Semi-aromatic polyamide resin composition for plated molded products, and plated molded products
The semi-aromatic polyamide resin composition addresses low melting point and adhesion issues by incorporating non-fibrous fillers and optimized processing, resulting in enhanced plating properties and solder reflow resistance for electronic and automotive components.
Patent Information
- Application Number
- JP2021546557
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-17
- Filing Date
- 2020-08-21
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-08-21
AI Technical Summary
Existing polyamide resin compositions for metal plating in electronic components face challenges with low melting points, poor solder reflow resistance, and inadequate adhesion, which limits their use in advanced applications requiring electromagnetic shielding and improved plating performance.
A semi-aromatic polyamide resin composition is developed, incorporating a specific C/N ratio, non-fibrous inorganic fillers, and controlled terminal groups to enhance plating properties, water resistance, and solder reflow resistance, achieved by blending semi-aromatic polyamide resin with non-fibrous fillers like kaolin and diatomaceous earth, and optimizing processing conditions.
The composition achieves excellent metal plating adhesion, low water absorption, and high solder reflow resistance, enabling stable performance in electronic components and automotive parts, with improved moldability and appearance.
Smart Images

Figure 0007586086000001 
Figure 0007586086000002 
Figure 0007586086000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a semi-aromatic polyamide resin composition having good plating properties, low water absorption and excellent solder reflow resistance. [Background technology]
[0002] Taking advantage of their excellent properties and ease of melt molding, polyamide resins have been used in clothing, industrial fiber, engineering plastics, etc. In recent years, with technological developments in various fields, the uses of polyamide resins have expanded even further, and they are now used in a variety of applications, from automobile parts around the engine to electrical and electronic parts such as smartphones.
[0003] As various technologies advance, the performance of electrical and electronic equipment and office automation equipment is improving. In the automotive industry, for example, motors are used as driving sources, and there is a need to reduce the impact that electromagnetic waves generated from various components have on surrounding parts or the human body.
[0004] In order to address these issues, studies have been conducted to impart electromagnetic shielding properties to the components of various devices, and metals with excellent electromagnetic shielding properties and resins containing conductive fillers have been used. Although it is possible to achieve electromagnetic shielding using these methods, there are still issues with regard to improving automobile fuel efficiency, reducing the weight of products, and resin processability.
[0005] On the other hand, metal deposition or metal plating on the surface of resin molded products is known as a method for imparting electromagnetic shielding properties to component parts of equipment. This method is used in various fields because it is easier to reduce the weight of the parts than to make them out of metal, and it can also provide sufficient electromagnetic shielding properties.
[0006] Various metal vapor deposition and metal plating techniques for resins have been developed. Patent Document 1 discloses a polyamide resin composition that is made of polyamide, an inorganic filler, and a modified styrene-olefin copolymer and has excellent adhesion properties with metal plating. However, the polyamide resin composition described in the document has a melting point lower than 280°C, and therefore is difficult to withstand the solder reflow process used in the manufacture of circuit board components.
[0007] Patent Document 2 discloses a resin composition for metal deposition containing a polyamide resin, a styrene-based resin, and a filler. However, the resin composition for metal deposition described in this document describes good adhesion to a metal film formed by a metal deposition technique, and the metal film formation process is essentially different from that of the metal plating technique of the present invention. In addition, all of the resin compositions for metal deposition described in the examples have melting points lower than 280°C, making it difficult to withstand the solder reflow process.
[0008] Patent Document 3 discloses a resin composition for forming a plating layer, which contains a semi-aromatic polyamide composed of terephthalic acid and a diamine component having an alkylene group having 4 to 25 carbon atoms, and an inorganic filler. However, the resin composition described in this document only describes the use of glass fiber in the examples, and does not sufficiently ensure plating adhesion.
[0009] Patent Document 4 discloses a molded article having a metal layer on the surface thereof, which is obtained from a polyamide resin composition comprising a polyamide resin composed of terephthalic acid and 1,9-nonanediamine and a filler. However, the resin composition described in this document is limited to a polyamide resin.
[0010] Patent Document 5 discloses a method for forming an electroless plating layer using a resin composition in which a filler is mixed with a semi-aromatic polyamide resin selected from polyamide 10T, polyamide 9T, polyamide 6T, polyamide 4T, or polyphthalamide. However, the technique described in this document has limitations in terms of equipment, since it is necessary to set the mold temperature to 180 to 240°C when molding a base to be plated using the resin composition.
[0011] As described above, although various inventions have been made regarding metal vapor deposition and metal plating on resin, various problems and limitations remain. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Special Publication No. 8-11782 [Patent Document 2] JP 2006-131821 A [Patent Document 3] Patent No. 3009707 [Patent Document 4] Patent No. 3400133 [Patent Document 5] Patent No. 6190154 Summary of the Invention [Problem to be solved by the invention]
[0013] The present invention has been invented in view of the current state of the prior art, and its purpose is to provide a semi-aromatic polyamide resin composition that has good plating properties, low water absorption, and excellent solder reflow resistance. Furthermore, in recent years, there has been a demand for higher plating properties and appearance of plated molded products, and for this reason, moldability at the molded product stage before plating is also important, and the semi-aromatic polyamide resin composition of the present invention can also solve this problem.
[0014] In order to achieve the above object, the present inventors have thoroughly investigated the composition of the semi-aromatic polyamide resin as well as the type and amount of filler, and as a result have been able to provide a semi-aromatic polyamide resin composition that has good plating properties, low water absorption and excellent solder reflow resistance.
