Composite material

The composite material, combining chlorosulfonated polyethylene and cuprous oxide/zinc borate porous boron nitride nanosheets, addresses the limitations of conventional flash spinning materials by enhancing shrinkage resistance, tear strength, and antibacterial properties, making it suitable for protective clothing and other applications.

JP7586922B2Active Publication Date: 2024-11-19JIANGSU QINGYUN NEW MATERIAL TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022556113
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-28
Filing Date
2021-11-30
Publication Date
2024-11-19
Estimated Expiration
2041-11-30

AI Technical Summary

Technical Problem

Conventional flash spinning materials exhibit poor shrinkage resistance, tear strength, and inadequate antifungal and antibacterial properties, limiting their application in protective clothing and other fields.

Method used

A composite material produced by flash evaporation technology, incorporating chlorosulfonated polyethylene and cuprous oxide/zinc borate porous boron nitride nanosheets, with specific shrinkage rates, heat shrinkage strengths, and tear strengths, enhanced by a controlled hot pressing process.

Benefits of technology

The composite material demonstrates improved shrinkage resistance, tear strength, and long-term antibacterial and antifungal properties, expanding its application in protective materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586922000002
    Figure 0007586922000002
  • Figure 0007586922000003
    Figure 0007586922000003
  • Figure 0007586922000004
    Figure 0007586922000004
Patent Text Reader

Abstract

The present invention relates to a composite material, the raw material of which includes polyethylene, the shrinkage ratio R being 0.2-0.7, and the standard heat shrinkage strength σ r 0.5~3.5N / mm 2 and the antifungal grade is less than grade 2. This application has good shrinkage and excellent antibacterial and antifungal effects, and is therefore widely used.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of flash spinning, a composite material produced using flash evaporation technology. [Background technology]

[0002] Since the outbreak of the COVID-19 epidemic in early 2020, the research and development of new high-quality emergency protective materials has become an urgent task. As a research project that focuses equally on urgency, importance, and universality, emergency protective textiles have attracted widespread attention from the textile and product industries throughout the country and even the world. The speed at which the new coronavirus mutates is astonishing, so much so that in just a year and a half, almost half of the Greek letters used in the naming of the new coronavirus have been used without knowledge, from alpha to lambda. However, at present, the research and development of protective clothing for new epidemic viruses in China and the world is not sufficient. The development of antibacterial and antiviral protective clothing, reusable protective clothing, and protective materials with high barrier properties, high comfort, and high strength has become the focus of research and development of many scientific research institutions and enterprises. Flash spinning technology was invented by scientists from DuPont in the United States in the 1960s and is a method for producing high-tech nonwoven fabrics. The nonwoven fabric produced by this method has the characteristics of paper, film and cloth at the same time, and has the characteristics of light weight, high strength, waterproof, breathable, tear resistance, puncture resistance, etc., and has a wide range of applications, which is suitable for personal protection, medical packaging, national defense, construction, printing and other fields. However, the technology is relatively complicated, and the raw materials are mainly imported from the United States. In particular, China needs to make a breakthrough in this field as soon as possible, especially in the face of a choked international environment. The project team launched a flash evaporation project in 2018 and is currently generating sales. During this time, it mainly uses polyethylene as raw material, dissolves it through a solvent, and then flash spins it. The flash material produced has a wider range of applications than traditional products. At the same time, traditional flash materials have technical problems such as poor shrinkage and reduced tear strength, as well as poor anti-mold and antibacterial effects. Through the improvement of spinning polymer raw materials and the selection of spinning solvent and spinning temperature, the performance of the flash material can be improved and its application range can be expanded. Summary of the Invention [Problem to be solved by the invention]

[0003] The present invention overcomes the deficiencies of the prior art and aims to provide a composite material produced by flash evaporation technology. [Means for solving the problem]

[0004] The object of the present invention is realized through the following technical solutions. A composite material, characterized in that the raw material of the composite material includes polyethylene; The shrinkage ratio R is 0.2 to 0.7. Standard heat shrink strength σ r 0.5~3.5N / mm 2 and Contraction ratio R=[(L0-L1) / L0], Standard heat shrink strength is σ r =[F r / S]*[Actual gram weight / 50g / m 2 ], The anti-mold grade is less than grade 2. In the formula, each of the symbols is L0 is the initial length of the test piece (unit: mm); S is the initial cross-sectional area of ​​the specimen (unit: mm 2 ), L1 is the length of the test piece after thermal shrinkage (unit: mm), F r is the thermal contraction force (unit: N), The shrinkage ratio R of the composite material is in the range of 0.2 to 0.3.

[0005] The shrinkage ratio R of the composite material is in the range of 0.3 to 0.4.

[0006] The shrinkage ratio R of the composite material is in the range of 0.4 to 0.5.

[0007] The shrinkage ratio R of the composite material is in the range of 0.5 to 0.6.

[0008] The shrinkage ratio R of the composite material is in the range of 0.6 to 0.7.

[0009] Standard heat shrink strength σ of composite materialsr is 0.5~1.5N / mm 2 It is.

[0010] Standard heat shrink strength σ of composite materials r is 1.5~2.5N / mm 2 It is.

[0011] Standard heat shrink strength σ of composite materials r is 2.5~3.5N / mm 2 It is.

[0012] It is a composite material with a standard tear strength P of 7 to 12 KN / m.

[0013] P=[F / d]*[actual gram weight / 50g / m 2 ], F is the average tear force (unit: N); d is the thickness of the test piece (unit: mm);

[0014] The standard tear strength P of the composite material is 7~8.5KN / m.

[0015] The standard tear strength P of the composite material is 8.5~10KN / m.

[0016] The standard tear strength P of the composite material is 10~12KN / m.

[0017] It is a composite material, and the anti-fungal grade of the composite material is Grade 0.

[0018] The composite material has a mold resistance grade of Grade 1.

[0019] A composite material, the raw material of which further includes composite chlorosulfonated polyethylene, and the mass fraction of the composite chlorosulfonated polyethylene in the mixture of the composite chlorosulfonated polyethylene and polyethylene is 6-8%.

[0020] The composite chlorosulfonated polyethylene is composed of cuprous oxide / zinc borate porous boron nitride nanosheets, a compatibilizer, and chlorosulfonated polyethylene particles, where the mass fraction of cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene is 11-13%.

