the neutralization step uses nickel-cobalt mixed hydroxide (MHP) as the neutralizing agent.

[0028] Here, the increase in turbidity of the leachate (overflow liquid) obtained by performing a pre-neutralization process (pre-neutralization treatment) to remove free acid contained in the leaching slurry and then performing solid-liquid separation occurs when the pH of the leaching slurry fluctuates higher in the pre-neutralization treatment. On the other hand, in order to promote the precipitation of iron contained in the leaching slurry, it is necessary to adjust the pH of the leaching slurry to a higher value. Therefore, in order to prevent the increase in turbidity of the overflow liquid obtained by solid-liquid separation and to sufficiently precipitate and remove iron, it is necessary to prevent the pH of the leaching slurry from fluctuating excessively higher, and it is preferable to suppress the pH fluctuation and stably adjust the pH to a desired pH range.

[0029] As a result of the inventors' investigations, it was found that by using nickel-cobalt mixed hydroxide as a neutralizing agent in the preliminary neutralization treatment of the leaching slurry, the variation in pH of the leaching slurry can be effectively suppressed, and the pH of the leaching slurry can be prevented from fluctuating excessively high.

[0030] Therefore, according to this method, it is possible to perform preliminary neutralization treatment stably while suppressing the variation in pH, and it is possible to effectively convert the iron contained in the leaching slurry into precipitates and suppress an increase in turbidity of the overflow liquid (leachate) recovered through solid-liquid separation. This makes it possible to suppress a decrease in the recovery rate of the finally obtained nickel-cobalt mixed sulfide and to perform efficient and effective operation.

[0031] Furthermore, the nickel-cobalt mixed hydroxide used as the neutralizing agent can be produced through a known manufacturing process for nickel-cobalt mixed hydroxide using, as a raw material, a leached slurry obtained by subjecting nickel oxide ore to a leaching treatment. By using such nickel-cobalt mixed hydroxide as a neutralizing agent, efficient operation utilizing surplus intermediate raw materials becomes possible, and production efficiency can be improved.

[0032] Furthermore, since nickel-cobalt mixed hydroxide contains nickel and cobalt, even if it is added as a neutralizing agent to the process for producing nickel-cobalt mixed sulfide, it does not become an impurity component, and it also leads to an increase in the production amount of nickel-cobalt mixed sulfide.

[0033] ≪2. Nickel oxide ore smelting process≫ First, a hydrometallurgical process for nickel oxide ore including the above-mentioned step of performing the preliminary neutralization treatment (preliminary neutralization step) will be described. The hydrometallurgical process for nickel oxide ore is a method for leaching nickel and cobalt from nickel oxide ore, which is a raw material, and producing a mixed sulfide of nickel and cobalt (nickel-cobalt mixed sulfide) from the leachate. In the following, a process based on the HPLA method in which nickel oxide ore is leached with sulfuric acid under high temperature and high pressure will be described.

[0034] Fig. 1 is a process diagram showing an example of the flow of a hydrometallurgical process for nickel oxide ore. As shown in Fig. 1, the hydrometallurgical process for nickel oxide ore includes a leaching step S1 in which sulfuric acid is added to a slurry of nickel oxide ore and leaching is performed under high temperature and high pressure, a preliminary neutralization step S2 in which the pH of the leaching slurry is adjusted to a predetermined range and preliminary neutralization is performed, a solid-liquid separation step S3 in which the pH-adjusted leaching slurry is washed in multiple stages to separate the residue and obtain a leachate containing nickel, cobalt and impurity elements, a neutralization step S4 in which the pH of the leachate is adjusted and neutralized, and a sulfurization step S5 in which a sulfurizing agent is added to the neutralization final solution to generate a nickel-cobalt mixed sulfide. In addition, the process includes a final neutralization step S6 in which the leachate residue separated in the solid-liquid separation step S3 and the barren solution discharged in the sulfurization step S5 are collected and rendered harmless.

