2-component water-based paint composition
A two-component water-based coating composition with specific formulation enhances adhesion and anticorrosion properties by optimizing elastic modulus and gel fraction, addressing the limitations of epoxy resin-based water-based paints.
Patent Information
- Application Number
- JP2023051278
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Epoxy resin-based water-based paints do not fully demonstrate adhesion properties compared to solvent-based paints, lacking in both adhesion and anticorrosion performance.
A two-component water-based coating composition comprising an epoxy resin, a resin that reacts with the epoxy resin, a pigment, and water, with specific formulations to achieve an elastic modulus of 600 to 2400 N/mm², a gel fraction of 80% or more, and a solvent residual amount of less than 8.0%, enhancing adhesion and anticorrosion properties.
The composition forms a coating film with excellent adhesion and anticorrosion properties, suitable for various substrates, including metals and composite materials, with improved resistance to deformation and corrosion.
Smart Images

Figure 0007586952000001 
Figure 0007586952000002 
Figure 0007586952000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a two-component water-based coating composition, and more particularly to a two-component water-based coating composition capable of forming a coating film having excellent adhesion and corrosion resistance. [Background technology]
[0002] In the field of coatings for architectural and civil engineering structures, there has been a shift from solvent-based to water-based systems in order to reduce the health hazards to painters and residents and to reduce odors. Room temperature curing two-component water-based epoxy resin paints have been developed for metal coating materials, with excellent film strength, adhesion, and rust prevention properties.
[0003] Japanese Patent Laid-Open Publication No. 2021-1314 (Patent Document 1) describes an invention of an aqueous coating material containing a film-forming component and a powder component, wherein the film-forming component contains an aqueous epoxy resin emulsion as a resin component, and the formed coating has a gel fraction of 10% or more. The powder component contains an anti-rust pigment and calcium carbonate, and the powder component contains 50 to 300 parts by weight of the powder component per 100 parts by weight of the resin component, and the powder component contains 30 to 90% by weight of the calcium carbonate. This aqueous coating material is said to have excellent coating film strength, adhesion, anti-rust properties, etc. Furthermore, Japanese Patent Laid-Open Publication No. 2021-1315 (Patent Document 2) describes an invention in which the aqueous coating material described in Patent Document 1 is blended with a color pigment containing titanium oxide and a red iron oxide pigment.
[0004] JP 2009-149791 A (Patent Document 3) describes an invention of a two-component water-based anticorrosive paint that is composed of a combination of (I) a base agent containing an epoxy resin emulsion and a pigment, and (II) an amine curing agent, and that is mixed and applied immediately before use, characterized in that the pigment in the base agent (I) contains a phosphate-based rust-preventive pigment as part of its components, and the amine curing agent (II) contains as part of its components a polyamine (IIa) with a cyclic structure and an active hydrogen equivalent ranging from 80 to less than 1,000. The invention states that this two-component water-based anticorrosive paint has good curing properties even when dried at room temperature, and is capable of forming an anticorrosive coating film that has excellent corrosion resistance on substrates such as steel materials (e.g., iron and zinc-plated steel) and non-ferrous materials, and therefore can maintain the beauty of the coated object for a long period of time even in harsh environments.
[0005] JP 2019-515991 A (Patent Document 4) describes a two-component epoxy resin paint comprising (a) an epoxy resin component and (b) an amine component for curing the epoxy resin component, the amine component comprising (i) at least one polyamide curing agent and (ii) at least one Mannich base curing agent, wherein at least one of the polyamide curing agent and the Mannich base curing agent is derived from one or more polyfunctional amines, including at least one alicyclic polyfunctional amine, and the alicyclic polyfunctional amine is present in an amount of 30% by weight or more based on the total amount of the polyfunctional amine, and the weight ratio of the epoxy resin component (a) to the amine component (b) is 100:8 to 100:20. It also describes that this provides a two-component epoxy resin paint with a good balance between a long pot life and a fast drying speed.
[0006] Japanese Patent Application Laid-Open Publication No. 2018-53028 (Patent Document 5) describes an invention for a two-component reactive curing water-based coating composition for primer paint that contains an epoxy resin and an amine resin, in which the weight ratio of the epoxy resins having an epoxy equivalent of 400 to 1000 g / eq to the epoxy resins having an epoxy equivalent of 150 to 300 g / eq is 90:10 to 60:40, and describes that this makes it possible to provide a two-component reactive curing water-based coating composition for primer paint that gives a primer paint film with excellent chemical resistance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent Publication No. 2021-1314 [Patent Document 2] Patent Publication No. 2021-1315 [Patent Document 3] Japanese Patent Application Laid-Open No. 2009-149791 [Patent Document 4] Japanese Patent Application Publication No. 2019-515991 [Patent Document 5] Japanese Patent Application Publication No. 2018-53028 Summary of the Invention [Problem to be solved by the invention]
[0008] As mentioned above, epoxy resin-based water-based paint compositions have been proposed. However, although epoxy resins are generally known to have excellent adhesive properties, it was thought that when used in water-based paints, the adhesive properties of epoxy resins were not fully exhibited compared to when used in organic solvent-based paints.
[0009] Therefore, an object of the present invention is to provide a two-component water-based coating composition capable of forming a coating film having excellent adhesion and corrosion resistance. [Means for solving the problem]
[0010] The present inventors have conducted research to achieve the above object, and have found that the elastic modulus of a coating film formed from an epoxy resin-based two-component water-based coating composition is 600 to 2400 N / mm 2 The inventors found that by adjusting the viscosity of the coating to the above range, it was possible to form a coating film with excellent adhesion even with a water-based coating, and thus completed the present invention.
