Adhesive for polishing pads, double-sided adhesive sheet for polishing pads, multi-layered polishing pads, and single-layered polishing pads

A double-sided adhesive sheet for polishing pads using an acrylic copolymer, synthetic rubber, and curing agent addresses the need for rapid adhesive strength at room temperature and chemical resistance, ensuring effective polishing performance.

JP7586276B1Active Publication Date: 2024-11-19TOYO INK MFG CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023213212
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2024-11-19
Estimated Expiration
2043-12-18

AI Technical Summary

Technical Problem

Existing double-sided adhesive sheets for polishing pads face challenges in developing high adhesive strength quickly at room temperature and maintaining strength in acidic or alkaline environments, while avoiding warping or peeling during polishing processes.

Method used

A double-sided adhesive sheet composed of an acrylic copolymer, synthetic rubber, and a curing agent, with specific ratios and additives, is used to form adhesive layers that adhere at room temperature and maintain strength in harsh chemical conditions.

Benefits of technology

The adhesive sheet achieves rapid development of high adhesive strength at room temperature and maintains strength in acidic or alkaline solutions, preventing peeling and warping during polishing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586276000001
    Figure 0007586276000001
  • Figure 0007586276000002
    Figure 0007586276000002
  • Figure 0007586276000003
    Figure 0007586276000003
Patent Text Reader

Abstract

The object of the present invention is to provide a double-sided pressure-sensitive adhesive sheet that can exhibit high adhesive strength shortly after application even when applied near room temperature (e.g., 23°C) and can maintain a high level of adhesive strength even when immersed in an acidic or alkaline aqueous solution. SOLUTION: The pressure-sensitive adhesive for polishing pads contains an acrylic copolymer (A), a synthetic rubber (B), and a curing agent (C). It is preferable that the synthetic rubber (B) is contained in an amount of 0.05 to 20 parts by mass per 100 parts by mass of the acrylic copolymer (A).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a double-sided pressure-sensitive adhesive sheet for a polishing pad used when polishing objects such as silicon wafers, glass (for liquid crystal, reinforced), hard disks, etc. The present invention also relates to a pressure-sensitive adhesive for a polishing pad for forming the double-sided pressure-sensitive adhesive sheet for a polishing pad. [Background technology]

[0002] Conventionally, glass for liquid crystal displays, substrates for hard disks, optical lenses, silicon wafers, integrated circuits, etc. have been polished using polishing pads. Polishing pads are classified into multi-layer and single-layer types. Multi-layer polishing pads are formed by bonding a top pad and a cushion layer with a double-sided adhesive sheet or a double-sided adhesive sheet for forming a polishing pad. Multi-layer and single-layer polishing pads, i.e., top pads, are fixed to a platen by a double-sided adhesive sheet or a double-sided adhesive sheet for fixing the polishing pad. The double-sided adhesive sheet or double-sided adhesive sheet for forming a multi-layer type polishing pad is required to prevent the top pad from peeling off from the cushion layer during polishing. The double-sided adhesive sheet or double-sided adhesive sheet for fixing a polishing pad to a platen is required to prevent the polishing pad from peeling off from the platen during polishing. In addition, since an acidic or alkaline slurry is used in the polishing process, all of the adhesive sheets or adhesive sheets are required to be acid-resistant or alkaline-resistant.

[0003] Patent Document 1 describes a double-sided adhesive tape having a thermal adhesive layer on one side of a substrate and a pressure-sensitive adhesive layer on the other side as a double-sided adhesive sheet for fixing an abrasive member, and describes that the thermal adhesive layer is preferably configured as a type that is heated and melted, then cooled and solidified to adhere (hot melt adhesive). Specifically, it describes that a thermal adhesive layer for an abrasive member formed using a hot melt adhesive is thermocompressed to an adherend at 50°C, left in an environment of 23°C for 30 minutes, and then the adhesive strength is measured. Furthermore, Patent Document 2 describes the use of an adhesive containing an acrylic copolymer (A), a liquid xylene-based resin (B), and an isocyanate curing agent (C) as an adhesive sheet for attaching the adhesive sheet to a polishing pad without heat lamination or heat pressing. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-213192 A [Patent Document 2] JP 2016-183211 A Summary of the Invention [Problem to be solved by the invention]

[0005] Hot melt adhesives such as those described in Patent Document 1 are preferable in that they are heated and melted, and after the adherends are stacked together, they solidify quickly when the heat source is removed, completing the bonding process in a short time, and that they tend to exhibit a relatively large adhesive strength (i.e., peel strength). However, when the double-sided adhesive sheet is applied to the polishing pad, which is the adherend, there is a problem that application at high temperatures causes the polishing pad to warp or ripple, resulting in a decrease in polishing accuracy. Application at high temperatures also increases the environmental load and costs. Therefore, at the time of the invention described in Patent Document 1, application at 50°C was aimed for. However, in recent years, application at lower temperatures has been desired.

[0006] The adhesive sheet described in Patent Document 2 is excellent in that it can exert a large adhesive strength even when the adhesive sheet is attached to a polishing pad without heat lamination or heat pressing, and can maintain a high level of adhesive strength even when immersed in an acidic or alkaline aqueous solution. However, it takes about 24 hours for the adhesive to develop a stable and strong adhesive strength after application. In order to quickly carry out quality inspections and shipping decisions after application, there is a demand for adhesives for polishing pads that develop a stable adhesive strength as soon as possible after application.