[0035] (1) Leaching process In the leaching step S1, a high-temperature pressurized reaction tank such as an autoclave is used to add sulfuric acid to a slurry of nickel oxide ore (ore slurry), and a leaching treatment is performed by stirring under conditions of a temperature of approximately 230°C to 270°C and a pressure of approximately 3 MPa to 5 MPa, producing a leaching slurry consisting of a leachate and a leach residue.

[0036] Nickel oxide ores include so-called laterite ores such as limonite ore and saprolite ore. The nickel content of laterite ore is usually about 0.8% by mass to 2.5% by mass, and is contained as hydroxide or magnesium silicate mineral. The iron content is about 10% by mass to 50% by mass, and is mainly in the form of trivalent hydroxide, but some divalent iron is contained in magnesia siliceous mineral.

[0037] In the leaching process, for example, the leaching reactions represented by the following formulas (a) to (e) and high-temperature pyrohydrolysis reactions occur, resulting in the leaching of nickel, cobalt, etc. as sulfates and the immobilization of the leached iron sulfate as hematite. However, since the immobilization of iron ions does not proceed completely, the liquid portion of the obtained leaching slurry usually contains divalent and trivalent iron ions in addition to nickel, cobalt, etc.

[0038] Leaching reaction MO+H2SO4→MSO4+H2O (a) (In the formula, M represents Ni, Co, Fe, Zn, Cu, Mg, Cr, Mn, etc.) 2Fe(OH)3+3H2SO4→Fe2(SO4)3+6H2O ···(b) FeO+H2SO4→FeSO4+H2O (c) High-temperature thermohydrolysis reaction 2FeSO4+H2SO4+1 / 2O2→Fe2(SO4)3+H2O ···(d) Fe2(SO4)3+3H2O→Fe2O3+3H2SO4··(e)

[0039] The amount of sulfuric acid added in the leaching treatment is not particularly limited, but an excess amount is used so that the iron in the ore is leached. For example, 300 kg to 400 kg per ton of ore. From the viewpoint of the filterability of the leaching residue containing hematite generated in the subsequent solid-liquid separation step S3, it is preferable to adjust the pH of the resulting leachate to 0.1 to 1.0.

[0040] (2) Pre-neutralization process In the preliminary neutralization step S2, the pH of the leaching slurry obtained by the leaching treatment is adjusted to a predetermined range. In the leaching treatment, excess sulfuric acid is added to improve the leaching rate, so the leaching slurry contains excess sulfuric acid that was not involved in the leaching reaction, i.e., free acid, and has a low pH. In the preliminary neutralization step S2, a neutralizing agent is added to the leaching slurry to adjust the pH to a predetermined range, thereby removing the free acid.

[0041] Here, the leaching slurry to be neutralized is not particularly limited, but the slurry concentration is about 30% by mass to 50% by mass. The concentration of free acid contained in the leaching slurry is about 30 g / L to 60 g / L. The concentration of nickel contained in the leaching slurry is 5 g / L to 10 g / L, and the concentration of iron is 3 g / L to 10 g / L.

[0042] Although details will be described later, nickel-cobalt mixed hydroxide (MHP) is used as a neutralizing agent in the preliminary neutralization process S2. This preliminary neutralization process makes it possible to carry out the neutralization process stably while suppressing the variation in pH, and to effectively convert the iron contained in the leaching slurry into a precipitate while suppressing an increase in turbidity of the overflow liquid (leachate) recovered through solid-liquid separation.

[0043] In the preliminary neutralization treatment, a multi-stage neutralization treatment can be performed continuously using two or more reaction tanks arranged in series. Nickel-cobalt mixed hydroxide is added as neutralizing agent A to at least the first reaction tank located at the most upstream. A neutralizing agent other than nickel-cobalt mixed hydroxide, for example, limestone slurry, is added as neutralizing agent B to the second and subsequent reaction tanks arranged adjacent to the first reaction tank.

[0044] When multiple reaction tanks are used for multi-stage neutralization, the first reaction tank contains nickel-cobalt mixed hydroxide as neutralizer A, which is added to the leaching slurry so that the pH of the solution after neutralization is 2.0 to 2.5. In the second and subsequent reaction tanks, neutralizer B is added so that the pH of the solution after neutralization in the downstreammost reaction tank is 2.8 to 3.2.

