Asphalt Mixture
Sodium ferrite or potassium carbonate absorbers in asphalt mixtures enable carbon dioxide absorption and recovery at lower temperatures, addressing the deterioration issue and enhancing environmental performance.
Patent Information
- Application Number
- JP2021077034
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-04-30
AI Technical Summary
Conventional carbon dioxide absorbers in asphalt mixtures require high temperatures for regeneration, leading to asphalt deterioration, and existing methods fail to recover carbon dioxide absorption capacity under atmospheric pressure in recycled asphalt mixtures.
Incorporating sodium ferrite or potassium carbonate as carbon dioxide absorbers that operate at room temperature and release carbon dioxide below 200°C, allowing for the recovery of absorption capacity without deteriorating the asphalt, and integrating a carbon dioxide recovery system to manage emissions.
The asphalt mixture effectively absorbs carbon dioxide at lower temperatures, maintaining asphalt integrity while reducing emissions by recovering carbon dioxide absorption capacity and preventing its release into the atmosphere.
Smart Images

Figure 0007586762000001 
Figure 0007586762000002 
Figure 0007586762000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an asphalt mixture used for road paving, which is capable of absorbing carbon dioxide. [Background technology]
[0002] Asphalt mixtures used in asphalt pavement are stripped from roads as they become old and recycled at asphalt plants, with the recycling rate of asphalt mixtures reaching 98%. The heating temperature of recycled asphalt aggregate in the production of recycled asphalt mixture is 170 to 200°C, and if asphalt is heated to above 200°C, it will deteriorate. When asphalt deteriorates, its adhesiveness decreases and it becomes hard, brittle, and prone to cracking. Due to the recent increase in environmental awareness, carbon dioxide absorbents (e.g., Patent Document 1) have been attracting attention. However, in conventional carbon dioxide absorbents, after absorbing carbon dioxide (CO2), it is necessary to heat them to about 600°C in order to recover (regenerate) their absorption capacity. For example, lithium silicate (Li4SiO4) absorbs carbon dioxide at temperatures between room temperature and 700°C, and releases carbon dioxide at temperatures above 700°C. Therefore, even if a conventional carbon dioxide absorbent is added to an asphalt mixture, there is a problem that the asphalt deteriorates when it is heated to about 600°C to restore its carbon dioxide absorption capacity. In addition, asphalt mixtures containing zeolite, which absorbs carbon dioxide under atmospheric pressure and releases the absorbed carbon dioxide when the pressure is reduced to near vacuum, need to be reduced in pressure to near vacuum in order to recover (regenerate) their absorption capacity after absorbing carbon dioxide, but the production of regenerated asphalt mixtures is carried out under atmospheric pressure. Therefore, the absorbed carbon dioxide cannot be released, and therefore the carbon dioxide absorption capacity cannot be restored. Therefore, it is inconvenient to add a conventional carbon dioxide absorbent to a carbon dioxide absorbing asphalt mixture. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 6080122 Summary of the Invention [Problem to be solved by the invention]
[0004] As a result of research and development, the inventors discovered that sodium ferrite (NaFeO2) and potassium carbonate are materials with carbon dioxide absorption ability, which absorb carbon dioxide at room temperature and regenerate their carbon dioxide absorption ability at around 100°C (a temperature lower than the heating temperature of recycled asphalt aggregate). The present invention has been proposed in consideration of the problems of the conventional technology described above, and aims to provide an asphalt mixture that has carbon dioxide absorption capacity and can restore its carbon dioxide absorption capacity at a temperature lower than the heating temperature of the recycled asphalt aggregate. [Means for solving the problem]
[0005] The present invention In The asphalt mixture is In asphalt mixtures containing asphalt and aggregate, It contains a carbon dioxide absorbent that absorbs carbon dioxide at normal temperature and pressure and releases carbon dioxide at temperatures below 200°C. Including is. wherein the carbon dioxide absorbent is sodium ferrite or potassium carbonate; The content of the carbon dioxide absorbent is 30% to 100% of the stone powder content obtained by a normal mix design, The asphalt content is preferably set to an amount that can be obtained by normal mix design. Other possible carbon dioxide absorbents include cerium oxide, solid amines, and sodium carbonate.
[0006] Here, "normal mix design" is well known to those skilled in the art, and is shown, for example, in the "Pavement Construction Handbook (2006 Edition)" (Published by Japan Road Association) (First edition, first printing published December 4, 2001, 2006 edition published February 24, 2006) for new asphalt mixtures (asphalt mixtures made only from materials that have not yet been used as asphalt mixtures), and in the "Pavement Regeneration Handbook (2010 Edition)" (Published by Japan Road Association) (First edition, first printing published February 17, 2004, revised edition, first printing published November 30, 2010) for recycled asphalt mixtures.
[0007] When implementing the asphalt mixture of the present invention, it is possible to replace some or all of the amount of carbon dioxide absorbent mixed in the amount of stone powder obtained by a normal mix design with slaked lime, that is, to contain an amount of slaked lime equivalent to some or all of the amount of carbon dioxide absorbent mixed in the amount of stone powder minus the amount of carbon dioxide absorbent mixed in the amount of stone powder.
[0008] Method for producing asphalt mixture of the present invention About In a method for producing an asphalt mixture containing asphalt and aggregate, The process includes mixing either sodium ferrite or potassium carbonate, which is a carbon dioxide absorbent. I am . The method for producing the asphalt mixture of the present invention is also About In a method for producing an asphalt mixture containing asphalt and aggregate, Recycled materials, new materials, stone powder, or new asphalt. The process includes mixing a carbon dioxide absorbent that absorbs carbon dioxide at normal temperature and pressure and releases carbon dioxide at temperatures below 200°C. I am .
[0009] The method for producing the asphalt mixture of the present invention About , The carbon dioxide absorbent is sodium ferrite or potassium carbonate, The content of the carbon dioxide absorbent is 30% to 100% of the stone powder content obtained by a normal mix design, The asphalt content is preferably an amount obtainable by normal mix design. In addition, in the method for producing an asphalt mixture of the present invention, it is preferable to add the carbon dioxide absorbent after the asphalt and aggregate are mixed (wet mixing) (rather than dry mixing, in which the aggregate and carbon dioxide absorbent are mixed and then the asphalt is mixed). In the present invention, if a part or all of the amount of carbon dioxide absorbent mixed in subtracted from the amount of stone powder mixed in a normal mix design is replaced with slaked lime, it becomes possible to prevent peeling, and the material can be used as a road pavement even when there are concerns about water resistance.