[0015] That is, the present invention has the following configuration. (1) A semi-aromatic polyamide resin composition for plated molded products, comprising 10 to 200 parts by mass of a non-fibrous inorganic filler (B) per 100 parts by mass of a semi-aromatic polyamide resin (A), wherein the ratio (C / N ratio) of the number of carbon atoms (C) to the number of nitrogen atoms (N) in the semi-aromatic polyamide resin (A) is 7.3 or more. (2) The semi-aromatic polyamide resin composition according to (1), wherein the semi-aromatic polyamide resin (A) is a semi-aromatic polyamide resin containing 50 to 100 mol % of repeating units consisting of a diamine having 6 to 12 carbon atoms and terephthalic acid. (3) The semi-aromatic polyamide resin composition according to (1) or (2), wherein the semi-aromatic polyamide resin (A) has a terminal carboxyl group concentration of 5 to 200 eq / ton and a terminal amino group concentration of 0 to 100 eq / ton. (4) The semi-aromatic polyamide resin composition according to any one of (1) to (3), wherein the non-fibrous inorganic filler (B) is at least one selected from the group consisting of kaolin, wollastonite, glass beads, diatomaceous earth, and zeolite. (5) A plated molded product obtained by plating the semi-aromatic polyamide resin composition according to any one of (1) to (4). Effect of the Invention
[0016] According to the present invention, it is possible to provide a semi-aromatic polyamide resin composition having good plating properties, low water absorbency and solder reflow resistance, and a plated molded product using this semi-aromatic polyamide resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The semi-aromatic polyamide resin composition of the present invention will be described below.
[0018] The semi-aromatic polyamide resin (A) used in the present invention is not particularly limited, and is a semi-aromatic polyamide having an acid amide bond (-CONH-) and an aromatic ring (benzene ring) in the molecule. Examples of semi-aromatic polyamides include 6T-based polyamides (e.g., polyamide 6T / 6I consisting of terephthalic acid / isophthalic acid / hexamethylenediamine, polyamide 6T / 66 consisting of terephthalic acid / adipic acid / hexamethylenediamine, polyamide 6T / 6I / 66 consisting of terephthalic acid / isophthalic acid / adipic acid / hexamethylenediamine, polyamide 6T / M-5T consisting of terephthalic acid / hexamethylenediamine / 2-methyl-1,5-pent ... Examples include polyamide 6T / 6 made of samethylenediamine / ε-caprolactam, polyamide 6T / 4T made of terephthalic acid / hexamethylenediamine / tetramethylenediamine, 9T polyamide (terephthalic acid / 1,9-nonanediamine / 2-methyl-1,8-octanediamine), 10T polyamide (terephthalic acid / 1,10-decanediamine), 12T polyamide (terephthalic acid / 1,12-dodecanediamine), and polyamide made of sebacic acid / paraxylenediamine.
[0019] The C / N ratio described in this specification means the ratio of the number of carbon atoms (C) to the number of nitrogen atoms (N) in the repeating structural unit in the semi-aromatic polyamide (A) (hereinafter referred to as the C / N ratio). The C / N ratio represents the concentration of amide groups in the polyamide, and the higher the C / N ratio, the lower the concentration of amide groups. In general, amide groups are easily coordinated with water molecules, so the C / N ratio is an index of the water absorption of polyamide resins. When the water absorption of polyamide resins is high, that is, when the C / N ratio is small, the water in the molded body is rapidly heated in post-processing steps such as solder reflow, and the volume expands, which often causes problems with surface swelling (blisters). In addition, the dimensional change of the product due to water absorption causes problems during assembly and strength reduction. Therefore, the C / N ratio is important in manufacturing more stable products industrially.
[0020] The semi-aromatic polyamide resin (A) used in the present invention must have a C / N ratio of 7.3 or more. It is also preferable that it is 7.5 or more. The upper limit of the C / N ratio is not particularly limited, but is preferably 10.0 or less, more preferably 9.0 or less, even more preferably 8.5 or less, and particularly preferably 8.2 or less.
[0021] From the viewpoint of a C / N ratio of 7.3 or more, the semi-aromatic polyamide resin (A) used in the present invention is preferably the following semi-aromatic polyamide resin. The semi-aromatic polyamide resin (A) is preferably a semi-aromatic polyamide containing 50 to 100 mol% of repeating units consisting of a diamine having 6 to 12 carbon atoms and terephthalic acid. The semi-aromatic polyamide resin (A) is more preferably a semi-aromatic polyamide resin containing 50 to 100 mol% of repeating units consisting of a diamine having 6 to 12 carbon atoms and terephthalic acid, and 0 to 50 mol% of repeating units consisting of an aminocarboxylic acid or lactam having 10 or more carbon atoms, is even more preferably a semi-aromatic polyamide resin containing 50 to 98 mol% of repeating units consisting of a diamine having 6 to 12 carbon atoms and terephthalic acid, and 2 to 50 mol% of repeating units consisting of an aminocarboxylic acid or lactam having 10 or more carbon atoms, and is particularly preferably a semi-aromatic polyamide resin containing 55 to 98 mol% of repeating units consisting of a diamine having 6 to 12 carbon atoms and terephthalic acid, and 2 to 45 mol% of repeating units consisting of an aminocarboxylic acid or lactam having 10 or more carbon atoms. If the ratio of repeating units consisting of diamines having 6 to 12 carbon atoms and terephthalic acid in the semi-aromatic polyamide resin (A) is less than 50 mol%, the moisture in the molded product is rapidly heated in post-processing steps such as solder reflow, and the volume expands, often causing problems with surface swelling (blistering). In addition, the dimensional change of the product due to water absorption causes problems during assembly and a decrease in strength.
[0022] Examples of the diamine component having 6 to 12 carbon atoms constituting the semi-aromatic polyamide resin (A) include 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 2-methyl-1,8-octamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine, etc. These may be used alone or in combination.
[0023] As the aminocarboxylic acid having 10 or more carbon atoms or the lactam having 10 or more carbon atoms constituting the semi-aromatic polyamide resin (A), an aminocarboxylic acid or lactam having 11 to 18 carbon atoms is preferred. Among them, 11-aminoundecanoic acid, undecane lactam, 12-aminododecanoic acid, and 12-lauryllactam are preferred. From the viewpoint of a C / N ratio of 7.3 or more, it is preferred that one or more of aminocarboxylic acids having 11 to 18 carbon atoms or lactams having 11 to 18 carbon atoms are copolymerized as the copolymerization component.