[0011] Therefore, the coating composition of the present invention is a two-component water-based coating composition containing (A) an epoxy resin, (B) a resin that reacts with the epoxy resin, (C) a pigment, and (D) water, and when the coating composition is applied and dried for 7 days under conditions of 23°C and 50% humidity, the coating film has an elastic modulus of 600 to 2400 N / mm 2 The coating composition is
[0012] In a preferred embodiment of the coating composition of the present invention, the coating film has a gel fraction of 80% or more when the coating composition is applied and dried under conditions of 23°C and 50% humidity for 7 days.
[0013] In another preferred embodiment of the coating composition of the present invention, when the coating composition is applied and dried under conditions of 23°C and 50% humidity for 7 days, the amount of solvent remaining in the coating film is less than 8.0%.
[0014] In another preferred embodiment of the coating composition of the present invention, the resin (B) that reacts with the epoxy resin contains at least a modified polyamine having a cyclic structure.
[0015] In another preferred embodiment of the coating composition of the present invention, the resin that reacts with the epoxy resin (B) contains at least a modified polyamine having a cyclic structure, and the content of the modified polyamine having a cyclic structure in the resin that reacts with the epoxy resin (B) is 50 to 100 mass %. [Effects of the Invention]
[0016] According to the present invention, it is possible to provide a two-component water-based coating composition capable of forming a coating film having excellent adhesion and corrosion resistance. DETAILED DESCRIPTION OF THE INVENTION
[0017] The present invention is described in detail below. The present invention relates to a two-component water-based paint composition containing an epoxy resin, a resin reactive with the epoxy resin, a pigment, and water. In this specification, this paint composition is also referred to as the "two-component water-based paint composition of the present invention" or the "paint composition of the present invention." Furthermore, the "epoxy resin" is the (A) component and is also referred to as the "(A) epoxy resin." The "resin reactive with the epoxy resin" is the (B) component and is also referred to as the "(B) resin reactive with the epoxy resin." The "pigment" is the (C) component and is also referred to as the "(C) pigment." The "water" is the (D) component and is also referred to as the "(D) water."
[0018] In this specification, a water-based coating composition refers to a coating composition containing water as the main solvent. The water used in the coating composition of the present invention is not particularly limited, but suitable examples include tap water, ion-exchanged water, distilled water, and other pure water. Furthermore, when storing the coating composition for a long period of time, water that has been sterilized by ultraviolet irradiation or the like may be used to prevent the growth of mold and bacteria. The amount of water in the coating composition of the present invention is preferably 20 to 60% by mass, more preferably 30 to 50% by mass.
[0019] Furthermore, the amount of nonvolatile content in the coating composition of the present invention is preferably 40 to 80% by mass, more preferably 50 to 70% by mass. In this specification, the nonvolatile content refers to the components excluding volatile components such as solvents, and is the component that will ultimately form the coating film. In the present invention, the components that remain when the coating composition is dried in an oven at 110°C for 3 hours are considered to be nonvolatile content.
[0020] In this specification, a two-component coating composition is a coating composition consisting of a base agent and a curing agent. A two-component coating composition can be prepared by mixing the base agent, curing agent, and additives selected as necessary at the time of coating. In the present invention, (A) an agent containing an epoxy resin is the base agent, and (B) an agent containing a resin that reacts with the epoxy resin is the curing agent. (C) Pigment may be blended in either the base agent or the curing agent, but is usually contained in the base agent. (D) Water is usually contained in the base agent and the curing agent, but may also be used only in the base agent. Also, a portion of (D) Water may also be used as an additive when mixing the base agent and curing agent.
[0021] Epoxy resins are resins that have epoxy groups in their molecules and can be cured by reaction of the epoxy groups. Epoxy resins generally have high adhesion to substrates, particularly metal substrates, and also have the effect of shielding the substrate from environmental factors (e.g., water, oxygen, etc.) that affect the corrosion of substrates, particularly metal substrates (shielding effect), and are therefore known as resins with excellent corrosion resistance. However, when used in aqueous coating compositions, the effects of improving adhesion and corrosion resistance due to this epoxy resin have not been fully demonstrated. However, according to the present invention, by adjusting the elastic modulus and gel fraction of the coating film formed, it is possible to sufficiently improve adhesion and corrosion resistance even in aqueous coating compositions.
[0022] The epoxy resin is preferably a resin having at least two epoxy groups per molecule, and is obtained, for example, by reacting a polyhydric alcohol or a polyhydric phenol with a halohydrin, and specific examples include bisphenol A epoxy resins, halogenated bisphenol A epoxy resins, novolac epoxy resins, polyglycol epoxy resins, bisphenol F epoxy resins, epoxidized oil, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, etc. Furthermore, from the viewpoint of increasing the elastic modulus of the resulting coating film, the epoxy resin is preferably one having a rigid structure such as an aromatic ring.
[0023] The epoxy resin is preferably formulated in the form of an epoxy resin emulsion, an epoxy resin dispersion, or an aqueous epoxy resin solution. In this specification, "resin emulsion" refers to an emulsion in which a resin is dispersed in an aqueous medium primarily composed of water, "resin dispersion" refers to a dispersion in which a resin is dispersed in an aqueous medium primarily composed of water, and "aqueous resin solution" refers to a solution in which a resin is dissolved in an aqueous medium primarily composed of water. The epoxy resin emulsion is prepared by emulsifying an epoxy resin in an aqueous medium primarily composed of water using a conventional forced emulsification method (a method using an emulsifier and a high-speed mixer, etc.), without any particular limitation. Examples of emulsifiers include polyethers such as polyoxyethylene alkylphenol ether-based nonionic surfactants and polyoxyethylene-polyoxypropylene block copolymers; and adducts of at least one of these nonionic surfactants and these polyethers with a diisocyanate compound. The emulsifiers may be used alone or as a blend of two or more. Commercially available epoxy resin emulsions include Epolsion EA-1, 2, 3, 7, 12, 20, 55, and HD2 (manufactured by Henkel Japan Co., Ltd.); Yuka Resin KE-002, KE-116, E-1022, and KE-301C (manufactured by Yoshimura Oil Chemical Co., Ltd.); Adeka Resin EM-101-50 (manufactured by Adeka Corporation); jER W1155R55, jER W3435R67, and jER W2821R70 (manufactured by Mitsubishi Chemical Corporation). Commercially available epoxy resin dispersions include Beckpox EP2381 (manufactured by Allnex Corporation); and EPI-REZ6530-WH-53 (manufactured by Momentive Corporation).
