Active energy ray curable adhesive sheet and display device

The use of a diene copolymer with (meth)acrylate moieties in an active energy ray-curable adhesive sheet composition addresses high initial water vapor transmission and incomplete curing issues, ensuring low permeability and durability in display devices.

JP7585954B2Active Publication Date: 2024-11-19OJI HLDG CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021076769
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-28
Publication Date
2024-11-19
Estimated Expiration
2041-04-28

AI Technical Summary

Technical Problem

Conventional active energy ray-curable pressure-sensitive adhesive sheets have high initial water vapor transmission rates and insufficient water vapor permeability in areas not exposed to active energy rays due to incomplete curing.

Method used

Incorporating a diene copolymer with (meth)acrylate moieties at both ends and a specific (meth)acrylic polymer composition to achieve a water vapor transmission rate of 200 g/(m²·24hr) or less and an X1/X2 value of less than 1.5, ensuring low water vapor permeability before and after curing.

Benefits of technology

The adhesive sheet maintains low water vapor transmission rates before and after curing, even in areas not exposed to active energy rays, enhancing durability and reducing moisture-related damage in display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585954000001
    Figure 0007585954000001
Patent Text Reader

Abstract

To provide an active energy ray-curable adhesive sheet having low water vapor permeability, and a display device using the adhesive sheet.SOLUTION: The active energy ray-curable adhesive sheet of the present invention comprises a semi-cured product of an adhesive composition which contains at least a (meth)acrylic polymer, a photopolymerization initiator, and a diene copolymer having (meth)acrylate moieties at both terminals. When the water vapor permeability before curing with active energy rays is X1 and the water vapor permeability after curing with active energy rays is X2, X1 is 200 g / (m2 24 hr) or less and the value of X1 / X2 is less than 1.5.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an active energy ray-curable pressure-sensitive adhesive sheet and a display device. [Background technology]

[0002] Adhesive sheets are used, for example, for bonding components together, and are widely used in various fields. In recent years, such adhesive sheets have also been used for display devices such as liquid crystal displays (LCDs) and input devices such as touch panels. By using an adhesive sheet to bond each component of an optical display constituting a display device or an input device together, various devices can be manufactured easily and with high precision.

[0003] As an example of a pressure-sensitive adhesive sheet, an active energy ray-curable pressure-sensitive adhesive sheet is known (see, for example, Patent Document 1). Such an active energy ray-curable pressure-sensitive adhesive sheet has a property that the curing of the active energy ray-curable pressure-sensitive adhesive sheet progresses when irradiated with active energy rays (i.e., by post-curing). Therefore, when active energy rays are irradiated in a state in which adherends are bonded together with the active energy ray-curable pressure-sensitive adhesive sheet, the curing of the active energy ray-curable pressure-sensitive adhesive sheet progresses, and the adherends are bonded together more firmly. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2017 / 022770 Summary of the Invention [Problem to be solved by the invention]

[0005] However, although conventional active energy ray curable adhesive sheets often have a desired water vapor transmission rate after post-curing, there is a problem that the initial water vapor transmission rate, that is, the water vapor transmission rate before irradiation with active energy rays, is high.In addition, when a display device or the like equipped with an active energy ray curable adhesive sheet is irradiated with active energy rays to post-cure the adhesive sheet, if a bezel or the like of the display exists, the active energy rays do not hit the adhesive sheet at that part, so that the post-cure at that part is difficult to proceed, and as a result, the water vapor transmission rate at that part is insufficient, which may be a problem.From this point of view, it can be said that there is an urgent need to develop an active energy ray curable adhesive sheet with a low initial water vapor transmission rate.

[0006] The present invention has been made in view of the above, and an object of the present invention is to provide an active energy ray-curable pressure-sensitive adhesive sheet having low water vapor transmission rate, and a display device using the pressure-sensitive adhesive sheet. [Means for solving the problem]

[0007] As a result of extensive research into achieving the above-mentioned object, the inventors have discovered that the above-mentioned object can be achieved by using a diene-based copolymer having (meth)acrylate moieties at both ends, and have thus completed the present invention.

[0008] That is, the present invention includes, for example, the subject matter described in the following sections. Item 1 A semi-cured product of a pressure-sensitive adhesive composition including at least a (meth)acrylic polymer, a photopolymerization initiator, and a diene copolymer having (meth)acrylate moieties at both ends, When the water vapor transmission rate before curing with active energy rays is X1 and the water vapor transmission rate after curing with active energy rays is X2, X1 is 200g / (m 2 24 hours or less, An active energy ray-curable adhesive sheet having an X1 / X2 value of less than 1.5. Section 2 Item 2. The active energy ray-curable pressure-sensitive adhesive sheet according to item 1, wherein the pressure-sensitive adhesive composition contains less than 5 parts by mass of a monofunctional acrylic monomer having a molecular weight of less than 1000 per 100 parts by mass of the (meth)acrylic polymer. Section 3 Item 3. The active energy ray-curable pressure-sensitive adhesive sheet according to item 1 or 2, wherein the pressure-sensitive adhesive composition contains less than 5 parts by mass of a monofunctional acrylic monomer having an alkyl group having a linear or branched structure and a carbon number of 8 to 24 per 100 parts by mass of the (meth)acrylic polymer. Section 4 Item 4. The active energy ray-curable pressure-sensitive adhesive sheet according to any one of items 1 to 3, wherein the diene copolymer is a polymer having a 1,2 vinyl structure or a polymer having a structure in which a 1,2 vinyl structure has been hydrogenated. Section 5 The weight average molecular weight of the diene copolymer is 1,000 to 5,000; Item 5. The active energy ray-curable pressure-sensitive adhesive sheet according to any one of items 1 to 4, wherein the diene copolymer has a glass transition temperature of 0° C. or lower. Section 6 6. The active energy ray-curable pressure-sensitive adhesive sheet according to any one of items 1 to 5, wherein the pressure-sensitive adhesive composition contains 0.5 to 30 parts by mass of the diene copolymer relative to 100 parts by mass of the (meth)acrylic polymer. Section 7 Item 7. The active energy ray-curable pressure-sensitive adhesive sheet according to any one of items 1 to 6, which has a relative dielectric constant of 3.5 or less at 100 kHz after being cured with active energy rays. Section 8 Used for bonding components for liquid crystal or organic EL displays, Item 8. The active energy ray-curable pressure-sensitive adhesive sheet according to any one of items 1 to 7, wherein the member is glass, a polarizing plate, or a touch sensor. Section 9 Item 9. A display device comprising a post-cured product of the active energy ray-curable pressure-sensitive adhesive sheet according to any one of items 1 to 8 as a pressure-sensitive adhesive layer. Effect of the Invention

[0009] The active energy ray-curable pressure-sensitive adhesive sheet of the present invention has low water vapor permeability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "comprise" include the concepts of "containing", "comprises", "consists essentially of" and "consists only of".

[0011] 1. Active energy ray curable adhesive sheet The active energy ray-curable adhesive sheet of the present invention comprises a semi-cured product of an adhesive composition containing at least a (meth)acrylic polymer, a photopolymerization initiator, and a diene copolymer having (meth)acrylate moieties at both ends. The active energy ray-curable adhesive sheet of the present invention has a water vapor transmission rate of X1 before curing with active energy rays and X2 after curing with active energy rays, where X1 is 200 g / (m 2 ·24 hr) or less, and the value of X1 / X2 is less than 1.5. In this specification, curing an active energy ray-curable pressure-sensitive adhesive sheet with active energy rays is sometimes simply referred to as "post-curing".

