Phosphorus-based flame retardants, their products and their manufacturing method
A phosphorus-based flame retardant with a styrene functional group and phosphorus skeleton addresses the need for low dielectric constant and high fire resistance, producing resin sheets with superior dielectric properties for electronic and power equipment applications.
Patent Information
- Application Number
- JP2023152088
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-06-14
- Filing Date
- 2023-09-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-09-20
AI Technical Summary
Traditional flame retardants fail to meet stringent dielectric property requirements in modern applications, necessitating the development of new flame retardants with low dielectric constant and high fire resistance.
A phosphorus-based flame retardant with a styrene functional group and phosphorus skeleton is produced using a specific reaction process, incorporating phenolic functional groups, chloromethylstyrene, and potassium iodide, followed by solvent removal and compression to create a resin sheet with enhanced properties.
The resulting resin sheet exhibits a low dielectric constant and high fire resistance, suitable for electronic products and power equipment, outperforming conventional additives in dielectric performance.
Smart Images

Figure 0007586987000001 
Figure 0007586987000002 
Figure 0007586987000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a flame retardant, a product and a method for producing the same, and more particularly to a phosphorus-based flame retardant, a product and a method for producing the same. [Background technology]
[0002] Flame retardants are chemicals that prevent objects from burning and can be added to products such as building materials, textiles and vehicle interiors to improve their fire resistance.
[0003] Those skilled in the art have been eager to develop a low dielectric reaction retarder as a novel fire-resistant material having both low dielectric constant and high fire resistance. The flame retardant of the present invention can be applied to fields requiring high levels of fire resistance, such as electronic products and power equipment. Summary of the Invention [Problem to be solved by the invention]
[0004] Many countries have relevant fire resistance standards and regulations that require the use of flame retardants to improve the fire resistance of buildings and products. Therefore, the development of new flame retardant technologies has become an important field in today's chemical industry. Traditional flame retardants may not meet the stringent requirements for dielectric properties in the future. [Means for solving the problem]
[0005] The present invention provides a phosphorus-based flame retardant, its product and manufacturing method. The phosphorus-based flame retardant has a novel phosphorus-based flame retardant modified structure, which is a structure consisting of a styrene functional group and a phosphorus skeleton, and has low dielectric constant and high fire resistance.
[0006] The method for producing a phosphorus-based flame retardant of the present invention includes the following steps: A phenolic functional group-containing flame retardant and chloromethylstyrene are added to a reaction tank, and then butanone and potassium iodide are added as solvents and stirred. After stirring, the solvent is discharged and the mixture is placed in an oven to produce a phosphorus-based flame retardant. The phenolic functional group-containing flame retardant has a chemical structure shown in the following formula (1). Chloromethylstyrene has a chemical structure shown in the following formula (2). The phosphorus-based flame retardant has a chemical structure shown in the following formula (3) or formula (4). [ka] In formula (1), X is H, OH, F, Cl, or Br. When X in formula (1) is H, F, Cl, or Br, the resulting phosphorus-based flame retardant has the chemical structure shown in formula (3), where Y is H, F, Cl, or Br. When X in formula (1) is OH, the resulting phosphorus-based flame retardant has the chemical structure shown in formula (4).
[0007] In one embodiment of the present invention, the molar ratio of the phenolic functional group-containing flame retardant to chloromethylstyrene is 0.1-5.
[0008] In one embodiment of the present invention, the amount of the solvent added is 100 phr to 200 phr, based on the total weight of the phenolic functional group-containing flame retardant and chloromethylstyrene.
[0009] In one embodiment of the present invention, the amount of potassium iodide added is 1 phr to 10 phr, based on the total weight of the phenolic functional group-containing flame retardant and chloromethylstyrene.
[0010] In one embodiment of the present invention, the stirring speed is 60 rpm to 600 rpm, the stirring time is 12 hours to 48 hours, and the stirring temperature is 50°C to 90°C.
[0011] In one embodiment of the present invention, the oven temperature is 80° C. to 120° C., and the storage time in the oven is 1 hour to 6 hours.
[0012] The phosphorus-based flame retardant of the present invention is produced by the above-mentioned method for producing a phosphorus-based flame retardant. The phosphorus-based flame retardant has a chemical structure shown in the following formula (3) or formula (4). [ka] In formula (3), Y is H, F, Cl, or Br. [ka]
[0013] The product of the present invention comprises the above-mentioned phosphorus-based flame retardant. The product includes a resin sheet.