[0024] The epoxy resin may be a modified epoxy resin, such as a urethane-modified epoxy resin, an amine-modified epoxy resin, an isocyanate-modified epoxy resin, an acrylic-modified epoxy resin, a polyester-modified epoxy resin, or a dimer acid-modified epoxy resin.
[0025] The epoxy equivalent of the epoxy resin is preferably 100 to 1,000 g / eq, more preferably 200 to 700 g / eq, and even more preferably 300 to 600 g / eq. When the epoxy equivalent is 100 g / eq or more, sufficient coating film properties are easily obtained. On the other hand, when the epoxy equivalent is 1,000 g / eq or less, leveling properties are less likely to decrease and a uniform coating film is easily obtained. When multiple epoxy resins are used in combination, it is preferable that the average epoxy equivalent of each epoxy resin mixture be within the above-specified range. The epoxy equivalent of the epoxy resin can be determined according to JIS K 7236:2001, "Determination of the epoxy equivalent of an epoxy resin."
[0026] In the coating composition of the present invention, the amount of epoxy resin in the nonvolatile matter is preferably 30 to 70 mass %. The epoxy resins may be used alone or in combination of two or more.
[0027] Resins reactive with epoxy resins are resins that react with epoxy resins, particularly with their epoxy groups, to promote or control the curing reaction. Resins reactive with epoxy resins are preferably resins containing active hydrogens that react with epoxy groups, with polyamine resins being more preferred. Polyamine resins are resins containing at least two amino groups per molecule. Examples of polyamine resins include those produced by condensation polymerization of amines and aldehydes, etherification of amines with alcohols, ring-opening polymerization of amines with heterocyclic structures (e.g., ethyleneimine), condensation of amines with carboxylic acids, or the Mannich reaction of amines with formaldehyde and ketones or phenols. Polyamine resins that also contain amide bonds in their molecules, such as resins produced by condensation of amines and carboxylic acids, are also referred to as "polyamidoamine resins" or "polyamidoamines." Furthermore, ring-opening polymerization of alkylene oxides such as ethylene oxide and propylene oxide can be used to etherify amines with alcohols.
[0028] Examples of amines that can be used in producing the polyamine resin include aliphatic polyamines such as ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, triaminopropane, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, isophoronediamine, and 1,3-bisaminomethylcyclohexane; aromatic polyamines such as phenylenediamine, metaxylylenediamine, paraxylylenediamine, and diaminodiphenylmethane; and amines having a heterocyclic structure such as ethyleneimine.
[0029] The polyamine resin may also be a modified polyamine resin. The modified polyamine resin is a polyamine resin in which some of the amino groups have been modified. The amino groups can be modified by known methods, such as amidation of the amino groups, the Mannich reaction of the amino groups with a carbonyl compound, or the addition reaction of the amino groups with an epoxy group.
[0030] The resin reactive with the epoxy resin preferably contains at least a modified polyamine having a cyclic structure. By using a modified polyamine having a cyclic structure as the resin reactive with the epoxy resin, the elastic modulus of the resulting coating film can be increased. The modified polyamine is a polyamine resin in which some of the amino groups have been modified, and examples of such modifications include amidation of the amino groups, the Mannich reaction of the amino groups with a carbonyl compound, and the addition reaction of the amino groups with an epoxy group. The modified polyamine is preferably a Mannich-modified polyamidoamine.
[0031] The content of the modified polyamine having a cyclic structure in the resin that reacts with the epoxy resin is preferably 50 to 100% by mass, and more preferably 60 to 90% by mass.
[0032] It is more preferable that the resin reacting with the epoxy resin contains at least a modified polyamine having a cyclic structure. The use of a modified polyamine having a cyclic structure can enhance the effect of increasing the elastic modulus. A modified polyamine having a cyclic structure can be obtained by using a substance having a cyclic structure during its production. Examples of amines having a cyclic structure that can be used to produce polyamine resins include piperazines such as N-aminoethylpiperazine, aliphatic polyamines such as 1,3-bisaminoethylcyclohexane, isophoronediamine, 1-cyclohexylamino-3-aminopropane, 1,4-diaminocyclohexane, di(aminocyclohexyl)methane, 1,3-di(aminocyclohexyl)propane, 2,4-diaminocyclohexane, N,N'-diethyl-1,4-diaminocyclohexane, and 3,3'-dimethyl-4,4'-diaminocyclohexylmethane, and aromatic polyamines such as phenylenediamine, metaxylylenediamine, paraxylylenediamine, and diaminodiphenylmethane. Aliphatic polyamines having a cyclic structure are sometimes referred to as alicyclic polyamines. Examples of alcohols having a cyclic structure that can be used to produce polyamine resins include phenol and its derivatives. Examples of phenol derivatives include phenols in which the benzene ring is substituted with a hydrocarbon group, particularly phenols substituted with a linear or branched hydrocarbon group that may have one or more unsaturated bonds. Here, the hydrocarbon group is preferably a long-chain hydrocarbon group having 10 to 20 carbon atoms, particularly an alkyl group. A specific example of a phenol derivative is cardanol. Resins to be reacted with epoxy resins preferably have a cyclic structure, and more preferably have a rigid structure such as an aromatic ring, from the viewpoint of increasing the elastic modulus of the resulting coating film.