[0024] The semi-aromatic polyamide resin (A) used in the present invention can be copolymerized with other components in an amount of 50 mol % or less in the constituent units. Examples of copolymerizable diamine components include aliphatic diamines such as 1,13-tridecamethylenediamine, 1,16-hexadecamethylenediamine, 1,18-octadecamethylenediamine, and 2,2,4 (or 2,4,4)-trimethylhexamethylenediamine, alicyclic diamines such as piperazine, cyclohexanediamine, bis(3-methyl-4-aminohexyl)methane, bis-(4,4'-aminocyclohexyl)methane, and isophoronediamine, and aromatic diamines such as metaxylylenediamine, paraxylylenediamine, paraphenylenediamine, and metaphenylenediamine, and hydrogenated products thereof.
[0025] Examples of the copolymerizable acid component include aromatic dicarboxylic acids such as isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 2,2'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 5-sodium sulfonate isophthalic acid, and 5-hydroxyisophthalic acid; and aliphatic or alicyclic dicarboxylic acids such as fumaric acid, maleic acid, succinic acid, itaconic acid, adipic acid, azelaic acid, sebacic acid, 1,11-undecanedioic acid, 1,12-dodecanedioic acid, 1,14-tetradecanedioic acid, 1,18-octadecanedioic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 4-methyl-1,2-cyclohexanedicarboxylic acid, and dimer acid. Furthermore, examples of copolymerizable components include ε-caprolactam.
[0026] The aromatic polyamide resin (A) used in the present invention is preferably a semi-aromatic polyamide resin containing 50 to 100 mol % of repeating units consisting of hexamethylenediamine and terephthalic acid and 0 to 50 mol % of repeating units consisting of aminoundecanoic acid or undecane lactam, and is preferably a semi-aromatic polyamide resin containing 50 to 98 mol % of repeating units consisting of hexamethylenediamine and terephthalic acid and 2 to 50 mol % of repeating units consisting of aminoundecanoic acid or undecane lactam. It is more preferable that the polyamide resin is a semi-aromatic polyamide resin containing 55 to 80 mol % of repeating units composed of hexamethylenediamine and terephthalic acid and 20 to 45 mol % of repeating units composed of aminoundecanoic acid or undecane lactam, and it is even more preferable that the polyamide resin is a semi-aromatic polyamide resin containing 60 to 70 mol % of repeating units composed of hexamethylenediamine and terephthalic acid and 30 to 40 mol % of repeating units composed of aminoundecanoic acid or undecane lactam. If the ratio of repeating units consisting of hexamethylenediamine and terephthalic acid in the semi-aromatic polyamide resin (A) is less than 50 mol%, the moisture in the molded product is rapidly heated during post-processing such as solder reflow, causing the volume to expand, which often results in problems with surface swelling (blistering). In addition, the dimensional changes of the product due to water absorption can cause problems during assembly and a decrease in strength.
[0027] Examples of catalysts used in producing the semi-aromatic polyamide resin (A) include phosphoric acid, phosphorous acid, hypophosphorous acid, or their metal salts, ammonium salts, and esters. Specific examples of metal species of metal salts include potassium, sodium, magnesium, vanadium, calcium, zinc, cobalt, manganese, tin, tungsten, germanium, titanium, and antimony. Examples of esters include ethyl ester, isopropyl ester, butyl ester, hexyl ester, isodecyl ester, octadecyl ester, decyl ester, stearyl ester, and phenyl ester. In addition, from the viewpoint of improving melt retention stability, it is preferable to add an alkali compound such as sodium hydroxide, potassium hydroxide, or magnesium hydroxide.
[0028] The relative viscosity (RV) of the semi-aromatic polyamide resin (A) measured in 96% concentrated sulfuric acid at 20° C. is preferably 0.4 to 4.0, more preferably 1.0 to 3.0, and even more preferably 1.5 to 2.5. Methods for adjusting the relative viscosity of the polyamide within a certain range include a method for adjusting the molecular weight.
[0029] The terminal carboxyl group concentration and terminal amino group concentration of the semi-aromatic polyamide resin (A) are preferably from 5 to 200 eq / ton and from 0 to 100 eq / ton, respectively. If the terminal carboxyl group concentration is less than 5 eq / ton, the adhesion to the filler will be insufficient, the compatibility with the polyamide resin will be poor, and the filler will not disperse well. If the filler disperses poorly, the unevenness will not be fully developed after the etching process, and the metal plating may peel off. Furthermore, if the terminal carboxyl group concentration and terminal amino group concentration exceed 200 eq / ton and 100 eq / ton, respectively, gelation and deterioration may be promoted during molding processing, so the terminal carboxyl group concentration and terminal amino group concentration within the above ranges are appropriate.
[0030] The amount of terminal groups and the molecular weight of the semi-aromatic polyamide resin (A) can be adjusted by a method of polycondensation by adjusting the molar ratio of the amount of amino groups to the amount of carboxyl groups or a method of adding a terminal blocking agent.
[0031] The timing of adding the end-capping agent may include the time of charging the raw materials, the start of polymerization, the later stage of polymerization, or the end of polymerization. The end-capping agent is not particularly limited as long as it is a monofunctional compound that is reactive with the amino group or carboxyl group at the polyamide terminal, and may include monocarboxylic acids or monoamines, acid anhydrides such as phthalic anhydride, monoisocyanates, monoacid halides, monoesters, and monoalcohols. Examples of the end-capping agent include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexylcarboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid; acid anhydrides such as maleic anhydride, phthalic anhydride, and hexahydrophthalic anhydride; aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; and aromatic monoamines such as aniline, toluidine, diphenylamine, and naphthylamine.
[0032] The semi-aromatic polyamide resin (A) can be produced by a conventional method, and can be easily synthesized, for example, by subjecting raw material monomers to a co-condensation reaction. The order of the co-condensation polymerization reaction is not particularly limited, and all raw material monomers may be reacted at once, or some raw material monomers may be reacted first, followed by the remaining raw material monomers. The polymerization method is not particularly limited, and may proceed in a continuous process from raw material charging to polymer preparation, or an oligomer may be prepared once and then polymerized in a separate process using an extruder, or the oligomer may be polymerized by solid-phase polymerization. The ratio of each structural unit in the synthesized copolymerized polyamide can be controlled by adjusting the charging ratio of the raw material monomers.