[0010] The method for producing an asphalt mixture of the present invention is as follows: In a method for producing an asphalt mixture containing asphalt and aggregate, Recycled materials (recycled asphalt aggregate), new materials (coarse and fine aggregates that have not yet been used as materials for asphalt mixtures), stone powder, or new asphalt. 、 The method includes a step of mixing a carbon dioxide absorbent that absorbs carbon dioxide at 25°C and atmospheric pressure and releases carbon dioxide at less than 200°C and atmospheric pressure, The carbon dioxide absorbent is ,Na Thorium ferrite or potassium carbonate the law of nature, The content of the carbon dioxide absorbent is 30% to 100% of the stone powder content obtained by a normal mix design, The asphalt content is set to the amount obtained by normal mix design. In the case where a recycled material containing a carbon dioxide absorbent is mixed in the mixing step, the recycled material is mixed prior to the mixing step. 170~200℃ The method includes a heating step of heating the recycled material, and a step of restoring the carbon dioxide absorption capacity of the carbon dioxide absorbent material contained in the recycled material in the heating step (a step of restoring the carbon dioxide absorption capacity of the recycled material). It is characterized by: In this case, it is preferable to include a step of recovering the carbon dioxide released (from the recycled material) in the mixing step.
[0011] When the recycled material is mixed in the mixing step, the carbon dioxide capture device (4) is connected to the heating device (1), and in the carbon dioxide capture step, it is preferable that when the recycled material is heated by the heating device (1), carbon dioxide released by either the sodium ferrite or potassium carbonate in the recycled material in the heating device (1) is captured by the carbon dioxide capture device (4). And / or, it is preferable that the carbon dioxide capture device (4) is connected to the mixer (3), and the carbon dioxide absorbent, either sodium ferrite or potassium carbonate, releases the absorbed carbon dioxide in the mixer (3) by the heat contained in the heated regenerator, and the released carbon dioxide is captured by the carbon dioxide capture device (4).
[0012] In addition, the method of constructing or repairing an asphalt pavement of the present invention comprises: A method for repairing asphalt pavement comprising scraping heated pavement, spreading the scraped pavement evenly, and compacting the pavement, a heating step of heating the road surface (RD) on which the asphalt mixture has been spread and leveled by a heating device (15) to release carbon dioxide; The method is characterized by including a recovery step of recovering the carbon dioxide released in the heating step by a carbon dioxide recovery unit (first carbon dioxide recovery unit 16 and / or second carbon dioxide recovery unit 17).
[0013] In the method for constructing or repairing an asphalt pavement of the present invention, the recovery step comprises: A step of recovering carbon dioxide released from the carbon dioxide absorbent when the road surface (RD) is heated by the heating device (15) using a first carbon dioxide recovery device (16); A step of recovering, by a second carbon dioxide recovery device (17), carbon dioxide released from the carbon dioxide absorbent when the asphalt mixture is spread and leveled on a road surface by the asphalt mixture spreading device (14); It is preferred that the composition comprises:
[0014] In addition, in the method for constructing or repairing an asphalt pavement of the present invention, The method includes a mixing step of raking the heated asphalt mixture of the existing road surface (RD) with a road surface raking device (12) and mixing the raked asphalt mixture with a mixing device (3A, 3B); The recovery step preferably includes a step of recovering carbon dioxide generated in the mixers (3A, 3B) during the mixing step by using a second carbon dioxide recovery unit (17).
[0015] The method for constructing or repairing an asphalt pavement of the present invention preferably includes a method (remix method) in which the asphalt pavement of the road surface (RD) is heated by a heating device (15), the asphalt mixture that has been scraped off after heating by a road surface scraping device (12) is mixed in a mixing device (3A) with an asphalt mixture produced in an asphalt mixture production plant (AP production mixture) and / or a carbon dioxide absorbent, and then the resulting mixture is spread evenly at the current position (road surface RD) by an asphalt mixture spreading device (14). The method for constructing or repairing an asphalt pavement of the present invention preferably includes a method (so-called "repave method") in which the asphalt pavement of the road surface (RD) is heated by a heating device (15), the asphalt mixture that has been scraped off by a road surface scraping device (12) after heating is mixed in a mixing device (3B), and then spread and leveled at the current location (road surface RD) by an asphalt mixture spreading and leveling device (14), and the AP manufacturing mixture is supplied and layered on the spread and leveled asphalt mixture (NA) (NB). In this case, a carbon dioxide absorbent can be mixed in when mixing in the mixing device (3B). Furthermore, the method for constructing or repairing an asphalt pavement of the present invention can include a method of heating the asphalt pavement of the road surface (RD) with a heating device (15), and then spreading the asphalt mixture that has been heated and then scraped with a road surface scraping device (12) evenly on the current location (road surface RD) (the so-called "reshape method or reform method"). Effect of the Invention
[0016] According to the asphalt mixture of the present invention having the above-mentioned configuration, either the new asphalt mixture or the recycled asphalt mixture contains either sodium ferrite or potassium carbonate, which is a carbon dioxide absorbent, so that a road paved with the asphalt mixture produced by the present invention absorbs carbon dioxide on its pavement surface (RD). Because the road absorbs carbon dioxide, it can effectively respond to the demand for reducing carbon dioxide emissions.
[0017] Here, once a carbon dioxide absorbent has absorbed a certain amount of carbon dioxide, it cannot absorb any more carbon dioxide unless it is heated to restore its carbon dioxide absorption capacity. The asphalt mixture of the present invention contains either sodium ferrite or potassium carbonate as a carbon dioxide absorbent, and its carbon dioxide absorption capacity is restored at a temperature (for example, about 100°C) lower than the heating temperature of the recycled asphalt aggregate, which is lower than 200°C, the temperature at which asphalt deteriorates. Therefore, the asphalt mixture of the present invention can be heated to restore its carbon dioxide absorption capacity without deteriorating the asphalt.
[0018] In the asphalt mixture manufacturing method of the present invention, when the recycled material is mixed, the carbon dioxide absorbent, sodium ferrite and potassium carbonate, are heated to a temperature sufficient to recover their carbon dioxide absorption capacity in the heating step carried out prior to the mixing step, so that the carbon dioxide absorbent contained in the recycled material recovers its capacity. The carbon dioxide released when the carbon dioxide absorbent recovers its capacity is recovered by the carbon dioxide recovery device (4), so that the amount of carbon dioxide emissions in the facility (10) where the manufacturing method of the present invention is carried out can be kept low. In addition, it is possible to prevent the situation in which carbon dioxide diffuses outside the facility (10).
[0019] Furthermore, there is a risk of carbon dioxide being generated in the mixing step in the method for producing an asphalt mixture of the present invention, but the carbon dioxide generated in the mixing step is also captured by the carbon dioxide capture device (4). Therefore, according to the present invention, when producing a recycled asphalt mixture, a step of restoring the carbon dioxide absorption capacity of the carbon dioxide absorbent can be carried out simultaneously with the heating step and / or the mixing step.