[0033] From the viewpoint of increasing the elastic modulus of the coating film, the modified polyamine having a cyclic structure is preferably a polyamine resin obtained by the Mannich reaction of amines, formaldehyde, and a phenol derivative. Here, the cyclic structure is derived from a phenol derivative, and the amines are preferably chain compounds (or acyclic compounds) such as ethylenediamine. The phenol derivative is as described above, and cardanol is particularly preferred. Such modified polyamine resins are also called phenalkamine-based curing agents.
[0034] As described above, the use of modified polyamines, particularly modified polyamines having a cyclic structure, can increase the elastic modulus of the coating film. On the other hand, modified polyamines, particularly modified polyamines having a cyclic structure, tend to have low reactivity with epoxy resins. Therefore, it is preferable to use a modified polyamine, particularly a modified polyamine having a cyclic structure, in combination with a resin that does not fall under the category of modified polyamines as a resin that reacts with epoxy resins. This ensures the reactivity of the resin that reacts with epoxy resins. Here, the resin that can be used in combination with the modified polyamine is not particularly limited, and examples thereof include polyoxyethylene amines (also called polyether amines) such as polyoxyethylene diamine and polyoxypropylene diamine.
[0035] When the resin that reacts with the epoxy resin contains a modified polyamine and a resin that does not fall under the category of modified polyamine, it is preferable that the proportion of the modified polyamine in the entire resin that reacts with the epoxy resin is 50 to 99 mass %, and the proportion of the resin that does not fall under the category of modified polyamine is 1 to 50 mass %.
[0036] The resin that reacts with the epoxy resin is preferably blended in the form of an emulsion, a dispersion, or an aqueous solution.
[0037] The active hydrogen equivalent of the resin that reacts with the epoxy resin is preferably 80 to 350 g / eq, more preferably 100 to 250 g / eq. The active hydrogen equivalent of the resin that reacts with the epoxy resin is the number of grams [g / eq] of the resin containing 1 equivalent of active hydrogen, and is the value obtained by dividing the molecular weight of the resin that reacts with the epoxy resin by the number of hydrogen atoms in the amino group per molecule.
[0038] In the coating composition of the present invention, the amount of the resin reactive with the epoxy resin in the nonvolatile content is preferably 5 to 20 mass %. The resin reactive with the epoxy resin may be used alone or in combination of two or more.
[0039] The pigment is not particularly limited, and pigments commonly used in the paint industry such as anti-rust pigments, extender pigments, coloring pigments, etc. The pigments may be used alone or in combination of two or more.
[0040] Examples of anti-rust pigments include zinc powder, zinc oxide, barium metaborate, calcium silicate, aluminum phosphate, condensed aluminum phosphate, aluminum tripolyphosphate, zinc phosphate, zinc phosphite, potassium phosphite, calcium phosphite, aluminum phosphite, calcium zinc phosphate, zinc aluminum phosphate, zinc phosphomolybdate, aluminum phosphomolybdate, magnesium phosphate, and vanadate / phosphoric acid mixed pigments. Among these, phosphate-based anti-rust pigments are preferred from the viewpoint of corrosion prevention. Examples of phosphate-based anti-rust pigments include salts of phosphate compounds such as phosphoric acid, phosphorous acid, and polyphosphoric acid (magnesium salts, calcium salts, zinc salts, aluminum salts, phosphomolybdates, etc.). In the coating composition of the present invention, the amount of the anti-rust pigment in the non-volatile content is, for example, 1 to 20 mass%.
[0041] Examples of extender pigments include silica, talc, mica, calcium carbonate, and barium sulfate. Among these, calcium carbonate is preferred from the viewpoint of chemical resistance. In the coating composition of the present invention, the amount of the extender pigment in the nonvolatile matter is, for example, 10 to 50 mass %.
[0042] Examples of color pigments include titanium oxide, iron oxide, carbon black, yellow lead, molybdate orange, ultramarine, Prussian blue, phthalocyanine blue, phthalocyanine green, quinacridone red, naphthol red, benzimidazolone yellow, Hansa yellow, benzimidazolone orange, dioxazine violet, etc. In the coating composition of the present invention, the amount of color pigment in the nonvolatile content is, for example, 1 to 20 mass %.
[0043] At least a portion of the pigment can be a scaly pigment. Due to their scale shape, scaly pigments have the effect of inhibiting the penetration of corrosive factors such as water, oxygen, and chlorides, and of reducing the internal stress of the coating film. By reducing the internal stress of the coating film, the adhesion of the coating film can be further improved, and a thick coating film can be advantageously formed. Examples of scaly pigments include talc, mica, kaolin clay, glass flake, micaceous iron oxide, aluminum, and other metal pigments. Some scaly pigments are classified as anti-rust pigments, extender pigments, or coloring pigments, as described above. In the coating composition of the present invention, the amount of the scaly pigment in the nonvolatile content is, for example, 0 to 50% by mass.
[0044] In the present invention, from the viewpoint of increasing the elastic modulus of the resulting coating film, it is preferable to use a scaly pigment having an aspect ratio of more than 1 and less than 120. From the viewpoint of increasing the elastic modulus, scaly pigments having an aspect ratio of more than 30 are preferred, but because dispersibility is poor, an average aspect ratio of 1 to 30 is preferred.
[0045] In this specification, the average aspect ratio of a scaly pigment refers to the ratio (D / T) of the average particle diameter (D) to the average thickness (T) of the scaly pigment. Here, the average particle diameter is the 50% particle diameter (D) of the volume-based particle size distribution. 50) and is determined from the particle size distribution measured using a laser diffraction / scattering particle size distribution analyzer. The particle size of a scaly pigment is expressed as the spherical equivalent diameter measured by the laser diffraction / scattering method. The average thickness is the average value of the thicknesses measured for 100 or more scaly pigment particles using a scanning electron microscope (SEM).
[0046] The average particle size of the scaly pigment is preferably 3 to 40 μm, and more preferably 3 to 20 μm.