[0012] The active energy ray-curable pressure-sensitive adhesive sheet of the present invention has a low water vapor transmission rate even in the initial stage (before post-curing). Therefore, when the active energy ray-curable pressure-sensitive adhesive sheet of the present invention is post-cured, the active energy ray-curable pressure-sensitive adhesive sheet of the present invention has a low water vapor transmission rate even in areas not exposed to the active energy ray, and as a result, the active energy ray-curable pressure-sensitive adhesive sheet of the present invention has a low water vapor transmission rate even after post-curing.

[0013] Hereinafter, the active energy ray-curable pressure-sensitive adhesive sheet of the present invention will be referred to simply as "pressure-sensitive adhesive sheet".

[0014] <(Meth)acrylic polymer> The type of (meth)acrylic polymer is not particularly limited, and can be the same as the (meth)acrylic polymer used for forming a known adhesive sheet. In particular, the (meth)acrylic polymer is preferably a polymer that undergoes crosslinking reaction by a crosslinking agent described below, that is, the (meth)acrylic polymer is preferably a polymer that has a crosslinkable functional group. Examples of the crosslinkable functional group include a carboxy group, a hydroxyl group, a glycidyl group, and an amino group.

[0015] An example of a (meth)acrylic polymer is a polymer containing (meth)acrylic ester units (a) and monomer units (b) having a carboxyl group and / or a hydroxyl group. "(Meth)acrylic" means "acrylic" or "methacrylic", "(meth)acrylate" means "acrylate" or "methacrylate", and "(meth)allyl" means "allyl" or "methallyl".

[0016] The term "unit" in the (meth)acrylic ester unit (a) and the monomer unit (b) having a carboxy group and / or a hydroxyl group means a repeating unit constituting a polymer.

[0017] The (meth)acrylic ester (a) is a repeating unit derived from a (meth)acrylic ester compound. Examples of the (meth)acrylic ester compound include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, and isodecyl (meth)acrylate. Among these, the (meth)acrylic ester compound is preferably a (meth)acrylic ester compound having a linear or branched alkyl group having 4 to 10 carbon atoms, preferably 4 to 8 carbon atoms. The (meth)acrylic ester compound is preferably free of a hydroxyl group and a carboxy group.

[0018] The (meth)acrylic polymer may contain one or more types of (meth)acrylic ester units (a).

[0019] The monomer unit (b) having a carboxy group is a repeating unit derived from a monomer having a carboxy group. The monomer having a carboxy group may be, for example, a wide variety of known polymerizable monomers containing a carboxy group, specifically, acrylic acid, methacrylic acid, etc.

[0020] The monomer unit (b) having a hydroxyl group is a repeating unit derived from a monomer having a hydroxyl group. For example, the monomer having a hydroxyl group can be a wide variety of known hydroxyl group-containing polymerizable monomers, and specifically, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, polyalkylene glycol mono (meth)acrylate, etc. can be mentioned.

[0021] The (meth)acrylic polymer may contain, as the monomer unit (b), both a monomer unit having a carboxy group and a monomer unit having a hydroxyl group, or may contain only one of them. When the monomer unit (b) contains both a monomer unit having a carboxy group and a monomer unit having a hydroxyl group, the content ratio of these is not particularly limited, and a desired PSA sheet can be obtained regardless of the content ratio.

[0022] In the (meth)acrylic polymer, the content ratio of the (meth)acrylic ester unit (a) and the monomer unit (b) is not particularly limited. For example, the (meth)acrylic polymer may contain 50% by mass or more of the (meth)acrylic ester unit (a) with respect to the total mass of the (meth)acrylic ester unit (a) and the monomer unit (b), preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. In addition, the content ratio of the (meth)acrylic ester unit (a) with respect to the total mass of the (meth)acrylic ester unit (a) and the monomer unit (b) is preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 98% by mass or less.

[0023] In the present invention, the content of each structural unit in the (meth)acrylic polymer can be considered to be equal to the amount of polymerizable monomer derived from the structural unit used when producing the (meth)acrylic polymer.

[0024] The (meth)acrylic polymer may contain other structural units other than the (meth)acrylic ester unit (a) and the monomer unit (b) as long as the effect of the present invention is not impaired. Examples of other structural units include a wide range of structural units derived from compounds that are copolymerizable with the (meth)acrylic ester compound. Specific examples of such compounds include (meth)acrylonitrile, vinyl acetate, styrene, vinyl chloride, vinylpyrrolidone, vinylpyridine, etc., and other examples include amino group-containing (meth)acrylic esters, glycidyl group-containing (meth)acrylic esters, and alkoxyalkyl group-containing (meth)acrylic esters.

[0025] The content ratio of the (meth)acrylic ester units (a) and the monomer units (b) relative to the total mass of all structural units of the (meth)acrylic polymer is preferably 90 mass% or more, more preferably 95 mass% or more, and even more preferably 99 mass% or more. The (meth)acrylic polymer may be composed only of the (meth)acrylic ester units (a) and the monomer units (b).

[0026] In the (meth)acrylic polymer, the order of arrangement of each constituent unit is not particularly limited, and for example, a random copolymer, a block copolymer, a graft copolymer, etc. can be formed. In terms of ease of production, a random copolymer is preferable.

[0027] The weight average molecular weight of the (meth)acrylic polymer is not particularly limited. For example, the weight average molecular weight of the (meth)acrylic polymer is preferably 100,000 to 2,000,000, and more preferably 200,000 to 1,500,000, in terms of the initial adhesive strength of the pressure-sensitive adhesive sheet being easily increased. The weight average molecular weight of the (meth)acrylic polymer means the value before crosslinking with a crosslinking agent described later. The weight average molecular weight of the (meth)acrylic polymer is measured by gel permeation chromatography (GPC) under the following conditions, and is a value calculated based on polystyrene standards. Solvent: Tetrahydrofuran Column: Shodex KF801, KF803L, KF800L, KF800D (4 columns made by Showa Denko Co., Ltd.) Column temperature: 40℃ Sample concentration: 0.5% by mass Detector: RI-2031plus (JASCO) Pump: RI-2080plus (JASCO) Flow rate (flow rate): 0.8ml / min Injection volume: 10μl In the GPC measurement, a calibration curve is prepared using 10 samples of standard polystyrene, Shodex standard polystyrene (manufactured by Showa Denko KK) with Mw=1,320 to 2,500,000.

[0028] The pressure-sensitive adhesive composition may contain only one type of (meth)acrylic polymer, or may contain two or more types of (meth)acrylic polymer.

[0029] The method for producing the (meth)acrylic polymer is not particularly limited, and for example, the (meth)acrylic polymer can be obtained by a production method utilizing a known polymerization method. The (meth)acrylic polymer can also be obtained from commercial products, etc.

[0030] <Diene copolymer having (meth)acrylate moieties at both ends> A diene copolymer having (meth)acrylate moieties at both ends (hereinafter simply referred to as "diene copolymer") is a polymer whose polymer backbone is a diene polymer and has (meth)acrylate moieties at both ends. The (meth)acrylate moiety is, for example, a monovalent group represented by "CH2=C(CH3)COO-". It should be noted that the diene copolymer is a polymer other than a (meth)acrylic polymer, just to be sure.