[0020] In addition, according to the method for constructing or repairing an asphalt pavement of the present invention, the carbon dioxide absorption capacity of the carbon dioxide absorbents, sodium ferrite and potassium carbonate, is restored by heating the road surface (RD) on which the asphalt mixture containing the carbon dioxide absorbent has been spread using a heating device (15). Even if the carbon dioxide absorbed by the carbon dioxide absorbents, sodium ferrite and potassium carbonate, is released, it is captured by the carbon dioxide capture devices (16, 17), so that when repairing a damaged pavement, the carbon dioxide absorption capacity can be restored and the carbon dioxide can be prevented from being released into the atmosphere. Then, the asphalt pavement having carbon dioxide absorption capacity can be restored or repaired to the road surface. As a result, the pavement is repaired and the carbon dioxide absorption capacity of the asphalt mixture is restored (regenerated). The method for constructing or repairing asphalt pavement of the present invention is not only capable of repairing road surfaces paved with the asphalt mixture of the present invention having carbon dioxide absorption capacity, but is also capable of repairing road surfaces that do not have carbon dioxide absorption capacity, and furthermore, the repaired road surface can also be made into an asphalt pavement that has carbon dioxide absorption capacity. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a diagram showing the CO2 absorption rates of a test specimen containing sodium ferrite and a test specimen containing potassium carbonate in Experimental Example 1. [Diagram 2] FIG. 13 is a graph showing a comparison of CO2 absorption rates by varying the asphalt type and amount in Experimental Example 2 using potassium carbonate as a CO2 absorbent. [Diagram 3]FIG. 13 is a graph showing a comparison of standard Marshall stability by varying the asphalt type and asphalt amount in Experimental Example 2 using potassium carbonate as a CO2 absorbent. [Figure 4] FIG. 13 is a diagram showing the results of a residual Marshall stability test carried out in Experimental Example 3 by changing the amount of sodium ferrite added, the amount of slaked lime added, and the type of asphalt. [Diagram 5] FIG. 11 is a graph showing a comparison of CO2 absorption rates in dry mixing and wet mixing in Experimental Example 4. [Figure 6] FIG. 2 is an explanatory diagram showing a main part of an asphalt mixture manufacturing plant according to an embodiment. [Figure 7] FIG. 1 is an explanatory diagram of a system for repairing a pavement using an asphalt mixture according to an embodiment. [Figure 8] FIG. 8 is an explanatory diagram of a system for repairing a pavement made of an asphalt mixture according to an embodiment, which is different from the system shown in FIG. 7. [Figure 9] FIG. 9 is an explanatory diagram of a system for repairing a pavement made of an asphalt mixture according to an embodiment, which is yet another system different from the systems shown in FIGS. 7 and 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, embodiments and experimental examples of the present invention will be described with reference to the accompanying drawings. In the embodiment, sodium ferrite or potassium carbonate is used as the carbon dioxide (CO2) absorbent. It is also possible to use cerium oxide, solid amine, or sodium carbonate as the carbon dioxide absorbent in the illustrated embodiment or experimental example. First, with reference to Experimental Examples 1 and 2, the CO2 absorption rate and other characteristics of the CO2 absorbents, sodium ferrite and potassium carbonate, will be described.
[0023] [Experimental Example 1] The CO2 absorption rate was measured for two types of test specimens in which 6% of the stone powder in the dense-graded asphalt mixture was replaced with sodium ferrite or potassium carbonate, which are CO2 absorbents. In experimental example 1, carbon dioxide gas was supplied into a desiccator to adjust the CO2 concentration inside the desiccator to approximately 3000 to 4000 ppm, a test specimen was placed into the desiccator, the supply of carbon dioxide gas was stopped, the desiccator was sealed, and the desiccator was left in a sealed state for three hours, after which the change in CO2 concentration over time was measured. Here, the CO2 absorption rate (%) was calculated using the following formula. CO2 absorption rate (%) = [{(CO2 concentration at the start of measurement) - (CO2 concentration after 3 hours)} / (CO2 concentration at the start of measurement)] x 100
[0024] As shown in Figure 1, in Experimental Example 1, the amount of asphalt was varied as follows: 5.7%, 6.3%, (6.9%), (7.5%), (9.3%). In Figure 1, the CO2 absorption rate was measured three times for each amount of asphalt, and the average value of the three CO2 absorption rates is represented by the plot of "◯". The CO2 absorption rate of the asphalt mixture containing sodium ferrite was about 10%, and the CO2 absorption rate of the asphalt mixture containing potassium carbonate was 10 to 40%. In other words, Experimental Example 1 confirmed that the asphalt mixture containing sodium ferrite and potassium carbonate has CO2 absorption capacity.
[0025] Although not shown in the figure, another experiment conducted by the inventor revealed that the content of CO2 absorbent material should preferably be more than 30% and less than 100% of the stone powder mixture amount obtained by normal mix design, and that if the content of CO2 absorbent material is less than 30% of the stone powder mixture amount, the CO2 absorption performance is significantly reduced, and if it is more than 100% of the stone powder mixture amount (if it is replaced with materials other than stone powder, such as sand), the durability of the asphalt mixture cannot be guaranteed.
[0026] [Experimental Example 2] Next, potassium carbonate was used as a CO2 absorbent for dense-graded asphalt mixtures. Inexpensive and versatile straight asphalt (St.As), Polymer modified asphalt type II (modified type II asphalt) is made by adding modifiers such as thermoplastic elastomers to straight asphalt to improve durability. Polymer modified asphalt H type (modified H type asphalt) is an asphalt with an even larger amount of modifier added than modified type II asphalt and is used for drainage pavement (porous asphalt mixtures). In this case, the CO2 absorption rate (%) and stability (kN) were measured by varying the asphalt type and amount. In Experimental Example 2, the stability was determined by the Marshall stability test. The target value for stability was set at 4.9 kN or more. The results of Experimental Example 2 are shown in FIGS.
[0027] Figure 2 shows the results of calculating the CO2 absorption rate by varying the asphalt type and amount. In Figure 2, in the left area (area indicated by the symbol "St.As"), the CO2 absorption rate (%) was measured three times for each case where the straight asphalt content was 5.7%, 6.3%, 7.5%, and 9.3%, and each measured value and the average of the three measurements are shown. In the center area indicated by the symbol "Modified Type II", the CO2 absorption rate (%) was measured three times for each case where the modified Type II asphalt content was 5.7%, 6.3%, 6.9%, 7.5%, 8.1%, 8.7%, and 9.3%, and each measured value and the average of the three measurements are shown. In the right area (area indicated by the symbol "Modified Type H"), the CO2 absorption rate (%) was measured three times for each case where the modified Type H asphalt content was 5.7%, 6.3%, 6.9%, 7.5%, and 9.3%, and each measured value and the average of the three measurements are shown. Figure 2 reveals that there is no clear correlation between asphalt type and CO2 absorption rate.