[0014] The manufacturing method of the product of the present invention includes the following steps: Use butanone as a solvent, stir the above phosphorus-based flame retardant and crosslinking accelerator, and put into a vacuum oven to remove the solvent to obtain a mixture; Crush the mixture, fill it into a mold, and compress it in a hot press to manufacture a product; The crosslinking accelerator contains peroxide, the peroxide contains Luf, and the product contains a resin sheet.
[0015] In one embodiment of the present invention, the weight ratio of the phosphorus-based flame retardant to the crosslinking accelerator is 50-500.
[0016] In one embodiment of the present invention, the amount of the solvent added is 100 phr to 200 phr based on the total weight of the phosphorus-based flame retardant and the crosslinking accelerator.
[0017] In one embodiment of the present invention, the stirring speed is 40 rpm to 400 rpm, the stirring time is 0.5 hours to 2 hours, and the stirring temperature is 50°C to 75°C.
[0018] In one embodiment of the present invention, the oven temperature is 80° C. to 120° C., and the storage time in the oven is 1 hour to 6 hours.
[0019] In one embodiment of the present invention, the compression time of the hot press is 1 hour to 6 hours, and the temperature is 150°C to 300°C.
[0020] The compressed resin sheet needs to meet the specifications of thickness 0.3 μm to 1.3 μm and square dimensions 3 cm to 13 cm for subsequent dielectric constant measurements. Effect of the Invention
[0021] Based on the above, the present invention provides a phosphorus-based flame retardant, a product and a method for producing the same. The phosphorus-based flame retardant has a novel phosphorus-based flame retardant modified structure, which is a structure consisting of a styrene functional group and a phosphorus skeleton. Unlike conventional additives, the flame retardant of the present invention can be regarded as a reactive flame retardant resin with both low dielectric constant and high fire resistance, and can be applied to fields requiring high levels of fire resistance, such as electronic products and power equipment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, embodiments of the present invention will be described in detail, but these embodiments are merely examples and the present invention is not limited thereto.
[0023] In this specification, the ranges indicated as "a certain value to another value" are general expressions to avoid listing all the values in the range one by one. Thus, the description of a specific numerical range includes any numerical value within that numerical range and any smaller numerical range defined by any numerical value within that numerical range, and the same applies to any numerical value and any smaller numerical range explicitly described in the specification.
[0024] The method for producing a phosphorus-based flame retardant of the present invention includes the following steps: A phenolic functional group-containing flame retardant and chloromethylstyrene are added to a reaction vessel, and butanone and potassium iodide as a solvent are added and stirred. After stirring, the solvent is discharged and the vessel is placed in an oven to produce a phosphorus-based flame retardant. The phenolic functional group-containing flame retardant has a chemical structure shown in the following formula (1). Chloromethylstyrene has a chemical structure shown in the following formula (2). The phosphorus-based flame retardant has a chemical structure shown in the following formula (3) or formula (4). [ka] In formula (1), X is H, OH, F, Cl, or Br. When X in formula (1) is H, F, Cl, or Br, the resulting phosphorus-based flame retardant has the chemical structure shown in formula (3), where Y is H, F, Cl, or Br. When X in formula (1) is OH, the resulting phosphorus-based flame retardant has the chemical structure shown in formula (4).
[0025] In this embodiment, the molar ratio of the phenolic functional group-containing flame retardant to chloromethylstyrene is, for example, 0.1 to 5. The amount of the solvent added relative to the total weight of the phenolic functional group-containing flame retardant and chloromethylstyrene is, for example, 100 phr to 200 phr, and the amount of potassium iodide added is, for example, 1 phr to 10 phr. The stirring speed is, for example, 60 rpm to 600 rpm, the stirring time is, for example, 12 hours to 48 hours, and the stirring temperature is, for example, 50°C to 90°C. The oven temperature is, for example, 80°C to 120°C, and the storage time in the oven is, for example, 1 hour to 6 hours.
[0026] The present invention also provides a phosphorus-based flame retardant produced by the above-mentioned method for producing a phosphorus-based flame retardant, which has a chemical structure represented by the following formula (3) or (4). [ka] In formula (3), Y is H, F, Cl, or Br. [ka]
[0027] The present invention also provides a product comprising the above phosphorus-based flame retardant, which may include a resin sheet such as a 5G high-frequency board, but the present invention is not limited thereto.
[0028] The method for producing the product of the present invention includes the following steps: Use butanone as a solvent, stir the phosphorus-based flame retardant and crosslinking accelerator, and place in a vacuum oven to remove the solvent to obtain a mixture. The mixture is crushed and filled into a mold, and compressed by a hot press to produce a product. The crosslinking accelerator may include a peroxide, the peroxide may include Luf, and the product may include a resin sheet such as a 5G high-frequency board.
