Manufacturing method of optical laminate, adhesive application device, and manufacturing device of optical laminate

A sealed adhesive storage system with a secondary tank and controlled circulation maintains adhesive quality, addressing viscosity issues in optical laminate manufacturing to ensure consistent adhesion and efficiency.

JP7586831B2Active Publication Date: 2024-11-19NITTO DENKO CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021558248
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-19
Filing Date
2020-10-28
Publication Date
2024-11-19
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

Existing methods for manufacturing optical laminates face issues with adhesive viscosity changes due to moisture absorption and solvent evaporation, leading to reduced adhesion and increased costs, which impair manufacturing efficiency.

Method used

A method involving a sealed adhesive storage system with a larger secondary tank to maintain adhesive freshness, using active energy ray-curable adhesives with specific properties, and a controlled circulation system to ensure consistent adhesive quality.

Benefits of technology

Maintains good adhesion between optical films while reducing adhesive costs and preserving manufacturing efficiency by minimizing moisture absorption and solvent evaporation effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586831000001
    Figure 0007586831000001
  • Figure 0007586831000002
    Figure 0007586831000002
  • Figure 0007586831000003
    Figure 0007586831000003
Patent Text Reader

Abstract

[Problem] To provide a production method or the like for an optical layered product in which good adhesion is maintained, with a reduced running cost incurred for an adhesive and without a reduction in the manufacturing efficiency of the optical layered product. [Solution] The present invention comprises an adhesive application step for applying an actinic ray curable adhesive ad by using an adhesive application device 100 on at least a first optical film F1 or a second optical film F2, which are attached together to produce an optical layered product F. The adhesive application device comprises: an application machine 6 for applying an adhesive; a first tank 20 for storing the adhesive and supplying the adhesive to the application machine; and a second tank 30 that is for tightly sealing and storing the adhesive and supplying the adhesive to the first tank, and that has a larger storage amount of the adhesive than that of the first tank. In the adhesive application step, the adhesive is circulated between the first tank and the application machine, and when the amount of the adhesive stored in the first tank is not more than a predetermined value, the adhesive is supplied from the second tank to the first tank.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an optical laminate by bonding a first optical film and a second optical film with an adhesive, such as producing a polarizing film by bonding a polarizer and a protective film with an adhesive, an adhesive applicator, and an apparatus for producing an optical laminate. In particular, the present invention relates to a method for producing an optical laminate, an adhesive applicator, and an apparatus for producing an optical laminate, which are capable of maintaining good adhesion between the first optical film and the second optical film in the optical laminate while reducing the running cost of the adhesive and without impairing the production efficiency of the optical laminate. [Background technology]

[0002] Conventionally, polarizing films including a polarizer have been used as a constituent material of liquid crystal displays, polarized sunglasses, etc. A polarizing film is composed of, for example, a polarizer dyed with a dichroic material such as iodine and a protective film that protects the polarizer. As described in Patent Documents 1 to 3, for example, a polarizing film can be obtained by coating a polarizer and / or a protective film with an active energy ray-curable adhesive, bonding the polarizer and the protective film together, and irradiating the adhesive between the polarizer and the protective film with active energy rays to cure the adhesive. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-160313 A [Patent Document 2] JP 2012-144690 A [Patent Document 3] International Publication No. 2017 / 199979 Summary of the Invention [Problem to be solved by the invention]

[0004] Here, the active energy ray curable adhesive is applied to the polarizer and / or protective film by an adhesive applicator. In general, the adhesive applicator includes a coater such as a gravure coater and a tank that stores the adhesive and supplies the adhesive to the coater, and circulates the adhesive between the tank and the coater. For this reason, while the adhesive is stored in the tank or while the adhesive is circulating, the adhesive absorbs moisture from the atmosphere or the solvent components of the adhesive evaporate, causing the viscosity of the adhesive to change.

[0005] If the viscosity of the adhesive is too high or too low, the adhesion between the polarizer and the protective film decreases. Since a polarizing film is required to have stable optical properties, it is necessary to maintain good adhesion between the polarizer and the protective film. Therefore, for example, the timing at which the adhesive strength between the polarizing film and the protective film decreases is determined empirically, and the adhesive stored in the tank is replaced with new adhesive by this timing. However, frequent replacement of the adhesive stored in the tank increases the running costs of the adhesive, and since the production line for polarizing films must be stopped when replacing the adhesive, frequent replacement of the adhesive reduces the production efficiency of polarizing films.

[0006] In addition, an auxiliary tank that stores a smaller amount of adhesive than the tank may be installed between the tank and the coater. The adhesive may be supplied from the tank to the auxiliary tank, and then from the auxiliary tank to the coater, while the adhesive that was not applied by the coater is returned to the tank, thereby circulating the adhesive between the tank, the auxiliary tank, and the coater. Generally, the tank is mobile and is transported from the location where the adhesive is dissolved to the location where the coater is installed, and is replaced with the old tank. In contrast, the auxiliary tank is stationary, so it is possible to install a level meter to measure the liquid level of the adhesive stored in the auxiliary tank. Therefore, when an auxiliary tank is installed, it is possible to mechanically detect and prevent the depletion of the adhesive. However, even in the above case, while the adhesive is stored in the tank or the auxiliary tank, or while the adhesive is circulating, the adhesive may absorb moisture from the atmosphere or the solvent component of the adhesive may volatilize, causing a change in the viscosity of the adhesive. This may result in problems such as an increase in the running costs of the adhesive and a loss in the production efficiency of the polarizing film, as described above.

[0007] In the above explanation, a polarizing film obtained by bonding a polarizer and a protective film together via an adhesive is used as an example. However, the above problem is not limited to polarizing films, but is a problem common to optical laminates obtained by bonding a first optical film and a second optical film together via an adhesive. Therefore, an object of the present invention is to provide a method for manufacturing an optical laminate, an adhesive application device, and an apparatus for manufacturing an optical laminate that can maintain good adhesion between a first optical film and a second optical film in the optical laminate while reducing the running costs of the adhesive and without compromising the manufacturing efficiency of the optical laminate. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention includes an adhesive coating step of coating at least one of a first optical film and a second optical film with an active energy ray curable adhesive by an adhesive coater, and an optical laminate fabricating step of bonding the first optical film and the second optical film together via the adhesive and irradiating the adhesive with active energy rays to cure the adhesive, thereby fabricating an optical laminate, wherein the adhesive coater includes a coater that coats the adhesive, a first tank that stores the adhesive and supplies the adhesive to the coater, and a storage tank that seals and stores the adhesive and supplies the adhesive to the first tank, and a storage tank that stores the adhesive higher than the first tank. abilityand a second tank having a larger capacity, in which, in the adhesive application process, the adhesive is applied while being circulated between the first tank and the applicator, and when the amount of the adhesive stored in the first tank falls below a predetermined value, the adhesive is supplied from the second tank to the first tank.