[0007] The present invention has been made in consideration of these problems, and its object is to provide a double-sided pressure-sensitive adhesive sheet that can develop high adhesive strength shortly after application, even when applied at around room temperature (e.g., 23°C), and that can maintain a high level of adhesive strength even when immersed in an acidic or alkaline aqueous solution. [Means for solving the problem]

[0008] [1] The present invention relates to an adhesive for a polishing pad, comprising an acrylic copolymer (A), a synthetic rubber (B), and a curing agent (C). It is preferable that the synthetic rubber (B) is contained in an amount of 0.05 to 20 parts by mass based on 100 parts by mass of the acrylic copolymer (A). The present invention preferably further comprises a tackifier resin.

[0009] [2] The present invention relates to a double-sided pressure-sensitive adhesive sheet for a polishing pad, comprising a base sheet, a first adhesive layer located on one side of the base sheet, and a second adhesive layer located on the other side of the base sheet, The first adhesive layer is an adhesive layer formed from the adhesive for a polishing pad according to [1], A double-sided pressure-sensitive adhesive sheet for a polishing pad according to the following (1) or (2): (1) Double-sided adhesive sheet for polishing pads to fix the top pad to the cushion layer (2) Double-sided adhesive sheet for polishing pads to secure the top pad to the platen In the case of (1) above, the first adhesive layer is in contact with the top pad, and the second adhesive layer is in contact with the cushion layer, In the case of (2) above, the first adhesive layer contacts the top pad, and the second adhesive layer contacts the base plate. The present invention relates to a double-sided pressure-sensitive adhesive sheet for a polishing pad.

[0010] [3] The present invention provides a polishing pad comprising a top pad, a polishing pad having a first adhesive layer in contact with one surface of the top pad, and a polishing pad having a first adhesive layer in contact with the first adhesive layer of the top pad; The invention relates to a multi-layer polishing pad in which a second adhesive layer of a double-sided adhesive sheet for a polishing pad is in contact with one surface of a cushion layer, The double-sided adhesive sheet for a polishing pad includes a base sheet, a first adhesive layer located on one side of the base sheet, and a second adhesive layer located on the other side of the base sheet, The present invention relates to a multi-layer polishing pad, in which the first adhesive layer is an adhesive layer formed from the adhesive for a polishing pad according to [1].

[0011] [4] The present invention relates to a single-layer polishing pad in which a first adhesive layer of a double-sided adhesive sheet for a polishing pad is in contact with one surface of a top pad, The double-sided adhesive sheet for a polishing pad includes a base sheet, a first adhesive layer located on one side of the base sheet, and a second adhesive layer located on the other side of the base sheet, The first adhesive layer relates to a single-layer type polishing pad, which is an adhesive layer formed from the adhesive for a polishing pad according to [1]. Effect of the Invention

[0012] The present invention makes it possible to provide a double-sided pressure-sensitive adhesive sheet that can develop high adhesive strength to a top pad shortly after application, even when applied at near room temperature (e.g., 23°C), and that can maintain a high level of adhesive strength even when immersed in an acidic or alkaline aqueous solution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] <Acrylic copolymer (A)> In the present invention, the acrylic copolymer (A) is a (meth)acrylic polymer that can be synthesized using an acrylic monomer, and examples of the acrylic monomer include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, propyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, (meth)acrylamide, vinyl acetate, and acrylonitrile, but are not limited thereto. They may be used alone or in combination of two or more. When synthesizing, polymerization methods such as solution polymerization, emulsion polymerization, bulk polymerization, or polymerization by ultraviolet irradiation can be used, but in the present invention, it is preferable to use solution polymerization, which is easy to control the reaction and physical properties.

[0014] The acrylic copolymer (A) preferably contains a monomer having a carboxyl group (hereinafter referred to as a carboxyl group-containing monomer). The carboxyl group-containing monomer is preferably used in an amount of 0.1 to 10 parts by weight. When the amount is 0.1 part by weight or more, the crosslink density with the curing agent is improved, thereby increasing the cohesive force, and the polishing pad and the adhesive surface are less likely to shift laterally during the polishing process, and the acid resistance is improved. On the other hand, when the amount is 10 parts by weight or less, the crosslink density with the curing agent is not excessive, so the anchoring property to the top pad is increased, peeling is less likely to occur between the top pad and the adhesive layer during the polishing process, and the alkali resistance and acid resistance are improved. From the above viewpoint, 0.5 to 8 parts by weight is more preferable.

[0015] The carboxyl group-containing monomer may be any monomer having a carboxyl group, such as (meth)acrylic acid, itaconic acid, maleic acid, etc., with (meth)acrylic acid being preferred. These monomers may be used alone or in combination of two or more.

[0016] In addition, it is preferable that the acrylic copolymer (A) contains a monomer having a hydroxyl group (hereinafter referred to as a hydroxyl group-containing monomer). It is preferable to use 0.01 to 1.5 parts by weight of the hydroxyl group-containing monomer. When it is 0.01 part by weight or more, the crosslink density with the curing agent increases, and lateral displacement between the polishing pad and the adhesive surface is unlikely to occur during the polishing process. When it is 1.5 parts by weight or less, the crosslink density with the curing agent does not become excessive, so that the anchoring property to the top pad increases, peeling is unlikely to occur between the top pad and the adhesive layer during the polishing process, and the alkali resistance and acid resistance are improved. From the above viewpoint, 0.05 to 1 part by weight is more preferable.