[0031] The pressure-sensitive adhesive sheet of the present invention contains a diene copolymer, which reduces the water vapor transmission rate before irradiation with active energy rays (before post-curing) and also improves the step conformability. In addition, the diene copolymer tends to provide the pressure-sensitive adhesive sheet with a low dielectric constant.

[0032] The diene copolymer is preferably a polymer having a 1,2 vinyl structure or a polymer having a hydrogenated 1,2 vinyl structure. In this case, the water vapor permeability of the pressure-sensitive adhesive sheet before post-curing is likely to be lower, and the step conformability is particularly likely to be improved. The 1,2 vinyl structure is, for example, a monovalent group represented by CH2=CH-, and the hydrogenated 1,2 vinyl structure is, for example, a monovalent group represented by CH3-CH2-. When the diene copolymer is a polymer having a 1,2 vinyl structure or a polymer having a hydrogenated 1,2 vinyl structure, these structures can be, for example, in the side chain of the diene copolymer.

[0033] In particular, the diene copolymer preferably has a polybutadiene polymer skeleton with the (meth)acrylate moieties at both ends, which makes it easier to particularly reduce the water vapor transmission rate of the pressure-sensitive adhesive sheet before post-curing, particularly improve the step conformability, and also makes it possible to further reduce the relative dielectric constant of the pressure-sensitive adhesive sheet.

[0034] The (meth)acrylate moieties at both ends may be directly bonded to the diene polymer backbone, or may be indirectly bonded via another moiety. When the (meth)acrylate moiety is indirectly bonded via another moiety, it may be bonded to the diene polymer via a urethane bond, for example. The (meth)acrylate moieties at both ends may be the same or different.

[0035] The weight average molecular weight of the diene copolymer is not particularly limited, and can be, for example, 1000 to 5000. This makes it easier for the pressure-sensitive adhesive sheet to have a low water vapor transmission rate before post-curing, and to have improved conformability to unevenness. The weight average molecular weight of the diene copolymer is measured by gel permeation chromatography (GPC) under the following conditions, and is a value calculated based on polystyrene standards, and is the same as the weight average molecular weight of the (meth)acrylic polymer.

[0036] The glass transition temperature of the diene copolymer is not particularly limited, and is preferably, for example, 0° C. or lower. This makes it easier for the pressure-sensitive adhesive sheet to have a lower water vapor transmission rate before post-curing, and to have improved conformability to uneven surfaces. The glass transition temperature of the diene copolymer can be measured by a differential scanning calorimeter (DSC).

[0037] The viscosity of the diene copolymer is preferably, for example, 1,000 to 500,000 mPa·s / 45° C. In this case, the initial adhesive strength of the pressure-sensitive adhesive sheet is likely to be increased, the step-following ability is particularly likely to be improved, and the relative dielectric constant of the pressure-sensitive adhesive sheet can also be reduced. The viscosity here refers to a value measured with a B-type viscometer (RB-80L manufactured by TOKI).

[0038] The pressure-sensitive adhesive composition may contain only one type of diene copolymer, or may contain two or more types of diene copolymers.

[0039] The method for producing the diene copolymer is not particularly limited, and for example, the diene copolymer can be obtained by a production method using a known polymerization method. The diene copolymer can be obtained from commercial products, such as the TE series manufactured by Nippon Soda Co., Ltd.

[0040] In the pressure-sensitive adhesive composition, the content of the diene copolymer is not particularly limited. For example, the pressure-sensitive adhesive composition preferably contains 0.5 to 30 parts by mass of the diene copolymer relative to 100 parts by mass of the (meth)acrylic polymer. In this case, the water vapor transmission rate of the pressure-sensitive adhesive sheet before post-curing is likely to be lower, the step conformability is likely to be improved, and the relative dielectric constant of the pressure-sensitive adhesive sheet can be lowered. The pressure-sensitive adhesive composition more preferably contains 1 part by mass or more of the diene copolymer relative to 100 parts by mass of the (meth)acrylic polymer, even more preferably contains 2 parts by mass or more, particularly preferably contains 4 parts by mass or more, and more preferably contains 20 parts by mass or less, even more preferably contains 18 parts by mass or less, and particularly preferably contains 16 parts by mass or less.

[0041] <Photopolymerization initiator> The photopolymerization initiator is a component that plays a role of initiating, for example, the polymerization reaction of the diene copolymer by irradiation with active energy rays (i.e., post-curing). In the present invention, the term "active energy rays" refers to electromagnetic waves or charged particle rays that have an energy quantum, and examples of such rays include ultraviolet rays, electron beams, visible light, X-rays, and ion beams. Among these, ultraviolet rays or electron beams are preferred from the viewpoint of versatility, and ultraviolet rays are particularly preferred.

[0042] The type of photopolymerization initiator is not particularly limited, and may be a wide variety of known photopolymerization initiators, such as acetophenone-based initiators, benzoin ether-based initiators, benzophenone-based initiators, hydroxyalkylphenone-based initiators, thioxanthone-based initiators, and amine-based initiators.

[0043] Specific examples of acetophenone initiators include diethoxyacetophenone and benzyl dimethyl ketal. Specific examples of benzoin ether initiators include benzoin and benzoin methyl ether. Specific examples of benzophenone initiators include benzophenone, o-benzoyl methyl benzoate, 2,4,6-trimethylbenzophenone mesityl (phenyl) ketone, 4-methylbenzophenone, and the like, and may be a mixture of 2,4,6-trimethylbenzophenone mesityl (phenyl) ketone and 4-methylbenzophenone. Specific examples of hydroxyalkylphenone initiators include 1-hydroxy-cyclohexyl-phenyl-ketone. Specific examples of thioxanthone initiators include 2-isopropylthioxanthone and 2,4-dimethylthioxanthone. Specific examples of amine initiators include triethanolamine and 4-dimethylbenzoic acid ethyl.

[0044] The photopolymerization initiator contained in the pressure-sensitive adhesive composition may be one type alone or two or more types. The photopolymerization initiator may be available, for example, as a commercially available product.

[0045] In the pressure-sensitive adhesive composition, the content of the photopolymerization initiator is not particularly limited and is appropriately selected depending on the type and content of the diene copolymer, the amount of active energy radiation applied during semi-curing or post-curing, etc. For example, the pressure-sensitive adhesive composition may contain 0.05 to 10 parts by mass, and preferably 0.1 to 5 parts by mass, of the photopolymerization initiator relative to 100 mass of the (meth)acrylic polymer.

[0046] <Adhesive composition> The pressure-sensitive adhesive composition may contain a crosslinking agent in addition to the (meth)acrylic polymer, diene copolymer, and photopolymerization initiator.

[0047] The crosslinking agent is, for example, a compound that has the property of reacting with the (meth)acrylic polymer by heat. Examples of the crosslinking agent include an isocyanate compound, an epoxy compound, an oxazoline compound, an aziridine compound, a metal chelate compound, and a butylated melamine compound. In terms of high reactivity with the (meth)acrylic polymer, it is preferable to use an isocyanate compound or an epoxy compound as the crosslinking agent. When the crosslinking agent contains a metal chelate, it is also preferable to use, for example, a known crosslinking retarder in combination.

[0048] Examples of the isocyanate compound include tolylene diisocyanate, xylylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, etc. Examples of the epoxy compound include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerin diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, tetraglycidyl xylene diamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, trimethylolpropane polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitol polyglycidyl ether, etc.

[0049] The crosslinking agent contained in the pressure-sensitive adhesive composition may be one type alone or two or more types. The crosslinking agent may be, for example, commercially available.