[0045] In this way, the variation in pH of the leaching slurry can be more effectively suppressed, and the stability of the neutralization treatment can be improved. This promotes the precipitation of iron in the leaching slurry, and effectively suppresses an increase in turbidity of the overflow liquid from a solid-liquid separator such as a thickener, which is obtained in the next solid-liquid separation step S3. Furthermore, by suppressing an increase in turbidity of the overflow liquid, the treatment in the next step and thereafter can be performed efficiently, and a decrease in the recovery rate of nickel-cobalt mixed sulfides can be prevented.

[0046] (3) Solid-liquid separation process In the solid-liquid separation step S3, a solid-liquid separation device such as a thickener is used to wash the leaching slurry, whose pH has been adjusted in the preliminary neutralization step S2, in multiple stages, while performing a solid-liquid separation process to separate the leaching solution containing valuable metals such as nickel and cobalt from the leaching residue.

[0047] Specifically, first, the leaching slurry is diluted with a washing liquid, and then the leaching residue in the leaching slurry is concentrated as a precipitate in the thickener. This allows the nickel content adhering to the leaching residue to be reduced according to the degree of dilution. In practical operation, the recovery rate of nickel and cobalt can be improved by connecting thickeners having such functions in multiple stages. As the washing liquid, it is preferable to use an aqueous solution with a pH of 1 to 3 that does not affect the process, and for example, the low-pH barren liquid obtained in the sulfurization step S5 can be repeatedly used.

[0048] The overflow liquid obtained from the solid-liquid separator such as a thickener is recovered as a leachate and transferred to the next step. In this embodiment, since the treatment using nickel-cobalt mixed hydroxide as a neutralizing agent is performed in the above-mentioned preliminary neutralization step S2, it is possible to suppress an increase in the turbidity of the overflow liquid.

[0049] (4) Neutralization process In the neutralization step S4, a neutralizing agent such as magnesium oxide or calcium carbonate is added to the leachate separated and recovered in the solid-liquid separation step S3 while suppressing oxidation of the leachate, thereby obtaining a neutralized precipitate slurry containing trivalent iron and a neutralization end liquid, which is a mother liquor for recovering nickel.

[0050] Specifically, in the neutralization step S4, a neutralizing agent such as calcium carbonate is added to the leachate while suppressing oxidation of the leachate so that the pH of the resulting neutralized end solution is 4.0 or less, preferably 3.0 to 3.5, and more preferably 3.1 to 3.2, to form a neutralized end solution that serves as a mother liquor for recovering nickel and cobalt, and a neutralized precipitate slurry that contains trivalent iron as an impurity element.

[0051] The neutralization end solution is recovered by performing solid-liquid separation on the slurry (neutralization precipitate slurry) obtained by the neutralization treatment. As described above, the neutralization end solution is a solution based on the leachate obtained by subjecting the raw material nickel oxide ore to the leaching treatment with sulfuric acid in the leaching step S1, and is a sulfuric acidic solution containing nickel and cobalt.

[0052] (5) Sulfurization process In the sulfurization step S5, the neutralization end liquid, which is the mother liquid for recovering nickel and cobalt, is used as the starting liquid for the sulfurization reaction, and a sulfurizing agent such as hydrogen sulfide gas is added to the starting liquid for the sulfurization reaction to cause a sulfurization reaction, thereby producing a mixed sulfide of nickel and cobalt with few impurities and a barren liquid in which the concentrations of nickel and cobalt are stabilized at low levels. If zinc is contained in the neutralization end liquid, zinc can be selectively separated as a sulfide prior to separating nickel and cobalt as sulfides.