[0009] In the present invention, too, while the adhesive is stored in the first tank or while the adhesive is circulating between the first tank and the coater, the adhesive between the first tank and the coater may absorb moisture from the atmosphere or the solvent components of the adhesive may volatilize. However, according to the present invention, when the adhesive stored in the first tank is applied to the first optical film and / or the second optical film, and the amount of the adhesive stored in the first tank becomes equal to or less than a predetermined value, the adhesive is supplied from the second tank to the first tank. Since the adhesive is stored in a sealed state in the second tank, it is difficult to absorb moisture in the atmosphere and the solvent component is difficult to volatilize. In addition, the adhesive that is not applied by the coater returns to the first tank instead of the second tank, so that the second tank is not mixed with the adhesive that has absorbed moisture in the atmosphere or the adhesive whose solvent component has volatilized due to the circulatory use between the first tank and the coater. Therefore, the adhesive that is almost new is supplied from the second tank to the first tank, and this almost new adhesive is newly circulated between the first tank and the coater. Since the amount of the adhesive stored in the second tank is larger than that of the first tank, the adhesive in the second tank can be used for a long time without being replaced until the adhesive in the second tank runs out. Therefore, according to the present invention, it is possible to maintain good adhesion between the first optical film and the second optical film in the optical laminate, while reducing the running costs of the adhesive and not compromising the manufacturing efficiency of the optical laminate.

[0010] In the present invention, the "adhesive application process of applying an active energy ray curable adhesive to at least one of the first optical film and the second optical film by an adhesive application device" includes, for example, any of the following processes: (1) a process of applying an active energy ray curable adhesive to both the first optical film and the second optical film by an adhesive application device; (2) a process of applying an active energy ray curable adhesive to the first optical film by an adhesive application device, and applying an easy-adhesion composition to the second optical film by the adhesive application device of the present invention; and (3) a process of applying an active energy ray curable adhesive to the second optical film by an adhesive application device, and applying an easy-adhesion composition to the first optical film by the adhesive application device of the present invention.

[0011] Preferably, in the adhesive application step, the adhesive has a viscosity at 25° C. of 1 mPa·s to 100 mPa·s at the start of application. If the viscosity in the above-mentioned preferred method can be maintained, good adhesion between the first optical film and the second optical film can be easily maintained.

[0012] Preferably, in the adhesive application step, the adhesive has a coating thickness of 0.1 μm to 5 μm. In the case of the above-mentioned preferred method, when the coating thickness is thin, a gravure coater is preferably used as a coater, but when a gravure coater is used, the adhesive tends to remain (overflow) without being applied to the first optical film and / or the second optical film, and therefore the adhesive is recycled, and the present invention is preferably used.

[0013] Preferably, the adhesive contains a hydroxyl group. When an adhesive contains hydroxyl groups, it is prone to absorbing moisture from the atmosphere, and therefore the present invention is preferably used in the case of adhesives that contain hydroxyl groups.

[0014] Preferably, the adhesive has an SP value of 29.0 (MJ / m 3 ) 1 / 2 More than 32.0(MJ / m 3 ) 1 / 2or less than 21.0 (MJ / m 3 ) 1 / 2 More than 23.0(MJ / m 3 ) 1 / 2 The polymerizable compound includes the following radical polymerizable compound. When the adhesive has the above SP value (solubility parameter), when a polarizer is used as the first optical film and a protective film is used as the second optical film, the SP value becomes close to that of the materials of polarizers and protective films that are generally used, which contributes to improving the adhesiveness. In addition, the SP value is relatively large and the adhesive is easily absorbed by moisture in the atmosphere, so that the present invention is preferably used.

[0015] Preferably, the adhesive contains water. When the adhesive contains water and a polarizer is used as the first optical film, the water swells and plasticizes the polarizer surface, making it easier to form various physical and chemical bonds such as hydrogen bonds, ionic bonds, and covalent bonds between the polarizer and the adhesive, resulting in improved adhesion.

[0016] Preferably, the adhesive contains at least one organometallic compound selected from the group consisting of metal alkoxides and metal chelates. When the adhesive contains the above-mentioned organometallic compound, the adhesiveness and water resistance are improved.

[0017] Preferably, the adhesive is cationically polymerizable. compound Contains: The adhesive contains a cationic polymerizable functional group (e.g., an epoxy group, an oxetanyl group, an oxetane group, a vinyl ether group, a spiro orthoester group). A cationic polymerizable compound having When this compound is contained, in the case where a polarizer is used as the first optical film, a stronger interaction occurs between the acid groups present on the polarizer surface and the adhesive, resulting in interlayer adhesion that is not easily peeled off even in the presence of moisture.

[0018] The present invention is suitably used in the case where the first optical film is a polarizer, the second optical film is a protective film, and the optical laminate is a polarizing film. However, the present invention is not limited to this, and the combination of the first optical film and the second optical film can be applied to various combinations of optical films, such as polarizers, protective films, retardation films, anti-glare films, brightness enhancement films, viewing angle enhancement films, and transparent conductive films.

[0019] Further, in order to solve the above-mentioned problems, the present invention provides an adhesive applicator that applies an active energy ray curable adhesive to at least one of a first optical film and a second optical film, the adhesive applicator including a coater that applies the adhesive, a first tank that stores the adhesive and supplies the adhesive to the coater while circulating the adhesive between the coater and the first tank, and a storage tank that seals and stores the adhesive and supplies the adhesive to the first tank, the storage tank being larger than the first tank. ability and a control device that supplies the adhesive from the second tank to the first tank when the adhesive is applied from the applicator and the amount of the adhesive stored in the first tank falls below a predetermined value.

[0020] Furthermore, in order to solve the above problem, the present invention also provides an apparatus for manufacturing an optical laminate, comprising: the adhesive applicator; and an active energy ray irradiation device that irradiates the adhesive between the first optical film and the second optical film bonded together via the adhesive with active energy rays to harden the adhesive. Effect of the Invention

[0021] According to the present invention, it is possible to maintain good adhesion between the first optical film and the second optical film in the optical laminate, while reducing the running costs of the adhesive and not compromising the production efficiency of the optical laminate. [Brief description of the drawings]

[0022] [Figure 1]FIG. 1 is a diagram illustrating an example of the schematic configuration of a manufacturing apparatus for an optical laminate (polarizing film) to which a manufacturing method for an optical laminate (polarizing film) according to one embodiment of the present invention is applied. [Diagram 2] FIG. 2 is a diagram showing a schematic diagram of a specific configuration example of the adhesive applicator 100 shown in FIG. [Diagram 3] 3 is a diagram showing an example of a change in the refractive index of an adhesive measured by the refractometer 23 shown in FIG. 2 and a change in the moisture content of the adhesive calculated from the measured refractive index. FIG. [Figure 4] The measurement results of the peel strength obtained in Examples 1 to 4 and Comparative Examples 1 to 4 are shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, a method for producing an optical laminate, an adhesive applicator, and an apparatus for producing an optical laminate according to one embodiment of the present invention will be described with reference to the accompanying drawings, taking as an example a case in which the first optical film is a polarizer, the second optical film is a protective film, and the optical laminate is a polarizing film. Therefore, in this embodiment, the "optical laminate" will be referred to as a "polarizing film", the "first optical film" will be referred to as a "polarizer", and the "second optical film" will be referred to as a "protective film". In this specification, a numerical range represented by "lower limit X to upper limit Y" means a range from lower limit X to upper limit Y. When a plurality of numerical ranges are separately described, it is understood that any lower limit and any upper limit can be selected to set "any lower limit to any upper limit." In addition, it should be noted that each drawing is for reference purposes only, and the dimensions, scale, and shapes of components and the like shown in each drawing may differ from the actual ones.