[0047] The coating composition of the present invention preferably has a pigment volume concentration (PVC) of 10 to 40%, more preferably 25 to 35%. In the present invention, from the viewpoint of increasing the elastic modulus of the resulting coating film, a high PVC is preferred, and from this viewpoint, the PVC is preferably 28% or more.
[0048] In this specification, pigment volume concentration (PVC) is the ratio of the total volume of pigment to the total volume of nonvolatile matter in a coating composition, and can be calculated from the composition and specific gravity of the components that make up the nonvolatile matter.
[0049] The coating composition of the present invention has a coating film elastic modulus of 600 to 2400 N / mm when the coating composition is applied and dried for 7 days under conditions of 23°C and 50% humidity. 2 and 900 to 2400 N / mm 2 Preferably, the strength is 1300 to 2400 N / mm 2 The present inventors have set the modulus of elasticity of the coating film to 600 N / mm 2 It was found that by increasing the modulus of elasticity to 2400 N / mm, the adhesion of the coating film can be improved. The modulus of elasticity is a physical property that indicates resistance to deformation. Therefore, it is thought that the higher the modulus of elasticity, the higher the resistance to deformation, which improves the adhesion of the coating film. In addition, the modulus of elasticity of the coating film is 2400 N / mm 2 If the coating has a viscosity of 1000 ppm or less, the coating exhibits excellent adhesion, does not cause poor film formation, and exhibits excellent corrosion prevention properties.
[0050] (How to determine the elastic modulus of a coating film) The coating composition is applied to a substrate (e.g., a polypropylene plate) using an applicator to a dry film thickness of 50 to 70 μm, and then allowed to dry for 7 days at 23°C and 50% humidity. A 50 mm x 10 mm strip test piece is cut from the resulting coating to prepare a measurement sample. A tensile test is performed at 23°C and 50% humidity at a speed of 5 mm / min, and the stress-strain ratio is calculated from the slope (proportionality constant) within the proportional range of stress and strain.
[0051] Conventional epoxy resin-based water-based coating compositions have a modulus of elasticity of the coating film formed of 600 N / mm 2 However, the present inventors have found that by using a modified polyamine, particularly a modified polyamine having a cyclic structure, as a resin that reacts with the epoxy resin, the elastic modulus of the resulting coating film can be increased to 600 N / mm 2 It has been found that it is possible to form a coating film having an elastic modulus of 2400 N / mm or more. However, when the coating film is dried at a high temperature (for example, a temperature of 50°C or higher) or when the pigment volume concentration (PVC) exceeds 40%, the elastic modulus of the formed coating film is 2400 N / mm or more. 2 It is expected that the elastic modulus will exceed 2400N / mm 2 A coating film exceeding this temperature tends to become hard and brittle, loses toughness, and may result in poor film formation or cracks.
[0052] The coating composition of the present invention preferably has a gel fraction of 80% or more, and preferably 90% or more, when applied and dried for 7 days at 23°C and 50% humidity. The gel fraction is an index of the reactivity between the epoxy resin and the resin that reacts with the epoxy resin. In the present invention, if the gel fraction of the coating film is less than 80%, the reactivity between these resins cannot be said to be sufficient, and problems such as redissolution when a paint is applied on top of the coating film or insufficient water resistance and corrosion resistance may occur.
[0053] For example, when a modified polyamine, especially a modified polyamine having a cyclic structure, is used as a resin that reacts with an epoxy resin, the effect of increasing the elastic modulus is obtained, but the reactivity with the epoxy resin tends to be low, and the gel fraction of the coating film may fall below 80%. In such cases, it is preferable to use a resin that does not fall under the category of a modified polyamine having a cyclic structure as a resin that reacts with the epoxy resin. This will increase the elastic modulus of the coating film to 600 to 2400 N / mm. 2 It is also possible to make the gel fraction of the coating film 90% or more while still being within the above range.
[0054] (How to determine the gel fraction of a coating film) The coating composition is applied to a substrate (e.g., a polypropylene plate) using an applicator to a dry film thickness of 50 to 70 μm, and after drying for 7 days at 23°C and 50% humidity, the coating is peeled off from the substrate and the mass of the resulting coating is measured; this mass is designated W0. The coating is then immersed in tetrahydrofuran (THF) at 23°C for 1 day. After immersion, the coating is removed from the THF, completely dried, and its mass is measured. The mass of the coating at this point is designated Wd. The mass loss ΔW (= W0 - Wd) is then divided by W0 to convert the result into a percentage to calculate the mass loss rate. The gel fraction is a value calculated from the difference between 100% and the mass loss rate. Calculation formula: Gel fraction = 100 - (W0 - Wd) / W0 x 100
[0055] The coating composition of the present invention preferably has a residual solvent content of less than 8.0%, preferably 7.0% or less, and more preferably 6.5% or less, when the coating composition is applied and dried for 7 days under conditions of 23°C and 50% humidity. If a large amount of solvent remains, problems such as a decrease in elastic modulus due to a plasticizing effect and insufficient adhesion may occur. The residual solvent content can be kept low by reducing the proportion of volatile components such as water and film-forming aids used in the coating composition.
[0056] (How to determine the amount of solvent remaining in the coating film) The coating composition is applied to a substrate (e.g., a polypropylene plate) using an applicator to a dry film thickness of 50 to 70 μm. The mass of the coating composition used for application is designated as the coating mass W0. After application, the coating is dried for 7 days under conditions of 23°C and 50% humidity, and the mass of the resulting coating is measured, which is designated as the measured coating mass W. The theoretical value of the final dry coating mass is calculated from the mass of the nonvolatile components in the coating composition used for application, and this is designated as the theoretical coating mass Wz. The remaining solvent amount is calculated by dividing the difference between the measured and theoretical coating masses (W-Wz) by the coating mass W0 and converting the result into a percentage. Calculation formula: Remaining solvent amount = (W-Wz) / W0 x 100
[0057] Other components that may be blended into the coating composition of the present invention, depending on the purpose, include resins other than component (A) or component (B), crosslinking agents other than component (B), film-forming aids, antifreezing agents, surface conditioners (also known as wetting agents), dispersants, antifoaming agents, viscosity modifiers, thickeners, rust inhibitors other than anti-rust pigments, anti-flash rust agents, anti-settling agents, anti-skinning agents, anti-sagging agents, anti-color separation agents, matting agents, adhesion promoters, leveling agents, drying agents, catalysts, plasticizers, anti-mold agents, antibacterial agents, antiviral agents, preservatives, insecticides, antistatic agents, and conductivity-imparting agents.