[0017] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycidyl (meth)acrylate, N-methylolacrylamide, and hydroxypropyl (meth)acrylate. Among these, from the viewpoint of appropriate crosslinking with the curing agent, a hydroxyl group-containing monomer having an alkylene group having 1 to 3 carbon atoms is preferred because it can further improve cohesive strength, heat resistance, and adhesion. And, 2-hydroxyethyl (meth)acrylate is more preferred. These monomers may be used alone or in combination of two or more.

[0018] In the present invention, for the copolymerization, a conventionally known polymerization initiator such as a peroxide-based polymerization initiator or an azobis-based polymerization initiator can be used. Examples of the organic peroxide polymerization initiator include benzoyl peroxide, di-t-butyl peroxide, cumene hydroperoxide, t-butyl peroxybenzoate, t-butyl peroxy neodecanoate, and t-butyl peroxy 2-ethylhexanoate. Examples of the azo polymerization initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis(2-methylpropionamidine) disulfate, and 2,2'-azobis(N,N'-dimethyleneisobutylamidine). These polymerization initiators may be used alone or in combination of two or more kinds.

[0019] In the present invention, the weight average molecular weight of the acrylic copolymer (A) is preferably 300,000 to 2,000,000, and more preferably 600,000 to 1,500,000. If the weight average molecular weight is 300,000 or more, the cohesive force increases, improving heat resistance, and lateral displacement between the polishing pad and the adhesive surface during the polishing process is less likely to occur. On the other hand, if the weight average molecular weight is 2,000,000 or less, the cohesive force is not too high, so the anchoring ability to the top pad increases, and peeling between the top pad and the adhesive layer is less likely to occur during the polishing process. In the present invention, the weight average molecular weight is the weight average molecular weight calculated as polystyrene by GPC measurement, and the GPC measurement conditions are as follows: Apparatus: SHIMADZU Prominence (manufactured by Shimadzu Corporation), column: TOSO HTS K-GELGMHXL (manufactured by Tosoh Corporation), solvent: tetrahydrofuran, flow rate: 0.5 mL / min, temperature: 40°C, sample concentration: 0.1 wt%, sample injection amount: 100 μL.

[0020] <Synthetic rubber (B)> In the present invention, the synthetic rubber (B) functions as a tackifier resin. The synthetic rubber (B) includes liquid rubber (B1) and styrene-based elastomer (B2). The liquid rubber (B1) is not particularly limited, but is preferably a diene-based liquid rubber, and preferably has a number average molecular weight of 100 to 60000. In the present invention, the liquid state of the liquid rubber (B1) is defined as a state in which the bottom area is 10 cm 2 This is the physical property in which, when a sample is placed in a cylindrical container with a height of 80 cm to a height of 20 cm and the container is placed horizontally at room temperature (23°C), the sample reaches one edge of the top of the container within 10 minutes. Examples of such liquid rubber (B1) include polyisoprenes manufactured by Kuraray Co., Ltd., such as LIR-30 (number average molecular weight: 28,000, viscosity at 38° C. (hereinafter the same): 70 Pa s), LIR-50 (number average molecular weight: 54,000, viscosity: 500 Pa s), LIR-390 (number average molecular weight: 48,000, viscosity: 400 Pa s), LIR-403 (number average molecular weight: 34,000, viscosity: 200 Pa s), and LIR-410 (number average molecular weight: 30,000, viscosity: 430 Polybutadienes manufactured by Kuraray Co., Ltd. include LBR-302 (number average molecular weight: 5,500, viscosity: 0.6 Pa·s), LBR-307 (number average molecular weight: 8,000, viscosity: 1.5 Pa·s), LBR-305 (number average molecular weight: 26,000, viscosity: 40 Pa·s), LBR-352 (number average molecular weight: 9,000, viscosity: 6 Pa·s), and LBR-361 (number average molecular weight: 5,500, viscosity: 5.5 Pa·s), and polybutadienes manufactured by Nippon Soda Co., Ltd. include NISSO Examples of the liquid rubber (B1) include PB B-3000 (number average molecular weight: 3200, viscosity at 45°C (hereinafter the same): 21 Pa·s), NISSO PB B-1000 (number average molecular weight: 1200, viscosity: 1 Pa·s), Poly bd R-45HT (number average molecular weight: 2800, viscosity at 30°C (hereinafter the same): 5 Pa·s), which is a hydroxyl-terminated polybutadiene manufactured by Idemitsu Kosan Co., Ltd., Epol (number average molecular weight: 2500, viscosity: 75 Pa·s), which is a hydrogenated isoprene polyol manufactured by Idemitsu Kosan Co., Ltd., and Poly ip (number average molecular weight: 2500, viscosity: 7.5 Pa·s), which is a hydroxyl-terminated polyisoprene manufactured by Idemitsu Kosan Co., Ltd. The liquid rubber (B1) may be used alone or in combination of two or more kinds. The viscosity values ​​are measured one minute after starting measurement by weighing an appropriate amount of sample, setting the temperature to each temperature, and then appropriately selecting the rotor and rotation speed according to the viscosity measured using a TVB-10M viscometer manufactured by Toki Sangyo Co., Ltd.