[0021] A method for producing a composite material, the technical solutions of which are as follows:

[0022] First, the spinning raw material is dissolved in a spinning solvent to obtain a spinning solution, then the spinning solution is flash spun at 180-240°C to lay flash fibers, and finally a hot pressing process is performed by a hot roller to obtain a composite material produced by a flash evaporation method. The hot pressing process by a hot roller specifically means hot pressing by an upper hot roller and a lower hot roller, and the absolute value ΔT of the difference between the surface temperature T above of the upper hot roller and the surface temperature T below of the lower hot roller is 5-10°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 100-140°.

[0023] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene.

[0024] The mass fraction of the spinning raw material in the spinning solution is 10 to 15%.

[0025] The spinning solvent is selected from some mixture of aromatic hydrocarbons, aliphatic hydrocarbons, cycloaliphatic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, esters, ethers, ketones, nitriles, amides, fluorocarbons.

[0026] The spinning solvent is a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3-dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane.

[0027] The preparation method of the composite chlorosulfonated polyethylene particles specifically includes the following steps:

[0028] First, the porous boron nitride nanosheet is dispersed in a sodium hydroxide solution by microwave stirring, and alkali treatment is performed. In addition, copper sulfate and zinc sulfate are added to the sodium hydroxide solution, respectively, and filtered to obtain a mixture, which is then pulverized. The first stage calcination is performed first, the first stage calcination temperature is 130-150°C, the first stage calcination time is 0.5-1 hour, and then heated to perform the second stage calcination, the second stage calcination temperature is 550-700°C, the second stage calcination time is 1-2 hours, and the primary product is produced. Next, the primary product is added to a boric acid solution, filtered and separated, and pulverized, and then the third stage calcination is performed. The third stage calcination temperature is 400-500°C, and the third stage calcination time is 2-4 hours, and the porous boron nitride nanosheet of cuprous oxide / zinc borate is obtained. Finally, the cuprous oxide / zinc borate porous boron nitride nanosheets, compatibilizer, and chlorosulfonated polyethylene particles are melt extruded and granulated to obtain composite chlorosulfonated polyethylene.

[0029] The mass fraction of the porous boron nitride nanosheet boron nitride in the sodium hydroxide solution is 5-20%, and the mass fraction of sodium hydroxide in the sodium hydroxide solution is 1-15%. The boron nitride has a porous layered structure and serves as an adsorption carrier. The purpose of the surface alkali treatment is to realize the subsequent adsorption of metal ions in the mixed solution of copper sulfate and zinc sulfate. The specific surface area of ​​the porous boron nitride nanosheet is 400-2500 m 2 / g, and the porous boron nitride nanosheets have mesopores of 0.3-15 nm and a total pore volume of 0.2-2.4 ml / g with micropores of 0.5-1.5 nm, where the mesopores account for 20-90% of the total pore volume. The purpose of the first calcination stage of this application is mainly to produce zinc oxide, and the purpose of the second calcination stage is mainly to produce cuprous oxide. This is the purpose of the staged calcination to produce various products.

[0030] The mass ratio of copper sulfate to zinc sulfate is 1:2 to 1:5.

[0031] The mass ratio of zinc sulfate to porous boron nitride nanosheets is 1:2 to 1:5.

[0032] The mass fraction of the primary product in the boric acid solution is 3-6%.

[0033] The mass fraction of boric acid in the boric acid solution is 10-20%.

[0034] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 11-13%.

[0035] The mass fraction of the compatibilizer in the composite chlorosulfonated polyethylene particles is 0.5-1%.

[0036] The antifungal and antibacterial functional material is a material that supports zinc borate doped with cuprous oxide on a boron nitride substrate, and uses zinc borate doped with cuprous oxide to penetrate the cell walls of microorganisms, thereby providing both antifungal and antibacterial effects. The porous boron nitride nanosheet has a large specific surface area and porous properties, so it has sustained release antifungal and antibacterial effects. This application has better antifungal and antibacterial effects than the mixture of pure raw materials (cuprous oxide and zinc borate). When the mass fraction of the porous boron nitride nanosheet of cuprous oxide / zinc borate in the composite chlorosulfonated polyethylene is low, its distribution tends to be uniform, and the possibility of mutual contact in the composite chlorosulfonated polyethylene is low, so it can obviously withstand a certain tear force, absorb more stress, and reduce the intermolecular movement of the polymer when force is applied to the final product, which delays the occurrence of cracks and has a great positive effect on improving the properties such as tear strength of the final product. When the mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheet in the composite chlorosulfonated polyethylene is high, it is easy to cause the phenomenon of local aggregation, which destroys the balanced distribution structure of the product, reduces its performance, and therefore fails to achieve the intended purpose. This is the reason why the mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheet in the composite chlorosulfonated polyethylene particles is selected to be in the range of 11-13%. As for the parameters of the hot pressing process, when ΔT exceeds 10°C, the temperature difference between the two sides is large, so the stress of the fiber structure is large, the shrinkage rate and shrinkage strength are large, and the tear strength is reduced. When the α angle is larger than 140°, the surface area covered by the hot roller is small, the heat curing time of the roller surface is short, and the stress release is insufficient, so the shrinkage rate and shrinkage strength are large, and the tear strength is small.

[0037] Chlorosulfonated polyethylene is a white or yellow elastomer, which can be dissolved in aromatic hydrocarbons and chlorinated hydrocarbons, but cannot be dissolved in fats and alcohols, can be swollen but not dissolved in ketones and ethers, has excellent ozone resistance, atmospheric aging resistance, chemical corrosion resistance, etc., has good physical and mechanical properties, aging resistance, heat resistance and low temperature resistance, and has excellent oil resistance, fire resistance and wear resistance. Because of its excellent elasticity, it can improve the shrinkage of the product, which is one of the important factors for the application to select this raw material, and at the same time, it is soluble in aromatic hydrocarbons and chlorinated hydrocarbons, which is similar to the polyethylene as the raw material for flash spinning in this application being soluble in spinning solvent.

[0038] The method for producing modified functional materials by flash spinning includes the following technical solutions:

[0039] First, the spinning raw material is dissolved in a spinning solvent to disperse and dissolve, and a spinning solution is obtained. The mass fraction of the spinning raw material in the spinning solution is 11.5% to 13.5%. Then, the spinning solution is flash spun at 185 to 250°C to lay flash fiber. Finally, a hot pressing process is performed with a hot roller to obtain a modified functional material by flash spinning.

[0040] The hot pressing process with hot rollers specifically refers to hot pressing with an upper hot roller and a lower hot roller, in which the absolute value ΔT of the difference between the surface temperature T of the upper hot roller and the surface temperature T of the lower hot roller is 5-10°C, and both T and T are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 100-140°.