[0053] The sulfurization treatment in the sulfurization step S5 can be carried out using a sulfurization reaction tank or the like, and the sulfurization reaction is caused by, for example, blowing hydrogen sulfide gas into the gas phase of the sulfurization reaction starting liquid charged in the sulfurization reaction tank and dissolving the hydrogen sulfide gas in the solution. By such sulfurization treatment, nickel and cobalt contained in the sulfurization reaction starting liquid are fixed as mixed sulfides. After the sulfurization reaction is completed, the slurry containing the generated nickel-cobalt mixed sulfide is charged into a settling device such as a thickener and subjected to a settling separation treatment, and only the nickel-cobalt mixed sulfide is separated and recovered from the bottom of the thickener.

[0054] In this embodiment, nickel-cobalt mixed sulfide can be produced by going through each of the above-mentioned treatment steps. In particular, in this embodiment, since a preliminary neutralization treatment using nickel-cobalt mixed hydroxide as a neutralizing agent is performed in the preliminary neutralization step S2, the variation in pH of the leaching slurry can be effectively suppressed. This makes it possible to more effectively promote the precipitation of iron and reduce the concentration of iron in the leachate, and also to suppress an increase in the turbidity of the overflow liquid obtained through solid-liquid separation, i.e., the leachate, so that the treatment in the next step and thereafter can be efficiently performed. In addition, a decrease in the recovery rate of nickel-cobalt mixed sulfide can be prevented.

[0055] The aqueous solution components separated through the sulfurization step S5 are overflowed from the top of the thickener and collected as barren liquid. The collected barren liquid is a solution with an extremely low concentration of valuable metals such as nickel, and contains impurity elements such as iron, magnesium, and manganese that have not been sulfurized. This barren liquid is transferred to the final neutralization step S6 and is detoxified.

[0056] (6) Final neutralization step In the final neutralization step S6, the leaching residue separated by the solid-liquid separation treatment in the above-mentioned solid-liquid separation step S3 and the barren liquid containing impurity elements such as iron, magnesium, manganese, etc., recovered in the sulfurization step S5 are subjected to a neutralization treatment (detoxification treatment) to adjust the pH to a predetermined range that satisfies the discharge standard. The method for adjusting the pH is not particularly limited, but it can be adjusted to the predetermined range by adding a neutralizing agent such as calcium carbonate slurry, for example.

[0057] ≪3. Treatment in the preliminary neutralization process (preliminary neutralization treatment)≫ In the hydrometallurgical process for nickel oxide ore, as described above, in the pre-neutralization step S2, the pH of the leaching slurry is adjusted to remove excess sulfuric acid that was not involved in the reaction in the leaching process, i.e., free acid (pre-neutralization treatment).

[0058] Specifically, in the preliminary neutralization treatment, the pH of the obtained leaching slurry is adjusted to be maintained as high as possible. If the pH of the leaching slurry is too low, not only will it be necessary to make the treatment equipment used in the next step acid-resistant, which will increase costs, but the precipitation of iron, an impurity contained in the leaching slurry, will not proceed, and the iron content in the leachate will increase. Therefore, by adjusting the pH to a higher value by the preliminary neutralization treatment, the precipitation of iron will be promoted so that, for example, the iron content of the leaching residue obtained by solid-liquid separation of the leaching slurry will be 40% by mass to 55% by mass.

[0059] On the other hand, it is known that the pH of the leaching slurry can cause an increase in turbidity of the overflow liquid (leachate) from a solid-liquid separator such as a thickener in the solid-liquid separation step S3 following the preliminary neutralization step S2. The increase in turbidity of the overflow liquid reduces the treatment efficiency of the subsequent steps, and ultimately reduces the recovery rate of nickel-cobalt mixed sulfides.

[0060] It has been found that an increase in turbidity of the overflow liquid occurs when the pH of the leaching slurry obtained through the preliminary neutralization treatment fluctuates higher. As described above, in order to promote the precipitation of iron contained in the leaching slurry obtained through the leaching step S1, it is necessary to adjust the pH of the leaching slurry to a higher value. However, on the other hand, in order to prevent an increase in the turbidity of the overflow liquid obtained in the next solid-liquid separation step S3, it is necessary to prevent the pH of the leaching slurry from fluctuating excessively higher, and it is desirable to suppress the pH variation and stably adjust the pH to the desired pH range.