[0033] The non-fibrous inorganic filler (B) can be used without any particular limitation as long as it is an inorganic filler other than a fibrous inorganic filler, but the average aspect ratio of the non-fibrous inorganic filler (B) is preferably 100 or less, more preferably 50 or less. The non-fibrous inorganic filler (B) preferably has an average particle size of 50 μm or less, more preferably 30 μm or less, and even more preferably 10 μm or less. The amount of the non-fibrous inorganic filler (B) is 10 to 200 parts by mass, preferably 20 to 160 parts by mass, and more preferably 40 to 160 parts by mass, relative to 100 parts by mass of the semi-aromatic polyamide resin (A). If the amount is less than 10 parts by mass, the adhesion strength of the metal plating is reduced and the reinforcing effect is reduced, which is not preferable. On the other hand, if the amount is more than 200 parts by mass, the processability and the surface smoothness of the molded product are reduced, which is not preferable. In the semi-aromatic polyamide resin composition of the present invention, the amount of the non-fibrous inorganic filler (B) is the content in the semi-aromatic polyamide resin composition as it is.
[0034] The non-fibrous inorganic filler (B) used in the present invention is blended to improve the metal plating adhesion, strength, and dimensional stability of the semi-aromatic polyamide resin composition, and at least one selected from the non-fibrous inorganic fillers is used. Examples of the non-fibrous inorganic filler (B) include aluminum silicate salts (kaolin, zeolite), calcium silicate salts (wollastonite), magnesium silicate salts (talc), mica, calcium carbonate, barium sulfate, silicon dioxide (diatomaceous earth), glass beads, and glass balloons. The semi-aromatic polyamide resin composition of the present invention has good metal plating adhesion, and from the viewpoint of particularly excellent plating adhesion, the non-fibrous inorganic filler (B) is preferably at least one selected from kaolin, diatomaceous earth, wollastonite, glass beads, and zeolite, more preferably at least one selected from kaolin, diatomaceous earth, and wollastonite, and even more preferably at least one selected from kaolin and diatomaceous earth. Kaolin has excellent appearance when molded, and does not dissolve in the etching solution used in the plating process, so it is easy to create unevenness and has excellent plating adhesion. The same is true for diatomaceous earth, and since the filler itself has many unevennesses, it is easier to ensure plating adhesion. These can be used not only alone, but also in combination with several types.
[0035] The non-fibrous inorganic filler (B) is preferably treated with an organic agent or a coupling agent in order to improve its affinity with the semi-aromatic polyamide resin (A). Alternatively, it is preferable to use a coupling agent in combination with the non-fibrous inorganic filler (B) during melt compounding. As the coupling agent, any of silane-based coupling agents, titanate-based coupling agents, and aluminum-based coupling agents may be used, and among these, aminosilane coupling agents and epoxysilane coupling agents are particularly preferable.
[0036] An example of a method for plating the surface of the semi-aromatic polyamide resin composition of the present invention with a metal is to bring an etching solution into contact with the surface of a molded article formed using the semi-aromatic polyamide resin composition, etch (roughen the surface) the surface of the molded article, form a concave-convex structure on the surface of the molded article, and then plate the surface with a metal. It is presumed that the concave-convex structure formed by etching exerts a mechanical bonding effect, resulting in excellent plating adhesion.
[0037] The semi-aromatic polyamide resin composition of the present invention is one in which the semi-aromatic polyamide resin (A) is blended with the non-fibrous inorganic filler (B) in a predetermined blending amount as described above, thereby forming irregularities on the surface of the molded article after etching, and improving the adhesion of metal plating through the mechanical bonding effect.
[0038] The semi-aromatic polyamide resin composition of the present invention can contain various additives used in conventional polyamide resin compositions within the range that does not impair the properties of the composition. Examples of additives include reinforcing agents, stabilizers, release agents, sliding property improvers, colorants, plasticizers, crystal nucleating agents, polyamides different from the semi-aromatic polyamide resin (A), and thermoplastic resins other than polyamides. The possible blending amounts of these components in the semi-aromatic polyamide resin composition are as described below, but the total amount of these components in the semi-aromatic polyamide resin composition is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less.
[0039] Examples of the reinforcing agent include fibrous inorganic fillers, specifically glass fibers, potassium titanate fibers, acicular wollastonite, and fibrous wollastonite. These reinforcing agents may be used alone or in combination. The amount of the reinforcing agent to be added may be selected from the optimum amount, but it is possible to add up to 5 parts by mass per 100 parts by mass of the semi-aromatic polyamide resin (A). If the amount exceeds 5 parts by mass, problems will arise in the metal plating appearance and moldability, which is not preferable. It is more preferable not to add a fibrous inorganic filler.
[0040] Examples of the stabilizer include organic antioxidants such as hindered phenol antioxidants, sulfur antioxidants, and phosphorus antioxidants, heat stabilizers, light stabilizers such as hindered amines, benzophenones, and imidazoles, ultraviolet absorbers, metal deactivators, and copper compounds. Examples of the copper compound include copper salts of organic carboxylic acids such as cuprous chloride, cuprous bromide, cuprous iodide, cupric chloride, cupric bromide, cupric iodide, cupric phosphate, cupric pyrophosphate, copper sulfide, copper nitrate, and copper acetate. In addition, it is preferable to contain an alkali metal halide compound as a component other than the copper compound, and examples of the alkali metal halide compound include lithium chloride, lithium bromide, lithium iodide, sodium fluoride, sodium chloride, sodium bromide, sodium iodide, potassium fluoride, potassium chloride, potassium bromide, and potassium iodide. These additives may be used alone or in combination of several types. The amount of stabilizer to be added may be selected optimally, but it is possible to add up to 5 parts by mass per 100 parts by mass of the semi-aromatic polyamide resin (A).
[0041] Examples of the release agent include long-chain fatty acids or their esters or metal salts, amide compounds, polyethylene wax, silicone, and polyethylene oxide. As the long-chain fatty acid, those having 12 or more carbon atoms are particularly preferable, and examples thereof include stearic acid, 12-hydroxystearic acid, behenic acid, and montanic acid, and the carboxylic acid may be partially or entirely esterified with monoglycol or polyglycol, or may form a metal salt. Examples of the amide compounds include ethylene bis-terephthalamide and methylene bis-stearylamide. These release agents may be used alone or as a mixture. The amount of the release agent to be added may be selected from the optimum amount, but it is possible to add up to 5 parts by mass per 100 parts by mass of the semi-aromatic polyamide resin (A).