[0058] The coating composition of the present invention can be prepared by preparing the base agent and curing agent in advance and then mixing the base agent, curing agent, and optional additives at the time of application. The base agent and curing agent can be prepared by mixing various components appropriately selected as necessary.
[0059] The coating composition of the present invention preferably has a viscosity of 1 to 1000 (Pa·s, 23°C) at a shear rate of 0.1 (1 / s), and a viscosity of 0.05 to 10 (Pa·s, 23°C) at a shear rate of 1000 (1 / s).
[0060] In this specification, viscosity is measured using a rheometer (for example, ARES rheometer manufactured by TA Instruments) after adjusting the liquid temperature to 23°C.
[0061] The means for applying the coating composition of the present invention is not particularly limited, and known coating means such as brush coating, roller coating, trowel coating, spatula coating, flow coater coating, and spray coating (e.g., air spray coating, airless spray coating) can be used.
[0062] The means for drying the coating composition of the present invention is not particularly limited, and may be either natural drying at ambient temperature or forced drying using a dryer or the like.
[0063] The coating composition of the present invention is capable of forming a coating film with excellent adhesion and preferably also has improved corrosion resistance, making it suitable as an undercoat coating.
[0064] Substrates to be coated with the coating composition of the present invention include, for example, plastic substrates such as epoxy resin, ABS resin, polycarbonate, polyvinyl chloride, polystyrene, acrylic resin, e.g., polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), polyolefin, e.g., polypropylene (PP), metal substrates such as steel, galvanized steel, tin-plated steel, stainless steel, magnesium alloy, aluminum, aluminum alloy, titanium, titanium alloy, etc., inorganic substrates other than metals such as cement, mortar, concrete, slate, gypsum, calcium silicate, glass, ceramic, calcium carbonate, marble, artificial marble, etc., wood substrates such as wood, paper substrates, composite substrates combining two or more of these substrates, etc. Examples of composite substrates include composite substrates such as wood fiber reinforced cement board, fiber reinforced cement board, fiber reinforced cement-calcium silicate board, etc., metal substrates that have been subjected to various surface treatments, such as oxidation treatment, and plastic substrates whose surfaces are coated with inorganic substances (e.g., plastic substrates coated with glass).
[0065] The coating composition of the present invention is capable of forming a coating film that has excellent adhesion and preferably also excellent corrosion resistance, and therefore the substrate to be coated is preferably a metal substrate or a composite substrate made of a metal and another material.
[0066] The substrate may have various shapes, for example, two-dimensional substrates such as films, sheets, and plates, and three-dimensional substrates that are complex three-dimensional objects, etc. The surface of the substrate may be smooth or may have irregularities.
[0067] The surface of the substrate may be subjected to pretreatments such as degreasing, chemical conversion treatment and polishing, or may be painted with a sealer, primer or zinc-rich paint, or plated or metal sprayed.
[0068] The substrate may have an old paint film on its surface. The old paint film may cover a part or the whole of the surface of the substrate. In this specification, the old paint film means a paint film that is already present on the substrate when painting, particularly repair, is performed.
[0069] When a substrate has an old coating film on its surface, the substrate surface, including the old coating film, can be coated with the coating composition of the present invention. If the old coating film is sound, the coating composition of the present invention can be applied to the old coating film without peeling or removing the old coating film from the substrate surface. Since contaminants such as dust and dirt adhere to the old coating film, removing the contaminants can improve the adhesion of a new coating film to the old coating film. Methods for removing contaminants include high-pressure water washing, alkaline washing with caustic soda or the like, acid washing with inorganic or organic acids, washing with bleaching agents such as perchloric acid, and washing by scraping and wiping with a cloth.
[0070] The old paint film preferably contains a resin, for example, acrylic resin, silicone resin, acrylic silicone resin, styrene acrylic copolymer resin, polyester resin, fluororesin, rosin resin, petroleum resin, coumarone resin, phenolic resin, urethane resin, melamine resin, urea resin, epoxy resin, cellulose resin, xylene resin, alkyd resin, aliphatic hydrocarbon resin, butyral resin, maleic acid resin, fumaric acid resin, vinyl resin, amine resin, ketimine resin, and resins obtained by modifying these resins (modified resins), etc. The resins may be used alone or in combination of two or more.
[0071] The old paint film may contain various additives as other components, such as pigments, dispersants, surface conditioners, antioxidants, plasticizers, rust inhibitors, solvents, antibacterial agents, antiviral agents, viscosity adjusters, fillers, antifoaming agents, charge control agents, stress relaxation agents, penetrating agents, light-guiding materials, lustrous materials, magnetic materials, phosphors, ultraviolet absorbers, and radical scavengers.
[0072] The coating composition of the present invention has a coating film elastic modulus of 600 to 2400 N / mm when dried for 7 days under conditions of 23°C and 50% humidity. 2 Therefore, resistance to external stress is increased, and as a result, it is possible to form a coating film that has excellent adhesion to the substrate and old coating film, and preferably also excellent corrosion resistance. In addition, by selecting an appropriate intermediate or top coat paint according to the external environment, it is possible to not only impart adhesion and corrosion resistance to the substrate and old coating film, but also to create a coating film that has properties adapted to the environment, such as antifouling properties, water repellency, weather resistance, environmental barrier properties, etc.