[0029] In this embodiment, the weight ratio of the phosphorus-based flame retardant to the crosslinking accelerator is, for example, 50 to 500. The amount of the solvent added relative to the total weight of the phosphorus-based flame retardant and the crosslinking accelerator is 100 phr to 200 phr. The stirring speed is, for example, 40 rpm to 400 rpm, the stirring time is, for example, 0.5 hours to 2 hours, and the stirring temperature is, for example, 25°C to 75°C. The oven temperature is, for example, 80°C to 120°C, and the storage time in the oven is, for example, 1 hour to 6 hours. The compression time of the hot press is, for example, 1 hour to 6 hours, and the temperature is, for example, 150°C to 300°C.
[0030] The phosphorus-based flame retardant and its product of the present invention will be described in detail below with reference to examples, although the present invention is not limited to the following examples.
[0031] Working Example
[0032] The following examples are provided to demonstrate that the phosphorus-based flame retardant of the present invention enables a resin sheet product to have both a low dielectric constant and high fire resistance.
[0033] Test Method
[0034] Dielectric constant Dk: The dielectric constant Dk at a frequency of 10 GHz was tested using a dielectric analyzer HP Agilent E4991A.
[0035] Dielectric loss Df: The dielectric loss Df at a frequency of 10 GHz was tested using a dielectric analyzer HP Agilent E4991A.
[0036] Preparation, testing and evaluation of phosphorus-based flame retardants and their products
[0037] Example 1
[0038] 1 mole of a phenolic functional group-containing flame retardant having a chemical structure shown in formula (1) and 2.5 moles of chloromethylstyrene were added to a reaction vessel. Next, butanone and potassium iodide as a solvent were added and stirred at 80°C for 24 hours. After stirring, the solvent was discharged and placed in an oven. The temperature of the oven was 100°C. After confirming that the solvent was removed, a phosphorus-based flame retardant having a chemical structure shown in formula (3) was produced. Next, 25 grams of the obtained phosphorus-based flame retardant and 0.25 grams of a crosslinking accelerator Luf were stirred for 30 minutes using butanone as a solvent, and then placed in a vacuum oven at 100°C for 3 hours to remove the solvent and obtain a mixture. Next, this mixture was crushed, filled into a mold, and compressed at 200°C for 2 hours using a hot press to produce a resin sheet.
[0039] Example 2
[0040] Basically, the preparation conditions and methods of the phosphorus-based flame retardant and its product are the same as those in Example 1. The difference is that in Example 2, the phenolic functional group-containing flame retardant has the chemical structure shown in formula (1), where X in formula (1) is OH. Therefore, the phosphorus-based flame retardant produced has the chemical structure shown in formula (4).
[0041] Comparative Example 1
[0042] Basically, the preparation conditions and methods of the phosphorus-based flame retardant and its product are the same as those in Example 1. The difference is that the phenolic functional group-containing flame retardant having the chemical structure shown in formula (1) and chloromethylstyrene are replaced with a flame retardant having the chemical structure shown in formula (5) and a commercial product Noryl SA9000 SABIC having the chemical structure shown in formula (6), respectively. [ka]
[0043] Comparative Example 2
[0044] Basically, the preparation conditions and methods of the phosphorus-based flame retardant and its product are the same as those of Comparative Example 1. The difference is that the flame retardant having the chemical structure shown in formula (5) is replaced with a flame retardant having the chemical structure shown in formula (7). [ka]
[0045] Comparative Example 3
[0046] Basically, the preparation conditions and methods of the phosphorus-based flame retardant and its product are the same as those of Comparative Example 1. The difference is that the flame retardant having the chemical structure shown in formula (5) is replaced with the flame retardant having the chemical structure shown in formula (8). [ka]
[0047] The test results of Example 1, Example 2, and Comparative Examples 1 to 3 are shown in Table 1 below. Under the same reaction preparation conditions, it can be seen that in Example 1 and Example 2, the phosphorus-based flame retardant consisting of the phenolic functional group-containing flame retardant of the present invention and chloromethylstyrene has a structure consisting of a styrene functional group and a phosphorus skeleton, and therefore has both a low dielectric constant and high fire resistance. In contrast, it can be seen that Comparative Examples 1 to 3, which use the conventional DOPO flame retardant, cannot react with existing resins and have the disadvantage of being inferior in dielectric constant and dielectric loss.