[0042] The semi-aromatic polyamide resin composition of the present invention may be polymer-blended with a polyamide having a different composition from the semi-aromatic polyamide resin (A). The amount of the polyamide having a different composition from the semi-aromatic polyamide resin (A) added may be selected from the optimum amount, but it is possible to add up to 50 parts by mass per 100 parts by mass of the semi-aromatic polyamide resin (A).
[0043] The semi-aromatic polyamide resin composition of the present invention may contain a thermoplastic resin other than polyamide. Examples of polymers other than polyamide include polyphenylene sulfide (PPS), liquid crystal polymer (LCP), aramid resin, polyetheretherketone (PEEK), polyetherketone (PEK), polyetherimide (PEI), thermoplastic polyimide, polyamideimide (PAI), polyetherketoneketone (PEKK), polyphenylene ether (PPE), polyethersulfone (PES), polysulfone (PSU), polyarylate (PAR), polyethylene terephthalate, polybutylene terephthalate ... Examples of the thermoplastic resin include polyethylene naphthalate, polybutylene naphthalate, polycarbonate (PC), polyoxymethylene (POM), polypropylene (PP), polyethylene (PE), polymethylpentene (TPX), polystyrene (PS), polymethyl methacrylate, acrylonitrile-styrene copolymer (AS), acrylonitrile-butadiene-styrene copolymer (ABS), ethylene-butylene copolymer (EBR), ethylene-propylene copolymer (EPR), and styrene-ethylene-butylene copolymer (SEBS). These thermoplastic resins can be blended in a molten state by melt kneading, but the thermoplastic resin may be made fibrous or granular and dispersed in the polyamide resin composition of the present invention. The amount of the thermoplastic resin to be added can be selected from the optimum amount, but it is possible to add up to 50 parts by mass to 100 parts by mass of the semi-aromatic polyamide resin (A).
[0044] When a thermoplastic resin other than the aromatic polyamide resin (A) is added to the semi-aromatic polyamide resin composition of the present invention, it is preferable that a reactive group capable of reacting with the polyamide is copolymerized, and the reactive group is a group capable of reacting with the amino group, carboxyl group, and main chain amide group, which are the terminal groups of the polyamide resin.Specific examples of the reactive group include a carboxylic acid group, an acid anhydride group, an epoxy group, an oxazoline group, an amino group, and an isocyanate group, and among them, an acid anhydride group has the highest reactivity.
[0045] The semi-aromatic polyamide resin composition of the present invention can be produced by blending the above-mentioned components by a conventionally known method, for example, by adding each component during the polycondensation reaction of the semi-aromatic polyamide resin (A), by dry blending the semi-aromatic polyamide resin (A) with other components, or by melt-kneading each component using a twin-screw extruder.
[0046] The semi-aromatic polyamide resin composition of the present invention can be molded into a molded article by a known molding method such as injection molding. When a molded article is manufactured using the semi-aromatic polyamide resin composition of the present invention, the mold temperature in injection molding is preferably 180°C or less, more preferably 170°C or less, even more preferably 160°C or less, and particularly preferably 150°C or less. If the mold temperature exceeds the above upper limit, molding defects such as the molded article remaining in the mold may occur. There is no particular limit to the lower limit of the mold temperature, but from the viewpoint of the fluidity of the resin, the appearance of the molded article, and the suppression of dimensional change in the actual use environment, it is preferably 50°C or more, more preferably 70°C or more, even more preferably 100°C or more, and particularly preferably 120°C or more.
[0047] The semi-aromatic polyamide resin composition of the present invention can be used as a metal-plated molded product obtained by plating the surface of a molded product obtained using the composition with a metal. The metal-plated molded product has excellent metal plating adhesion, low water absorption, and solder reflow resistance compared to conventional metal-plated molded products.
[0048] The method for producing a metal-plated molded product using the semi-aromatic polyamide resin composition of the present invention is not particularly limited, and can be produced by known techniques. As an example, the catalyst accelerator method in which the surface is roughened by chemical etching treatment using chromic acid, permanganic acid, hydrochloric acid, etc., and then the roughened surface is used to perform steps such as neutralization, catalyst application, activation, electroless plating, acid activation, and electroplating in order, or the direct plating method in which the electroless plating step in the catalyst accelerator method is omitted, the surface is modified by ultraviolet light or a laser light having a specific wavelength, and then the modified surface is used to perform steps such as catalyst application, activation, electroless plating, acid activation, and electroplating in order, or the direct plating method in which the electroless plating step in the catalyst accelerator method is omitted, or the like, can be mentioned. In addition, etching and metal plating can be performed on the entire surface of the molded product for plating or on a part of it.
[0049] The thickness of the metal plating of the metal-plated molded product using the semi-aromatic polyamide resin composition of the present invention may be selected to an optimum thickness, but is preferably 0.5 to 200 μm, more preferably 1 to 150 μm.
[0050] Metal-plated molded articles using the semi-aromatic polyamide resin composition of the present invention have excellent metal adhesion due to the non-fibrous inorganic filler blended in the semi-aromatic polyamide resin composition.
[0051] The metal plating peel strength of a metal-plated molded product using the semi-aromatic polyamide resin composition of the present invention is measured by the method described in the Examples section below. The metal plating peel strength is an item related to the good plating properties of the semi-aromatic polyamide resin composition of the present invention, and the metal plating peel strength must be 4.0 N / cm or more. It is also preferably 4.5 N / cm or more, more preferably 5.0 N / cm or more, even more preferably 5.5 N / cm or more, and particularly preferably 5.7 N / cm or more. If the metal plating peel strength is below the lower limit, the adhesion between the semi-aromatic polyamide resin composition and the metal plating is low, and the metal plating may lift or peel off.