[0028] Figure 3 shows the relationship between asphalt type, asphalt amount, and stability. In FIG. 3, the indication "no substitution" indicates that potassium carbonate, which is a CO2 absorbent, is not included, and the indication "6% potassium carbonate" indicates that 6% potassium carbonate is included. The horizontal axis of FIG. 3 indicates the asphalt content, and the vertical axis indicates the stability (kN). Figure 3 reveals that the stability of modified type II asphalt and modified type H asphalt is above the target value of 4.9 kN.
[0029] [Experimental Example 3] The inventor further: A sample of dense-graded asphalt mixture containing 5.7% modified type II asphalt and 6% sodium ferrite (NaFeO2) was added. A sample of dense-graded asphalt mixture containing 5.7% modified type II asphalt and 4% sodium ferrite (NaFeO2) was added. A sample of dense-graded asphalt mixture containing 5.7% modified type II asphalt with the addition of 4% sodium ferrite (NaFeO2) and 2% hydrated lime was used. A sample of dense-graded asphalt mixture containing 6.9% special modified asphalt and 4% sodium ferrite (NaFeO2) was added. A sample of dense-graded asphalt mixture containing 6.9% special modified asphalt with the addition of 4% sodium ferrite (NaFeO2) and 2% hydrated lime. The residual stability was measured for the following: The results of Experimental Example 3 are shown in Figure 4. In Figure 4, the dotted line extending horizontally (left and right) indicates the line at which the residual stability is 75% (the threshold value for whether or not there is a problem with the water resistance of the asphalt mixture).
[0030] In Experimental Example 3, The residual stability of the sample containing 5.7% modified type II asphalt and 6% sodium ferrite was 49.1%. The residual stability of the sample containing 5.7% modified type II asphalt and 4% sodium ferrite was 63.7%. The residual stability of the sample containing 5.7% modified type II asphalt and dense-graded asphalt mixture with 4% sodium ferrite and 2% hydrated lime was 82.5%; The residual stability of the sample in which 4% sodium ferrite was added to a dense-graded asphalt mixture containing 6.9% special modified asphalt was 80.6%; The residual stability of the sample containing 6.9% special modified asphalt and adding 4% sodium ferrite and 2% hydrated lime was 86.4%; It was. Here, in the case of modified type II asphalt, only the sample with 2% added slaked lime had a residual stability of 75% or more, indicating that there was no problem with water resistance. From this, it was confirmed that in cases where water resistance is a problem, adding slaked lime is sufficient. In addition, in the case of special modified asphalt, there were no problems with water resistance whether hydrated lime was added or not (residual stability of 75% or more).
[0031] Although not clearly shown in the figures, the inventors' experiments confirmed that water resistance can be improved by replacing part or all of the amount of stone powder obtained by subtracting the amount of carbon dioxide absorbent material from the amount of stone powder obtained by normal mix design with hydrated lime.
[0032] From Experimental Examples 1 to 3, it was found that potassium carbonate and sodium ferrite have the necessary CO2 absorption capacity as a CO2 absorbent, and that asphalt mixtures to which these have been added have the necessary stability as road pavement materials, for example, when mixed with modified type II asphalt.
[0033] Next, in Experimental Example 4, the mixing procedure for producing an asphalt mixture using either potassium carbonate or sodium ferrite as a CO2 absorbent was confirmed. [Experimental Example 4] When mixing coarse aggregate, fine aggregate, filler (stone powder), CO2 absorbent, and asphalt to make the asphalt mixture, the amount of asphalt was varied from 5.7%, (6.3%), 7.5%, and 9.3%. First, coarse aggregate, fine aggregate, filler, and CO2 absorbent are mixed dry and then asphalt is added (dry mixing). In the case of adding CO2 absorbent material after mixing coarse aggregate, fine aggregate, and filler with asphalt and thoroughly covering the aggregate with asphalt (wet state) (wet mixing), The CO2 absorption rates were compared in the same manner as in Experimental Example 1.
[0034] When potassium carbonate was used as the CO2 absorbent, the asphalt content was 5.7%, (6.3%), 7.5%, and 9.3%, respectively. As shown in Figure 5, the CO2 absorption rate of wet mixing was greater than that of dry mixing (higher CO2 absorption capacity). Furthermore, although not shown in FIG. 5, in Experimental Example 4, it was easier to coat the asphalt with wet mixing than with dry mixing, making it easier to prepare test specimens. Experimental Example 4 clarified that wet mixing is more preferable than dry mixing. Therefore, in an embodiment of the present invention, the CO2 absorbent was added after the asphalt and aggregate were mixed. However, it is also possible to manufacture the asphalt mixture of the present invention by dry mixing. In addition, according to an experiment conducted by the inventor separately from Experimental Example 4, the CO2 absorption capacity of sodium ferrite was higher in wet mixing than in dry mixing. Also, it was easy to prepare the test specimen.
[0035] From Experimental Examples 1 to 4, for the asphalt mixture according to the embodiment of the present invention, either sodium ferrite or potassium carbonate was selected as the CO2 absorbent. And, it was confirmed from Experimental Example 3 that when there is a problem with water resistance, it can be dealt with by adding hydrated lime. Furthermore, it was confirmed from Experimental Example 4 that it is desirable to add the CO2 absorbing material after the asphalt and aggregate are mixed (wet mixing).
[0036] Next, with reference to FIG. 6, the production of a recycled asphalt mixture according to an embodiment will be described. In FIG. 6, an asphalt mixture manufacturing plant 10 (manufacturing facility) has a recycled material heating device 1, a new material heating device 2, a mixer 3, and a carbon dioxide capture device 4 (CO2 capture device). In the asphalt mixture manufacturing plant 10, only the essential parts of which are shown in FIG. 6, recycled materials (asphalt mixture that has already been paved and removed from the road surface) and new materials containing stone powder (coarse aggregate and fine aggregate that have not yet been used as an ingredient in asphalt mixtures) are mixed to manufacture an asphalt mixture, or the asphalt mixture is manufactured using only recycled materials, or the asphalt mixture is manufactured using only new materials containing stone powder, or a CO2 absorbent (either sodium ferrite or potassium carbonate) and / or hydrated lime is added to the recycled materials and / or new materials. Although not explicitly shown, in the manufacturing plant 10 in Fig. 6, the CO2 absorbent is added after the asphalt and aggregate are mixed, so it is manufactured by "wet mixing". However, it is also possible to manufacture it by dry mixing, in which aggregate and CO2 absorbent are mixed and then asphalt is mixed.