[0048] [Table 1]
[0049] In summary, the present invention provides a phosphorus-based flame retardant, its product and manufacturing method. The phosphorus-based flame retardant has a novel phosphorus-based flame retardant modified structure, which is a structure consisting of a styrene functional group and a phosphorus skeleton. Unlike conventional additives, the flame retardant of the present invention can be considered as a reactive flame retardant resin with both low dielectric constant and high fire resistance. The resin sheet product has a dielectric constant (@10GHz) of less than 3.0 / a and a dielectric loss (@10GHz) of less than 0.0080, which is superior to conventional flame retardants (dielectric constant (@10GHz) greater than 3.0 / dielectric loss (@10GHz) greater than 0.0100), and can be applied in fields requiring high levels of fire resistance, such as electronic products and power equipment. [Industrial Applicability]
[0050] The phosphorus-based flame retardant of the present invention can be applied to fields requiring a high level of fire resistance, such as electronic products and power equipment.
Claims
1. Adding a phenolic functional group-containing flame retardant and chloromethylstyrene to a reaction vessel, adding butanone and potassium iodide as a solvent, and stirring; After stirring, the solvent is discharged and placed in an oven to produce a phosphorus-based flame retardant; The phenolic functional group-containing flame retardant has a chemical structure shown in the following formula (1), the chloromethylstyrene has a chemical structure shown in the following formula (2), and the phosphorus-based flame retardant has a chemical structure shown in the following formula (3) or formula (4). 【Chemical 1】 In formula (1), X is H, OH, F, Cl, or Br; When X in formula (1) is H, F, Cl, or Br, the resulting phosphorus-based flame retardant has a chemical structure shown in formula (3), in which Y is H, F, Cl, or Br, When X in formula (1) is OH, the resulting phosphorus-based flame retardant has the chemical structure shown in formula (4).
2. 2. The method for producing a phosphorus-based flame retardant according to claim 1, wherein the molar ratio of the phenolic functional group-containing flame retardant to the chloromethylstyrene is 0.1 to 5.
3. 2. The method for producing a phosphorus-based flame retardant according to claim 1, wherein the amount of the solvent added is 100 phr to 200 phr based on the total weight of the phenolic functional group-containing flame retardant and the chloromethylstyrene.
4. 2. The method for producing a phosphorus-based flame retardant according to claim 1, wherein the amount of potassium iodide added is 1 phr to 10 phr based on the total weight of the phenolic functional group-containing flame retardant and the chloromethylstyrene.
5. 2. The method for producing a phosphorus-based flame retardant according to claim 1, wherein the stirring speed is 60 rpm to 600 rpm, the stirring time is 12 hours to 48 hours, and the stirring temperature is 50°C to 90°C.
6. 2. The method for producing a phosphorus-based flame retardant according to claim 1, wherein the oven temperature is 80 to 120°C, and the storage time in the oven is 1 to 6 hours.
7. A phosphorus-based flame retardant having a chemical structure shown in the following formula (3) or formula (4): 【Chemistry 2】 In formula (3), Y is H, F, Cl or Br. 【Chemistry 3】
8. A product comprising the phosphorus-based flame retardant according to claim 7, The article comprises a resin sheet.
9. A method of manufacturing a product, comprising: Stirring the phosphorus-based flame retardant and the crosslinking accelerator according to claim 7 using butanone as a solvent, placing the mixture in a vacuum oven, and removing the solvent to obtain a mixture; grinding the mixture and filling it into a mold, and hot pressing it to produce the product; The method for manufacturing a product, wherein the crosslinking accelerator comprises a peroxide, the peroxide comprises Luf, and the product comprises a resin sheet.
10. The method for manufacturing a product according to claim 9, wherein the weight ratio of the phosphorus-based flame retardant to the crosslinking accelerator is 50 to 500.
11. The method for manufacturing a product according to claim 9, wherein the amount of the solvent added is 100 phr to 200 phr based on the total weight of the phosphorus-based flame retardant and the crosslinking accelerator.
12. 10. The method for producing the product of claim 9, wherein the stirring speed is 40 rpm to 400 rpm, the stirring time is 0.5 hours to 2 hours, and the stirring temperature is 25°C to 75°C.
13. The method for producing a product according to claim 9, wherein the temperature of the oven is between 80°C and 120°C, and the storage time in the oven is between 1 hour and 6 hours.
14. The method for manufacturing a product according to claim 9, wherein the compression time of the hot press is 1 hour to 6 hours, and the temperature is 150°C to 300°C.
Citation Information
Patent Citations
Triarylphosphine oxide derivative having fluorine- containing alkyl group and method for producing the same
JP2002212194A
Functional organic phosphorus compound and its manufacturing method
JP2006001876A
Use of hydroxyphenylphosphine oxide mixtures and their flame retardants for epoxy resins
JP2013500272A
Flame retardant, composite flame retardant, flame retardant antistatic composition, and method of flame resistance
JP2018021175A
Halogen-free flameproofing agent and method for flameproofing fiber by using the same
WO2008047897A1