[0052] Metal-plated molded products using the semi-aromatic polyamide resin composition of the present invention can be used for a variety of applications, such as automobile parts, electric and electronic parts, office automation equipment parts, and electromagnetic wave shielding parts, taking advantage of the excellent metal plating adhesion. EXAMPLES
[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The measured values described in the examples were measured by the following methods.
[0054] (1) Terminal amino group concentration (AEG), terminal carboxyl group concentration (CEG) Semi-aromatic polyamide resin (A) is dissolved in a solvent of deuterated chloroform (CDCl3) / hexafluoroisopropanol (HFIP) = 1 / 1 (volume ratio), and polyformic acid is added dropwise, 1 The concentration of each end group was measured by H-NMR.
[0055] (2) Relative Viscosity (RV) 0.25 g of the semi-aromatic polyamide resin was dissolved in 25 ml of 96% sulfuric acid, and the viscosity was measured at 20° C. using an Ostwald viscometer.
[0056] (3) Melting point (Tm) 5 mg of the semi-aromatic polyamide resin was placed in an aluminum sample pan and sealed. The resin was measured using a differential scanning calorimeter (DSC) DSC-Q100 (TA Instruments Japan, Inc.) at a heating rate of 20°C / min up to 350°C, and the maximum peak temperature of the heat of fusion was determined as the crystalline melting point.
[0057] (4) Metal plating peel strength Using a Toshiba Machine injection molding machine EC-100, the cylinder temperature was set to the melting point of the resin + 20°C, the mold temperature was set to 140°C, and a flat plate with a length of 100 mm, width of 100 mm, and thickness of 2 mm was injection molded to prepare a test specimen for evaluation. The obtained test specimen was wiped with isopropyl alcohol, and then degreased at 60°C for 3 minutes using 50g / l OPC-250 cleaner (manufactured by Okuno Pharmaceutical Co., Ltd.). The test specimen was then immersed in a 70°C chromic acid solution consisting of 400g / l chromic acid, 200ml / l concentrated sulfuric acid, and 0.3g / l Top Shut (manufactured by Okuno Pharmaceutical Co., Ltd.) for 5 minutes to perform surface treatment. The surface-treated test specimen was acid washed at room temperature for 3 minutes with a 5% aqueous solution of 38% hydrochloric acid, and then immersed in a treatment solution consisting of 200ml / l B-200 Neutralizer (manufactured by Okuno Pharmaceutical Co., Ltd.) adjusted to 45°C for 5 minutes. Next, the specimen was immersed for 4 minutes in a treatment solution consisting of a tin-palladium complex salt solution (A30 Catalyst, manufactured by Okuno Pharmaceutical Co., Ltd.), hydrochloric acid, and water (volume ratio = 1:1:5) prepared at 25 ° C (catalyzing). After that, the specimen was immersed for 4 minutes in a 10% aqueous solution of 38% hydrochloric acid prepared at 50 ° C (accelerating), and then immersed for 10 minutes in an electroless nickel plating solution consisting of TMP Chemical Nickel A solution, B solution (manufactured by Okuno Pharmaceutical Co., Ltd.) and water (volume ratio = 1:1:4) prepared at 40 ° C to form a nickel plating layer of about 1 μm on the surface of the specimen, and further electrolytic copper plating was applied to form a copper plating layer. A strip specimen measuring 100 mm in length, 10 mm in width, and 2 mm in thickness was cut out from the obtained metal-plated specimen to be used as a peel strength evaluation specimen. The metal plating peel strength was measured using the prepared peel strength evaluation specimen in accordance with the JIS H8630 90 degree peel strength test method.
[0058] (5) Metal plating appearance Using a Toshiba Machine injection molding machine EC-100, the cylinder temperature was set to the melting point of the resin + 20°C, the mold temperature was set to 140°C, and a flat plate with a length of 100 mm, width of 100 mm, and thickness of 2 mm was injection molded to prepare a test specimen for evaluation. The obtained test specimen was wiped with isopropyl alcohol, and then degreased at 60°C for 3 minutes using 50g / l OPC-250 cleaner (manufactured by Okuno Pharmaceutical Co., Ltd.). The test specimen was then immersed in a 70°C chromic acid solution consisting of 400g / l chromic acid, 200ml / l concentrated sulfuric acid, and 0.3g / l Top Shut (manufactured by Okuno Pharmaceutical Co., Ltd.) for 5 minutes to perform surface treatment. The surface-treated test specimen was acid washed at room temperature for 3 minutes with a 5% aqueous solution of 38% hydrochloric acid, and then immersed in a treatment solution consisting of 200ml / l B-200 Neutralizer (manufactured by Okuno Pharmaceutical Co., Ltd.) adjusted to 45°C for 5 minutes. Next, the test piece was immersed for 4 minutes in a treatment solution consisting of a tin-palladium complex salt solution (A30 Catalyst, manufactured by Okuno Pharmaceutical Co., Ltd.), hydrochloric acid, and water (volume ratio = 1:1:5) prepared at 25°C (catalyzing). After that, the test piece was immersed for 4 minutes in a 10% aqueous solution of 38% hydrochloric acid prepared at 50°C (accelerating), and then immersed for 10 minutes in an electroless nickel plating solution consisting of TMP Chemical Nickel A and B solutions (manufactured by Okuno Pharmaceutical Co., Ltd.) and water (volume ratio = 1:1:4) prepared at 40°C, forming a nickel plating layer of about 1 μm on the surface of the test piece, and further electrolytic copper plating was applied to form a copper plating layer. The appearance of the obtained metal-plated test piece was observed, and the appearance was evaluated based on the presence or absence of lifting of the metal plating. ○: No lifting of metal plating ×: Metal plating peeling
[0059] (6) Solder reflow resistance Using a Toshiba Machine injection molding machine EC-100, the cylinder temperature was set to the melting point of the resin + 20℃, the mold temperature was set to 140℃, and a UL combustion test piece with a length of 127 mm, width of 12.6 mm, and thickness of 0.8 mmt was injection molded to prepare a test piece. The test piece was left in an atmosphere of 85℃ and 85%RH (relative humidity) for 72 hours. The test piece was preheated in an air reflow furnace (Atec AIS-20-82C) by raising the temperature from room temperature to 150℃ over 60 seconds, and then preheated to 190℃ at a heating rate of 0.5℃ / min. The temperature was then raised to a specified set temperature at a rate of 100℃ / min, held at the specified temperature for 10 seconds, and then cooled. The set temperature was increased in 5℃ increments from 240℃, and the highest set temperature at which no swelling or deformation of the surface occurred was used as an index of solder heat resistance as the reflow heat resistance temperature. ○: Reflow heat resistance temperature is 260℃ or higher ×: Reflow heat resistance temperature is less than 260℃
[0060] (7) Formability Using a Toshiba Machine EC-100 injection molding machine, the cylinder temperature was set to the resin's melting point + 20°C, the mold temperature was set to 140°C, and a flat plate measuring 100 mm in length, 100 mm in width, and 2 mm in thickness was injection molded to prepare a test specimen for evaluation. The appearance of the obtained test specimen was visually observed and evaluated according to the following criteria. ◯: No filler floating was observed on the surface of the molded article. ×: Filler floating is observed on the surface of the molded product.