[0061] The inventors have studied neutralizing agents used in the preliminary neutralization treatment and found that the use of a specific neutralizing agent makes it possible to suppress the variation in pH and perform the neutralization treatment stably. Specifically, the method according to the present embodiment is characterized in that nickel-cobalt mixed hydroxide (MHP) is used as the neutralizing agent in the preliminary neutralization treatment. By using nickel-cobalt mixed hydroxide as the neutralizing agent in this way, it is possible to effectively remove free acid while suppressing the variation in pH, and it is possible to prevent the pH of the leaching slurry from fluctuating excessively high.

[0062] The preliminary neutralization treatment will be described more specifically. The preliminary neutralization treatment is performed, for example, using a free acid removal equipment. Fig. 2 is a diagram showing an example of the configuration of the free acid removal equipment. As described above, the free acid removal equipment is equipment for removing free acid in a leaching slurry obtained by high-pressure acid leaching of nickel oxide ore.

[0063] As shown in Fig. 2, the free acid removal equipment 1 includes two or more reaction tanks 11 for continuously treating the leaching slurry, an agent addition section 12 for adding a neutralizing agent to the leaching slurry to be treated, and a control section 13 for controlling the amount of neutralizing agent added via the agent addition section. Note that the preliminary neutralization treatment is not limited to a multi-stage treatment using two or more reaction tanks as shown in Fig. 2, and treatment may be performed in a single reaction tank.

[0064] [Reaction tank] The reaction tank 11 contains the leaching slurry obtained by the leaching treatment, i.e., a mixed slurry of the leaching solution and the leaching residue, and a preliminary neutralization treatment is performed based on pH adjustment. The free acid removal equipment 1 includes two or more reaction tanks 11 (11 (1) ,11 (2) ) are installed in series, and the neutralization treatment of the leaching slurry is carried out continuously in multiple stages.

[0065] Specifically, first, the first reactor 11, which is the reactor located at the most upstream and is treated first, (1)The leaching slurry is then neutralized by adding a neutralizing agent. (1) The leaching slurry after the treatment in the second reaction tank 11 is continuously provided. (2) The reactor 11 is then transferred to the (2) In the case where three or more reaction tanks are provided, the neutralization process is carried out in a continuous multi-stage manner in the same manner. In this specification, the nth reaction tank is referred to as "reaction tank 11". (n) In the configuration diagram shown in FIG. 2, the first reactor 11 is (1) (the upstream reactor) and the second reactor 11 (2) The diagram shows the configuration of the equipment, which consists of two tanks: the downstream reactor and the downstream reactor.

[0066] [Drug Addition Section] The chemical additive unit 12 adds a predetermined amount of neutralizing agent to the reaction tank 11 containing the leaching slurry. By adding the neutralizing agent to the leaching slurry via the chemical additive unit 12, the leaching slurry contained in the reaction tank 11 is neutralized.

[0067] The chemical addition section 12 includes two or more reaction vessels 11 (11 (1) ,11 (2) ) can be provided individually in each of the reaction vessels 11, and a predetermined amount of neutralizing agent can be added to the corresponding reaction vessel 11 via each chemical addition section 12.

[0068] In the method according to the present embodiment, as described above, nickel-cobalt mixed hydroxide is used as the neutralizing agent. In a free acid removal facility in which a plurality of reaction tanks 11 are continuously provided as shown in FIG. 2, at least the first reaction tank 11 located at the most upstream (1) In addition, nickel-cobalt mixed hydroxide (MHP) is added as a neutralizing agent A to the first reaction tank 11. (1) The second and subsequent reaction tanks 11 are provided in succession to the (2) , a neutralizer other than nickel-cobalt mixed hydroxide is added as neutralizer B.