[0041] The spinning raw materials are composite chlorosulfonated polyethylene and polypropylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polypropylene is 6-8%.

[0042] The spinning solvent is a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3-dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane. Effect of the Invention

[0043] Compared with the prior art, the positive effects of the present invention are as follows:

[0044] This application is widely applicable because the addition of chlorosulfonated polyethylene can improve the shrinkage of the product, and the addition of cuprous oxide / zinc borate porous boron nitride nanosheets can obviously improve the long-term antibacterial and antifungal effects of the product. [Brief description of the drawings]

[0045] [Figure 1] FIG. 1 is an SEM image of the product of Example 3. [Diagram 2] FIG. 13 is a comparative SEM image with the product of Comparative Example 7. [Diagram 3] FIG. 2 is a schematic diagram of the hot press of the hot roller of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0046] The following provides an embodiment for implementing the composite material of the present invention. 1. Shrinkage rate R and standard heat shrink strength σ r Testing: For the test of shrinkage rate and heat shrink strength, refer to the national standard GB / T34848-2017 (test method for heat shrinkable film performance), and the basic process of the test is as follows:

[0047] The initial dimension length of the test piece is L0 (unit is centimeter), the initial cross-sectional area of ​​the test piece is S (unit is square millimeter), and after the test piece is heated, it is cooled to a temperature of 40 ° C after reaching the maximum heat shrinkage force, the size of the test piece after heat shrinkage is L1 (unit is centimeter), and the maximum heat shrinkage force is Fr (unit is Newton), and the largest force generated during the cooling process is the cold contraction force, F c (The unit is Newton). For the test piece, 10 test pieces are taken and the average value is calculated, and then the return method is performed. The standard heat shrinkage strength is calculated by the formula: σ r =[F r / S]*[Actual gram weight / 50g / m 2 ] and obtain the standard heat shrinkage strength of the test specimen.

[0048] 2. Standard tear strength P test: For the test of tear strength, refer to the standard GB / T16578.1-2008 / ISO6363-1:1983 (Part 1 of the measurement of plastic films and sheets with high tear resistance: Trouser method tear test), and the basic steps of the test are as follows:

[0049] At a test speed of 200 mm / min, the average force required to make the crack penetrate the test specimen is expressed as F. For the test specimen, 10 test specimens are taken and the average value is calculated. Then, the return method is carried out and the standard tear strength P is calculated by the formula: P = [F / d] * [actual gram weight / 50 g / m 2 ], F is the average tear force (in Newtons), and d is the gram weight of the specimen / 50g / m 2 ], thickness (in millimeters).

[0050] 3. Whiteness W test: For the test of whiteness, refer to the national standard GB / T22880-2008 (measurement of CIE whiteness of paper and paperboard, D65 / 10° outdoor sunlight), and under the conditions specified in the standard, the whiteness is obtained by measuring the CIE tristimulus values.

[0051] 4. Antifungal grade AMA test: For the test of antifungal grade, refer to the standard GB / T24346-2009 (evaluation of antifungal properties of textiles), and the specific test conditions are as follows:

[0052] The strains used in the antifungal tests were Aspergillus niger CGMCC3.5487, Chaetomyces cerevisiae CGMCC3.3601, Penicillium funiculosum CGMCC3.3875, and Trichoderma viride CGMCC3.2941.

[0053] Anti-mold constant temperature and humidity environment parameters: 28℃±1℃, 90%±2%; incubation time 28 days.

[0054] 5. Antibacterial rate A test: For the test of antibacterial rate, refer to the standard GB / T20944.2-2007 (Part 2 of the evaluation of textile antibacterial properties: Absorption method), and the specific test conditions are as follows:

[0055] The bacterial species used in the antibacterial tests are Staphylococcus aureus, Klebsiella pneumoniae and Escherichia coli.

[0056] Culture conditions: 37℃±2℃, 90%±2%; culture time 18-24 hours.

[0057] The antibacterial rate (i.e., antibacterial rate) means that 95% or more has antibacterial properties, and over 99% means that it has excellent antibacterial properties.

[0058] <Example 1> A method for producing a composite material, the technical solutions of which are as follows:

[0059] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, then the spinning solution is flash spun at 200°C to lay the flash fiber, and finally, a hot pressing process is performed by hot rollers to obtain a composite material. The hot pressing process by hot rollers specifically refers to the hot pressing process performed by the upper hot roller 1 and the lower hot roller 2, and the absolute value ΔT of the difference between the surface temperature T above the upper hot roller and the surface temperature T below the lower hot roller is 6°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 120°, where the α angle is specifically shown in FIG. 3.

[0060] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 6%.

[0061] The mass fraction of the spinning raw material in the spinning solution is 12%.

[0062] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3-dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0063] The preparation method of the composite chlorosulfonated polyethylene particles specifically includes the following steps:

[0064] First, the porous boron nitride nanosheet is dispersed in a sodium hydroxide solution by microwave stirring, and alkali treatment is performed. In addition, copper sulfate and zinc sulfate are added to the sodium hydroxide solution, respectively, and filtered to obtain a mixture, which is then pulverized. The first stage of calcination is performed first, the first stage of calcination temperature is 130-150°C, the first stage of calcination time is 0.5-1 hour, and then heated to perform the second stage of calcination, the second stage of calcination temperature is 550-700°C, the second stage of calcination time is 1-2 hours, and the primary product is produced. Next, the primary product is added to a boric acid solution, filtered and separated, and pulverized, and then the third stage of calcination is performed. The third stage of calcination temperature is 400-500°C, and the third stage of calcination time is 2-4 hours, and the porous boron nitride nanosheet of cuprous oxide / zinc borate is obtained. Finally, the cuprous oxide / zinc borate porous boron nitride nanosheets, compatibilizer, and chlorosulfonated polyethylene particles are melt extruded and granulated to obtain composite chlorosulfonated polyethylene.

[0065] The mass fraction of boron nitride of the porous boron nitride nanosheets in the sodium hydroxide solution is 6%, and the mass fraction of sodium hydroxide in the sodium hydroxide solution is 5%.

[0066] The mass ratio of copper sulfate to zinc sulfate is 1:2.

[0067] The mass ratio of zinc sulfate to porous boron nitride nanosheets is 1:2.

[0068] The mass fraction of the primary product in the boric acid solution is 3%.

[0069] The mass fraction of boric acid in the boric acid solution is 12%.