[0024] 1 is a diagram showing a schematic configuration example of a polarizing film manufacturing apparatus to which the polarizing film manufacturing method according to the present embodiment is applied, in which the arrows in FIG. 1 indicate the transport direction of each film. The polarized film manufacturing apparatus according to this embodiment includes an adhesive applicator 100 and an active energy ray irradiation device 8, as well as various conventionally known components that are included in general polarized film manufacturing apparatuses. The polarizing film manufacturing apparatus according to the present invention may be of a type in which a polarizer F1 is manufactured and then a protective film F2 is continuously bonded to the polarizer F1, or a polarizer F1 is separately prepared and then a protective film F2 is bonded to the polarizer F1. The former type is a type in which a series of steps from manufacturing the polarizer F1 to bonding the protective film F2 to obtain a polarizing film F are performed on one manufacturing line, while the latter type is a type in which the polarizer F1 is manufactured on one manufacturing line and the step of bonding the protective film F2 to the polarizer F1 to obtain a polarizing film F is performed on another manufacturing line. The manufacturing apparatus shown in FIG. 1 is of a roll-to-roll type, in which a series of steps from the manufacture of the polarizer F1 to the bonding of at least the protective film F2 to obtain the polarizing film F are carried out on a single manufacturing line.

[0025] In manufacturing the polarizing film F using the manufacturing equipment shown in FIG. 1, first, the raw film F0 wound around the unwinding roller 1 is unwound and immersed in a treatment bath in a treatment tank 2 (for example, consisting of a swelling treatment tank, a dyeing treatment tank, a crosslinking treatment tank, a stretching treatment tank, and a cleaning treatment tank, in that order from the upstream side in the conveying direction of the raw film F0), where the film is dyed with a dichroic substance such as iodine or a dichroic dye and uniaxially stretched. Next, the film is dried in an oven 3 to obtain a polarizer F1. The polarizer F1 is an optical element that has the property of transmitting light (polarized light) vibrating in only one specific direction and blocking light vibrating in other directions. The polarizer F1 of this embodiment is in the form of a flexible film.

[0026] The raw film F0 is a long strip. In this specification, a long strip means a rectangular shape whose longitudinal length is sufficiently longer than its lateral length (direction perpendicular to the longitudinal direction). The longitudinal length of the long strip is, for example, 10 m or more, and preferably 50 m or more. The raw film F0 is not particularly limited, but is preferably a film containing a hydrophilic polymer film (e.g., a polyvinyl alcohol-based film, etc.) because of its excellent dyeability with a dichroic substance, and more preferably a hydrophilic polymer film. An example of a film containing a hydrophilic polymer film is a film in which a hydrophilic polymer film and a non-hydrophilic polymer film are laminated. In this case, it is preferable that the hydrophilic polymer film is laminated on the front and / or back surface of the non-hydrophilic polymer film. In this case, the hydrophilic polymer film laminated on the front and / or back surface of the non-hydrophilic polymer film may be a thin film having a thickness of about several μm.

[0027] The hydrophilic polymer film is not particularly limited, and a conventionally known film can be used. Specifically, examples of the hydrophilic polymer film include polyvinyl alcohol (PVA)-based films, partially formalized PVA-based films, polyethylene terephthalate (PET) films, ethylene-vinyl acetate copolymer-based films, and partially saponified films thereof. In addition to these, polyene-oriented films such as dehydrated PVA and dehydrochlorinated polyvinyl chloride, and stretch-oriented polyvinylene-based films can also be used. Among these, PVA-based polymer films are preferred because they are particularly excellent in dyeability with dichroic substances. Examples of raw material polymers for PVA-based polymer films include polymers obtained by polymerizing vinyl acetate and then saponifying it, and polymers obtained by copolymerizing vinyl acetate with a small amount of a copolymerizable monomer such as an unsaturated carboxylic acid or an unsaturated sulfonic acid. The degree of polymerization of the PVA-based polymer is not particularly limited, but is preferably 500 to 10,000, and more preferably 1,000 to 6,000, in terms of solubility in water, etc. The degree of saponification of the PVA-based polymer is preferably 75 mol% or more, and more preferably 98 mol% to 100 mol%. The thickness of the untreated raw film F0 is not particularly limited, but is, for example, 15 μm to 110 μm.

[0028] When the processing tank 2 is composed of a swelling processing tank, a dyeing processing tank, a crosslinking processing tank, a stretching processing tank, and a cleaning processing tank (not shown) in that order from the upstream side in the transport direction of the raw film F0, each tank has, for example, the configuration described below.

[0029] <Swelling treatment tank> The swelling treatment tank is a treatment tank that contains a swelling treatment liquid. The swelling treatment liquid swells the raw film F0. For example, water can be used as the swelling treatment liquid. Furthermore, water to which an appropriate amount of an iodine compound such as glycerin or potassium iodide has been added may be used as the swelling treatment liquid. When glycerin is added, its concentration is preferably 5% by weight or less, and when an iodine compound such as potassium iodide is added, its concentration is preferably 10% by weight or less.

[0030] <Dyeing treatment tank> The dyeing treatment tank is a treatment tank containing a dyeing treatment liquid. The dyeing treatment liquid dyes the raw film F0. The dyeing treatment liquid may be a solution containing a dichroic substance as an active ingredient. Examples of the dichroic substance include iodine and organic dyes. Preferably, the dyeing treatment liquid is a solution in which iodine is dissolved in a solvent. Water is generally used as the solvent, but an organic solvent compatible with water may be further added. The concentration of iodine in the dyeing treatment liquid is not particularly limited, but is preferably 0.01% by weight to 10% by weight, more preferably 0.02% by weight to 7% by weight, and even more preferably 0.025% by weight to 5% by weight. In order to further improve the dyeing efficiency, an iodine compound may be added to the dyeing treatment liquid as necessary. An iodine compound is a compound that contains iodine and an element other than iodine in the molecule, and examples thereof include potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, and titanium iodide.