[0021] As the styrene-based elastomer (B2), a known styrene-based copolymer can be suitably used, and there is no particular limitation. Specific examples include styrene-butadiene-styrene copolymer (hereinafter simply referred to as SBS), styrene-butadiene-styrene-butadiene copolymer (hereinafter simply referred to as SBSB), styrene-butadiene / butylene-styrene copolymer (hereinafter simply referred to as SBBS), styrene-ethylene / butylene-styrene copolymer (hereinafter simply referred to as SEBS), styrene-ethylene / propylene-styrene copolymer (hereinafter simply referred to as SEPS), styrene-ethylene-ethylene / propylene-styrene copolymer (hereinafter simply referred to as SEEPS), and styrene-isoprene-styrene block copolymer (hereinafter simply referred to as SIS). The weight average molecular weight of the styrene-based elastomer (B2) is preferably 20,000 to 120,000. The lower limit of the weight average molecular weight is more preferably 30,000 or more, even more preferably 45,000 or more, and particularly preferably 60,000 or more. By having a weight average molecular weight of 25,000 or more, the holding power of the entire adhesive layer is improved. On the other hand, the condition of the weight average molecular weight is more preferably 90,000 or less, even more preferably 75,000 or less, and particularly preferably 65,000 or less. By having a weight average molecular weight of 120,000 or less, it is possible to avoid deterioration of compatibility with the acrylic copolymer (A).

[0022] The synthetic rubber (B) is preferably 0.05 to 20 parts by weight per 100 parts by weight of the acrylic copolymer (A). By being 0.05 parts by weight or more, even when applied at a low temperature, high adhesive strength to the top pad can be exhibited in a short time after application, and peeling of the adhesive surface between the top pad and the cushion layer, and between the top pad and the platen in the polishing process can be effectively prevented. By being 20 parts by weight or less, compatibility with the acrylic copolymer (A) becomes easy, and retention power can be easily improved. From the above viewpoint, 0.1 to 15 parts by weight is more preferable.

[0023] <Other tackifier resins> In the present invention, in addition to the above synthetic rubber (B), resins generally known as tackifier resins can be used as necessary within the limits that do not impair the required performance. Examples of common tackifier resins include rosin-based resins such as petroleum resins, rosin esters, polymerized rosins, hydrogenated rosins, disproportionated rosins, maleic acid modified rosins, fumaric acid modified rosins, and rosin phenolic resins; terpene-based resins such as α-pinene resins, β-pinene resins, dipentene resins, aromatic modified terpene resins, hydrogenated terpene resins, terpene phenolic resins, acid modified terpene resins, and styrenated terpene resins; and further examples include coumarone-indene resins, styrene-based resins, and alkylphenol resins, but are not limited thereto. Two or more of these tackifier resins may be used in combination, and it is preferable to use a petroleum resin or a copolymer thereof.

[0024] Examples of petroleum resins include FTR-6100 (softening point 100°C), FTR-6110 (softening point 110°C), and FTR-6125 (softening point 125°C) manufactured by Mitsui Chemicals, Petrotac 70 (softening point 70°C), Petrotac 90 (softening point 95°C), Petrotac 120V (softening point 120°C), Petcol 100T (softening point 100°C), Petcol 120 (softening point 120°C), Petcol 130 (softening point 125°C), Petcol LX (softening point 95°C) manufactured by Toho Chemical Industry, Toho Resin 120S (softening point 120°C) manufactured by Arizona Chemical, Sylvares SA-85 (softening point 85°C), Sylvares SA-100 (softening point 100°C), Sylvares Examples of the resin include SA-120 (softening point 120° C.), Sylvares SA-140 (softening point 140° C.), and Neopolymer S (softening point 92° C.) manufactured by ENEOS Corp., but are not limited thereto. Petroleum resins having a softening point of 80° C. to 150° C. are preferred, and two or more of these may be used in combination.

[0025] When petroleum resin is used in combination with synthetic rubber (B), the anchoring property for the top pad is increased, peeling between the top pad and the adhesive layer is less likely to occur during the polishing process, and alkali and acid resistance are also improved. In addition, the cohesive force is improved, making it less likely that lateral shifting of the adhesive surface between the top pad and the adhesive layer occurs during the polishing process.

[0026] The other tackifier resin is preferably used in an amount of 5 to 80 parts by weight per 100 parts by weight of the acrylic copolymer (A). When the amount is 5 parts by weight or more, the anchoring property to the top pad is increased, peeling is unlikely to occur between the top pad and the adhesive layer during the polishing process, and acid resistance and alkali resistance are improved. When the amount is 80 parts by weight or less, the adhesion and cohesive force are not reduced due to the tackifier resin, so that lateral displacement and peeling are unlikely to occur between the top pad and the adhesive layer during the polishing process. From the above viewpoint, 10 to 40 parts by weight is more preferable, and 10 to 30 parts by weight is even more preferable.

[0027] <Hardening agent (C)> The curing agent (C) of the present invention functions as a crosslinking agent, and examples thereof include isocyanate-based curing agents, epoxy-based curing agents, aziridine-based curing agents, and metal chelate curing agents. Examples of isocyanate-based curing agents include, but are not limited to, adducts of isocyanate compounds such as tolylene diisocyanate, xylylene diisocyanate, and hexamethylene diisocyanate with polyols such as trimethylolpropane. As the adduct, the isocyanate compound is preferably tolylene diisocyanate, and the polyol is preferably trimethylolpropane. Examples of epoxy compounds include ethylene glycol diglycidyl ether, triglycidyl ether, trimethylolpropane triglycidyl ether, and glycerin diglycidyl ether. Examples of metal chelate compounds include compounds in which polyvalent metals such as aluminum, zinc, iron, tin, titanium, antimony, magnesium, and vanadium are derivatized into acetylacetone or ethyl acetoacetate. Examples of aziridine compounds include N,N'-toluene-2,4-bis(1-aziridinecarboxylate), N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxylate)triethylenemelamine, bisisopropyl-1-(2-methylaziridine), and tri-1-aziridinylphosphine oxide. Two or more of the above crosslinking agents may be used in combination.