[0037] As described above, in the manufacturing plant 10 of FIG. 6, the asphalt mixture may be manufactured using only recycled materials, may be manufactured using only new materials including stone powder, may add a CO2 absorbent to the recycled materials and / or new materials, or may add hydrated lime. When using recycled materials, new materials, new asphalt, and new CO2 absorbing materials, the order of feeding them into the mixer 3 is as follows: In that order, recycled materials, new materials including stone powder, new asphalt, and new CO2 absorbing materials. The order is new material including stone powder, recycled material, new asphalt, and new CO2 absorbing material, and the order to be adopted varies depending on the conditions of each manufacturing plant 10.
[0038] In FIG. 6, the regenerated material is transported from a regenerated material supply source (not shown) via a route R1 to the regenerated material heating device 1, and a heating step of heating the regenerated material is performed. In the heating process by the regenerator heating device 1, the CO2 absorbents (sodium ferrite, potassium carbonate) contained in the regenerator and which have already absorbed CO2 and no longer have any CO2 absorption capacity release the absorbed CO2, thereby recovering their CO2 absorption capacity. The heating temperature in the heating process in the recycled material heating device 1 is, for example, about 170 to 200°C. A heating temperature of 170 to 200°C is high enough to restore the CO2 absorption capacity of the CO2 absorbents (sodium ferrite, potassium carbonate) contained in the recycled material, and is also a typical heating temperature for recycled asphalt materials. In other words, in the production of the recycled asphalt mixture according to the embodiment shown in Figure 6, it is not necessary to heat the asphalt to a temperature at which it deteriorates, its adhesiveness decreases, it becomes hard and brittle, and it becomes prone to cracking.
[0039] The CO2 released from the CO2 absorbing material in the heating process in the regenerator heating device 1 is sent to the CO2 capture device 4 via the CO2 exhaust pipe P1 and treated there. The recycled material (asphalt mixture that has already been paved and removed from the road surface) whose CO2 absorption capacity has been restored after undergoing the heating process in the recycled material heating device 1 is transported to the mixing device 3 via route R2. In Figure 6, an on-off valve V1 is provided on route R2. For example, when producing an asphalt mixture using only new materials, no recycled material is added to the asphalt mixture, so on-off valve V1 is closed. When recycled material is used (added), on-off valve V1 is opened. Here, on-off valve V1 is an example, and any mechanism for stopping the supply of recycled material (for example, various supply cut-off mechanisms) can be installed on route R2 in place of on-off valve V1. The same applies to on-off valves V2, V6, V8, V9, and V10. The on-off valve V1 is informationally connected to a control unit (CU) via a control line CL1, and receives an on-off control signal from the control unit CU. Here, the control device CU can be configured with a computer or the like having an information processing function. However, the control device CU may also be a control panel operated by an operator. It is also possible for the control device CU to be configured with an operator, who can manually operate the on-off valve V1 (or V2, V6, V8, V9, V10) or the supply cutoff mechanism.
[0040] In Fig. 6, new materials (coarse aggregates and fine aggregates that have not yet been used as materials for an asphalt mixture) are transported from a new material supplier (not shown) via route R3 to the new material heating device 2. The transported new materials are heated by the new material heating device 2 (heating process). The heating temperature in the heating process of the new material heating device 2 is, for example, about 170 to 200° C., similar to that of the recycled material heating device 1. Here, the new material does not contain a carbon dioxide absorbent. Therefore, unlike the recycled material heating device 1, the new material heating device 2 is not provided with a piping system (CO2 exhaust piping) that communicates with the CO2 capture device 4. However, assuming that CO2 is emitted when heating in the new material heating device 2, a piping system (CO2 exhaust piping) that communicates between the new material heating device 2 and the CO2 capture device 4 can be provided, although this is not shown in the figure. The new material that has been subjected to the heating process in the new material heating device 2 is transported to the mixer 3 via a route R4. An on-off valve V2 is provided in the route R4, and the on-off valve V2 receives a control signal from the control device CU via a control line CL2. The on-off valve V2 is the same as the on-off valve V1 described above. Here, when manufacturing an asphalt mixture with CO2 absorption capacity using only new materials without using recycled materials, the new materials (coarse aggregate, fine aggregate) are heated in the new material heating device 2, and the heated new materials are mixed with stone powder, new asphalt, and CO2 absorbent (new CO2 absorbent) in the mixing device 3.
[0041] The recycled material heated in the recycled material heating device 1 and the new material heated in the new material heating device 2 are transported to the mixer 3, where they are mixed (mixing process). Then, a new asphalt mixture, that is, an AP production mixture, is produced. The mixer 3 is connected to a CO2 absorbent supply source 32 via a path R6 having an on-off valve V6 therein, and the on-off valve V6 is informationally connected to a control device CU via a control line CL6. The mixer 3 is also connected to a new asphalt supply source 34 via a route R8 having an on-off valve V8 therein, and the on-off valve V8 is informationally connected to the control device CU via a control line CL8. Furthermore, the mixer 3 is connected to a slaked lime supply source 36 via a route R9 having an on-off valve V9 disposed therein, and the on-off valve V9 is informationally connected to the control device CU via a control line CL9. In addition, the mixer 3 is connected to the stone powder supply source 38 via a route R10 having an on-off valve V10, and the on-off valve V10 is informationally connected to the control device CU via a control line CL10. Note that the wiring of the control lines CL6, CL8, CL9, and CL10 is not limited to the positions shown in the figure. The on-off valves V6, V8, V9, and V10 are similar to the on-off valve V1 described above.
[0042] In this way, by connecting the CO2 absorbent supply source 32, new asphalt supply source 34, slaked lime supply source 36, and stone powder supply source 38 to the mixer 3, the manufacturing plant 10 in Figure 6 can handle cases where new asphalt should be added, cases where CO2 absorbent should be added, cases where slaked lime should be added due to problems with water resistance, cases where stone powder should be added, etc. When it is not necessary to add new asphalt, CO2 absorbent, slaked lime, or stone powder, the on-off valves V6, V8, V9, and V10 can be closed so that they are not supplied to the mixer 3. Although not shown in FIG. 9, a regenerating additive can be added to the mixing device 3. Therefore, according to the manufacturing plant 10 of Figure 6, it is possible to produce asphalt mixtures containing CO2 absorbents in the following cases: when produced using only new asphalt, new CO2 absorbents and other new materials; when produced using new CO2 absorbents and other new materials and asphalt recycled materials without any CO2 absorbents mixed in; when produced using new CO2 absorbents and other new materials and recycled materials with CO2 absorbents mixed in; and when produced using only recycled materials with CO2 absorbents mixed in.