[0070] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 11%.

[0071] The mass fraction of the compatibilizer in the composite chlorosulfonated polyethylene particles is 0.5%.

[0072] Performance data from product testing of this Example 1 is shown in Table 1.

[0073] <Example 2> A method for producing a composite material, the technical solutions of which are as follows:

[0074] First, the spinning raw material is dissolved in a spinning solvent to disperse and dissolve to obtain a spinning solution, then the spinning solution is flash spun at 205°C to lay flash fiber, and finally a hot pressing process is performed by hot rollers to obtain a composite material. The hot pressing process by hot rollers specifically refers to hot pressing by upper hot rollers and lower hot rollers, and the absolute value ΔT of the difference between the surface temperature T above of the upper hot roller and the surface temperature T below of the lower hot roller is 7°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 122°.

[0075] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 6.5%.

[0076] The mass fraction of the spinning raw material in the spinning solution is 12.5%.

[0077] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3-dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0078] The preparation method of the composite chlorosulfonated polyethylene particles specifically includes the following steps:

[0079] First, the porous boron nitride nanosheet is dispersed in a sodium hydroxide solution by microwave stirring, and alkali treatment is performed. In addition, copper sulfate and zinc sulfate are added to the sodium hydroxide solution, respectively, and filtered to obtain a mixture, which is then pulverized. The first stage calcination is performed first, the first stage calcination temperature is 130-150°C, the first stage calcination time is 0.5-1 hour, and then heated to perform the second stage calcination, the second stage calcination temperature is 550-700°C, the second stage calcination time is 1-2 hours, and the primary product is produced. Next, the primary product is added to a boric acid solution, filtered and separated, and pulverized, and then the third stage calcination is performed. The third stage calcination temperature is 400-500°C, and the third stage calcination time is 2-4 hours, and the porous boron nitride nanosheet of cuprous oxide / zinc borate is obtained. Finally, the cuprous oxide / zinc borate porous boron nitride nanosheets, compatibilizer, and chlorosulfonated polyethylene particles are melt extruded and granulated to obtain composite chlorosulfonated polyethylene.

[0080] The mass fraction of boron nitride of the porous boron nitride nanosheets in the sodium hydroxide solution is 8%, and the mass fraction of sodium hydroxide in the sodium hydroxide solution is 5%.

[0081] The mass ratio of copper sulfate to zinc sulfate is 1:2.5.

[0082] The mass ratio of zinc sulfate to porous boron nitride nanosheets is 1:2.5.

[0083] The mass fraction of the primary product in the boric acid solution is 3.5%.

[0084] The mass fraction of boric acid in the boric acid solution is 12%.

[0085] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 11.5%.

[0086] The mass fraction of the compatibilizer in the composite chlorosulfonated polyethylene particles is 0.6%.

[0087] Performance data for product testing of this Example 2 is shown in Table 1.

[0088] <Example 3> A method for producing a composite material, the technical solutions of which are as follows:

[0089] First, the spinning raw material is dissolved in a spinning solvent to obtain a spinning solution, then the spinning solution is flash spun at 210°C to lay flash fiber, and finally a hot pressing process is performed by hot rollers to obtain a composite material. The hot pressing process by hot rollers specifically refers to hot pressing by upper hot rollers and lower hot rollers, and the absolute value ΔT of the difference between the surface temperature T above of the upper hot roller and the surface temperature T below of the lower hot roller is 8°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 124°.

[0090] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0091] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0092] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3-dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0093] The preparation method of the composite chlorosulfonated polyethylene particles specifically includes the following steps:

[0094] First, the porous boron nitride nanosheet is dispersed in a sodium hydroxide solution by microwave stirring, and alkali treatment is performed. In addition, copper sulfate and zinc sulfate are added to the sodium hydroxide solution, respectively, and filtered to obtain a mixture, which is then pulverized. The first stage of calcination is performed first, the first stage of calcination temperature is 130-150°C, the first stage of calcination time is 0.5-1 hour, and then heated to perform the second stage of calcination, the second stage of calcination temperature is 550-700°C, the second stage of calcination time is 1-2 hours, and the primary product is produced. Next, the primary product is added to a boric acid solution, filtered and separated, and pulverized, and then the third stage of calcination is performed. The third stage of calcination temperature is 400-500°C, and the third stage of calcination time is 2-4 hours, and the porous boron nitride nanosheet of cuprous oxide / zinc borate is obtained. Finally, the cuprous oxide / zinc borate porous boron nitride nanosheets, compatibilizer, and chlorosulfonated polyethylene particles are melt extruded and granulated to obtain composite chlorosulfonated polyethylene.

[0095] The mass fraction of boron nitride of the porous boron nitride nanosheets in the sodium hydroxide solution is 10%, and the mass fraction of sodium hydroxide in the sodium hydroxide solution is 5%.

[0096] The mass ratio of copper sulfate to zinc sulfate is 1:3.5.

[0097] The mass ratio of zinc sulfate to porous boron nitride nanosheets is 1:3.5.

[0098] The mass fraction of the primary product in the boric acid solution is 5%.

[0099] The mass fraction of boric acid in the boric acid solution is 12%.

[0100] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 12%.

[0101] The mass fraction of the compatibilizer in the composite chlorosulfonated polyethylene particles is 0.7%.

[0102] Performance data for product testing of this Example 3 is shown in Table 1.

[0103] The product of Example 3 is left in a normal temperature environment for one year, specifically, the temperature is 25±2°C and the humidity is (60±5)%RH. The antifungal grade of the test piece is tested again and determined to be grade 1, with an antibacterial rate of 98.2%, and the antibacterial and antifungal properties do not decrease significantly, providing long-term antibacterial and antifungal effects.

[0104] <Example 4> A method for producing a composite material, the technical solutions of which are as follows:

[0105] First, the spinning raw material is dissolved in a spinning solvent to disperse and dissolve to obtain a spinning solution, then the spinning solution is flash spun at 215°C to lay flash fiber, and finally a hot pressing process is performed by hot rollers to obtain a composite material. The hot pressing process by hot rollers specifically refers to hot pressing by upper hot rollers and lower hot rollers, and the absolute value ΔT of the difference between the surface temperature T above of the upper hot roller and the surface temperature T below of the lower hot roller is 8°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 126°.

[0106] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7.5%.

[0107] The mass fraction of the spinning raw material in the spinning solution is 13.5%.