[0031] <Cross-linking treatment tank> The crosslinking treatment tank is a treatment tank containing a crosslinking treatment liquid. The crosslinking treatment liquid crosslinks the dyed raw film F0. As the crosslinking treatment liquid, a solution containing a boron compound as an active ingredient can be used. For example, as the crosslinking treatment liquid, a solution in which a boron compound is dissolved in a solvent can be used. As the solvent, water is generally used, but an organic solvent compatible with water may be further added. Examples of the boron compound include boric acid and borax. The concentration of the boron compound in the crosslinking treatment liquid is not particularly limited, but is preferably 1% by weight to 10% by weight, more preferably 2% by weight to 7% by weight, and even more preferably 2% by weight to 6% by weight. Furthermore, since a polarizer having uniform optical properties can be obtained, an iodine compound may be added to the crosslinking treatment liquid as necessary.

[0032] <Stretching tank> The stretching treatment tank is a treatment tank that contains a stretching treatment solution. The stretching treatment liquid is not particularly limited, but for example, a solution containing a boron compound as an active ingredient can be used. As the stretching treatment liquid, for example, a solution in which a boron compound and, if necessary, various metal salts, zinc compounds, etc. are dissolved in a solvent can be used. As the solvent, water is generally used, but an organic solvent compatible with water may be further added. The concentration of the boron compound in the stretching treatment liquid is not particularly limited, but is preferably 1% by weight to 10% by weight, more preferably 2% by weight to 7% by weight. From the viewpoint of suppressing the elution of iodine adsorbed to the film, an iodine compound may be added to the stretching treatment liquid as necessary.

[0033] <Cleaning treatment tank> The cleaning treatment tank is a treatment tank that contains a cleaning treatment liquid. The cleaning treatment liquid is used to clean the raw film F0 after stretching. The cleaning treatment liquid is a treatment liquid for cleaning treatment liquids such as dyeing treatment liquid and crosslinking treatment liquid that are attached to the raw film F0. As the cleaning treatment liquid, water such as ion-exchanged water, distilled water, and pure water is typically used.

[0034] The oven 3 is provided downstream of the cleaning treatment tank constituting the above-described treatment tank 2. The oven 3 is provided to dry the film after treatment. In the above-described example, the processing tank 2 includes a swelling processing tank, a dyeing processing tank, a crosslinking processing tank, a stretching processing tank, and a cleaning processing tank, but one or two of these processing tanks may be omitted. On the other hand, the processing tank 2 may further include an adjustment processing tank (not shown). The adjustment processing tank is a processing tank that contains an adjustment processing liquid. This adjustment processing tank is provided between the crosslinking processing tank and the stretching processing tank, or between the stretching processing tank and the cleaning processing tank. The adjustment processing liquid is a solution for adjusting the hue of the film, and a solution containing an iodine compound as an active ingredient can be used. The washed original film F0 was dried in an oven 3 to obtain a film, which was a polarizer F1.

[0035] 1, an active energy ray curable adhesive is applied to both sides of the polarizer F1 by an adhesive applicator 100 (corresponding to the adhesive application step of the present invention). Also, the active energy ray curable adhesive is applied to one side of the protective film F2 fed from a feed roller 5 by the adhesive applicator 100. Then, the protective film F2 coated with the adhesive is bonded to both sides of the polarizer F1 coated with the adhesive by a bonding roller 7. The coating thickness of the adhesive is not particularly limited, but if it is too small, the adhesive strength of the film decreases, and if it is too large, the thickness of the polarizing film F becomes relatively too large. From this viewpoint, it is preferable that the coating thickness of the adhesive on the polarizer F1 and the protective film F2 is each independently 0.1 μm to 5 μm. Furthermore, the viscosity of the adhesive at the start of coating is not particularly limited, but if it is too low or high, the adhesiveness of the adhesive will decrease from the start of coating. From this perspective, the viscosity of the adhesive at 25°C at the start of coating is preferably adjusted to 1 mPa·s to 100 mPa·s, more preferably 10 mPa·s to 50 mPa·s, and particularly preferably 15 mPa·s to 45 mPa·s. The specific configuration of the adhesive applicator 100 and the types of adhesive applied by the adhesive applicator 100 will be described later.

[0036] The protective film F2 is in the form of a long strip. The protective film F2 is a film that is less hydrophilic (has hydrophobicity) than the polarizer F1. The protective film F2 is preferably excellent in transparency, mechanical strength, thermal stability, moisture blocking properties, isotropy, and the like. Examples of the protective film F2 include polyester-based polymers such as polyethylene terephthalate and polyethylene naphthalate, cellulose-based polymers such as diacetyl cellulose and triacetyl cellulose, acrylic polymers such as polymethyl methacrylate, styrene-based polymers such as polystyrene and acrylonitrile-styrene copolymer (AS resin), and polycarbonate-based polymers. Examples of the polymer forming the protective film F2 include polyethylene, polypropylene, polyolefins having a cyclo- or norbornene structure, polyolefin-based polymers such as ethylene-propylene copolymers, vinyl chloride-based polymers, amide-based polymers such as nylon and aromatic polyamides, imide-based polymers, sulfone-based polymers, polyethersulfone-based polymers, polyetheretherketone-based polymers, polyphenylene sulfide-based polymers, vinyl alcohol-based polymers, vinylidene chloride-based polymers, vinyl butyral-based polymers, arylate-based polymers, polyoxymethylene-based polymers, epoxy-based polymers, and blends of the above polymers. The protective film F2 may contain one or more of any suitable additives. Examples of the additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, coloring inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants. The content of the thermoplastic resin in the protective film F2 is preferably 50 to 100% by weight, more preferably 50 to 99% by weight, further preferably 60 to 98% by weight, and particularly preferably 70 to 97% by weight. If the content of the thermoplastic resin in the protective film F2 is 50% by weight or less, the inherent high transparency of the thermoplastic resin may not be fully exhibited.

[0037] In addition, examples of the protective film F2 include polymer films described in JP-A-2001-343529, such as a resin composition containing (A) a thermoplastic resin having a substituted and / or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted and / or unsubstituted phenyl and nitrile group in the side chain. Specific examples include a film of a resin composition containing an alternating copolymer of isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer. As the film, a film made of a mixed extrusion product of the resin composition can be used. These films have a small phase difference and a small photoelastic coefficient, so they can eliminate problems such as unevenness caused by distortion of the polarizing film F, and have a small moisture permeability, so they have excellent moisture durability.

[0038] Next, as shown in FIG. 1, the adhesive between the polarizer F1 and the protective film F2 is irradiated with active energy rays from an active energy ray irradiation device 8 to cure, and then dried in an oven 9. The active energy rays are appropriately selected depending on the curability of the active energy ray curable adhesive. Examples of the active energy rays include electron beams, ultraviolet rays, and visible light. Finally, a long strip-shaped surface protective film F3 unwound from a pay-out roller 10 is laminated by a lamination roller 11 to one side of the polarizer F1 having protective films F2 laminated on both sides, thereby obtaining a long strip-shaped polarizing film F. The obtained polarizing film F is taken up by a take-up roller 12. The process of producing a polarizing film F by bonding a polarizer F1 and a protective film F2 via an adhesive and irradiating the adhesive with active energy rays to harden the adhesive corresponds to the optical laminate production process of the present invention.