[0043] The new asphalt mixture, i.e., AP production mixture, produced from either heated recycled material, heated new material, stone powder, new asphalt, CO2 absorbent, or slaked lime is transported from the mixing device 3 to a required site or storage facility (not shown) by a transport means (truck, etc.). The transportation to a site or storage facility (not shown) is indicated by the symbol "R5". When the recycled material is mixed in the mixer 3, the amount of heat contained in the heated recycled material may cause the CO2 absorbent to release in the mixer 3 any CO2 that was not released in the recycled material heating device 1. For this reason, the mixing process includes a process of capturing the CO2 released from the recycled material. A CO2 discharge pipe P2 (piping system) is provided that connects the mixer 3 and the CO2 capture device 4, and the CO2 released from the mixer 3 is sent to the CO2 capture device 4 via the CO2 discharge pipe P2 and captured by the CO2 capture device 4 (a process in which the CO2 released in the mixer 3 is captured by the CO2 capture device 4).
[0044] In Fig. 6, the piping system (CO2 exhaust piping P1) connecting the recycled material heating device 1 and the CO2 capture device 4 and the piping system (CO2 exhaust piping P2) connecting the mixer 3 and the CO2 capture device 4 are separate systems. However, the CO2 exhaust piping P1 and P2 can be merged before reaching the CO2 capture device 4 and connected to the CO2 capture device 4 as a single piping system (CO2 exhaust piping). Although not shown in the figure, an absorption tower may be formed by a piping system (CO2 exhaust piping P1) connecting the recycled material heating device 1 and the CO2 recovery device 4, a piping system (CO2 exhaust piping P2) connecting the mixing device 3 and the CO2 recovery device 4, and the CO2 recovery device 4. Although not clearly shown, the asphalt mixture of the present invention is produced by wet mixing in the production plant 10 in Figure 6. However, it is also possible to produce the asphalt mixture of the present invention by dry mixing in the production plant 10 in Figure 6.
[0045] As described above, the CO2 recovery device 4 is supplied with the CO2 discharged in the heating process of the recycled material heating device 1 and the CO2 discharged in the mixing process of the mixer 3. The CO2 recovery device 4 sends the supplied CO2 to a CO2 processing mechanism (not shown) via a CO2 exhaust pipe P3 (piping system). At that time, waste other than CO2 is detoxified in a device (not shown) and released into the atmosphere via the CO2 exhaust pipe P4. Although not clearly shown, the CO2 capture device 4 can be configured as an adsorption device that contains a material that adsorbs CO2.
[0046] The asphalt mixture produced in the manufacturing plant 10 shown in Figure 6 contains a CO2 absorbent, so if roads are paved with this asphalt mixture, CO2 will be absorbed by the paved surface, which will contribute to reducing CO2 emissions. In addition, the CO2 absorbent (either sodium ferrite or potassium carbonate) contained in the recycled asphalt mixture according to the illustrated embodiment recovers its CO2 absorption capacity at the heating temperature (e.g., 170 to 200°C) of the recycled asphalt aggregate. Therefore, when producing an asphalt mixture using the production plant 10 shown in FIG. 6, the CO2 absorption capacity can be restored without deteriorating the asphalt. 6, the CO2 released by the CO2 absorbent in the recycled material in the recycled material heating device 1 during the heating process is captured by the CO2 capture device 4, preventing the CO2 from dissipating outside the asphalt mixture manufacturing plant 10 during the heating process. Furthermore, the CO2 released in the mixing device 3 during the mixing process is also captured by the CO2 capture device 4, preventing the CO2 released during the mixing process from dissipating outside the asphalt mixture manufacturing plant 10.
[0047] Next, a system for repairing (or constructing) a pavement made of an asphalt mixture according to an embodiment will be described with reference to Figs. 7 to 9. In FIG. 7, a system 20 (pavement repair system) for repairing asphalt mixture pavement heats and warms the asphalt pavement of the existing road surface using a road surface heating vehicle or the like, scrapes it up, mixes the material with an AP manufacturing mixture, CO2 absorbent, etc. in a mixing device, and then spreads it evenly in the current location (remix method). The system 20 in Fig. 7 includes a heater vehicle 11, a trailing work vehicle (a so-called "remixer") 30, and a rolling machine 40. Here, a plurality of heater vehicles 11 can be used. The work vehicle 30 includes a road surface raking device 12, a mixing device 3A, and an asphalt mixture spreading device 14. The road surface raking device 12 is disposed in the front area of the work vehicle 30, and the asphalt mixture of the existing road surface raked by the road surface raking device 12 is supplied to the mixing device 3A. The mixer 3A is connected to the AP production mixture supply source 42 via a supply path indicated by an arrow R4A, and is connected to the CO2 absorbent supply source 32A via a supply path indicated by an arrow R6A. In the mixer 3A, the asphalt mixture of the existing road surface scraped by the road surface scraper 12, the AP production mixture supplied from the AP production mixture supply source 42, and the CO2 absorbent supplied from the CO2 absorbent supply source 32A are mixed and dropped onto the road surface, and then spread evenly by the asphalt mixture spreading device 14.
[0048] The work vehicle 30 follows the heater vehicle 11 . The heater vehicle 11 has a built-in hot air circulating heater 15, and further has a first CO2 capture device 16 built in behind the hot air circulating heater 15. The asphalt mixture spreading device 14 also has a second CO2 capture device 17 built in. The compaction machine 40 follows behind the work vehicle 30 . In Fig. 7, the pavement surface RD to be repaired by the pavement repair system 20 is a pavement surface on which the asphalt mixture according to the illustrated embodiment has been spread evenly, and a certain period of time has passed, causing it to absorb sufficient CO2 and lose its CO2 absorption capacity. Here, even if the pavement surface RD is a pavement surface according to the prior art that does not contain a CO2 absorbent, it can be repaired by the pavement repair system of Figs. 7 to 9 and newly given CO2 absorption capacity.
[0049] A hot air circulating heater 15 built into (mounted on) the heater vehicle 11 blows hot air (arrow A) toward the pavement surface RD (road surface) to be repaired, heating the pavement surface RD (heating step). The heating temperature by the hot air circulation heater 15 is, for example, 160 to 170°C, which is approximately the same temperature as the heating temperature in the recycled material heating device 1 in Fig. 6. In other words, the heating temperature of the hot air circulation heater 15 is set to a temperature lower than the temperature at which asphalt deteriorates (the temperature at which the adhesiveness decreases, the asphalt becomes hard and brittle, and the asphalt becomes more susceptible to cracking). By heating the pavement surface RD with the hot air circulation heater 15, the CO2 absorbed by the CO2 absorbent (either sodium ferrite or potassium carbonate) contained in the asphalt mixture of the pavement surface RD is released (arrow B). By releasing the CO2, the CO2 absorption capacity of the CO2 absorbent is restored.