[0050] In the pressure-sensitive adhesive composition, the content of the crosslinking agent is not particularly limited, and may be, for example, 0.01 to 5 parts by mass per 100 parts by mass of the total mass of the (meth)acrylic polymer. In this case, the processability of the obtained pressure-sensitive adhesive sheet is likely to be improved. The content of the crosslinking agent may be 0.05 to 3 parts by mass per 100 parts by mass of the total mass of the crosslinkable (meth)acrylic copolymer.

[0051] The pressure-sensitive adhesive composition may also contain a silane coupling agent. The type of silane coupling agent is not particularly limited, and for example, a wide variety of known compounds may be used. Examples of silane coupling agents include γ-acryloxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyldialkoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-glycidoxypropyltriakoxysilane, γ-methacryloxypropyltrialkoxysilane, γ-chloropropyltrialkoxysilane, γ-methacryloxypropyldialkoxysilane, γ-mercaptopropyltrialkoxysilane, and vinyltrialkoxysilane. The silane coupling agent may also be an oligomer of various alkoxysiloxanes. All of these silane coupling agents can be obtained from commercial products.

[0052] When the pressure-sensitive adhesive composition contains a silane coupling agent, the content ratio thereof can be 0.1 to 5 parts by mass per 100 parts by mass of the (meth)acrylic polymer. The silane coupling agent may be used alone or in combination of two or more kinds.

[0053] The adhesive composition may contain a solvent from the viewpoint of improving the coating property. Examples of the solvent include hydrocarbons such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; halogenated hydrocarbons such as dichloromethane, trichloroethane, trichloroethylene, tetrachloroethylene, and dichloropropane; alcohols such as methanol, ethanol, propanol, isopropyl alcohol, butanol, isobutyl alcohol, and diacetone alcohol; ethers such as diethyl ether, diisopropyl ether, dioxane, and tetrahydrofuran; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, isophorone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, amyl acetate, and ethyl butyrate; polyols and derivatives thereof such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monomethyl ether acetate.

[0054] When the pressure-sensitive adhesive composition contains a solvent, the content is not particularly limited, and can be, for example, 25 to 500 parts by mass, and more preferably 30 to 400 parts by mass, relative to 100 parts by mass of the (meth)acrylic polymer. The content of the solvent is preferably 10 to 90% by mass, and more preferably 20 to 80% by mass, relative to the total mass of the pressure-sensitive adhesive composition. The solvent may be used alone or in combination of two or more types, and when two or more types are used in combination, the total mass is preferably within the above range.

[0055] The adhesive composition may contain various additives for adhesives other than those described above, as long as they do not impair the effects of the present invention. Such additives may be selected as necessary from, for example, plasticizers, antioxidants, metal corrosion inhibitors, tackifiers, ultraviolet absorbers, light stabilizers such as hindered amine compounds, etc. In addition, dyes and pigments may be added for the purpose of coloring.

[0056] Other components contained in the pressure-sensitive adhesive composition include a polymerizable monomer. Examples of the polymerizable monomer include a polyfunctional polymerizable monomer and a monofunctional monomer. Hereinafter, the polymerizable monomer is referred to as a "polymerizable monomer M". As a precautionary note, the polymerizable monomer M means a component other than the diene copolymer. The type of the polymerizable monomer M is not particularly limited, and examples thereof include a wide range of known polyfunctional polymerizable monomers and monofunctional monomers used to manufacture pressure-sensitive adhesive sheets.

[0057] However, in the present invention, as described above, the pressure-sensitive adhesive composition is preferably free of a specific polymerizable monomer described below, in that the water vapor transmission rate of the pressure-sensitive adhesive sheet before post-curing is likely to be lower, and even if the specific polymerizable monomer is included, it is preferable that the amount of the specific polymerizable monomer used is small. Specifically, the specific polymerizable monomer referred to here is a monofunctional acrylic monomer having a molecular weight of less than 1000, and even if it is included, the content is preferably less than 5 parts by mass, more preferably 1 part by mass or less, even more preferably 0.1 parts by mass or less, and particularly preferably 0.05 parts by mass or less per 100 parts by mass of the (meth)acrylic polymer. It is particularly preferable that the pressure-sensitive adhesive composition does not include a monofunctional acrylic monomer having a molecular weight of less than 1000.

[0058] Other examples of the specific polymerizable monomer include monofunctional acrylic monomers having an alkyl group having a straight or branched structure with 8 to 24 carbon atoms, and even if such monomers are contained, the content thereof is preferably less than 5 parts by mass, more preferably 1 part by mass or less, further preferably 0.1 part by mass or less, and particularly preferably 0.05 part by mass or less, per 100 parts by mass of the (meth)acrylic polymer. It is particularly preferable that the pressure-sensitive adhesive composition does not contain a monofunctional acrylic monomer having an alkyl group having a straight or branched structure with 8 to 24 carbon atoms.

[0059] It is also preferable that the pressure-sensitive adhesive composition does not contain both a monofunctional acrylic monomer having a molecular weight of less than 1000 and a monofunctional acrylic monomer having an alkyl group having a linear or branched structure and having 8 to 24 carbon atoms.

[0060] Therefore, when the pressure-sensitive adhesive composition contains a polymerizable monomer M, it is most preferable that such polymerizable monomer M does not include a monofunctional acrylic monomer having a molecular weight of less than 1000 and a monofunctional acrylic monomer having an alkyl group having a linear or branched structure and a carbon number of 8 to 24. When the polymerizable monomer M is other than a monofunctional acrylic monomer having a molecular weight of less than 1000 and a monofunctional acrylic monomer having an alkyl group having a linear or branched structure and a carbon number of 8 to 24, the content thereof is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the (meth)acrylic polymer. It is also preferable that the pressure-sensitive adhesive composition does not contain a polymerizable monomer M.

[0061] The method for preparing the adhesive composition is not particularly limited. For example, the adhesive composition can be prepared by mixing a (meth)acrylic polymer synthesized in advance, a photopolymerization initiator, a diene copolymer having (meth)acrylate moieties at both ends, and other components (for example, a crosslinking agent, a silane coupling agent, a solvent, etc.) that are included as needed in a predetermined ratio. In this case, the (meth)acrylic polymer can be used in the state of a solution or dispersion. When the (meth)acrylic polymer is in the form of a solution or dispersion, the solution or dispersion can contain the solvent. The solution or dispersion of the (meth)acrylic polymer having a functional group can have a solid content concentration of, for example, 1 to 50 mass%.

[0062] <Adhesive sheet> The pressure-sensitive adhesive sheet of the present invention includes a layer-like semi-cured product formed from the pressure-sensitive adhesive composition. Such a semi-cured product also functions as a pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet.

[0063] The semi-cured product contains at least a cured product of a (meth)acrylic polymer, the photopolymerization initiator, and the diene-based copolymer (a diene-based copolymer having (meth)acrylate moieties at both ends). The cured product of a (meth)acrylic polymer is, for example, a crosslinked polymer produced by a reaction between the (meth)acrylic polymer and the crosslinking agent. However, the semi-cured product may contain unreacted (meth)acrylic polymer and crosslinking agent. The method for forming the semi-cured product will be described later in <Method for producing pressure-sensitive adhesive sheet>.

[0064] The pressure-sensitive adhesive sheet of the present invention may be formed only from the semi-cured product, or may have a layer other than the semi-cured product. Hereinafter, the semi-cured product may be referred to as the "pressure-sensitive adhesive layer".