[0073] When the coating composition of the present invention is used as an undercoat coating, a topcoat coating film can be formed on the undercoat coating film, or an intermediate coating film and a topcoat coating film can be formed in this order.
[0074] The paint for forming the intermediate coating film or the top coating film is preferably a water-based coating composition, similar to the coating composition of the present invention. These coating compositions can be appropriately blended with resins, crosslinking agents, pigments, water, film-forming aids, antifreezing agents, surface conditioners (also called wetting agents), dispersants, antifoaming agents, viscosity adjusters, thickeners, rust inhibitors, antisettling agents, antiskinning agents, antisagging agents, color-flux inhibitors, matting agents, adhesion promoters, leveling agents, drying agents, catalysts, plasticizers, antifungal agents, antibacterial agents, antiviral agents, preservatives, insecticides, ultraviolet absorbers, radical scavengers, antistatic agents, and conductivity-imparting agents, etc., depending on the purpose. [Example]
[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0076] <Example of preparation of coating composition> The base resin and curing agent were prepared by mixing the raw materials according to the formulations shown in Tables 1 and 2. The obtained base resin and curing agent were mixed with water for dilution in the mixing ratios shown in Table 3 to prepare coating compositions, which were then evaluated. The formulations and mixing ratios shown in Tables 1 to 3 are based on mass.
[0077] Details of the materials used in preparing the coating compositions are provided below. Epoxy resin 1: ADEKA Resin EM101-50 (epoxy resin emulsion manufactured by ADEKA: non-volatile content 47% by mass, epoxy equivalent weight 1075 g / eq) Epoxy resin 2: jER W2821R70 (epoxy resin emulsion manufactured by Mitsubishi Chemical Corporation: non-volatile content 70% by mass, epoxy equivalent weight 220-240 g / eq) Anti-rust pigment: Aluminum tripolyphosphate K-WHITE #84S (manufactured by Teika Co., Ltd.) Extender pigment 1: Calcium carbonate (average particle size 6 μm) Extender pigment 2: Talc (average particle size 13 μm, aspect ratio less than 20) Color pigment 1: Titanium dioxide (white pigment) Color pigment 2: Carbon black (black pigment) Color pigment 3: Iron oxide (Oukatsu color pigment) Color pigment 4: Iron oxide (rust pigment) Dispersant: FLORENE GW-1640 (Kyoeisha Chemical Co., Ltd.) Film-forming agent: Dipropylene glycol n-butyl ether Antifoaming agent: SN Deformer 1312 (manufactured by San Nopco) Thickener: SN Thickener 665T (San Nopco, urethane-modified polyether compound, non-volatile content 30%) Polyamine resin 1: Cardolite NX-8401 (amine resin emulsion manufactured by Cardolite; non-volatile content 57% by mass, active hydrogen equivalent 290 g / eq) Polyamine resin 2: Daitoclar X-7024 (amine resin emulsion manufactured by Daito Sangyo Co., Ltd.: non-volatile content 50%, active hydrogen equivalent 392 g / eq) Polyamine resin 3: JEFFAMINE T-403 (polyetheramine manufactured by HUNTSUMAN; non-volatile content 100% by mass, active hydrogen equivalent 81 g / eq) Polyamine resin 4: BECKOPOX EH623W (water-soluble amine resin manufactured by ALLNEX; non-volatile content 80% by mass, active hydrogen equivalent 200 g / eq) Rust inhibitor 1: HALOX 650 (organic rust inhibitor manufactured by ICL Phosphate Specialty, non-volatile content 100% by mass) Rust inhibitor 2: Sodium nitrite
[0078] <Coating film preparation method 1> The paint prepared in the above <Preparation Example of Paint Composition> was applied to a polypropylene plate (2.0 × 70 × 150 mm) using an applicator so that the dry film thickness was 50 to 70 μm, and the plate was dried in an environment of 23°C and 50% relative humidity for 7 days to obtain a painted plate.
[0079] <Coating film production method 2> A sandblasted board (3.2 x 70 x 150 mm) was air-sprayed with a modified epoxy resin paint (Epool Smile, manufactured by Dai Nippon Toryo Co., Ltd.) to a dry film thickness of 55-65 μm, dried at 23°C and 50% relative humidity for one day, and then forced-dried at 50°C for seven days to obtain a base coat. The paint prepared in the above <Paint Composition Preparation Example> was applied to the resulting base coat using an applicator to a dry film thickness of 50-70 μm, and then dried at 23°C and 50% relative humidity for seven days to obtain a painted board.
[0080] <Coating film production method 3> The paint prepared in the above <Preparation Example of Paint Composition> was air spray painted onto a sandblasted board (3.2 × 70 × 150 mm) to a dry film thickness of 55 to 65 μm, and dried in an environment of 23 °C and 50% relative humidity for 7 days to obtain a painted board. The back and periphery of the painted board were painted with the same paint and sealed.
[0081] <Elastic modulus> A 50mm x 10mm strip of coating film was cut out as a test piece from the coated plate prepared using coating film preparation method 1, and then a tensile test was carried out on the test piece at a speed of 5mm / min in an environment of 23°C and 50% humidity. The modulus of elasticity (N / mm 2 The results are shown in Table 3.