[0108] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3-dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0109] The preparation method of the composite chlorosulfonated polyethylene particles specifically includes the following steps:

[0110] First, the porous boron nitride nanosheet is dispersed in a sodium hydroxide solution by microwave stirring, and alkali treatment is performed. In addition, copper sulfate and zinc sulfate are added to the sodium hydroxide solution, respectively, and filtered to obtain a mixture, which is then pulverized. The first stage of calcination is performed first, the first stage of calcination temperature is 130-150°C, the first stage of calcination time is 0.5-1 hour, and then heated to perform the second stage of calcination, the second stage of calcination temperature is 550-700°C, the second stage of calcination time is 1-2 hours, and the primary product is produced. Next, the primary product is added to a boric acid solution, filtered and separated, and pulverized, and then the third stage of calcination is performed. The third stage of calcination temperature is 400-500°C, and the third stage of calcination time is 2-4 hours, and the porous boron nitride nanosheet of cuprous oxide / zinc borate is obtained. Finally, the cuprous oxide / zinc borate porous boron nitride nanosheets, compatibilizer, and chlorosulfonated polyethylene particles are melt extruded and granulated to obtain composite chlorosulfonated polyethylene.

[0111] The mass fraction of boron nitride of the porous boron nitride nanosheets in the sodium hydroxide solution is 12%, and the mass fraction of sodium hydroxide in the sodium hydroxide solution is 5%.

[0112] The mass ratio of copper sulfate to zinc sulfate is 1:4.

[0113] The mass ratio of zinc sulfate to porous boron nitride nanosheets is 1:4.

[0114] The mass fraction of the primary product in the boric acid solution is 5%.

[0115] The mass fraction of boric acid in the boric acid solution is 12%.

[0116] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 12.5%.

[0117] The mass fraction of the compatibilizer in the composite chlorosulfonated polyethylene particles is 0.8%.

[0118] Performance data for product testing of this Example 4 is shown in Table 1.

[0119] <Example 5> A method for producing a composite material, the technical solutions of which are as follows:

[0120] First, the spinning raw material is dissolved in a spinning solvent to disperse and dissolve to obtain a spinning solution, then the spinning solution is flash spun at 220°C to lay flash fiber, and finally a hot pressing process is performed by hot rollers to obtain a composite material. The hot pressing process by hot rollers specifically refers to hot pressing by upper hot rollers and lower hot rollers, and the absolute value ΔT of the difference between the surface temperature T above of the upper hot roller and the surface temperature T below of the lower hot roller is 8°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 128°.

[0121] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 8%.

[0122] The mass fraction of the spinning raw material in the spinning solution is 14%.

[0123] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3-dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0124] The preparation method of the composite chlorosulfonated polyethylene particles specifically includes the following steps:

[0125] First, the porous boron nitride nanosheet is dispersed in a sodium hydroxide solution by microwave stirring, and alkali treatment is performed. In addition, copper sulfate and zinc sulfate are added to the sodium hydroxide solution, respectively, and filtered to obtain a mixture, which is then pulverized. The first stage calcination is performed first, the first stage calcination temperature is 130-150°C, the first stage calcination time is 0.5-1 hour, and then heated to perform the second stage calcination, the second stage calcination temperature is 550-700°C, the second stage calcination time is 1-2 hours, and the primary product is produced. Next, the primary product is added to a boric acid solution, filtered and separated, and pulverized, and then the third stage calcination is performed. The third stage calcination temperature is 400-500°C, and the third stage calcination time is 2-4 hours, and the porous boron nitride nanosheet of cuprous oxide / zinc borate is obtained. Finally, the cuprous oxide / zinc borate porous boron nitride nanosheets, compatibilizer, and chlorosulfonated polyethylene particles are melt extruded and granulated to obtain composite chlorosulfonated polyethylene.

[0126] The mass fraction of boron nitride of the porous boron nitride nanosheets in the sodium hydroxide solution is 5 to 20%, and the mass fraction of sodium hydroxide in the sodium hydroxide solution is 5%.

[0127] The mass ratio of copper sulfate to zinc sulfate is 1:5.

[0128] The mass ratio of zinc sulfate to porous boron nitride nanosheets is 1:5.

[0129] The mass fraction of the primary product in the boric acid solution is 6%.

[0130] The mass fraction of boric acid in the boric acid solution is 12%.

[0131] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 13%.

[0132] The mass fraction of the compatibilizer in the composite chlorosulfonated polyethylene particles is 0.8%.

[0133] Performance data for product testing of this Example 5 is shown in Table 1.

[0134] <Comparative Example 1> A method for producing a composite material, the technical solutions of which are as follows:

[0135] First, the spinning raw material is dissolved in a spinning solvent to obtain a spinning solution, then the spinning solution is flash spun at 210°C to lay flash fiber, and finally a hot pressing process is performed by hot rollers to obtain a composite material. The hot pressing process by hot rollers specifically refers to hot pressing by upper hot rollers and lower hot rollers, and the absolute value ΔT of the difference between the surface temperature T above of the upper hot roller and the surface temperature T below of the lower hot roller is 8°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 124°.

[0136] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0137] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0138] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0139] The composite chlorosulfonated polyethylene particles are composed of cuprous oxide, zinc borate, a compatibilizer, and chlorosulfonated polyethylene particles, where the mass fraction of the mixture of cuprous oxide, zinc borate, and porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 12%.

[0140] The mass fraction of the compatibilizer in the composite chlorosulfonated polyethylene particles is 0.7%.

[0141] The mass ratio of cuprous oxide to zinc borate is 1:3.5.

[0142] The mass ratio of zinc borate to porous boron nitride nanosheets is 1:3.5.

[0143] Product test performance data for this Comparative Example 1 is shown in Table 1.

[0144] The product of Comparative Example 1 was left in a normal temperature environment for one year, specifically, the temperature was 25±2°C and the humidity was (60±5)% RH. The antifungal grade of the test piece was tested again and determined to be grade 4, with an antibacterial rate of 78.2%, indicating a clear decrease in antibacterial and antifungal properties and no antibacterial and antifungal effect.

[0145] <Comparative Example 2> A method for producing a composite material, the technical solutions of which are as follows:

[0146] First, the spinning raw material is dissolved in a spinning solvent to obtain a spinning solution, then the spinning solution is flash spun at 210°C to lay flash fiber, and finally a hot pressing process is performed by hot rollers to obtain a composite material. The hot pressing process by hot rollers specifically refers to hot pressing by upper hot rollers and lower hot rollers, and the absolute value ΔT of the difference between the surface temperature T above of the upper hot roller and the surface temperature T below of the lower hot roller is 8°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 124°.