[0050] In the heater vehicle 11, a first CO2 capture device 16 is mounted (built-in) behind the hot air circulation heater 15. The first CO2 capture device 16 captures the CO2 (arrow B) released when the pavement surface RD is heated by the hot air circulation heater 15, that is, the CO2 released from the CO2 absorbent contained in the asphalt mixture (capture process). The CO2 capture device, for example, adsorbs and captures CO2, and also functions as a CO2 storage device. Furthermore, the CO2 recovery device 16 can also recover the CO2 emitted when the hot air circulation heater 15 produces hot air. After being heated by the hot air circulating heater 15 and releasing CO2, the pavement surface RD is raked by the road surface raking device 12 in the work vehicle 30 following the heater vehicle 11.
[0051] As described above, the asphalt mixture scraped from the pavement surface RD by the road surface scraping device 12 is supplied to the mixer 3A, mixed with the AP production mixture and the CO2 absorbent, and spread and leveled by the asphalt mixture spreading device 14. The newly spread and leveled asphalt mixture is indicated by the symbol NA. The asphalt mixture mixed with the AP production mixture and CO2 absorbent in the mixing device 3A retains heat imparted by heating, etc., by the hot air circulating heater 15 of the heater vehicle 11, and therefore may release new CO2 from the CO2 absorbent contained therein. For this reason, a second CO2 capture device 17 is provided within the asphalt mixture spreading device 14, and the newly released CO2 (arrow C) is captured by the second CO2 capture device 17 and stored. Furthermore, the work vehicle 30 is equipped with a heater (not shown) for heating the asphalt mixture scraped off from the pavement surface RD, and the CO2 emitted from the heater is also captured by the second CO2 capture device 17. The asphalt mixture NA spread and leveled by the asphalt mixture spreading and leveling device 14 is compacted by the subsequent rolling machine 40, completing the repair of the pavement using the asphalt mixture according to the embodiment. Here, since the asphalt mixture scraped from the pavement surface RD by the road surface scraping device 12 is heated by the hot air circulation heater 15, there is a possibility that CO2 may be newly released in the mixer 3A as well. Therefore, the work vehicle 30 is provided with a pipe indicated by the arrow P2A in order to send the newly released CO2 in the mixer 3A to the second CO2 capture device 17. As a result, the newly released CO2 in the mixer 3A is also supplied to and captured by the second CO2 capture device 17.
[0052] According to the pavement repair system 20 of FIG. 7, when repairing a pavement with the asphalt mixture according to the embodiment shown in the figure, the pavement surface RD is heated by a hot air circulation heater 15 (heating process). Here, the temperature at which the pavement surface is heated to a degree that dissolves it is, for example, 160 to 170°C, so that the CO2 absorbent contained in the asphalt mixture according to the embodiment shown in the figure releases the absorbed CO2 and recovers the CO2 absorption capacity. The released CO2 is then captured by the first CO2 capture device 16 (capture process), suppressing the emission of CO2 from the CO2 absorbing pavement material on the road surface to the atmosphere. In addition, deterioration of the asphalt during heating is prevented. Furthermore, even if CO2 is newly emitted when the asphalt mixture of the pavement surface RD that has been heated and then scraped is mixed with the AP production mixture and the CO2 absorbent in the mixer 3A and / or when the asphalt mixture is spread and leveled by the asphalt mixture spreader 14, it is captured and stored by the second CO2 capture device 17. Therefore, in addition to suppressing CO2 emissions into the atmosphere when the CO2 absorbing pavement material of the road surface is heated, it is also possible to suppress CO2 emissions when the asphalt mixture is mixed by the mixer 3A in the work vehicle 30 and / or when the asphalt mixture is spread and leveled by the asphalt mixture spreader 14. The newly laid asphalt mixture NA is then compacted (rolled) by the following rolling machine 40, and the surface layer of the asphalt pavement having the CO2 absorption capacity is regenerated. This repairs the damaged pavement that has lost its CO2 absorption capacity.
[0053] Although not clearly shown in the figure, in FIG. 7, it is possible to block route R4A and not supply the AP manufacturing mixture, but to mix the asphalt mixture scraped from the existing pavement surface RD with the CO2 absorbent to make a new asphalt mixture. For example, if an asphalt pavement according to the conventional technology that does not contain a CO2 absorbent is scraped by the road surface scraping device 12 and the CO2 absorbent is mixed by the mixing device 3A, it can be spread evenly on the pavement surface RD as an asphalt mixture with CO2 absorption capacity and compacted. In this case, it is possible to mix only the CO2 absorbent without mixing the AP manufacturing mixture. Of course, the system 20 in Fig. 7 can be used to repair an existing asphalt pavement with CO2 absorption capacity. Even in the case of repairing an existing asphalt pavement with CO2 absorption capacity, it is possible to mix only the CO2 absorbent without mixing the AP manufacturing mixture. In addition, when the scraped asphalt mixture is mixed with a CO2 absorbent, only the AP production mixture can be mixed in the mixer 3A. Alternatively, only the CO2 absorbent can be mixed. Although not explicitly shown, the mixer 3 can be connected to an AP production mixture supply 42 and a CO2 absorbent supply 32A, as well as sources of other necessary additives (e.g., hydrated lime, regenerator additives, etc.).
[0054] The pavement repair system 20 shown in Fig. 7 is used to carry out the so-called remix method. In contrast, the repair system according to the embodiment of the present invention can be used to carry out a method (the so-called "repave method") in which the asphalt pavement of an existing road surface is heated and heated by a road surface heating vehicle, the material is spread evenly in the current location, and then an AP manufactured mixture is spread evenly on the spread asphalt mixture. A repair system 20A for carrying out the repair method is shown in Fig. 8. The repair system 20A in Fig. 8 will be described below, focusing mainly on the differences from the repair system 20 in Fig. 7. The mixer 3B of the work vehicle 30A in the repair system 20A in Fig. 8 is connected to the CO2 absorbent supply source 32A via a supply path indicated by an arrow R6A. In the mixer 3B, the asphalt mixture of the existing road surface scraped by the road surface scraper 12 and the CO2 absorbent supplied from the CO2 absorbent supply source 32A are mixed and dropped onto the road surface, and are spread and leveled by the asphalt mixture leveling device 14. The newly spread and leveled asphalt mixture is indicated by the symbol NA. An AP production mixture supply system R4B that communicates with the AP production mixture supply source 42A is arranged behind the asphalt mixture spreading device 14 (the rolling machine 40 side), and the AP production mixture NB (asphalt mixture produced in the asphalt mixture production plant: containing CO2 absorbent) is layered on top of the spread and leveled asphalt mixture NA. The layered asphalt mixtures NA and NB are compacted by the rolling machine 40.