[0065] The structure of the adhesive sheet is not particularly limited as long as it has the adhesive layer. The adhesive sheet may be a single-sided adhesive sheet or a double-sided adhesive sheet. When the adhesive sheet is a single-sided adhesive sheet, a multi-layer sheet in which a semi-cured product (adhesive layer) is laminated on a support may be used. In addition, another layer may be provided between the support and the adhesive layer. When the adhesive sheet is a double-sided adhesive sheet, a single-layer adhesive sheet made of a semi-cured product (adhesive layer), a multi-layer adhesive sheet in which a plurality of adhesive layers are laminated, a multi-layer adhesive sheet in which another adhesive layer is laminated between the adhesive layers, and a multi-layer adhesive sheet in which a support is laminated between the adhesive layers may be used. When the double-sided adhesive sheet has a support, a support using a transparent support is preferable. Such a double-sided adhesive sheet is excellent in transparency as the adhesive sheet as a whole, and can be suitably used for bonding optical members to each other.

[0066] Examples of the support include plastic films such as polystyrene, styrene-acrylic copolymers, acrylic resins, polyethylene terephthalate, polycarbonate, polyether ether ketone, and triacetyl cellulose; and optical films such as antireflection films and electromagnetic wave shielding films.

[0067] The adhesive layer may be covered with a release sheet, in which case an adhesive sheet with a release sheet is provided. Thus, an adhesive sheet with a release sheet can be formed using the adhesive sheet of the present invention. The release sheet can be a peelable laminated sheet having a release sheet substrate and a release agent layer provided on one side of the release sheet substrate, or a polyolefin film such as a polyethylene film or a polypropylene film as a low polar substrate. Paper or a polymer film is used as the release sheet substrate in the peelable laminated sheet.

[0068] As the release agent constituting the release agent layer, for example, a general-purpose addition type or condensation type silicone-based release agent or a compound containing a long-chain alkyl group is used. In particular, an addition type silicone-based release agent having high reactivity is preferably used. Specific examples of the silicone-based release agent include BY24-4527 and SD-7220 manufactured by Toray Dow Corning Silicone Co., Ltd., and KS-3600, KS-774, and X62-2600 manufactured by Shin-Etsu Chemical Co., Ltd. In addition, the silicone-based release agent may contain SiO2 units and (CH3)3SiO 1 / 2 Unit or CH2=CH(CH3)SiO 1 / 2 It is preferable that the silicone resin contains a silicone resin, which is an organosilicon compound having a unit. Specific examples of the silicone resin include BY24-843, SD-7292, SHR-1404, etc. manufactured by Dow Corning Toray Silicone Co., Ltd., and KS-3800, X92-183, etc. manufactured by Shin-Etsu Chemical Co., Ltd.

[0069] When the pressure-sensitive adhesive layer has release sheets on both sides, the release sheets may have different releasability. When the releasability from one side differs from the releasability from the other side, it becomes easy to first peel off only the release sheet with the higher releasability.

[0070] The thickness of the pressure-sensitive adhesive layer is not particularly limited since it can be appropriately set according to the application. For example, the thickness of the pressure-sensitive adhesive layer is preferably 10 to 1000 μm, more preferably 20 to 500 μm, and even more preferably 100 to 400 μm. In particular, the thickness of the pressure-sensitive adhesive layer means the total thickness of each layer when the pressure-sensitive adhesive layer has a multi-layer laminate structure.

[0071] In a pressure-sensitive adhesive sheet, when the water vapor transmission rate before curing with active energy rays is X1 and the water vapor transmission rate after curing with active energy rays is X2, X1 is 200 g / (m 2 1.24 hr) or less, and the value of X1 / X2 is less than 1.5. In this specification, the water vapor transmission rate of the pressure-sensitive adhesive sheet means the water vapor transmission rate when the pressure-sensitive adhesive sheet has a thickness of 100 μm.

[0072] X1 is 200g / (m 2 Since the X1 / X2 value is less than 1.5, the pressure-sensitive adhesive sheet of the present invention has low water vapor transmission rate even before post-curing.

[0073] Here, in the "curing by active energy rays" for measuring X2, the irradiation conditions of active energy rays are 120 mW / cm at a wavelength of 355 nm. 2 The illuminance is 3000mJ / cm 2 The illuminance meter used is the UV-PFA1 manufactured by iGraphics. Under these irradiation conditions, an iGraphics ECS-4011GX / N UV irradiator is used, to which a high pressure mercury lamp H04-L41 and a heat ray cut filter are attached. Hereafter, this irradiation condition is referred to as "irradiation condition A".

[0074] X1 is 195g / (m 2 24hr) or less, and 190g / (m 2.24 hr) or less. The value of X1 / X2 is preferably 1.4 or less, more preferably 1.3 or less, and even more preferably 1.2 or less. The lower limit of X1 / X2 is 1, for example.

[0075] The pressure-sensitive adhesive sheet contains at least a crosslinked structure of a (meth)acrylic polymer, the photopolymerization initiator, and the diene-based copolymer. In particular, by containing the diene-based copolymer, the value of X1 becomes small, and the value of X1 / X2 can also be small.

[0076] Therefore, even if there is a portion of the pressure-sensitive adhesive sheet that is not exposed to active energy rays when the pressure-sensitive adhesive sheet is post-cured, the water vapor transmission rate of that portion is also sufficiently low, and the post-cured portion can exhibit water vapor transmission rate, and as a result, the pressure-sensitive adhesive sheet can have a low water vapor transmission rate. This makes it possible to suppress damage to the device caused by water vapor when the pressure-sensitive adhesive sheet is applied to an electronic device such as a display device (e.g., an organic electroluminescence (EL) light-emitting device).

[0077] When the pressure-sensitive adhesive sheet does not contain the above-mentioned monofunctional acrylic monomer having a molecular weight of less than 1000 and / or the monofunctional acrylic monomer having an alkyl group having a linear or branched structure with a carbon number of 8 to 24, the value of X1 is particularly small, that is, the water vapor transmission rate is likely to be low. Although not intended to be a restrictive interpretation, when the pressure-sensitive adhesive sheet contains these monofunctional acrylic monomers, the monomers bring about a kind of plasticizing effect, so that if there is a part of the pressure-sensitive adhesive sheet that is not hit by active energy rays when the pressure-sensitive adhesive sheet is post-cured, the plasticizing effect of the monofunctional acrylic monomer acts on this part. It is presumed that this causes the water vapor transmission rate of the part to increase.

[0078] The pressure-sensitive adhesive sheet has a relative dielectric constant of, for example, 3.5 or less at 100 kHz after curing under the irradiation condition A. Since the pressure-sensitive adhesive sheet has such a low relative dielectric constant, the pressure-sensitive adhesive sheet of the present invention is suitable for use in various applications such as liquid crystal or organic EL display devices, and in particular makes it easier to prevent malfunction of touch sensors in mobile terminals.

[0079] The dielectric constant of the pressure-sensitive adhesive sheet after curing with active energy rays can be controlled, for example, by adjusting the type and content of the diene copolymer. The dielectric constant of the pressure-sensitive adhesive sheet after curing with active energy rays is a value measured at a frequency of 100 KHz under an environment of 23°C and 50% RH, and is calculated by the method specified in JIS C 2138.