[0069] Regarding the neutralizing agent, by using nickel-cobalt mixed hydroxide (MHP), which is the above-mentioned neutralizing agent A, the variation in pH of the leaching slurry can be suppressed, and excessively high fluctuations can be suppressed, and a stable neutralization treatment can be performed. In addition, nickel-cobalt mixed hydroxide can be produced through a known nickel-cobalt mixed hydroxide production process using a leaching slurry obtained by subjecting nickel oxide ore to leaching treatment as a raw material, and by using such nickel-cobalt mixed hydroxide as a neutralizing agent, efficient operation utilizing surplus intermediate raw materials becomes possible, and production efficiency can be improved while reducing the amount of new neutralizing agents used.

[0070] Furthermore, since nickel-cobalt mixed hydroxide contains nickel and cobalt, even if it is added as a neutralizing agent in the process of producing nickel-cobalt mixed sulfide, it does not become an impurity component and can be used as a nickel raw material, leading to an increase in the production volume of nickel-cobalt mixed sulfide.

[0071] The neutralizing agent B is not particularly limited, but is preferably a limestone slurry. The limestone slurry is an easy-to-handle and inexpensive neutralizing agent, and is particularly suitable for adjusting the pH of the leaching slurry to a range of about 2.8 to 3.2. When the limestone slurry is used as the neutralizing agent B, the concentration is not particularly limited, but is preferably 20% by mass or more and 35% by mass or less, and more preferably 25% by mass or more and 30% by mass or less. If the concentration of the limestone slurry is less than 20% by mass, the amount of the limestone slurry increases, and therefore the amount of the leaching slurry after adding the limestone slurry increases, that is, the amount of the process liquid to be treated increases, which is not preferable. On the other hand, if the concentration of the limestone slurry exceeds 35% by mass, the reactivity between the limestone slurry and the leaching slurry decreases, which is not preferable.

[0072] As described above, when performing preliminary neutralization treatment in a free acid removal facility in which a plurality of reaction tanks 11 are provided in series, at least the first reaction tank 11 located at the most upstream (1)Nickel-cobalt mixed hydroxide (MHP) was added as neutralizing agent A to the second and subsequent reaction tanks 11 (2) , and limestone slurry or the like is added as a neutralizing agent B. Specifically, the first reaction tank 11 (1) The neutralizing agent A, nickel-cobalt mixed hydroxide, is added so that the pH of the solution after neutralization in the reactor 11 located at the most downstream is 2.0 to 2.5. (2) The second and subsequent reaction tanks 11 are set so that the pH of the solution after neutralization is 2.8 to 3.2. (2) It is preferable to add neutralizing agent B to the mixture.

[0073] For example, when limestone slurry is used as the neutralizing agent B, the neutralization reaction of limestone is not so fast, so the second and subsequent reaction tanks 11 (2) If a large amount of limestone slurry is added to the thickener, foaming due to reaction will occur in the supernatant liquid of the thickener in the subsequent solid-liquid separation step S3, which is not preferable in terms of reducing turbidity. (1) By setting the pH after neutralization to 2.0 or more and 2.5 or less, the first reaction tank 11 can be (1) It is preferable to complete the neutralization reaction by

[0074] On the other hand, from the viewpoint of promoting precipitation of iron contained in the leaching slurry, it is preferable to adjust the pH of the leaching slurry to be subjected to solid-liquid separation to 2.8 to 3.2. (1) Nickel-cobalt mixed hydroxide was added to the second and subsequent reaction tanks 11 (2) By performing preliminary neutralization treatment by adding a neutralizing agent other than nickel-cobalt mixed hydroxide, such as limestone slurry, to the leaching slurry, it is possible to more effectively promote the precipitation of iron and suppress the variation in pH, thereby suppressing an increase in turbidity of the overflow liquid (leachate) recovered by solid-liquid separation of the leaching slurry.

[0075] The addition of the neutralizing agents A and B through the chemical addition section 12 is performed in the above-mentioned reaction tank 11 (11 (1) ,11 (2)) or may be added to a pipe or a gutter that introduces the leaching slurry into the reaction tank 11. Either mode of addition is included in the meaning of "adding to the reaction tank."