[0082] <Gel fraction> A 20 mm x 50 mm strip of coating film was cut out as a test piece from the coated plate prepared by Coating Film Preparation Method 1. The mass (W0) of the resulting coating film (test piece) was measured, and then the coating film (test piece) was immersed in tetrahydrofuran (THF) at 23°C for 1 day. After immersion, the coating film (test piece) was removed from the THF, washed with THF, and then completely dried. Its mass (Wd) was measured, and the gel fraction was calculated using the following formula and evaluated based on the following criteria. The results are shown in Table 3. Calculation formula: Gel fraction = 100 - (W0 - Wd) / W0 x 100 (standard) 〇: 85% or more △: 80% or more, less than 85% ×: Less than 80%
[0083] <Solvent Residual Rate> The mass (W) of the coating film on the coated plate prepared using Coating Film Preparation Method 1 and the mass (W0) of the paint used to prepare the coating film were measured, and the theoretical coating mass (Wz) when completely dried was calculated from the mass of the non-volatile content in the paint. The remaining amount of solvent was calculated using the following formula and evaluated based on the following criteria. The results are shown in Table 3. Calculation formula: Remaining solvent amount = (W-Wz) / W0 x 100 (standard) ○: Less than 6.0% △: 6.0% or more, less than 8.0% ×: 8.0% or more
[0084] <Adhesion> In an environment of 23°C and 50% RH, nine grids were created on the coating surface (test surface) of a coated plate prepared using Coating Preparation Method 2 by using a utility knife to make four cuts at 5mm intervals in both the vertical and horizontal directions, reaching down to the substrate base. A piece of cellophane tape with a crease on one side was firmly pressed against the grid surface and then forcefully peeled off at an angle of 60-90°. The adhesion of the coating was evaluated based on the area of the remaining coating according to the following criteria. The results are shown in Table 3. A coating with excellent adhesion was determined when the area of the remaining coating corresponded to four or more squares. (standard) ◎: The area of the remaining coating film corresponds to 8 or more squares. ○: The area of the remaining coating film corresponds to 6 or more but less than 8 squares. △: The area of the remaining coating film corresponds to 4 or more but less than 7 squares. ×: The area of the remaining coating film corresponds to less than 4 squares.
[0085] <Corrosion resistance> Test specimens were prepared by using a utility knife to make cuts in the lower half of the coating on the coated plate prepared using coating preparation method 3, reaching the sandblasted plate (base material). The condition of rust and blisters after 336 hours of neutral salt spray testing according to JIS Z 2371 was evaluated. The evaluation criteria are as follows, and the results are shown in Table 3. If the width of the rust and blisters in the cut area is within 3 mm, the coating has excellent corrosion protection. (standard) 〇: Rust and swelling width of cut area is less than 2mm △: Rust and swelling width of cut area is more than 2mm and less than 3mm ×: Rust or blister width in the cut area is 3mm or more, or there is an abnormality in the general area
[0086] [Table 1]
[0087] [Table 2]
[0088] [Table 3]
Claims
1. A two-component water-based coating composition comprising (A) an epoxy resin, (B) a resin that reacts with the epoxy resin, (C) a pigment, and (D) water, The (A) epoxy resin has an aromatic ring and is contained in an amount of 30 to 70 mass % in the non-volatile content of the two-component water-based coating composition, The (B) resin that reacts with the epoxy resin is i) containing a polyamine resin having an active hydrogen equivalent of 80 to 350 g / eq; and ii) at least a modified polyamine having a cyclic structure derived from an aromatic ring, the modified polyamine having a cyclic structure derived from an aromatic ring being contained in a proportion of 50 to 100% by mass based on the total mass of the resin (B) that reacts with the epoxy resin; the (C) pigment has a pigment volume concentration (PVC) of 25 to 35% and contains one or more pigments selected from the group consisting of anti-rust pigments, extender pigments, and color pigments, the contents of the anti-rust pigments, the extender pigments, and the color pigments in the non-volatile matter of the two-component water-based coating composition are 1 to 20% by mass, 10 to 50% by mass, and 1 to 20% by mass, respectively; In the two-component water-based coating composition, the amount of non-volatile matter is 40 to 80 mass %, The coating composition is applied to a polypropylene plate using an applicator so that the dry film thickness is 50 to 70 μm, and the coating film is dried for 7 days under conditions of 23°C and 50% humidity, and the elastic modulus of the coating film is 600 to 2400 N / mm 2 and Here, the elastic modulus of the coating film is determined by cutting out a strip of the coating film measuring 50 mm x 10 mm as a test piece, subjecting the test piece to a tensile test at an environment of 23°C and 50% humidity at a speed of 5 mm / min, and calculating the elastic modulus from the slope (proportionality constant) within the range in which stress and strain are proportional to each other.
2. The coating composition is applied to a polypropylene plate using an applicator so that the dry film thickness is 50 to 70 μm, and the coating film has a gel fraction of 80% or more when dried for 7 days under conditions of 23° C. and 50% humidity. Here, the gel fraction of the coating film was determined by cutting out a 20 mm x 50 mm strip of the coating film as a test piece, measuring the mass (W0) of the obtained coating film (test piece), immersing the coating film (test piece) in tetrahydrofuran (THF) at 23°C for one day, removing the coating film (test piece) from the THF after immersion, washing the coating film (test piece) with THF, and then completely drying the coating film. The mass (Wd) was then measured and calculated using the following formula:
2. The coating composition according to claim 1, wherein the gel fraction is calculated from the following formula: gel fraction = 100 - (W0 - Wd) / W0 x 100.
3. 3. The coating composition according to claim 1 or 2, characterized in that when the coating composition is applied to a polypropylene plate using an applicator so as to give a dry film thickness of 50 to 70 μm and dried for 7 days under conditions of 23° C. and 50% humidity, the coating film has a remaining solvent amount of less than 8.0%.
4. 3. The coating composition according to claim 1, wherein the pigment (C) comprises a scaly pigment.
5. 5. The coating composition according to claim 4, wherein the scaly pigment is at least one selected from the group consisting of talc, mica, kaolin clay, glass flake, micaceous iron oxide, aluminum and metal pigments other than aluminum.
Citation Information
Patent Citations
Material for two-part aqueous Anti-corrosive coating and method for Anti-corrosive coating
JP2009149791A
Two liquid reaction-curable aqueous coating composition for primer, and multilayer film forming method using the same and coated body
JP2018053028A
Two-component epoxy resin paint
JP2019515991A
Aqueous coating material
JP2021001314A
Aqueous coating material
JP2021001315A