[0039] In the example shown in FIG. 1, the active energy ray curable adhesive is applied to both the polarizer F1 and the protective film F2, but it is also possible to apply the adhesive only to both sides of the polarizer F1. In this case, of the total four adhesive applicators 100 shown in FIG. 1, the two adhesive applicators 100 on the lower side (downstream side in the film transport direction) in FIG. 1 are not necessary. It is also possible to apply the adhesive only to one side of the protective film F2. In this case, of the total four adhesive applicators 100 shown in FIG. 1, the two adhesive applicators 100 on the upper side (upstream side in the film transport direction) in FIG. 1 are not necessary. Furthermore, in the example shown in Figure 1, a protective film F2 is bonded to both sides of the polarizer F1, so a pair of adhesive applicators 100 are arranged on the left and right sides of Figure 1, and a pair of active energy ray irradiation devices 8 are arranged on the left and right sides. However, if a protective film F2 is bonded to only one side of the polarizer F1, it is sufficient to arrange only one adhesive applicator 100 and one active energy ray irradiation device 8 on either the left or right side of Figure 1.

[0040] Fig. 2 is a diagram showing a schematic diagram of a specific configuration example of the adhesive applicator 100. Fig. 2 shows the inside of each component in a see-through state as appropriate. As shown in FIG. 2, the adhesive applicator 100 of this embodiment includes a coater 6 that applies adhesive ad to a polarizer F1 or a protective film F2 (not shown in FIG. 2), a first tank 20 that stores the adhesive ad and supplies the adhesive ad to the coater 6 while circulating the adhesive ad between the coater 6 and the first tank 20, a second tank 30 that has a larger stored amount of adhesive ad than the first tank 20 and seals and stores the adhesive ad and supplies the adhesive ad to the first tank 20, and a control device 40 that causes the second tank 30 to supply adhesive ad to the first tank 20 when the amount of adhesive ad stored in the first tank 20 falls below a predetermined value.

[0041] A gravure coater is preferably used as the coater 6. The gravure coater has a gravure roll on whose surface a plurality of cells (recesses into which the supplied adhesive ad fits) are formed, and the gravure roll 61 comes into contact with the polarizer F1 or the protective film F2, whereby the adhesive ad in the cells is transferred to one side of the polarizer F1 or the protective film F2. In this manner, the adhesive ad is solidly applied from the gravure roll to one side of the polarizer F1 or the protective film F2, respectively.

[0042] The adhesive applicator 100 of this embodiment further includes a supply pipe 21, a pump 22, a refractometer 23, and a discharge pipe 24. The adhesive ad stored in the first tank 20 is sucked up by a pump 22 attached to the supply pipe 21 through the supply pipe 21, the lower end of which is inserted into the first tank 20 and immersed in the adhesive ad, and is supplied to the coater 6. A refractometer 23 is attached to the supply pipe 21, and the refractive index of the adhesive ad flowing through the supply pipe 21 is continuously measured by the refractometer 23. As the refractometer 23, various conventionally known refractometers can be applied, and for example, a process refractometer "PRM-100α" manufactured by ATAGO, whose measurement principle is a method of deriving the refractive index from the critical angle of total reflection using Snell's law, can be used.

[0043] On the other hand, the adhesive ad that has not been applied to the polarizer F 1 or the protective film F 2 by the coater 6 returns to the first tank 20 through a discharge pipe 24 , the lower end of which is inserted into the first tank 20 . In this manner, the adhesive ad is used while being circulated between the first tank 20 and the coater 6.

[0044] The adhesive applicator 100 of this embodiment further includes a bag 31, a cable tie 32, a first supply pipe 33, a weight 34, a joint 35, a second supply pipe 36, and a lid 37. The second tank 30 contains a bag 31 containing adhesive ad therein and having an upper end bound by a cable tie 32. As a result, the adhesive ad is sealed and stored in the second tank 30. A first supply pipe 33 having flexibility, such as a rubber hose, is inserted into the bag 31. A weight 34 is attached to the lower end of the first supply pipe 33 so that the lower end of the first supply pipe 33 is located near the bottom surface of the bag 31. The first supply pipe 33 passes through the upper end of the bag 31 and the cable tie 32, and its upper end is connected to a joint 35. A second supply pipe 36 having flexibility, such as a rubber hose, is also connected to this joint 35, and the first supply pipe 33 and the second supply pipe 36 communicate with each other via the joint 35. The adhesive ad stored in the second tank 30 (inside the bag body 31) is sucked up from the lower end of the first supply pipe 33, through the first supply pipe 33, the fitting 35 and the second supply pipe 36 by a pump 42 attached to the second supply pipe 36, and discharged from the lower end of the second supply pipe 36 to be supplied to the first tank 20.

[0045] The amount of adhesive ad stored in the second tank 30 (in the bag body 31) is larger than the amount of adhesive ad stored in the first tank 20. For example, the amount of adhesive ad stored in the second tank 30 is 180 liters, whereas the amount of adhesive ad stored in the first tank 20 is 30 liters or less. It is preferable that the amount of adhesive ad stored in the second tank 30 is about 2 to 50 times the amount of adhesive ad stored in the first tank 20.

[0046] When supplying the adhesive ad from the second tank 30 to the first tank 20, the lid 37 for closing the upper end opening of the second tank 30 is opened and the second supply pipe 36 is connected to the joint 35, as shown in Fig. 2. On the other hand, when preparing the adhesive ad in the second tank 30, the second supply pipe 36 is removed from the joint 35 and the lid 37 is closed. At this time, if a stopper (not shown) is provided on the lower surface of the lid 37 and the connection part of the joint 35 with the second supply pipe 36 is plugged with this stopper, the adhesive ad in the second tank 30 can be kept sealed.

[0047] The control device 40 of this embodiment includes a control device main body 41 configured with a computer or a PLC (Programmable Logic Controller), a pump 42, and a level gauge 43. As the level gauge 43, various conventionally known level gauges (liquid level gauges) can be applied, and for example, a guided pulse type level sensor "FL-001" manufactured by Keyence Corporation, which uses a guided pulse method as a measurement principle, can be used. The control device main body 41 receives an input of a liquid level measurement value of the adhesive ad stored in the first tank 20, measured by a level gauge 43. When the input liquid level measurement value falls below a preset threshold value (i.e., when the amount of adhesive ad stored in the first tank 20 falls below a predetermined value), the control device main body 41 transmits a control signal to the pump 42 to drive the pump 42. This drives the pump 42, and the adhesive ad stored in the second tank 30 (in the bag body 31) is sucked up from the lower end of the first supply pipe 33 through the first supply pipe 33, the joint 35, and the second supply pipe 36, discharged from the lower end of the second supply pipe 36, and supplied to the first tank 20. In this manner, the control device 40 causes the second tank 30 to supply the adhesive ad to the first tank 20 when the amount of the adhesive ad stored in the first tank 20 becomes equal to or less than a predetermined value.