[0061] In this example, semi-aromatic polyamide resin (A) was synthesized by the following method or a commercially available product. The physical properties of each semi-aromatic polyamide resin (A) are shown in Table 1.
[0062] [Table 1]
[0063] <Synthesis Example 1: Semi-aromatic polyamide resin (A1)> 8.55 kg of 1,6-hexamethylenediamine, 12.25 kg of terephthalic acid, 8.00 kg of 11-aminoundecanoic acid, 9 g of sodium hypophosphite as a catalyst, 140 g of acetic acid as a terminal regulator, and 16.20 kg of ion-exchanged water were charged into a 50-liter autoclave, pressurized from normal pressure to 0.05 MPa with N2, released the pressure, and returned to normal pressure. This operation was repeated three times to replace with N2, and then the mixture was uniformly dissolved at 135°C and 0.3 MPa under stirring. The solution was then continuously fed by a liquid feed pump, heated to 240°C by a heating pipe, and heated for 1 hour. The reaction mixture was then fed to a pressurized reactor and heated to 290°C, and a portion of the water was distilled off so as to maintain the internal pressure of the reactor at 3MPa, to obtain a low-order condensate. The low-order condensate was then fed directly to a twin-screw extruder (screw diameter 37 mm, L / D=60) while maintaining the molten state, and polycondensation was carried out under molten conditions while the resin temperature was kept at 335°C and water was removed from three vents, to obtain a semi-aromatic polyamide resin (A1). The obtained semi-aromatic polyamide resin (A1) was composed of 65.1 mol% of structural units consisting of 1,6-hexamethylenediamine and terephthalic acid, and 34.9 mol% of structural units consisting of 11-aminoundecanoic acid, and had a relative viscosity of 2.1, a melting point of 314°C, AEG 30 eq / ton, and CEG 140 eq / ton. The ratio of constituent monomers of polyamide resin was the same as that of AEG and CEG measurements. 1 This was confirmed by H-NMR.
[0064] <Synthesis Example 2: Semi-aromatic polyamide resin (A4)> Adipic acid / hexamethylenediamine = 25.1 / 19.9 mass%, terephthalic acid / hexamethylenediamine 32.4 / 22.6 mass%, benzoic acid 0.01 times molar, ion-exchanged water 60 mass%, and sodium hypophosphite 0.05 mass% were mixed in a 0.10m2 container with a clearance of 1-3% of the radius of the container and 95% of the side below the liquid level. 3 The mixture was charged into a batch-type pressurized polymerization tank, and after thorough nitrogen replacement, the temperature was raised to 160°C and the stirring pressure was 3.0 kg / cm. 2 The mixture was concentrated to a concentration of 85% by weight using a 100-G reactor. The temperature was then raised to a maximum of 300°C over 4 hours with stirring, and the maximum polymerization pressure was increased to 35 kg / cm.2 The discharge was ion-exchanged water, which was supplied at a rate of 3 l / hr by a metering pump, and the water vapor pressure was 35 kg / cm. 2 The reaction was carried out for 0.5 hours while maintaining at -G. The obtained semi-aromatic polyamide resin (A4) was composed of 55.1 mol % of structural units consisting of 1,6-hexamethylenediamine and terephthalic acid and 44.9 mol % of structural units consisting of 1,6-hexamethylenediamine and adipic acid, and had a relative viscosity of 2.3, a melting point of 305°C, an AEG of 25 eq / ton, and a CEG of 150 eq / ton.
[0065] <Synthesis Example 3: Semi-aromatic polyamide resin (A6)> The amount of 1,6-hexamethylenediamine was changed to 9.21 kg, and the amount of acetic acid as the end blocking agent was changed to 286 g. The mixture was subjected to vacuum drying in the same manner as in Synthesis Example 1, to obtain a low-order condensation product. 3 ) was used and reacted for 8 hours in an environment at 230°C and a vacuum of 0.07 KPa to obtain a semi-aromatic polyamide resin. The obtained semi-aromatic polyamide resin (A6) was composed of 66.6 mol% of structural units consisting of 1,6-hexamethylenediamine and terephthalic acid and 33.4 mol% of structural units consisting of 11-aminoundecanoic acid, and had a relative viscosity of 2.5, a melting point of 314°C, an AEG of 40 eq / ton, and a CEG of 0 eq / ton.
[0066] The present examples were carried out using semi-aromatic polyamide resin compositions prepared as exemplified below.
[0067] The components and mass ratios (parts by mass) shown in Tables 2 and 3 were melt-kneaded at the melting point of each polyamide raw material +20°C using a twin-screw extruder STS-35 manufactured by Coperion Co., Ltd. to obtain semi-aromatic polyamide resin compositions of Examples 1 to 10 and Comparative Examples 1 to 7. The raw materials used in producing the semi-aromatic polyamide resin compositions are as follows. The release agent and stabilizer used as other additives were used in a mass ratio of 1:5.