[0080] The gel fraction of the pressure-sensitive adhesive sheet is not particularly limited. The gel fraction of the pressure-sensitive adhesive sheet (before irradiation under the irradiation condition A) is, for example, 35% or more, preferably 40% or more, more preferably 45% or more, particularly preferably 50% or more, with an upper limit of, for example, 70%. The gel fraction of the pressure-sensitive adhesive sheet after curing under the irradiation condition A is, for example, 55% or more, preferably 60% or more, more preferably 65% ​​or more, particularly preferably 70% or more, with an upper limit of, for example, 95%.

[0081] The gel fraction is a value measured by the following method. First, about 0.1 g of the adhesive sheet is placed in a sample bottle, 30 ml of ethyl acetate is added, and the mixture is shaken for 24 hours. The contents of the sample bottle are then filtered through a 150 mesh stainless steel wire screen, and the residue on the screen is dried at 100°C for 1 hour to measure the dry mass (g). The gel fraction is calculated from the obtained dry mass using the following formula 1. Gel fraction (mass%) = (dry mass / collected mass of adhesive sheet) × 100 Equation 1

[0082] The haze of the pressure-sensitive adhesive sheet of the present invention is not particularly limited. For example, the haze of the pressure-sensitive adhesive sheet of the present invention after storage in a dry environment at 85° C. for 10 days and after storage in an environment at 60° C. and a relative humidity of 95% for 10 days is 1% or less, preferably 0.5% or less.

[0083] The pressure-sensitive adhesive sheet of the present invention has a haze of 1% or less, preferably 0.5% or less, after a durability test by exposure to ultraviolet light. The durability test by exposure to ultraviolet light is performed by subjecting the pressure-sensitive adhesive sheet to an environment of 60° C. and 0.63 mW / cm 2 The specimens are then exposed to light at an illumination intensity of 1000 x 1000 for four hours, and then stored under condensation at 50°C for four hours. This process is repeated a total of 12 times.

[0084] The total light transmittance of the pressure-sensitive adhesive sheet of the present invention is not particularly limited. For example, the total light transmittance (measured according to JIS K 7361-1:1997) of the pressure-sensitive adhesive sheet of the present invention after storing it in an environment of 85°C for 10 days and after storing it in an environment of 60°C and 95% relative humidity for 10 days is 85% or more, preferably 90% or more. In addition, the total light transmittance of the pressure-sensitive adhesive sheet of the present invention after the durability test by exposure to ultraviolet light described above is 85% or more, preferably 90% or more.

[0085] The pressure-sensitive adhesive sheet of the present invention * The value is not particularly limited. For example, the b value after storing the pressure-sensitive adhesive sheet of the present invention in an environment at 85° C. for 10 days and in an environment at 60° C. and a relative humidity of 95% for 10 days is * The value is 1 or less, preferably 0.5 or less. In addition, the adhesive sheet of the present invention is subjected to the durability test by exposure to ultraviolet light as described above. * The values ​​are all equal to or less than 1, and preferably equal to or less than 0.5.

[0086] The pressure-sensitive adhesive sheet of the present invention has the above-mentioned optical properties (haze, total light transmittance, b * value), the pressure-sensitive adhesive sheet can satisfy the transparency required when used for optical components, and also has excellent resistance to clouding due to humidity, making it suitable for optical applications.

[0087] 2. Manufacturing method of adhesive sheet The method for producing the pressure-sensitive adhesive sheet of the present invention is not particularly limited, and for example, a known method for producing an active energy ray-curable pressure-sensitive adhesive sheet can be widely adopted. For example, the pressure-sensitive adhesive sheet of the present invention can be obtained by a production method including a step of applying a pressure-sensitive adhesive composition to form a coating film, and a step of curing the coating film to form a semi-cured product.

[0088] The method of forming the coating film of the pressure-sensitive adhesive composition is not particularly limited, and for example, a known coating method can be widely adopted. For example, a coating film can be formed using a commercially available coating device such as a blade coater, an air knife coater, a roll coater, a bar coater, a gravure coater, a microgravure coater, a rod blade coater, a lip coater, a die coater, or a curtain coater. The amount of the pressure-sensitive adhesive composition applied is not particularly limited, and can be appropriately set according to the thickness of the pressure-sensitive adhesive layer of the target pressure-sensitive adhesive sheet. The coating film can be formed on a suitable substrate, and for example, the coating film can be formed on a release sheet.

[0089] The method of curing the coating film to form a semi-cured product is not particularly limited. In the present invention, it is preferable to form a semi-cured product by heating the coating film. The heating conditions are not particularly limited, and the coating film can be heated, for example, under conditions of 50°C or higher and 150°C or lower. The heating time can be appropriately set according to the heating temperature and the target residual solvent concentration of the pressure-sensitive adhesive layer, and can be, for example, 1 to 30 minutes. The heating treatment can be performed using a known heating device such as a heating furnace or an infrared lamp. After the heating treatment, the semi-cured product can be subjected to aging treatment under a predetermined environment as necessary.

[0090] The semi-cured product obtained as described above becomes the adhesive layer in the adhesive sheet. When the adhesive composition contains a volatile matter such as a solvent, it volatilizes during the process of forming the semi-cured product. As described above, the semi-cured product contains at least the crosslinked polymer generated by the reaction of the (meth)acrylic polymer with the crosslinking agent, the photopolymerization initiator, and the diene copolymer (a diene copolymer having (meth)acrylate moieties at both ends). However, the semi-cured product may contain unreacted (meth)acrylic polymer and crosslinking agent. In addition, the photopolymerization initiator and the diene copolymer may be consumed during the process of forming the semi-cured product. The photopolymerization initiator and the diene copolymer remaining in the semi-cured product are preferably 95% by mass or more, and more preferably 99% by mass or more, based on the photopolymerization initiator and the diene copolymer contained in the adhesive composition.

[0091] As described above, a semi-cured product (adhesive layer) is formed, and the adhesive sheet of the present invention can be obtained. If necessary, one or both sides of the semi-cured product (adhesive layer) can be protected with a release sheet or the like, and for example, the adhesive sheet with the release sheet described above is provided.

[0092] (How to use the adhesive sheet) The pressure-sensitive adhesive sheet of the present invention contains the photopolymerization initiator and the diene copolymer in a semi-cured product, and therefore has active energy ray curability. Therefore, the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet can be brought into contact with the surface of an adherend, and in this state, the pressure-sensitive adhesive layer can be post-cured, particularly completely cured, by irradiating the surface with active energy rays, thereby more firmly adhering to the adherend.

[0093] The active energy ray used for post-curing is not particularly limited, and from the viewpoint of versatility, ultraviolet rays or electron beams are preferred, and ultraviolet rays are particularly preferred. As the source of ultraviolet rays, for example, high pressure mercury lamps, low pressure mercury lamps, ultra-high pressure mercury lamps, metal halide lamps, carbon arcs, xenon arcs, electrodeless ultraviolet lamps, etc. can be used. As the electron beam, for example, electron beams emitted from various electron beam accelerators such as Cockcroft-Walt type, Van de Kraff type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type can be used.

[0094] The irradiation conditions of the active energy rays are not particularly limited and can be appropriately set depending on the wavelength. For example, the irradiation output of the ultraviolet rays is 100 mJ / cm2 in terms of the integrated light amount. 2 More than 10000mJ / cm 2 It is preferable to set the dose to 500 mJ / cm or less. 2 More than 5000mJ / cm 2 It is more preferable to have the following:

[0095] Since the adhesive layer of the adhesive sheet is in a semi-cured state, even if the adherend has steps, the adhesive layer can conform to the unevenness before being irradiated with active energy rays. In this way, by laminating the adhesive sheet and allowing it to conform to the unevenness, and then completely curing the adhesive layer with active energy rays, the cohesive force of the adhesive layer is increased, and the adhesiveness to the adherend is improved.