[0048] An active energy ray curable adhesive is used as the adhesive ad applied by the adhesive applicator 100 having the configuration described above. That is, in the second tank 30 of the adhesive applicator 100, an uncured active energy ray curable adhesive is prepared and stored. As the active energy ray-curable adhesive, a conventionally known adhesive can be used. The active energy ray-curable adhesive generally contains an active energy ray-curable component and a polymerization initiator, and further contains various additives as necessary. Active energy ray-curable components can be roughly divided into electron beam-curable, ultraviolet ray-curable, and visible light-curable components, and from the viewpoint of the curing mechanism, active energy ray-curable components can be roughly divided into radical polymerizable compounds and cationically polymerizable compounds.

[0049] The radical polymerizable compound may be a compound having a radical polymerizable functional group of a carbon-carbon double bond, such as a (meth)acryloyl group or a vinyl group. In addition, either a monofunctional radical polymerizable compound or a polyfunctional radical polymerizable compound having two or more functional groups may be used. In addition, these radical polymerizable compounds may be used alone or in combination of two or more. As the radical polymerizable compound, a compound having a (meth)acryloyl group is preferable, and examples thereof include a (meth)acrylamide derivative having a (meth)acrylamide group and a (meth)acrylate having a (meth)acryloyloxy group. When a radical polymerizable compound is used as the active energy ray curable adhesive, the polymerization initiator is appropriately selected according to the active energy ray. When the adhesive is cured by ultraviolet light or visible light, a polymerization initiator that is cleaved by ultraviolet light or visible light is used. Examples of such polymerization initiators include benzophenone-based compounds, aromatic ketone compounds, acetophenone-based compounds, aromatic ketal-based compounds, aromatic sulfonyl chloride-based compounds, and thioxanthone-based compounds.

[0050] Examples of the cationic polymerizable compound include monofunctional cationic polymerizable compounds having one cationic polymerizable functional group in the molecule, and polyfunctional cationic polymerizable compounds having two or more cationic polymerizable functional groups in the molecule. Examples of the cationic polymerizable functional group include epoxy groups, oxetanyl groups, oxetane groups, vinyl ether groups, and spiro orthoester groups. Examples of the cationic polymerizable compound having an epoxy group include aliphatic epoxy compounds, alicyclic epoxy compounds, and aromatic epoxy compounds. Examples of the cationic polymerizable compound having an oxetanyl group include 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetanyl)methoxymethyl]benzene, and 3-ethyl-3-(phenoxymethyl)oxetane. Examples of the cationic polymerizable compound having a vinyl ether group include 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, and 4-hydroxybutyl vinyl ether. When a cationic polymerizable compound is used as the active energy ray curable adhesive, a cationic polymerization initiator is blended. This cationic polymerization initiator generates cationic species or Lewis acid by irradiation with active energy rays such as visible light, ultraviolet light, and electron beams, and initiates a polymerization reaction with the epoxy group of the cationic polymerizable compound. As the cationic polymerization initiator, a photoacid generator and a photobase generator can be used.

[0051] In the present invention, an active energy ray-curable adhesive that is cured by light including visible light of 380 nm to 450 nm can also be used. In this case, it is preferable to use an active energy ray-curable adhesive that contains a radical polymerizable compound and a polymerization initiator. Such an active energy ray curable adhesive is disclosed, for example, in JP 2018-092186 A, and the active energy ray curable adhesive described in the above publication can be used as the active energy ray curable adhesive of the present invention. In this specification, due to space limitations, the description of the above publication is omitted, but the description of the adhesive in the above publication is incorporated into this specification as it is.

[0052] In the present invention, an active energy ray curable adhesive containing a hydroxyl group can also be used as the adhesive ad. For example, the adhesive of Example 1 described in paragraph 0152 and Table 1 of Patent Document 1 can be used as such an active energy ray curable adhesive. In this specification, the description of Patent Document 1 is omitted due to space limitations, but the description of the adhesive in Patent Document 1 can be directly incorporated into this specification.

[0053] In the present invention, the adhesive ad has an SP value of 29.0 (MJ / m 3 ) 1 / 2 More than 32.0(MJ / m 3 ) 1 / 2 or less than 21.0 (MJ / m 3 ) 1 / 2 More than 23.0(MJ / m 3 ) 1 / 2An active energy ray curable adhesive containing the following radical polymerizable compound can also be used. As such an active energy ray curable adhesive, for example, an active energy ray curable adhesive containing a radical polymerizable compound (A) or a radical polymerizable compound (C) described in paragraph 0015 of Patent Document 2 can be used. In this specification, due to space limitations, the description of Patent Document 2 is omitted, but the description of the adhesive in Patent Document 2 can be directly incorporated into this specification.

[0054] In addition, in the present invention, an active energy ray curable adhesive containing water can also be used as the adhesive ad. For example, a combination of a conventionally known active energy ray curable adhesive and the adhesive of Example 16 (easy-adhesion composition) described in Table 3 of Patent Document 3 can be used as such an active energy ray curable adhesive. In this specification, due to space limitations, the description of Patent Document 3 is omitted, but the description of the adhesive in Patent Document 3 can be directly incorporated into this specification.

[0055] Furthermore, in the present invention, an active energy ray curable adhesive containing at least one organometallic compound selected from the group consisting of metal alkoxides and metal chelates can be used as the adhesive ad. As such an active energy ray curable adhesive, for example, the adhesive of Example 1 described in paragraph 0152 and Table 1 of Patent Document 1 can be used.

[0056] According to the manufacturing method of the polarizing film F according to the present embodiment described above, when the adhesive ad stored in the first tank 20 is applied to the polarizer F1 and the protective film F2, and the amount of the adhesive ad stored in the first tank 20 becomes equal to or less than a predetermined value, the adhesive ad is supplied from the second tank 30 to the first tank 20. Since the adhesive ad is sealed and stored in the second tank 30, it is difficult to absorb moisture in the atmosphere and the solvent component is difficult to volatilize. In addition, the adhesive ad that has not been applied by the coater 6 returns to the first tank 20 instead of the second tank 30, so that the adhesive ad that has absorbed moisture in the atmosphere and the adhesive ad that has volatilized the solvent component due to the circulatory use between the first tank 20 and the coater 6 is not mixed into the second tank 30. Therefore, the adhesive ad that is almost new is supplied from the second tank 30 to the first tank 20, and this almost new adhesive ad is newly circulated between the first tank 20 and the coater 6. Since the amount of adhesive ad stored in the second tank 30 is larger than that in the first tank 20, the adhesive ad in the second tank 30 can be used for a long period of time without being replaced until the adhesive in the second tank 30 runs out. Therefore, according to the manufacturing method of the polarizing film F of this embodiment, it is possible to maintain good adhesion between the polarizer F1 and the protective film F2 in the polarizing film F while reducing the running costs of the adhesive ad and without compromising the manufacturing efficiency of the polarizing film F.