[0028] The crosslinking agent is preferably 0.1 to 10 parts by weight, more preferably 0.3 to 8 parts by weight, in total, based on 100 parts by weight of the acrylic copolymer (A). When the amount is 0.1 part by weight or more, the crosslinking density is improved, the cohesive force is increased, and lateral displacement between the top pad and the adhesive layer is unlikely to occur during the polishing process. On the other hand, when the amount is 10 parts by weight or less, the crosslinking density is not excessive, so the anchoring property to the top pad is increased, and peeling between the top pad and the adhesive layer is unlikely to occur during the polishing process.

[0029] <Other additives> The adhesive of the present invention may contain various additives, such as fillers, pigments, dyes, diluents, antioxidants, polymerization inhibitors, UV absorbers, UV stabilizers, coupling agents, etc., which are blended into known adhesive compositions as necessary, and two or more of these may be used. The amount of the additives added is not particularly limited as long as it is an amount that provides the required physical properties.

[0030] <About the composition of the adhesive sheet> The pressure-sensitive adhesive sheet of the present invention is a double-sided pressure-sensitive adhesive sheet for a polishing pad, comprising a base sheet, a first pressure-sensitive adhesive layer located on one side of the base sheet, and a second pressure-sensitive adhesive layer located on the other side of the base sheet, The first adhesive layer is an adhesive layer formed from the adhesive for a polishing pad, the adhesive comprising an acrylic copolymer (A), a synthetic rubber (B), and a curing agent (C); A double-sided pressure-sensitive adhesive sheet for a polishing pad according to the following (1) or (2): (1) Double-sided adhesive sheet for polishing pads to fix the top pad to the cushion layer (2) Double-sided adhesive sheet for polishing pads to secure the top pad to the platen In the case of (1) above, the first adhesive layer is in contact with the top pad, and the second adhesive layer is in contact with the cushion layer, In the case of (2) above, the first adhesive layer contacts the top pad, and the second adhesive layer contacts the base plate. This is a double-sided adhesive sheet for polishing pads. The second adhesive layer, which is in contact with the cushion layer or the base plate, can be formed from an adhesive containing an acrylic copolymer (A), a synthetic rubber (B), and a curing agent (C) like the first adhesive layer, or can be formed from an acrylic adhesive or a rubber-based adhesive.

[0031] Examples of the substrate sheet in the present invention include plastic films such as polyethylene, polypropylene, polyester, polystyrene, polyethylene terephthalate (hereinafter also referred to as PET), polyvinyl chloride, polycarbonate, cellophane, etc., papers such as fine paper, craft paper, crepe paper, glassine paper, etc., fabrics such as woven fabrics and nonwoven fabrics, and foams such as urethane foams and EPDM foams, and are not particularly limited thereto, but are preferably plastic films both sides of which are corona-treated. The thickness of the substrate is preferably 5 to 300 μm, more preferably 10 to 200 μm.

[0032] A top pad, also called an abrasive cloth, is a member that comes into direct contact with the object to be polished during polishing, and examples of such a pad include hard polyurethane sheets, synthetic leather, suede, velour, etc. A top pad may be used as a single layer fixed to a surface plate as in the above-mentioned (2), or may be attached to a cushion layer to form the outermost surface of a multi-layer type abrasive pad. Examples of the cushion layer include foams and nonwoven fabrics. Examples of the foams include urethane foams, polyethylene foams, polypropylene foams, etc. Examples of the nonwoven fabrics include those made from polyester, etc., and those made from natural materials such as wool, etc.

[0033] The double-sided pressure-sensitive adhesive sheet for a polishing pad of the present invention can be produced, for example, by the following method (1) or (2). (1) An adhesive system for forming a first adhesive layer and an adhesive system for forming a second adhesive layer are each applied to a release liner to form a first adhesive layer and a second adhesive layer, and then the first adhesive layer and the second adhesive layer are bonded to each side of a base sheet, respectively. (2) Either the adhesive for forming the first adhesive layer or the adhesive for forming the second adhesive layer is coated on one side of the base sheet to form the first adhesive layer or the second adhesive layer. The other adhesive, either the adhesive for forming the first adhesive layer or the adhesive for forming the second adhesive layer, is coated on a separate release liner to form the other adhesive layer, and the other adhesive layer formed on the release liner is attached to the side of the base sheet on which no adhesive layer is formed. Generally, each adhesive layer is protected with a release liner until the adhesive sheet is to be used.

[0034] The release liner has a release layer formed by applying a release agent to a substrate such as paper, plastic film, or synthetic paper. Examples of the release agent include silicone, alkyd resin, melamine resin, fluororesin, and acrylic resin. The removable pressure-sensitive adhesive of the present invention has an effect that the release force is not easily dependent on the type of release agent. The thickness of the release liner is not particularly limited, but is about 10 to 200 μm.

[0035] The adhesive can be applied by a known method such as a roll coater method, a comma coater method, a lip coater method, a die coater method, a reverse coater method, a silk screen method, a gravure coater method, etc. After application, the adhesive can be dried using a hot air oven, an infrared heater, etc., but is not limited thereto. The thickness of the adhesive layer is preferably 25 to 200 μm, more preferably 50 to 150 μm.