[0147] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0148] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0149] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0150] The preparation method of the composite chlorosulfonated polyethylene particles specifically includes the following steps:

[0151] First, the porous boron nitride nanosheet is dispersed in a sodium hydroxide solution by microwave stirring, and alkali treatment is performed. In addition, zinc sulfate is added to the sodium hydroxide solution, and the mixture is filtered and separated to obtain a mixture, which is then pulverized. The first stage of calcination is performed first, the first stage of calcination temperature is 130-150°C, and the first stage of calcination time is 0.5-1 hour, and then the mixture is heated to perform the second stage of calcination, the second stage of calcination temperature is 550-700°C, and the second stage of calcination time is 1-2 hours, to produce a primary product. Next, the primary product is added to a boric acid solution, and after filtering and separating, it is pulverized, and then the third stage of calcination is performed. The third stage of calcination temperature is 400-500°C, and the third stage of calcination time is 2-4 hours, to obtain a porous boron nitride nanosheet of cuprous oxide / zinc borate. Finally, the cuprous oxide / zinc borate porous boron nitride nanosheets, compatibilizer, and chlorosulfonated polyethylene particles are melt extruded and granulated to obtain composite chlorosulfonated polyethylene.

[0152] The mass fraction of boron nitride of the porous boron nitride nanosheets in the sodium hydroxide solution is 10%, and the mass fraction of sodium hydroxide in the sodium hydroxide solution is 5%.

[0153] The mass ratio of zinc sulfate to porous boron nitride nanosheets is 1:3.5.

[0154] The mass fraction of the primary product in the boric acid solution is 5%.

[0155] The mass fraction of boric acid in the boric acid solution is 12%.

[0156] The mass fraction of zinc borate / porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 12%.

[0157] The mass fraction of the compatibilizer in the composite chlorosulfonated polyethylene particles is 0.7%.

[0158] The performance data for the product test of this Comparative Example 2 is shown in Table 1.

[0159] <Comparative Example 3> A method for producing a composite material, the technical solutions of which are as follows:

[0160] First, the spinning raw material is dissolved in a spinning solvent to obtain a spinning solution, then the spinning solution is flash spun at 210°C to lay flash fiber, and finally a hot pressing process is performed by hot rollers to obtain a composite material. The hot pressing process by hot rollers specifically refers to hot pressing by upper hot rollers and lower hot rollers, and the absolute value ΔT of the difference between the surface temperature T above of the upper hot roller and the surface temperature T below of the lower hot roller is 8°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 124°.

[0161] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0162] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0163] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0164] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3, with the only difference being as follows:

[0165] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 8%.

[0166] Product test performance data for this Comparative Example 3 is shown in Table 1.

[0167] <Comparative Example 4> A method for producing a composite material, the technical solutions of which are as follows:

[0168] First, the spinning raw material is dissolved in a spinning solvent to obtain a spinning solution, then the spinning solution is flash spun at 210°C to lay flash fiber, and finally a hot pressing process is performed by hot rollers to obtain a composite material. The hot pressing process by hot rollers specifically refers to hot pressing by upper hot rollers and lower hot rollers, and the absolute value ΔT of the difference between the surface temperature T above of the upper hot roller and the surface temperature T below of the lower hot roller is 8°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 124°.

[0169] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0170] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0171] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0172] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3, with the only difference being as follows:

[0173] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 9%.

[0174] The performance data for the product test of this Comparative Example 4 is shown in Table 1.

[0175] <Comparative Example 5> A method for producing a composite material, the technical solutions of which are as follows:

[0176] First, the spinning raw material is dissolved in a spinning solvent to obtain a spinning solution, then the spinning solution is flash spun at 210°C to lay flash fiber, and finally a hot pressing process is performed by hot rollers to obtain a composite material. The hot pressing process by hot rollers specifically refers to hot pressing by upper hot rollers and lower hot rollers, and the absolute value ΔT of the difference between the surface temperature T above of the upper hot roller and the surface temperature T below of the lower hot roller is 8°C, and both T above and T below are less than 135°C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 124°.

[0177] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0178] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0179] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0180] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3, with the only difference being as follows:

[0181] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 10.5%.

[0182] Product test performance data for this Comparative Example 5 is shown in Table 1.

[0183] <Comparative Example 6> A method for producing a composite material, the technical solutions of which are as follows:

[0184] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 210°C to lay the flash fiber. Finally, a hot pressing process is performed with hot rollers to obtain a composite material. The hot pressing process with hot rollers specifically refers to hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 8°C, and T 上 and T 下 are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, which is 124°.

[0185] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0186] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0187] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0188] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3, with the only difference being as follows:

[0189] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 13.5%.

[0190] Product test performance data for this Comparative Example 6 is shown in Table 1.

[0191] <Comparative Example 7> A method for producing a composite material, the technical solutions of which are as follows:

[0192] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 210°C to lay the flash fiber. Finally, a hot pressing process is performed with hot rollers to obtain a composite material. The hot pressing process with hot rollers specifically refers to hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 8°C, and T 上 and T 下 are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, which is 124°.

[0193] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0194] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0195] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0196] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3, with the only difference being as follows:

[0197] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 14.5%.

[0198] SEM images of the control product, SEM of Example 3 is in Figure 1. SEM of Comparative Example 7 is in Figure 2. When the content of the porous boron nitride nanosheets of cuprous oxide / zinc borate is high, the content of the final product is relatively high, which does not serve the intended purpose, as can be seen from Figure 3 of the SEM test. From Figure 1 of the SEM of Example 3, it can be seen that the distribution is uniform and no aggregation phenomenon occurs.

[0199] Product test performance data for this Comparative Example 7 is shown in Table 1.

[0200] <Comparative Example 8> A method for producing a composite material, the technical solutions of which are as follows:

[0201] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 210°C to lay the flash fiber. Finally, a hot pressing process is performed with hot rollers to obtain a composite material. The hot pressing process with hot rollers specifically refers to hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 8°C, and T 上 and T 下are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, which is 124°.

[0202] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0203] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0204] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0205] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3, with the only difference being as follows:

[0206] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 16%.

[0207] Product test performance data for this Comparative Example 8 is shown in Table 1.

[0208] <Comparative Example 9> A method for producing a composite material, the technical solutions of which are as follows:

[0209] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 210°C to lay the flash fiber. Finally, a hot pressing process is performed with hot rollers to obtain a composite material. The hot pressing process with hot rollers specifically refers to hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 8°C, and T 上 and T 下 are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, which is 124°.