[0057] Fig. 3 is a diagram showing an example of the change in refractive index of the adhesive ad measured by the refractometer 23 shown in Fig. 2 and the change in moisture content of the adhesive ad calculated from the measured refractive index. In Fig. 3, the vertical axis for the refractive index (the vertical axis on the left side of Fig. 3) represents the amount of change from the initial refractive index. The refractive index and moisture content of the adhesive ad are related by the formula Y = aX + b (where a and b are coefficients determined by the adhesive ad), where X is the refractive index and Y is the moisture content. Using this formula, it is possible to calculate the moisture content from the measured refractive index. The refractive index (shown by a solid line in FIG. 3) and moisture content (shown by a dashed line in FIG. 3) of the adhesive ad were measured and calculated in a state in which the adhesive ad was circulated between the first tank 20 and the coater 6 without being coated from the coater 6 from the start of circulation of the adhesive ad between the first tank 20 and the coater 6 until the "start time of continuous operation" (after 19 hours had elapsed). After the "start time of continuous operation" had elapsed, the measurements and calculations were performed in a state in which the adhesive ad was coated from the coater 6 while circulating between the first tank 20 and the coater 6. The time point indicated by the outlined arrow in FIG. 3 indicates the timing at which the pump 42 was driven to supply the adhesive ad from the second tank 30 to the first tank 20. As shown in Figure 3, over time, the refractive index of the adhesive ad decreases (the moisture content increases) as it absorbs moisture from the atmosphere. However, by supplying nearly new adhesive ad from the second tank 30 to the first tank 20 at the time indicated by the white arrow, the refractive index of the applied adhesive ad increases (the moisture content decreases), and it can be expected that good adhesive properties can be maintained. EXAMPLES

[0058] The present invention will be described in more detail below with reference to examples and comparative examples, although the present invention is not limited to the following examples.

[0059] [Materials used] <Active energy ray curing adhesive A> 55% by weight of 1,9-nonanediol diacrylate, 10% by weight of hydroxyethyl acrylamide, and 30% by weight of acryloylmorpholine (active energy ray curable components) were mixed with 3% by weight of IRGACURE 907 and 2% by weight of KAYACURE DETX-S (polymerization initiator) and stirred for 3 hours to obtain active energy ray curable adhesive A. The viscosity of this active energy ray-curable adhesive A at 25°C at the start of coating was 20 mPa·s.

[0060] <Active energy ray curing adhesive B> 52% by weight of 1,9-nonanediol diacrylate, 10% by weight of hydroxyethyl acrylamide, 30% by weight of acryloyl morpholine, 3 parts by weight of 3-acrylamidophenylboronic acid (active energy ray curable component), 3% by weight of IRGACURE 907, and 2% by weight of KAYACURE DETX-S (polymerization initiator) were mixed and stirred for 3 hours to obtain active energy ray curable adhesive B. The viscosity of this active energy ray-curable adhesive B at 25°C at the start of coating was 22 mPa·s.

[0061] <Active energy ray curing adhesive C> 53% by weight of 1,9-nonanediol diacrylate, 10% by weight of hydroxyethyl acrylamide, 30% by weight of acryloyl morpholine, 1 part by weight of 3-acrylamidophenylboronic acid (active energy ray curable component), 1 part by weight of Orgatix TA-30: tetraoctyl titanate, 3% by weight of IRGACURE 907, and 2% by weight of KAYACURE DETX-S (polymerization initiator) were mixed and stirred for 3 hours to obtain active energy ray curable adhesive C. The viscosity of this active energy ray-curable adhesive C at 25°C at the start of coating was 20 mPa·s.

[0062] <Active energy ray curing adhesive D> 62% by weight of glycerin triacrylate, 10% by weight of 4-hydroxybutyl acrylate, 20% by weight of 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, 3% by weight of IRGACURE 907, 2% by weight of KAYACURE DETX-S (polymerization initiator), and 3% by weight of CPI-100P (photoacid generator) were mixed and stirred for 3 hours to obtain active energy ray-curable adhesive D. The viscosity of this active energy ray-curable adhesive D at 25°C at the start of coating was 35 mPa·s. The viscosities of the active energy ray-curable adhesives A to D at 25° C. at the start of coating were measured using an E-type viscometer.

[0063] <Polarizer X> Using an existing polarizer manufacturing apparatus equipped with a payout roller 1, a treatment tank 2, and an oven 3 shown in FIG. 1, a polyvinyl alcohol film having an average degree of polymerization of 2400 and a saponification degree of 99.9 mol% and a thickness of 45 μm was immersed in warm water at 30° C. for 60 seconds to swell. The film was then immersed in an aqueous solution of iodine / potassium iodide (weight ratio=0.5 / 8) with a concentration of 0.3%, and dyed while being stretched to 3.5 times. Thereafter, the film was stretched in an aqueous solution of boric acid ester at 65° C. to a total stretch ratio of 6 times. After stretching, the film was dried in an oven at 40° C. for 3 minutes to obtain a long strip-shaped polyvinyl alcohol-based polarizer (thickness 18 μm) X. When the easy-adhesion treatment was performed on the polarizer X, the easy-adhesion composition of Example 16 described in Table 3 of Patent Document 3 was used.

[0064] <Protection films Y and Z> As the protective film Y to be attached to one side of the polarizer X, a cyclic polyolefin film (manufactured by Zeon Corporation) having a thickness of 52 μm was used, and the surface to be attached to the polarizer X was subjected to a dry treatment such as a corona treatment. As the protective film Z to be attached to the other surface of the polarizer X, a triacetyl cellulose film having a thickness of 60 μm (manufactured by FUJIFILM Corporation) was used.

[0065] [Example 1] A polarizing film was produced by bonding the polarizer X and the protective films Y and Z together using an active energy ray curable adhesive A and curing the adhesive A. The polarizer X was not subjected to an easy-adhesion treatment. A 90-degree peel test was then performed on the polarizing film produced using the initial adhesive A (the adhesive corresponding to the "start of continuous operation" in FIG. 3) to measure the peel strength between the polarizer X and the protective film Y and the peel strength between the polarizer X and the protective film Z. In addition, a 90-degree peel test was performed on the polarizing film produced using the adhesive A after 32 hours of continuous operation to measure the peel strength between the polarizer X and the protective film Y and the peel strength between the polarizer X and the protective film Z.

[0066] [Example 2] A polarizing film was produced and the peel strength was measured in the same manner as in Example 1, except that active energy ray-curable adhesive B was used.

[0067] [Example 3] A polarizing film was produced and the peel strength was measured in the same manner as in Example 1, except that active energy ray-curable adhesive C was used.

[0068] [Example 4] A polarizing film was produced in the same manner as in Example 1, except that the active energy ray-curable adhesive D was used and the polarizer X was subjected to an easy-adhesion treatment, and the peel strength was measured.

[0069] [Comparative Example 1] A polarized film was produced and the peel strength was measured in the same manner as in Example 1, except that the second tank 30 was not sealed to store the adhesive, and the adhesive that was not coated by the coater 6 was returned to the second tank 30 instead of the first tank 20 (i.e., the adhesive was circulated between the second tank 30, the first tank 20, and the coater 6).