[0036] <Multi-layer polishing pad> The multi-layered polishing pad of the present invention is a multi-layered polishing pad in which a first adhesive layer of a double-sided adhesive sheet for a polishing pad is laminated on one surface of a top pad, The double-sided adhesive sheet for a polishing pad includes a base sheet, a first adhesive layer located on one side of the base sheet, and a second adhesive layer located on the other side of the base sheet, The first adhesive layer is an adhesive layer formed from the adhesive for a polishing pad, the adhesive comprising an acrylic copolymer (A), a synthetic rubber (B), and a curing agent (C); The second adhesive layer is in contact with the cushion layer.

[0037] The multi-layer polishing pad of the present invention can be produced, for example, as follows. The release liner covering the first adhesive layer is peeled off, and the top pad is superimposed on the first adhesive layer. When superimposing, no special heating is required, but heating can be used. After superimposing, the layers are left at room temperature for about 3 hours to develop stable peel strength. Next, the release liner covering the second adhesive layer is peeled off, and the cushion layer is superimposed on the second adhesive layer. When a conventional adhesive is used to form the second adhesive layer, it is preferable to leave the cushion layer on the second adhesive layer for about 24 hours at room temperature. Alternatively, the release liner covering the second adhesive layer is first peeled off, and the cushion layer is superimposed on the second adhesive layer. When a conventional adhesive is used to form the second adhesive layer, it is preferable to leave the cushion layer on the second adhesive layer at about room temperature for about 24 hours. Next, the release liner covering the first adhesive layer is peeled off, and the top pad is superimposed on the first adhesive layer. When superimposing, no special heating is required, but heating can be performed. After superimposing, leaving it at about room temperature for about 3 hours allows stable peel strength to be developed. In addition, if an adhesive containing an acrylic copolymer (A), synthetic rubber (B), and a curing agent (C) is used to form the second adhesive layer, as in the case of the first adhesive layer, the time for leaving the second adhesive layer at around room temperature after superimposing the cushion layer on top of the second adhesive layer can be reduced to about 3 hours.

[0038] The other side of the cushion layer of the multi-layered polishing pad can be attached to the surface plate, and the multi-layered polishing pad can be fixed to the surface plate. When attaching the cushion layer of the multi-layered polishing pad to the surface plate, various double-sided adhesive sheets can be used.

[0039] <Single-layer polishing pad> The double-sided pressure-sensitive adhesive sheet for a polishing pad of the present invention can also be used to form a single-layer type polishing pad. That is, the release liner covering the first adhesive layer is peeled off, and the top pad is laminated onto the first adhesive layer. When laminating, no special heating is required, but heating is also possible. After laminating, it is possible to form a single-layer polishing pad with stable peel strength by leaving it at around room temperature for about 3 hours. The second adhesive layer of the single-layered polishing pad can be attached to the surface plate, and the single-layered polishing pad can be fixed to the surface plate. When attaching the single-layered polishing pad to the surface plate, various double-sided adhesive sheets can be used. EXAMPLES

[0040] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples. In the examples, parts and % indicate parts by weight and % by weight, respectively.

[0041] (Measurement of weight average molecular weight) The measurements were carried out in the same manner as described in the specification. (Method of measuring viscosity) The measurements were carried out in the same manner as described in the specification. (Method of measuring softening point) The values ​​were measured in accordance with JISK2207.

[0042] <Production Example 1> Using a reaction apparatus equipped with a stirrer, reflux condenser, nitrogen inlet tube, thermometer, and dropping tube, 50% by weight of the total amount of each monomer in Table 1, 0.03 parts of Perbutyl O as an initiator, and 50 parts of ethyl acetate as a solvent were charged into a reaction vessel under a nitrogen atmosphere, and the remaining monomers, 35 parts of ethyl acetate, and 0.07 parts of Perbutyl O were added and mixed to the dropping tube. After heating the reaction vessel and confirming reflux, the monomer mixture was dropped from the dropping tube over about 1 hour, and the reaction was continued at about 80 ° C. After the reaction was completed, the mixture was cooled and diluted with ethyl acetate to obtain a solution of acrylic copolymer A1. The non-volatile content of the solution of acrylic copolymer A1 was 47%, and the weight average molecular weight of acrylic copolymer A1 was 600,000.

[0043] <Production Examples 2 to 7> In the same manner as in Production Example 1, solutions of acrylic copolymers A2 to A7 were obtained according to the monomer formulations in Table 1.

[0044] [Table 1]

[0045] The abbreviations in Table 1 are as follows: 2EHA: 2-Ethylhexyl acrylate BA: Butyl acrylate EA: Ethyl acrylate VAC: Vinyl acetate AA: Acrylic acid 2HEA: 2-hydroxyethyl acrylate

[0046] <Example 1> As shown in Table 2, the solution containing 100 parts by weight of the acrylic copolymer A1 obtained in Production Example 1 was mixed with 1.4 parts of LIR-410 (polyisoprene manufactured by Kuraray Co., Ltd., number average molecular weight 30,000, viscosity 430 Pa·s) as liquid rubber (B1-1), 19.4 parts of Haritac PCJ (polymerized rosin ester manufactured by Harima Chemical Group Co., Ltd., softening point 123°C) as other tackifier resins, 7.5 parts of Neopolymer S (aromatic hydrocarbon resin manufactured by ENEOS Co., Ltd., softening point 92°C), 0.5 parts by weight of Mytec GP-1 (ethyl acetate solution of tolylene diisocyanate trimethylolpropane adduct with 37.5% non-volatile content manufactured by Mitsubishi Chemical Co., Ltd.), 0.4 parts of antioxidant, and an appropriate amount of ethyl acetate to obtain an adhesive with a non-volatile content of 47%. The values ​​in Table 2 represent parts.