[0076] [Control Unit] The control unit 13 controls the addition of neutralizing agents A and B from the chemical addition unit 12 and the amount of the neutralizing agents added. (1) ,11 (2) ) and are connected so as to transmit electrical signals to the respective chemical addition units 12. Then, based on a control signal from the control unit 13, the amounts of neutralizing agents A and B added from the chemical addition unit 12 to the reaction tank 11 are controlled.

[0077] Each reaction tank 11 may be provided with a pH meter 14, which measures the pH of the leaching slurry in the reaction tank 11 over time and transmits a signal related to the measurement results to the control unit 13. Based on the pH measurement results, the control unit 13 performs feedback control of the amount of neutralizing agent added to each reaction tank 11 via the chemical addition unit 12. The control unit 13 may also perform a homogeneity variance test based on the pH measurement results and feedback control the amount of neutralizing agent added by measuring the variation in pH.

[0078] In the method according to the present embodiment, for example, the above-mentioned free acid removing equipment 1 is used to carry out the preliminary neutralization treatment. The method is characterized in that a nickel-cobalt mixed hydroxide is used as the neutralizing agent.

[0079] In this way, by performing the preliminary neutralization treatment using the nickel-cobalt mixed hydroxide as a neutralizing agent, the variation in pH of the leaching slurry can be suppressed, and the pH can be prevented from fluctuating excessively high, and the turbidity of the overflow liquid (leachate) recovered by solid-liquid separation of the leaching slurry can be suppressed. In addition, the nickel-cobalt mixed hydroxide can be produced by using the leaching slurry obtained by subjecting nickel oxide ore to leaching treatment as a raw material and through a known manufacturing process for nickel-cobalt mixed hydroxide. By using such a nickel-cobalt mixed hydroxide as a neutralizing agent, efficient operation using surplus intermediate raw materials is possible, and the amount of new neutralizing agents used can be reduced, thereby improving production efficiency. Furthermore, since the nickel-cobalt mixed hydroxide contains nickel and cobalt, it can be used as a nickel raw material, which can lead to an increase in the production volume of nickel-cobalt mixed sulfides.

[0080] In addition, when performing a continuous multi-stage neutralization treatment using two or more reactors arranged in series as shown in FIG. 2, at least the first reactor 11 located at the most upstream (1) Nickel-cobalt mixed hydroxide is added as neutralizing agent A to the first reaction tank 11. (1) The second and subsequent reaction tanks 11 are provided in succession to the (2) In the above, a neutralizing agent other than nickel-cobalt mixed hydroxide is added as neutralizing agent B. In this way, it is possible to more effectively promote the precipitation of iron, and also to suppress the variation in pH and the increase in turbidity of the overflow liquid (leachate). EXAMPLES

[0081] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0082] [Example 1] In the preliminary neutralization step in the hydrometallurgical process of nickel oxide ore (see FIG. 1), a preliminary neutralization treatment was carried out using nickel-cobalt mixed hydroxide (MHP) as a neutralizing agent. For the nickel-cobalt mixed hydroxide, a leaching slurry obtained by subjecting nickel oxide ore to a leaching treatment was used as the raw material, and surplus intermediate raw material generated from a known manufacturing process of nickel-cobalt mixed hydroxide was used. Table 1 below shows the analytical values ​​of the chemical composition of the nickel-cobalt mixed hydroxide used in the examples.

[0083] [Table 1]

[0084] The preliminary neutralization treatment was carried out using equipment in which two reaction tanks were arranged in series, as shown in Figure 2. In Example 1, the leaching slurry (pH 0.8) obtained through the leaching process was charged into the first reaction tank on the upstream side, and nickel-cobalt mixed hydroxide was added and dissolved in the reaction tank to carry out neutralization treatment. Note that 99.8% of the nickel was dissolved from the nickel-cobalt mixed hydroxide added as a neutralizing agent.