[0210] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0211] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0212] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0213] The preparation method of the composite chlorosulfonated polyethylene particles specifically includes the following steps:

[0214] First, the porous boron nitride nanosheet is dispersed in a sodium hydroxide solution by microwave stirring, and alkali treatment is performed. In addition, copper sulfate and zinc sulfate are added to the sodium hydroxide solution, respectively, and filtered to obtain a mixture, which is then pulverized. The first stage of calcination is performed first, the first stage of calcination temperature is 130-150°C, the first stage of calcination time is 0.5-1 hour, and then the second stage of calcination is performed by heating. The second stage of calcination temperature is 550-700°C, and the second stage of calcination time is 1-2 hours, and the primary product is produced. Next, the primary product is added to a boric acid solution, filtered and separated, and pulverized, and then the third stage of calcination is performed. The third calcination temperature is 400-500°C, and the third calcination time is 2-4 hours, and the porous boron nitride nanosheet of cuprous oxide / zinc borate is obtained. Finally, the cuprous oxide / zinc borate porous boron nitride nanosheets, compatibilizer, and chlorosulfonated polyethylene particles are melt extruded and granulated to obtain composite chlorosulfonated polyethylene.

[0215] The mass fraction of boron nitride of the porous boron nitride nanosheets in the sodium hydroxide solution is 10%, and the mass fraction of sodium hydroxide in the sodium hydroxide solution is 5%.

[0216] The mass ratio of copper sulfate to zinc sulfate is 1:0.5.

[0217] The mass ratio of zinc sulfate to porous boron nitride nanosheets is 1:3.5.

[0218] The mass fraction of the primary product in the boric acid solution is 5%.

[0219] The mass fraction of boric acid in the boric acid solution is 12%.

[0220] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 12%.

[0221] The mass fraction of the compatibilizer in the composite chlorosulfonated polyethylene particles is 0.7%.

[0222] Product test performance data for this Comparative Example 9 is shown in Table 1.

[0223] <Comparative Example 10> A method for producing a composite material, the technical solutions of which are as follows:

[0224] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 210°C to lay the flash fiber. Finally, a hot pressing process is performed with hot rollers to obtain a composite material. The hot pressing process with hot rollers specifically refers to hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 8°C, and T 上 and T 下 are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, which is 124°.

[0225] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0226] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0227] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0228] The preparation method of the composite chlorosulfonated polyethylene particles specifically includes the following steps:

[0229] First, the porous boron nitride nanosheet is dispersed in a sodium hydroxide solution by microwave stirring, and alkali treatment is performed. In addition, copper sulfate and zinc sulfate are added to the sodium hydroxide solution, respectively, and filtered to obtain a mixture, which is then pulverized. The first stage of calcination is performed first, the first stage of calcination temperature is 130-150°C, the first stage of calcination time is 0.5-1 hour, and then the second stage of calcination is performed by heating. The second stage of calcination temperature is 550-700°C, and the second stage of calcination time is 1-2 hours, and the primary product is produced. Next, the primary product is added to a boric acid solution, filtered and separated, and pulverized, and then the third stage of calcination is performed. The third calcination temperature is 400-500°C, and the third calcination time is 2-4 hours, and the porous boron nitride nanosheet of cuprous oxide / zinc borate is obtained. Finally, the cuprous oxide / zinc borate porous boron nitride nanosheets, compatibilizer, and chlorosulfonated polyethylene particles are melt extruded and granulated to obtain composite chlorosulfonated polyethylene.

[0230] The mass fraction of boron nitride of the porous boron nitride nanosheets in the sodium hydroxide solution is 10%, and the mass fraction of sodium hydroxide in the sodium hydroxide solution is 5%.

[0231] The mass ratio of copper sulfate to zinc sulfate is 1:1.

[0232] The mass ratio of zinc sulfate to porous boron nitride nanosheets is 1:3.5.

[0233] The mass fraction of the primary product in the boric acid solution is 5%.

[0234] The mass fraction of boric acid in the boric acid solution is 12%.

[0235] The mass fraction of the cuprous oxide / zinc borate porous boron nitride nanosheets in the composite chlorosulfonated polyethylene particles is 12%.

[0236] The mass fraction of the compatibilizer in the composite chlorosulfonated polyethylene particles is 0.7%.

[0237] Product test performance data for this Comparative Example 10 is shown in Table 1.

[0238] <Comparative Example 11> A method for producing a composite material, the technical solutions of which are as follows:

[0239] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 210°C to lay the flash fiber. Finally, a hot pressing process is performed with hot rollers to obtain a composite material. The hot pressing process with hot rollers specifically refers to hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 13°C, and T 上 and T 下 are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, which is 124°.

[0240] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0241] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0242] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0243] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3.

[0244] Product test performance data for this Comparative Example 11 is shown in Table 1.

[0245] <Comparative Example 12> A method for producing a composite material, the technical solutions of which are as follows:

[0246] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 210°C to lay the flash fiber. Finally, a hot pressing process is performed with hot rollers to obtain a composite material. The hot pressing process with hot rollers specifically refers to hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 2°C, and T 上 and T 下 are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, which is 124°.

[0247] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0248] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0249] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0250] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3.

[0251] Product testing performance data for this Comparative Example 12 is shown in Table 1.

[0252] <Comparative Example 13> A method for producing a composite material, the technical solutions of which are as follows:

[0253] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 210°C to lay the flash fiber. Finally, a hot pressing process is performed with hot rollers to obtain a composite material. The hot pressing process with hot rollers specifically refers to hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 8°C, and T 上 and T 下 are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, which is 150°.

[0254] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0255] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0256] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0257] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3.

[0258] Product test performance data for this Comparative Example 13 is shown in Table 1.

[0259] <Comparative Example 14> A method for producing a composite material, the technical solutions of which are as follows:

[0260] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 210°C to lay the flash fiber. Finally, a hot pressing process is performed with hot rollers to obtain a composite material. The hot pressing process with hot rollers specifically refers to hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 8°C, and T 上 and T 下 are both less than 135° C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 90°.

[0261] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0262] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0263] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0264] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3.

[0265] Product testing performance data for this Comparative Example 14 is shown in Table 1.

[0266] <Example 6> The method for producing modified functional materials by flash spinning includes the following technical solutions:

[0267] First, the spinning raw material is dissolved in a spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 200°C to lay flash fibers. Finally, a hot pressing process is carried out by hot rollers to obtain a modified functional material by flash spinning. The hot pressing process by hot rollers is specifically carried out by hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 6°C, and T 上 and T 下 are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, and the α angle is 120°.