[0047] The resulting adhesive was then coated onto a commercially available release liner using a comma coater so that the adhesive layer would be 80 μm thick after drying, and then dried in a drying oven at 100° C. for 2 minutes to remove the solvent, and then laminated to one side of a 25 μm PET film. Separately, a commercially available release liner was coated using a comma coater so that the adhesive layer would be 80 μm thick after drying, and then dried in a drying oven at 100° C. for 2 minutes to remove the solvent, and then laminated to the other side of a 25 μm PET film to obtain a double-sided adhesive sheet with a total thickness of 185 μm, and the performance of the double-sided adhesive sheet was evaluated according to the method described below.

[0048] <Examples 2 to 13> As shown in Table 2, pressure sensitive adhesives and double-sided pressure sensitive adhesive sheets were obtained in the same manner as in Example 1 except that the type of synthetic rubber (B) was changed, and the performance of the double-sided pressure sensitive adhesive sheets was evaluated.

[0049] <Examples 14 to 19> As shown in Table 3, pressure sensitive adhesives and double-sided pressure sensitive adhesive sheets were obtained in the same manner as in Example 1, except that the type of acrylic copolymer was changed, and the performance of the double-sided pressure sensitive adhesive sheets was evaluated.

[0050] <Examples 20 to 23> As shown in Table 3, pressure sensitive adhesives and double-sided pressure sensitive adhesive sheets were obtained in the same manner as in Example 1 except that the amount of liquid rubber (B1-1) was changed, and the performance of the double-sided pressure sensitive adhesive sheets was evaluated.

[0051] <Example 24> As shown in Table 3, a pressure-sensitive adhesive and a double-sided pressure-sensitive adhesive sheet were obtained in the same manner as in Example 1, except that no antioxidant was used, and the performance of the double-sided pressure-sensitive adhesive sheet was evaluated.

[0052] <Examples 25 to 31> As shown in Table 4, pressure sensitive adhesives and double-sided pressure sensitive adhesive sheets were obtained in the same manner as in Example 1, except that the type and amount of tackifier resin was changed, and the performance of the double-sided pressure sensitive adhesive sheets was evaluated.

[0053] <Examples 32 to 36> As shown in Table 4, pressure sensitive adhesives and double-sided pressure sensitive adhesive sheets were obtained in the same manner as in Example 1 except that the type and amount of curing agent (C) was changed, and the performance of the double-sided pressure sensitive adhesive sheets was evaluated.

[0054] <Comparative Examples 1 to 2> As shown in Table 4, in Comparative Example 1, no synthetic rubber (B) was used, and in Comparative Example 2, no curing agent (C) was used, but in the same manner as in Example 1, an adhesive and a double-sided adhesive sheet were obtained, and the performance of the double-sided adhesive sheet was evaluated.

[0055] The abbreviations in Tables 2 to 4 are as follows. Synthetic rubber (B) B1-1: LIR-410 Polyisoprene manufactured by Kuraray Co., Ltd., number average molecular weight: 30,000, viscosity: 430 Pa·s B1-2: LIR-390 Polyisoprene manufactured by Kuraray Co., Ltd., number average molecular weight: 48,000, viscosity: 400 Pa·s B1-3: LIR-30 Polyisoprene manufactured by Kuraray Co., Ltd., number average molecular weight: 28,000, viscosity: 70 Pa·s B1-4: LIR-403 Polyisoprene manufactured by Kuraray Co., Ltd., number average molecular weight: 34,000, viscosity: 200 Pa·s B1-5: LBR-305 Polybutadiene manufactured by Kuraray Co., Ltd., number average molecular weight: 26,000, viscosity: 40 Pa·s B1-6: LBR-352 Polybutadiene manufactured by Kuraray Co., Ltd., number average molecular weight: 9,000, viscosity: 6 Pa·s B1-7: LBR-361 Polybutadiene manufactured by Kuraray Co., Ltd., number average molecular weight: 5,500, viscosity: 5.5 Pa·s B1-8: NISSO PB B-3000 Polybutadiene manufactured by Nippon Soda Co., Ltd., number average molecular weight 3200, viscosity 21 Pa·s B1-9: NISSO PB B-1000 Polybutadiene manufactured by Nippon Soda Co., Ltd., number average molecular weight 1200, viscosity 1 Pa·s B1-10: Poly bd R-45HT, hydroxyl-terminated polybutadiene manufactured by Idemitsu Kosan Co., Ltd., number average molecular weight 2800, viscosity 5 Pa·s B1-11: Epol Hydrogenated isoprene polyol manufactured by Idemitsu Kosan Co., Ltd., number average molecular weight 2500, viscosity 75 Pa·s B1-12: Poly ip, hydroxyl-terminated polyisoprene manufactured by Idemitsu Kosan Co., Ltd., number average molecular weight 2500, viscosity 7.5 Pa·s B2: G-1650 (Kraton styrene-ethylene / butylene-styrene block copolymer, weight average molecular weight 96,000) In addition, B1-1 to B1-12 have a base area of ​​10 cm 2 When a sample was placed in a cylindrical container 80 cm high to a height of 20 cm and the container was placed horizontally at room temperature (23°C), the sample reached one edge of the top of the container within 10 minutes.