[0055] When performing the repair method using the repair system 20A shown in Figure 8, the existing pavement RD that is heated and scraped away can be applied to pavement that has CO2 absorbent material mixed in or pavement that does not have CO2 absorbent material mixed in. It is also possible to block the supply route arrow R6A and not mix the CO2 absorbing material into the scraped asphalt mixture. Although not explicitly shown, it is possible to connect a CO2 absorbent supply 32A to the mixer 3B as well as a supply of other necessary additives (eg, hydrated lime, regenerating additives, etc.). The mechanism of CO2 capture in the repair system 20A shown in Fig. 8 is the same as that of the system 20 in Fig. 7. Other configurations and effects are also the same as those of the repair system 20 in Fig. 7.
[0056] In addition to the system 20 implementing the remix method shown in FIG. 7 and the system 20A implementing the repair method shown in FIG. 8, there is also a repair system 20B for implementing a method (so-called "reshape method or reform method") in which the asphalt pavement of an existing road surface is heated and heated with a heater vehicle, the asphalt pavement of the existing road surface is scraped up with a road surface scraping device 12, and the asphalt pavement of the existing road surface is laid down evenly in its current location, as shown in FIG. 9, as an embodiment of the present invention. The repair system 20B in FIG. 9 will be described mainly with respect to the differences from the system 20 in FIG. 7 and the system 20A in FIG. The work vehicle 30B in the repair system 20B in Fig. 9 is not provided with a mixing device, and the asphalt mixture scraped off from the pavement surface RD by the road surface scraping device 12 is fed into the asphalt mixture spreading device 14 and spread and leveled. The newly spread and leveled asphalt mixture is indicated by the symbol NA.
[0057] As with the system 20 in FIG. 7 and the system 20A in FIG. 8, even if new CO2 is released when the asphalt mixture is spread by the asphalt mixture spreading device 14, the CO2 is captured and stored by the second CO2 capture device 17. However, since the work vehicle 30B is not provided with a mixing device, unlike the system 20 in FIG. 7 and the system 20A in FIG. 8, no CO2 capture piping connecting the mixing device and the second CO2 capture device 17 is provided. In the system 20B shown in FIG. 9, no CO2 absorbing material is added to the scraped asphalt mixture, so it can be applied to repair asphalt pavement in which a CO2 absorbing material has been mixed. Other configurations and effects of the repair system 20B shown in FIG. 9 are similar to those of the repair system 20 in FIG. 7 and the repair system 20A in FIG.
[0058] It should be noted that the illustrated embodiment is merely an example and is not intended to limit the technical scope of the present invention. [Explanation of symbols]
[0059] 1... Recycled material heating device (heating device) 2...New material heating device 3, 3A, 3B...Mixing device 4. CO2 capture equipment (carbon dioxide capture equipment) 10. Asphalt mixture manufacturing plant 11. Heated vehicle 12. Road surface clearing device 14. Asphalt mixture spreading device 15. Hot air circulation heater (heating device) 16. The first CO2 capture unit 17. Second CO2 capture unit 20, 20A, 20B Pavement Repair System 30, 30A, 30B...Work vehicle 40...Roller compaction machine RD...Road surface to be repaired
Claims
1. A method for producing an asphalt mixture containing asphalt and aggregate, comprising: Recycled materials, new materials, stone powder, or new asphalt. Mixing a carbon dioxide absorbent that absorbs carbon dioxide at 25° C. and atmospheric pressure and releases carbon dioxide at less than 200° C. and atmospheric pressure; The carbon dioxide absorbent is sodium ferrite or potassium carbonate, The content of the carbon dioxide absorbent is 30% to 100% of the stone powder content obtained by a normal mix design, The asphalt content is set to the amount obtained by normal mix design. When a recycled material containing a carbon dioxide absorbent is mixed in the mixing step, the method includes a heating step of heating the recycled material to 170 to 200°C prior to the mixing step, and includes a step of recovering the carbon dioxide absorption capacity of the carbon dioxide absorbent contained in the recycled material in the heating step, A method for producing an asphalt mixture, comprising the step of recovering carbon dioxide released in the mixing step.
2. When a recycled material containing a carbon dioxide absorbent is mixed in the mixing step, the method includes a heating step of heating the recycled material prior to the mixing step, and includes a step of recovering the carbon dioxide absorption capacity of the carbon dioxide absorbent contained in the recycled material in the heating step, The method for producing an asphalt mixture according to claim 1, wherein when a recycled material containing a carbon dioxide absorbent is mixed in the mixing step, a carbon dioxide capture device is connected to a heating device, and when the recycled material is heated by the heating device, the carbon dioxide released by the carbon dioxide absorbent in the recycled material in the heating device is captured by the carbon dioxide capture device.
3. The method for producing a carbon dioxide gas according to claim 2, further comprising a step of: the carbon dioxide capture device is connected to a mixing device; the carbon dioxide gas absorbent releases the carbon dioxide gas absorbed in the mixing device by the heat contained in the heated regenerator; and the released carbon dioxide gas is captured by the carbon dioxide capture device.
4. A method for repairing an asphalt pavement, comprising scraping a pavement composed of an asphalt mixture produced by the manufacturing method according to any one of claims 1 to 3, spreading the scraped pavement evenly, and compacting the pavement, A heating step of heating the road surface on which the asphalt mixture has been spread using a heating device to release carbon dioxide; A method for constructing or repairing an asphalt pavement that absorbs carbon dioxide, comprising a capture step of capturing the carbon dioxide released in the heating step using a carbon dioxide capture device.
5. The recovery step includes: A step of capturing, by a first carbon dioxide capture device, carbon dioxide released from the carbon dioxide absorbent when the road surface is heated by the heating device; A step of capturing, by a second carbon dioxide capture device, carbon dioxide released from the carbon dioxide absorbing material when the asphalt mixture is spread and leveled on a road surface by the asphalt mixture spreading device; 5. The method of construction or repair of claim 4, comprising:
6. The method includes a mixing step of scraping the heated asphalt mixture of the existing road surface with a road surface scraping device and mixing the scraped asphalt mixture with a mixing device; 6. The method of construction or repair according to claim 4 or claim 5, wherein the capture step includes a step of capturing carbon dioxide generated in the mixer during the mixing step by a second carbon dioxide capture device.
Citation Information
Patent Citations
JP1967003769Y1
JP1974042713A
Magnetic recording medium
JP1985080122A
Road surface reproducing device
JP1989278606A
Air cleaning method
JP2003053144A