[0070] [Comparative Example 2] A polarized film was produced and the peel strength was measured in the same manner as in Example 2, except that the second tank 30 was not sealed to store the adhesive, and the adhesive that was not applied by the coater 6 was returned to the second tank 30 instead of the first tank 20 (i.e., the adhesive was circulated between the second tank 30, the first tank 20, and the coater 6).

[0071] [Comparative Example 3] A polarized film was produced and the peel strength was measured in the same manner as in Example 3, except that the second tank 30 was not sealed to store the adhesive, and the adhesive that was not applied by the coater 6 was returned to the second tank 30 instead of the first tank 20 (i.e., the adhesive was circulated between the second tank 30, the first tank 20, and the coater 6).

[0072] [Comparative Example 4] A polarized film was produced and the peel strength was measured in the same manner as in Example 4, except that the second tank 30 was not sealed to store the adhesive, and the adhesive that was not applied by the coater 6 was returned to the second tank 30 instead of the first tank 20 (i.e., the adhesive was circulated between the second tank 30, the first tank 20, and the coater 6).

[0073] [Evaluation of measurement results] FIG. 4 shows the results of measuring the peel strength obtained in Examples 1 to 4 and Comparative Examples 1 to 4. The peel force (90-degree peel test) was measured by cutting the leading end (the part produced initially) and the trailing end (the part produced after about 32 hours of operation) of a long strip of polarizing film to prepare test pieces, and the test pieces were measured. The peel forces shown in the columns "Initial XY 90-degree peel test" and "Initial XZ 90-degree peel test" in Fig. 4 refer to the peel forces measured on the test pieces obtained by cutting the leading end of the polarizing film. The peel forces shown in the columns "XY 90-degree peel test after 32 hours of continuous operation" and "XZ 90-degree peel test after 32 hours of continuous operation" in Fig. 4 refer to the peel forces measured on the test pieces obtained by cutting the trailing end of the polarizing film.

[0074] Specifically, the above test piece was cut into a size of 200 mm in the direction parallel to the stretching direction of the polarizer and 15 mm in the direction perpendicular to the stretching direction, and the test piece was attached to a glass plate. When measuring the peel strength between the polarizer X and the protective film Y, a cutter knife was used to make a cut between the polarizer X and the protective film Y of the test piece, and a Tensilon was used to peel the polarizer X and the protective film Y in the 90° direction at a peeling speed of 500 mm / min, and the peel strength was measured. When measuring the peel strength between the polarizer X and the protective film Z, a cutter knife was used to make a cut between the polarizer X and the protective film Z of the test piece, and a Tensilon was used to peel the polarizer X and the protective film Z in the 90° direction at a peeling speed of 500 mm / min, and the peel strength was measured.

[0075] As shown in FIG. 4, according to Examples 1 to 4, not only the polarized film produced using the initial adhesive, but also the polarized film produced using the adhesive after 32 hours of continuous operation had a sufficiently large peel strength, and good adhesion was maintained between the polarizer and the protective film. In contrast, in Comparative Examples 1 to 4, the polarizing films prepared using the initial adhesive had good adhesion between the polarizer and the protective film, but the polarizing films prepared using the adhesive after 32 hours of continuous operation had a smaller peel force and reduced adhesion between the polarizer and the protective film. [Explanation of symbols]

[0076] ad...Active energy ray curing adhesive F1···Polarizer (first optical film) F2... Protective film (second optical film) F···Polarizing film (optical laminate) 6. Coating machine 20. Tank No. 1 22, 42... Pump 30. Second Tank 40...Control device 43 Level gauge 100 Adhesive coating device

Claims

1. an adhesive coating step of coating at least one of the first optical film and the second optical film with an active energy ray curable adhesive by an adhesive coating device; an optical laminate preparation step of bonding the first optical film and the second optical film together via the adhesive and irradiating the adhesive with active energy rays to cure the adhesive, thereby preparing an optical laminate; The adhesive applicator comprises: A coating machine that applies the adhesive; a first tank that stores the adhesive and supplies the adhesive to the coater; a second tank that seals and stores the adhesive and supplies the adhesive to the first tank, the second tank having a larger adhesive storage capacity than the first tank; In the adhesive coating process, the adhesive is coated while being circulated between the first tank and the coater, and when the amount of the adhesive stored in the first tank becomes equal to or less than a predetermined value, the adhesive is supplied from the second tank to the first tank. A method for producing an optical laminate.

2. In the adhesive application step, the viscosity of the adhesive at 25°C at the start of application is 1 mPa·s to 100 mPa·s; A method for producing the optical laminate according to claim 1 .

3. In the adhesive coating step, the coating thickness of the adhesive is 0.1 μm to 5 μm. A method for producing the optical laminate according to claim 1 or 2.

4. The adhesive contains a hydroxyl group. A method for producing the optical laminate according to claim 1 .

5. The adhesive has an SP value of 29.0 (MJ / m 3 ) 1/2 32.0 (MJ / m 3 ) 1/2 or less than 21.0 (MJ / m 3 ) 1/2 23.0 (MJ / m 3 ) 1/2 Contains a radical polymerizable compound which is A method for producing the optical laminate according to claim 1 .

6. The adhesive contains water. A method for producing the optical laminate according to claim 1 .

7. The adhesive contains at least one organometallic compound selected from the group consisting of metal alkoxides and metal chelates. A method for producing the optical laminate according to claim 1 .

8. The adhesive contains a cationic polymerizable compound. A method for producing the optical laminate according to claim 1 .

9. the first optical film is a polarizer, the second optical film is a protective film, The optical laminate is a polarizing film. A method for producing the optical laminate according to claim 1 .

10. An adhesive applicator that applies an active energy ray-curable adhesive to at least one of a first optical film and a second optical film, A coating machine that applies the adhesive; a first tank that stores the adhesive and supplies the adhesive to the coater while circulating the adhesive between the first tank and the coater; a second tank that seals and stores the adhesive and supplies the adhesive to the first tank and has a larger adhesive storage capacity than the first tank; a control device that supplies the adhesive from the second tank to the first tank when the adhesive is applied from the applicator and the amount of the adhesive stored in the first tank becomes equal to or less than a predetermined value; An adhesive application device comprising:

11. The adhesive applicator according to claim 10, an active energy ray irradiation device that irradiates the adhesive between the first optical film and the second optical film bonded together via the adhesive with active energy rays to cure the adhesive; An apparatus for manufacturing an optical laminate comprising:

Citation Information

Patent Citations

  • Liquid supply system for photo-curing adhesive

    CN204134843U

  • Active energy ray-curing adhesive agent composition, polarization plate, optical film and image display device

    JP2012144690A

  • Curable resin composition, polarizing film and production method of the same, optical film and image display device

    JP2017160313A

  • Adhesive optical film, method for producing the adhesive optical film, image display device, adhesive coating liquid and method for producing the adhesive coating liquid

    WO2010140450A1

  • Adhesive layer, adhesive member, method for producing same, and image display device

    WO2010140454A1