[0096] By using the pressure-sensitive adhesive sheet as described above, a laminate can be obtained in which the adherend and the post-cured pressure-sensitive adhesive sheet are laminated together. Thus, the laminate contains the post-cured product of the active energy ray-curable pressure-sensitive adhesive sheet as a pressure-sensitive adhesive layer.

[0097] The type of the adherend in the laminate is not particularly limited, and may be, for example, various optical members. Examples of the optical members include components of optical products such as touch panels and image display devices, and specifically, liquid crystal or organic EL display members. Examples of the liquid crystal or organic EL display members include glass, polarizing plates, and touch sensors.

[0098] The pressure-sensitive adhesive sheet of the present invention is preferably used for bonding liquid crystal or organic EL display members, because the water vapor transmission rate before irradiation with active energy rays is low, and even if there are areas not exposed to active energy rays, the water vapor transmission rate of the areas is low, and it is also possible to adjust the dielectric constant to a low level. Since the pressure-sensitive adhesive sheet can form an adhesive layer with a low water vapor transmission rate, when applied to electronic devices such as display devices, damage to the devices caused by water vapor can be suppressed. Therefore, display devices and the like are suitable as the laminate.

[0099] The pressure-sensitive adhesive sheet of the present invention can be used for liquid crystal or organic EL displays as described above, as well as for various other applications requiring a pressure-sensitive adhesive sheet. EXAMPLES

[0100] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.

[0101] (Production Example 1) 2-Ethylhexyl methacrylate (2-EHMA), 2-ethylhexyl acrylate (2-EHA), and 2-hydroxyethyl methacrylate (2-HEMA) were mixed in a mass ratio of 70:20:10, and 2,2'-azobis(2,4-dimethylvaleronitrile) was dissolved in the solution as a radical polymerization initiator. The solution was heated to 60°C for random copolymerization, resulting in a (meth)acrylic polymer with a weight average molecular weight (Mw) of 450,000 and a glass transition temperature (Tg) of -20°C.

[0102] (Components of Pressure-Sensitive Adhesive Composition) The components contained in the pressure-sensitive adhesive compositions used in the Examples and Comparative Examples were as follows. <(Meth)acrylic polymer> The (meth)acrylic polymer used was the (meth)acrylic polymer obtained in Production Example 1.

[0103] <Diene copolymer> The diene copolymer used was one of the following two types: ·“TEAI-1000” manufactured by Nippon Soda (Mw1000, Tg-14℃) Nippon Soda Co., Ltd. "TE-2000" (Mw2000, Tg-9℃)

[0104] <Crosslinking agent> The crosslinking agent used was a xylylene diisocyanate compound ("D-110N" manufactured by Mitsui Chemicals, Inc.).

[0105] <Silane coupling agent> The silane coupling agent used was "X-41-1810" manufactured by Shin-Etsu Chemical.

[0106] <Photopolymerization initiator> One of the following two types of photopolymerization initiator was used. · Omnirad184 (IGM resin) · Esacure TZT (IGM resin)

[0107] <Monofunctional acrylic monomer> One of the following two types of monofunctional acrylic monomers was used. Isostearyl acrylate (ISTA, manufactured by Osaka Organic Chemical Industry Co., Ltd., molecular weight 324) Isobornyl acrylate (IBXA (abbreviated as IBXA), manufactured by Osaka Organic Chemical Industry Co., Ltd., molecular weight 208)

[0108] <Polymonofunctional Monomer> As the polymonofunctional monomer, a trifunctional monomer M321 (trimethylolpropane propylene oxide modified triacrylate, molecular weight 546) manufactured by Toagosei Co., Ltd. was used.

[0109] Example 1 A pressure-sensitive adhesive composition was prepared according to the blending conditions shown in Table 1. Specifically, 100 parts by mass (in terms of polymer components) of the (meth)acrylic polymer obtained in Production Example 1, 1 part by mass of a diene copolymer ("TEAI-1000" manufactured by Nippon Soda Co., Ltd.), 0.2 parts by mass of a crosslinking agent, 0.2 parts by mass of a silane coupling agent, 0.4 parts by mass of a photopolymerization initiator (Omnirad184), and ethyl acetate as a solvent (E) were mixed to give a solid content concentration of 46% by mass to obtain a pressure-sensitive adhesive composition.

[0110] The pressure-sensitive adhesive composition was applied to a 100 μm-thick polyethylene terephthalate film (first release sheet, manufactured by Oji F-Tex Co., Ltd.: 100RL-07(2)) having a release agent layer treated with a silicone-based release agent in a coating amount of 200 μm / m after drying. 2 The adhesive was applied uniformly with an applicator so that the adhesive layer was uniformly applied. A doctor blade YD type manufactured by Yoshimitsu Seiki Co., Ltd. was used for application, and the adhesive layer was heated at 100°C for 3 minutes in an air-circulating thermostatic oven. This formed an adhesive layer on the surface of the first release sheet. A second release sheet (50RL-07(L) manufactured by Oji F-Tex Co., Ltd.) having a thickness of 50 μm was attached to the surface of this adhesive layer to obtain an adhesive sheet with a release sheet having a configuration of a first release film / adhesive sheet (adhesive layer) / second release film in which a semi-cured product (adhesive layer) was sandwiched between a pair of release films having a difference in release strength. This adhesive sheet was subjected to an aging treatment in which the adhesive sheet was left to stand for 7 days under conditions of 23°C and a relative humidity of 50%. The adhesive sheet had a thickness of 200 μm.

[0111] (Examples 2 to 9, Comparative Examples 1 to 4) Pressure-sensitive adhesive sheets with release sheets were obtained in the same manner as in Example 1, except that the types and amounts of the components of the pressure-sensitive adhesive composition were changed to the formulation shown in Table 1. The thickness of each pressure-sensitive adhesive sheet was as shown in Table 1.

[0112] (Evaluation method) The pressure-sensitive adhesive sheets obtained in the respective Examples and Comparative Examples were evaluated as follows. <Water vapor permeability (before post-curing)> The water vapor transmission rate of the adhesive sheet before post-curing was calculated by the cup method based on JIS Z0208-1976. Using an 80 μm tack film (TD80ULM (manufactured by Fujifilm) as a substrate, the light release film of the adhesive sheet was peeled off and the exposed surface was attached to the substrate, and then the heavy release film of the adhesive sheet was peeled off to produce a laminate, and the water vapor transmission rate (X1) was measured using the laminate. When the laminate was set in the cup, the outside of the cup was the tack film and the inside was the adhesive layer of the adhesive sheet. The measurement was performed in the presence of 5 g of calcium chloride in an environment of 40° C. and 90% RH, and the laminate was stored in that environment for 24 hours, and the water vapor transmission rate per 100 μm of adhesive sheet was calculated from the change in mass of the laminate before and after storage.