[0068] Semi-aromatic polyamide resin (A1): Semi-aromatic polyamide resin prepared according to Synthesis Example 1 above Semi-aromatic polyamide resin (A2): PA10T (KINGFA Vicnyl®, Tm = 310°C) Semi-aromatic polyamide resin (A3): PA6T / 6I (EMS, Grivory(R) G21, amorphous) Semi-aromatic polyamide resin (A4): Semi-aromatic polyamide resin prepared according to Synthesis Example 2 above Semi-aromatic polyamide resin (A5): PA6T / 6 (BASF Ultramide(R) KR4351, Tm = 295°C) Semi-aromatic polyamide resin (A6): Semi-aromatic polyamide resin prepared according to Synthesis Example 3 above
[0069] Non-fibrous inorganic filler (B1): Calcined kaolin (BASF, Translink(R) 445, surface-treated, average particle size 1.4 μm) Non-fibrous inorganic filler (B2): Calcined kaolin (BASF, Translink(R) 77, surface-treated, average particle size 0.8 μm) Non-fibrous inorganic filler (B3): Diatomaceous earth (EP Minerals, Celatom(R) MW-25, no surface treatment, average particle size 11 μm) Non-fibrous inorganic filler (B4): Wollastonite (Kinseimatec Co., Ltd., KTK(R), surface-treated, average particle size 0.5 to 8.0 μm) Non-fibrous inorganic filler (B5): Glass beads (Potters-Barotini, GB- 731A, surface treated, average particle size 32μm) Non-fibrous inorganic filler (B6): Zeolite (manufactured by Shin Tohoku Chemical Industry Co., Ltd., Zeofil(R) CP50, no surface treatment, average particle size 5 μm) Fibrous inorganic filler (B7): Glass filler (Nippon Electric Glass Co., Ltd., T-275H, surface-treated) Fibrous inorganic filler (B8): Fibrous wollastonite (NYCO, NYGLOS(R) 8, surface-treated)
[0070] Release agent: Magnesium stearate Stabilizer: Pentaerythrityl tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (Irganox1010, manufactured by Chiba Speciality Chemicals)
[0071] [Table 2]
[0072] [Table 3]
[0073] <Examples 1 to 10 and Comparative Examples 1 to 7> (Examples 6 to 8 are reference examples) As is clear from Table 2, Examples 1 to 10 exhibit excellent metal plating peel strength, metal plating appearance, and moldability, and also have reflow solder resistance, and are therefore excellent in properties. Furthermore, Examples 1 to 10 also exhibit excellent moldability, which is an index of higher plating and appearance, as has been required in recent years. On the other hand, Comparative Example 1 does not contain non-fibrous inorganic filler (B), and is therefore poor in metal plating peel strength and metal plating appearance, and is insufficient. Comparative Example 2 uses a semi-aromatic polyamide different from Examples 1 to 8, and is excellent in metal plating peel strength, metal plating appearance, and moldability, but is poor in reflow solder resistance. Comparative Example 3 uses a semi-aromatic polyamide different from Examples 1 to 8, and is excellent in metal plating appearance and moldability, but is poor in metal plating peel strength and reflow solder resistance. Comparative Example 4 uses a semi-aromatic polyamide different from Examples 1 to 8, and is excellent in metal plating appearance, but is poor in metal plating peel strength, reflow solder resistance, and moldability, by adding a fibrous filler to the semi-aromatic polyamide different from Examples 1 to 8. Comparative Example 5 uses a semi-aromatic polyamide different from those used in Examples 1 to 8, and is excellent in metal plating peel strength and metal plating appearance, but is poor in reflow solder resistance and moldability. Comparative Examples 6 and 7 use a fibrous inorganic filler, and are good in metal plating peel strength, metal plating appearance, and reflow solder resistance, but are poor in moldability and insufficient. [Industrial Applicability]
[0074] The semi-aromatic polyamide resin composition of the present invention, by blending a specific inorganic filler in addition to the composition of a semi-aromatic polyamide resin, exhibits good metal plating adhesion and plating appearance and also satisfies solder reflow resistance, making it possible to advantageously produce molded articles requiring metal plating on an industrial scale.
Claims
1. A semi-aromatic polyamide resin composition comprising 10 to 200 parts by mass of a non-fibrous inorganic filler (B) per 100 parts by mass of a semi-aromatic polyamide resin (A), wherein a ratio (C / N ratio) of the number of carbon atoms (C) to the number of nitrogen atoms (N) in the semi-aromatic polyamide resin (A) is 7.3 or more; the semi-aromatic polyamide resin (A) is a semi-aromatic polyamide resin containing 50 to 100 mol % of a repeating unit consisting of a diamine having 6 to 12 carbon atoms and terephthalic acid, and 0 to 50 mol % of a repeating unit consisting of an aminocarboxylic acid or lactam having 10 or more carbon atoms; the diamine having 6 to 12 carbon atoms is at least one selected from 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 2-methyl-1,8-octamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, and 1,12-dodecamethylenediamine; 1. A semi-aromatic polyamide resin composition for plated molded products, wherein the non-fibrous inorganic filler (B) is at least one selected from the group consisting of kaolin and diatomaceous earth.
2. 2. The semi-aromatic polyamide resin composition for plated molded products according to claim 1, wherein the semi-aromatic polyamide resin (A) has a terminal carboxyl group concentration of 5 to 200 eq / ton and a terminal amino group concentration of 0 to 100 eq / ton.
3. The semi-aromatic polyamide resin composition for plated molded products according to claim 1 or 2, wherein the semi-aromatic polyamide resin (A) is a semi-aromatic polyamide resin containing 50 to 100 mol % of a repeating unit consisting of a diamine having 6 to 12 carbon atoms and terephthalic acid, and 0 to 50 mol % of a repeating unit consisting of aminoundecanoic acid or undecane lactam.
4. A plated molded product obtained by plating the semi-aromatic polyamide resin composition for plated molded products according to any one of claims 1 to 3.
Citation Information
Patent Citations
Preparation of silver halide color photographic sensitive material
JP1986090154A
Platable resin composition and its use
JP1991197558A
Anti-rolling hydrofoil device with safety device
JP1996011782A
Molded form
JP1996081627A
Resin composition for metal vapor deposition, metal-deposited molded product and method for producing the metal-deposited molded product
JP2006131821A