[0268] The spinning raw materials are composite chlorosulfonated polyethylene and polypropylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polypropylene is 6%.

[0269] The mass fraction of the spinning raw material in the spinning solution is 12%.

[0270] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0271] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 1.

[0272] Performance data for product testing of this Example 11 is shown in Table 1.

[0273] <Example 7> The method for producing modified functional materials by flash spinning includes the following technical solutions:

[0274] First, the spinning raw material is dissolved in the spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 210°C to lay down the flash fiber. Finally, the hot pressing process is carried out by the hot rollers to obtain the modified functional material by flash spinning. The hot pressing process by the hot rollers is specifically carried out by the hot pressing with the upper hot rollers and the lower hot rollers, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 7°C, and T 上 and T 下 are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, which is 122°.

[0275] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 7%.

[0276] The mass fraction of the spinning raw material in the spinning solution is 13%.

[0277] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0278] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 3.

[0279] Performance data for product testing of this Example 7 is shown in Table 1.

[0280] <Example 8> The method for producing modified functional materials by flash spinning includes the following technical solutions:

[0281] First, the spinning raw material is dissolved in a spinning solvent to obtain a spinning solution, and then the spinning solution is flash spun at 220°C to lay flash fibers. Finally, a hot pressing process is carried out by hot rollers to obtain a modified functional material by flash spinning. The hot pressing process by hot rollers is specifically carried out by hot pressing with an upper hot roller and a lower hot roller, and the surface temperature T 上 and the surface temperature of the lower hot roller T 下 The absolute value of the difference ΔT is 8°C, and T 上 and T 下 are all less than 135° C. The tangents on both sides of the upper hot roller form an α angle, which is 124°.

[0282] The spinning raw materials are composite chlorosulfonated polyethylene and polyethylene, and the mass fraction of composite chlorosulfonated polyethylene in the mixture of composite chlorosulfonated polyethylene and polyethylene is 8%.

[0283] The mass fraction of the spinning raw material in the spinning solution is 14%.

[0284] The spinning solvent was a mixture of 1-pentene, trichlorofluoromethane, dichloromethane, cyclopentane, 2,3 dihydrodecafluoropentane, and 1,1,1,3,3-pentafluorobutane in a weight ratio of 6:5:4:3:1:1.

[0285] The preparation method of the composite chlorosulfonated polyethylene particles is the same as that in Example 5.

[0286] Performance data for product testing of this Example 8 is shown in Table 1.

[0287] JPEG0007586922000001.jpg153170

[0288] It should be noted that the above is only a preferred embodiment of the present invention, and those skilled in the art may make some improvements and modifications without departing from the gist of the present invention, and these improvements and modifications should also be considered to be within the protection scope of the present invention. [Explanation of symbols]

[0289] 1 Upper hot roller 2 Lower Hot Rollers

Claims

1. A composite material obtained by flash spinning using polyethylene and a composite chlorosulfonated polyethylene composed of a porous boron nitride nanosheet carrying cuprous oxide / zinc borate, a compatibilizer, and chlorosulfonated polyethylene particles, the raw material of the composite material containing polyethylene, the shrinkage ratio R being 0.2 to 0.7, and the standard heat shrinkage strength σ r is 0.5 to 3.5 N / mm 2 and the antifungal grade is less than grade 2, where the shrinkage rate R=[(L 0 -L 1 ) / L 0 ] and the standard heat shrinkage strength σ r = [F r / S] * [actual weight / 50g / m 2 ], and each of the symbols in the formula is L 0 is the initial length of the specimen, S is the initial cross-sectional area of ​​the specimen, and L 1 is the length of the test piece after thermal shrinkage, F r is a thermal shrinkage force.

2. 2. The composite material according to claim 1, characterized in that the shrinkage ratio R of the composite material is in the range of 0.2 to 0.

3.

3. 2. The composite material according to claim 1, characterized in that the shrinkage ratio R of the composite material is in the range of 0.3 to 0.

4.

4. 2. The composite material according to claim 1, characterized in that the shrinkage ratio R of the composite material is in the range of 0.4 to 0.

5.

5. 2. The composite material according to claim 1, characterized in that the shrinkage ratio R of the composite material is in the range of 0.5 to 0.

6.

6. 2. The composite material according to claim 1, characterized in that the shrinkage ratio R of the composite material is in the range of 0.6 to 0.

7.

7. The standard heat shrink strength of composite materials is 0.5 to 1.5 N / mm 2 2. The composite material according to claim 1 ,

8. The standard heat shrink strength of composite materials is 1.5 to 2.5 N / mm 2 2. The composite material according to claim 1 ,

9. The standard heat shrink strength of composite materials is 2.5 to 3.5 N / mm 2 2. The composite material according to claim 1 ,

10. The standard tear strength P of the composite material is 7-12 KN / m, where P = [F / d] * [actual weight / 50 g / m 2 2. The composite material according to claim 1, wherein F is the average tear strength and d is the thickness of the test specimen.

11. The composite material according to claim 10, characterized in that the standard tear strength P of the composite material is 7 to 8.5 KN / m.

12. The composite material according to claim 10, characterized in that the standard tear strength P of the composite material is 8.5 to 10 KN / m.

13. The composite material according to claim 10, characterized in that the standard tear strength P of the composite material is 10 to 12 KN / m.

14. 2. The composite material according to claim 1, characterized in that the composite material has a mold resistance grade of Grade 0.

15. 2. The composite material according to claim 1, characterized in that the composite material has a mold resistance grade of Grade 1.

16. 2. The composite material of claim 1, wherein the composite chlorosulfonated polyethylene is composed of porous boron nitride nanosheets carrying zinc borate doped with cuprous oxide, a compatibilizer and chlorosulfonated polyethylene particles.

Citation Information

Patent Citations

  • Preparation method of high modulus polyethylene fiber

    CN103757735A

  • Preparation technology of antibacterial and mildew-proof masterbatch, antibacterial and mildew-proof type cross-linking hot shrink film and preparation technology of antibacterial and mildew-proof type cross-linking hot shrink film

    CN110387053A

  • Insulating film for wrapping dry-type transformers

    CN111016374A

  • A process for flash-spinning dry polymeric plexifilamentary film-fibril strands

    EP0357364A2

  • Flash spinning

    JP1990139408A