[0113] <Water vapor transmission rate (after post-curing)> The water vapor transmission rate of the adhesive sheet after post-curing was calculated by the cup method based on JIS Z0208-1976. A pair of release sheets from the adhesive sheet with release sheet was peeled off, and the adhesive sheet was post-cured by irradiating it with active energy rays under the same conditions as the irradiation condition A. A laminate was produced by laminating a tack film (TD80ULM (manufactured by Fujifilm) with a thickness of 80 μm as a substrate to one side of the post-cured adhesive sheet, and the water vapor transmission rate was measured. When the laminate was set in the cup, the tack film was on the outside of the cup, and the adhesive layer of the adhesive sheet was on the inside. The measurement environment was 40°C and 90% RH, and the laminate was stored in this environment in the presence of 5 g of calcium chloride for 24 hours, and the water vapor transmission rate per 100 μm of adhesive sheet was calculated from the change in mass of the laminate before and after storage. The irradiation conditions under irradiation condition A were 120 mW / cm at a wavelength of 355 nm. 2 The illuminance is 3000mJ / cm 2 The illuminance meter used was the UV-PFA1 manufactured by iGraphics Co., Ltd. In this irradiation condition A, an iGraphics Co., Ltd. ECS-4011GX / N was used as the ultraviolet irradiator, and a high-pressure mercury lamp H04-L41 and a heat-cut filter were attached to it.

[0114] <Adhesion to glass (initial adhesion)> A PET film ("A4300#100" manufactured by Toyobo Co., Ltd.) was used as a backing material, and the adhesive sheet (before post-curing) was attached to a glass plate (soda glass manufactured by Hiraoka Special Glass Manufacturing Co., Ltd., 1.1 mm thick) with a 2 kg load roll. After leaving this at 25°C for 24 hours, the peel strength was measured at 180° peeling at a tensile speed of 300 mm / min (and 3000 mm / min) using a tensile tester (model: RTC-1210, manufactured by A&D) in accordance with JIS Z 0237, and this was taken as the initial adhesive strength (X1) of the adhesive sheet.

[0115] <Adhesion to glass (after post-curing)> A PET film ("A4300#100" manufactured by Toyobo Co., Ltd.) was used as a backing material, and the adhesive sheet (before post-curing) was attached to a glass plate (soda glass manufactured by Hiraoka Special Glass Manufacturing Co., Ltd., 1.1 mm thick) with a 2 kg load roll, and then the adhesive sheet was irradiated with active energy rays from the backing material side under the same conditions as those of the irradiation condition A to post-cure. After leaving the post-cured adhesive sheet at 25°C for 24 hours, a tensile tester (model: RTC-1210, manufactured by A&D) was used to measure the peel strength when peeled at 180 degrees at a tensile speed of 300 mm / min (and 3000 mm / min) in accordance with JIS Z 0237, and the adhesive strength (X2) of the post-cured adhesive sheet was determined. The irradiation conditions under irradiation condition A were 120 mW / cm at a wavelength of 355 nm. 2 The illuminance is 3000mJ / cm 2 The illuminance meter used was the UV-PFA1 manufactured by iGraphics Co., Ltd. In this irradiation condition A, an iGraphics Co., Ltd. ECS-4011GX / N was used as the ultraviolet irradiator, and a high-pressure mercury lamp H04-L41 and a heat-cut filter were attached to it.

[0116] <Gel fraction> Approximately 0.1 g of the adhesive sheet (before or after post-curing) was collected in a sample bottle, 30 ml of ethyl acetate was added, and the mixture was shaken for 24 hours. The contents of the sample bottle were then filtered through a 150-mesh stainless steel wire screen, and the residue on the wire screen was dried at 100°C for 1 hour to measure the dry mass (g), and the gel fraction was calculated from the obtained dry mass using the above formula 1. The post-curing of the adhesive sheet in the measurement of the gel fraction was performed under the above irradiation condition A.

[0117] <Dielectric constant> The post-cured adhesive sheet was sandwiched between two copper foils and autoclaved (40°C, 0.5 MPa, 30 min). It was then measured based on JIS C 2138 using a dielectric constant measurement system (Toyo Corporation, Model 1260). The relative dielectric constant was calculated using the method specified in JIS C 2138 at a frequency of 100 kHz, in an environment of 23°C and 50% RH.

[0118] [Table 1]

[0119] Table 1 shows the manufacturing conditions and evaluation results of the pressure-sensitive adhesive sheets obtained in each of the Examples and Comparative Examples. All of the pressure-sensitive adhesive sheets obtained in the Examples had low water vapor transmission rate before post-curing (i.e., in a semi-cured state), low relative dielectric constant, and also had high transparency and excellent step conformability. In contrast, the pressure-sensitive adhesive sheets obtained in the Comparative Examples were made from pressure-sensitive adhesive compositions that did not contain a diene copolymer, and further contained a monofunctional acrylic monomer and / or a polymonofunctional monomer, and therefore had high water vapor transmission rate before post-curing (i.e., in a semi-cured state).

Claims

1. The adhesive composition includes a semi-cured product of a pressure-sensitive adhesive composition including at least a (meth)acrylic polymer, a photopolymerization initiator, and a diene copolymer having (meth)acrylate moieties at both ends, The weight average molecular weight of the diene copolymer is 1,000 to 5,000; When the water vapor transmission rate before curing with active energy rays is X1 and the water vapor transmission rate after curing with active energy rays is X2, X1 is 200 g / (m 2 - 24 hr) or less, An active energy ray-curable pressure-sensitive adhesive sheet, wherein the value of X1 / X2 is less than 1.

5.

2. 2. The active energy ray-curable pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive composition contains less than 5 parts by mass of a monofunctional acrylic monomer having a molecular weight of less than 1,000 per 100 parts by mass of the (meth)acrylic polymer.

3. 3. The active energy ray-curable pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive composition contains less than 5 parts by mass of a monofunctional acrylic monomer having an alkyl group having a linear or branched structure and a carbon number of 8 to 24 per 100 parts by mass of the (meth)acrylic polymer.

4. The active energy ray-curable adhesive sheet according to any one of claims 1 to 3, wherein the diene copolymer is a polymer having a 1,2 vinyl structure or a polymer having a structure in which a 1,2 vinyl structure has been hydrogenated.

5. An active energy ray-curable adhesive sheet described in any one of claims 1 to 4, wherein the glass transition temperature of the diene-based copolymer is 0°C or lower.

6. The active energy ray-curable pressure-sensitive adhesive sheet according to any one of claims 1 to 5, wherein the pressure-sensitive adhesive composition contains 0.5 to 30 parts by mass of the diene copolymer relative to 100 parts by mass of the (meth)acrylic polymer.

7. The active energy ray-curable pressure-sensitive adhesive sheet according to any one of claims 1 to 6, which has a relative dielectric constant of 3.5 or less at 100 kHz after being cured with active energy rays.

8. Used for bonding components for liquid crystal or organic EL displays, The active energy ray-curable pressure-sensitive adhesive sheet according to any one of claims 1 to 7, wherein the member is glass, a polarizing plate, or a touch sensor.

9. A display device comprising a post-cured product of the active energy ray-curable pressure-sensitive adhesive sheet according to any one of claims 1 to 8 as a pressure-sensitive adhesive layer.

Citation Information

Patent Citations

  • Double-sided adhesive sheet and image display apparatus

    JP2015040240A

  • Active energy ray-curable composite resin composition, and active energy ray-curable composite resin adhesive using the composition, or adhesive tape for bonding optical members

    JP2017226785A

  • Adhesive composition, adhesive sheet and laminate

    JP2019182929A

  • Pressure-sensitive adhesive sheet, process for producing laminate including pressure-sensitive adhesive layer, laminate including pressure-sensitive adhesive layer, image display device, and touch panel

    WO2017022770A1