[0085] [Comparative Example 1] In Comparative Example 1, preliminary neutralization was performed using the same equipment as in Example 1, and limestone slurry was added to the first tank on the upstream side so that the pH of the solution after neutralization was 3.0, and then nickel-cobalt mixed hydroxide was added to the solution transferred from the first tank in the second tank and dissolved therein to perform neutralization. The rest of the procedure is the same as in Example 1. Note that 1.7% of nickel was dissolved from the nickel-cobalt mixed hydroxide added to the second reaction tank.

[0086] [evaluation] Table 2 below shows the analytical values ​​of the solution immediately after the nickel-cobalt mixed hydroxide was added and dissolved.

[0087] [Table 2]

[0088] As can be seen from the treatment results of Example 1 and Comparative Example 1, by adding nickel-cobalt mixed hydroxide as a neutralizing agent to the first reaction tank (pH 0.8) of the preliminary neutralization step and carrying out dissolution and neutralization, nickel and cobalt are effectively dissolved from the nickel-cobalt mixed hydroxide that is the surplus intermediate raw material, and it can be effectively used as a raw material for manufacturing nickel-cobalt mixed sulfide. This is expected to improve production volume and also reduce the amount of new chemicals used as neutralizing agents.

Claims

1. A method for hydrometallurgy of nickel oxide ore, comprising the steps of: producing nickel-cobalt mixed sulfides from a leaching slurry obtained by leaching nickel oxide ore, the method comprising the steps of: a leaching step of adding sulfuric acid to the nickel oxide ore to perform a leaching treatment; a preliminary neutralization step of neutralizing the leached slurry obtained by the leaching treatment by adding a neutralizing agent to the leached slurry to remove free acids contained in the leached slurry; In the preliminary neutralization step, nickel-cobalt mixed hydroxide is used as the neutralizing agent, In the preliminary neutralization step, a multi-stage neutralization process is continuously performed using two or more reaction tanks arranged in series, and the nickel-cobalt mixed hydroxide is added as a neutralizing agent A to at least the first reaction tank located at the most upstream, A neutralizer different from the nickel-cobalt mixed hydroxide is added as a neutralizer B to the second and subsequent reaction tanks that are connected to the first reaction tank, The neutralizing agent A is added so that the pH of the solution after neutralization in the first reaction tank is 2.0 or more and 2.5 or less; The neutralizing agent B is added to the second or subsequent reaction tanks so that the pH of the solution after neutralization in the reaction tank located at the most downstream is 2.8 to 3.

2. A hydrometallurgical process for nickel oxide ores.

2. The nickel-cobalt mixed hydroxide is produced through a production process using the leaching slurry as a raw material.

2. The method for hydrometallurgy of nickel oxide ore according to claim 1.

3. The neutralizing agent B is a limestone slurry; 2. The method for hydrometallurgy of nickel oxide ore according to claim 1.

4. The concentration of the free acid in the leaching slurry is 30 g / L to 60 g / L; 4. The method for hydrometallurgy of nickel oxide ore according to claim 1.

5. The leaching slurry contains nickel at a concentration of 5 g / L to 10 g / L and iron at a concentration of 3 g / L to 10 g / L; 5. A method for hydrometallurgy of nickel oxide ore according to claim 1.

6. The slurry concentration of the leaching slurry is 30% by mass to 50% by mass; 6. A method for hydrometallurgy of nickel oxide ore according to claim 1.

7. A method for hydrometallurgy of nickel oxide ore as described in any of claims 1 to 6, in which the pH or pH variation of the leaching slurry in the two or more reaction tanks is measured over time, and the amounts of neutralizing agent A and neutralizing agent B added to each of the two or more reaction tanks are feedback controlled based on the measurement results.

Citation Information

Patent Citations

  • Method for recovering nickel from acidic aqueous solution deriving from sulfuric acid

    JP2010180439A

  • Method for producing hematite for iron manufacture

    JP2013194283A

  • Wet smelting plant for nickel oxide ore and method of operating wet smelting plant

    JP2014173136A

  • Wet refining method of nickel oxide ore

    JP2016006233A

  • Apparatus and method for removing free acid, and method for producing nickel-and-cobalt-mixed sulfide