[0056] Hardener (C) C1: Mytec GP-105A, a 37.5% non-volatile solution of tolylene diisocyanate trimethylolpropane adduct manufactured by Mitsubishi Chemical Corporation in ethyl acetate C2: Tetrad X, a toluene / IPA mixed solution of multifunctional epoxy resin from Mitsubishi Gas Chemical Co., Ltd. with 5% non-volatile content C3: Chemitite PZ33, a toluene / IPA mixed solution of polyfunctional aziridine resin with 5% non-volatile content manufactured by Nippon Shokubai Co., Ltd.

[0057] (Other tackifier resin D) D1: Haritac PCJ (Harima Chemical Group polymerized rosin ester, softening point 123°C) D2: Neopolymer S, an aromatic hydrocarbon resin manufactured by ENEOS Corporation, with a softening point of 92°C D3: Alcon P100 Hydrogenated petroleum resin manufactured by Arakawa Chemical Industries, Ltd., softening point 100°C D4: Super Ester A125, a special rosin ester manufactured by Arakawa Chemical Industries, Ltd., with a softening point of 125°C D5: ECR5380 Hydrogenated alicyclic resin manufactured by ExxonMobil Corporation, softening point 86℃

[0058] [Evaluation method] <Preparation of test specimen> A sample measuring 10 mm in length and 25 mm in width was cut out from each double-sided PSA sheet obtained in each Example and Comparative Example, and the release liner was peeled off at three different environmental temperatures (23° C., 50° C., and 100° C.) The exposed adhesive layer was placed on a top pad (a commercially available hard urethane pad) and pressed back and forth once with a 2 kg roll. In the case of 23°C, the test pieces were left in an environment of 23°C for 3 hours or 24 hours, and then prepared for measurement. In the case of 50°C and 100°C, the sample was transferred to an environmental temperature of 23°C immediately after compression bonding, and left in an environment of 23°C - 50% for 3 hours to prepare a test piece for measurement.

[0059] <<Initial>> After leaving the test pieces in an environment of 23°C-50% for a specified time, the peel strength was immediately measured in the same environment using a tensile test at a peel speed of 300 / min and a peel angle of 180° in accordance with the measurement method of JIS Z1528.

[0060] <<After alkali immersion>> The test piece that had been left in an environment of 23°C-50% for 3 hours was then immersed in an aqueous solution adjusted to pH 11.5 with sodium hydroxide at 40°C for 24 hours. After that, the sample was removed from the aqueous solution and washed with water, and the peel strength at a peel angle of 180 degrees was measured in the same manner as for the initial case.

[0061] <<After acid immersion>> The test pieces that had been left in an environment of 23°C-50% for the specified 3 hours were then immersed for 24 hours in a 40°C aqueous solution adjusted to pH 1.5 with sulfuric acid. After that, the samples were taken out of the aqueous solution and washed with water, and the peel strength at a peel angle of 180 degrees was measured in the same manner as for the initial case.

[0062] [Table 2]

[0063] [Table 3]

[0064]

Table 4

Claims

1. The present invention comprises an acrylic copolymer (A), a synthetic rubber (B), and a curing agent (C), The synthetic rubber (B) is contained in an amount of 0.05 to 20 parts by mass relative to 100 parts by mass of the acrylic copolymer (A), The adhesive for a polishing pad, wherein the synthetic rubber (B) is either a liquid rubber (B1) or a styrene-based elastomer (B2).

2. The adhesive for a polishing pad according to claim 1 , further comprising a tackifier resin.

3. A double-sided adhesive sheet for a polishing pad, comprising a base sheet, a first adhesive layer located on one side of the base sheet, and a second adhesive layer located on the other side of the base sheet, The first adhesive layer is an adhesive layer formed from the adhesive for a polishing pad according to claim 1 or 2, A double-sided pressure-sensitive adhesive sheet for a polishing pad according to the following (1) or (2): (1) Double-sided adhesive sheet for polishing pads to fix the top pad to the cushion layer (2) Double-sided adhesive sheet for polishing pads to fix the top pad to the platen In the case of (1), the first adhesive layer is in contact with the top pad, and the second adhesive layer is in contact with the cushion layer; In the case of (2), the first adhesive layer contacts the top pad, and the second adhesive layer contacts the base. Double-sided adhesive sheet for polishing pads.

4. A first adhesive layer of a double-sided adhesive sheet for a polishing pad is in contact with one surface of the top pad, A multi-layer polishing pad in which a second adhesive layer of a double-sided adhesive sheet for a polishing pad is in contact with one surface of a cushion layer, The double-sided adhesive sheet for a polishing pad includes a base sheet, a first adhesive layer located on one side of the base sheet, and a second adhesive layer located on the other side of the base sheet, 3. A multi-layer polishing pad, wherein the first adhesive layer is an adhesive layer formed from the adhesive for a polishing pad according to claim 1.

5. A single-layer polishing pad in which a first adhesive layer of a double-sided adhesive sheet for a polishing pad is in contact with one surface of a top pad, The double-sided adhesive sheet for a polishing pad includes a base sheet, a first adhesive layer located on one side of the base sheet, and a second adhesive layer located on the other side of the base sheet, 3. A single-layer polishing pad, wherein the first adhesive layer is an adhesive layer formed from the adhesive for a polishing pad according to claim 1.

Citation Information

Patent Citations

  • Double-sided adhesive tape

    JP2013213192A

  • Pressure-sensitive adhesive sheet for fastening polishing pad

    JP2015078348A

  • Adhesive layer, adhesive sheet, and method of producing adhesive layer

    JP2015218306A

  • Adhesive agent for fixing polishing pad, and adhesive sheet for fixing polishing pad

    JP2016183211A

  • Double-sided adhesive tape for glass polishing material

    JP2017057295A