How iron ore is processed
A poly(meth)acrylic acid-based thickener in an O/W emulsion addresses the mixing challenges of polyacrylamide flocculants, effectively preventing iron ore slurry formation and improving transportation stability with reduced environmental impact.
Patent Information
- Application Number
- JP2020048004
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-18
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-03-18
AI Technical Summary
Existing polyacrylamide-based flocculants used for suppressing iron ore slurry formation are difficult to mix uniformly due to gelling when diluted with water, leading to increased water content and reduced effectiveness.
Application of a poly(meth)acrylic acid-based thickener in the form of an O/W emulsion to iron ore, which adsorbs to particle surfaces and agglomerates particles under neutral to alkaline conditions, maintaining low viscosity and facilitating uniform mixing.
The method effectively suppresses iron ore slurry formation, enhances transportation stability, and reduces environmental impact by avoiding nitrogen oxide generation during sintering, while being cost-effective and easy to apply.
Smart Images

Figure 0007587102000001 
Figure 0007587102000002 
Figure 0007587102000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for processing iron ore. [Background technology]
[0002] After being extracted from a mine, iron ore is transported by transportation means (cargo ships, freight trains, trucks, etc.). Iron ore has a low water retention capacity, and when it is unloaded from a ship, the water in it causes it to turn into a slurry, which can stick to conveyor belts and make transportation difficult, or the piles in the yard can collapse due to rain.
[0003] As a method for solving the above problems, a method is known in which a chemical is applied to the iron ore to agglomerate the iron ore particles.
[0004] For example, Patent Document 1 discloses a "method for granulating coal and / or iron ore slurry, comprising adding a W / O type emulsion of an acrylic acid-based and / or acrylamide-based polymer to a coal and / or iron ore slurry and mixing the mixture."
[0005] Furthermore, Patent Document 2 discloses a method for lifting moist bulk materials such as ore and coal from a cargo ship using a bridge crane or an unloader's grab bucket, which, if suspended spring water containing suspended powder is generated during the lifting operation, comprises adding a polymer flocculant to the location where the suspended spring water is generated to cause the particles to coagulate and aggregate, and mixing the bulk materials in the vicinity of this location or in other locations before lifting the material.
[0006] Furthermore, Patent Document 3 discloses a method for treating moist bulk materials, such as ores and coals containing moisture, which comprises the steps of: loading moist bulk materials such as ores and coals onto a ship via a conveyor belt; adding a flocculant diluted to a mass ratio (water / flocculant) of 20 to 200 to the moist bulk materials on the conveyor belt and / or at a junction of the conveyor belt, thereby adhering the flocculant to the moist bulk materials. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 5927807 [Patent Document 2] Patent No. 5910810 [Patent Document 3] Patent No. 6505668 Summary of the Invention [Problem to be solved by the invention]
[0008] Patent Documents 1 to 3 disclose the use of a polyacrylamide-based flocculant (a polyacrylamide-based W / O type emulsion) as a drug. In polyacrylamide-based flocculants, the polymer components of the agent are adsorbed to the particle surface by electrostatic force or hydrogen bonds, and the polymers become entangled and flocculate the particles. The agent is applied on the belt conveyor or its junction, but since the amount applied is very small (about 0.05 to 0.5% by mass of the ore), it is considered effective to dilute the agent to lower its viscosity in order to mix it uniformly.
[0009] However, in reality, polyacrylamide-based flocculants are W / O emulsions in which polyacrylamide-based polymers are dispersed in oil, and when water is added, they gel and become difficult to mix. Therefore, in order to add water to the flocculant to reduce its viscosity, it is necessary to dilute it by 50 times or more by mass. In this case, the addition of water used for dilution increases the water content relative to the ore, which reduces the effectiveness of the agent.
[0010] In addition, polyacrylamide-based flocculants gel the moment they come into contact with the moisture contained in the iron ore, making it difficult for the agent to penetrate into the interior of the iron ore, which is also another reason why uniform mixing is difficult.
[0011] For this reason, the effect of polyacrylamide-based flocculants in inhibiting the formation of a slurry of iron ore is currently insufficient.
[0012] Therefore, an object of the present invention is to provide a method for treating iron ore which is highly effective in suppressing the formation of a slurry of iron ore. [Means for solving the problem]
[0013] The means for solving the problems include the following aspects. <1> A method for treating iron ore, comprising adding a poly(meth)acrylic acid-based thickener, which is an O / W type emulsion in which a poly(meth)acrylic acid-based polymer is dispersed in water, to iron ore containing moisture, thereby agglomerating the iron ore particles in the iron ore. <2> The poly(meth)acrylic acid-based thickener is applied to the iron ore before the iron ore is loaded onto a ship. <1> 2. A method for treating iron ore according to claim 1. <3> The amount of the poly(meth)acrylic acid-based thickener applied is an amount such that the poly(meth)acrylic acid-based polymer is 0.002 to 0.02 parts by mass relative to 100 parts by mass of the iron ore. <1> or <2> 2. A method for treating iron ore according to claim 1. <4> In the poly(meth)acrylic acid-based thickener, the mass ratio of the water to the poly(meth)acrylic acid-based polymer (water / poly(meth)acrylic acid-based polymer) is 5 or more and less than 20. <1> ~ <3> 13. The method for treating iron ore according to claim 12. Effect of the Invention
[0014] According to the present invention, a method for treating iron ore that is highly effective in inhibiting the iron ore from becoming a slurry can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described as an example. In this specification, unless otherwise specified, a numerical range expressed using "to" means a range including the numerical values before and after "to" as the lower and upper limits. Thus, for example, 0.65 to 1.50% means a range of 0.65% or more and 1.50% or less. Unless otherwise specified, "%" in the composition of a component means % by mass.
[0016] The iron ore processing method according to this embodiment is a method for processing iron ore in which a poly(meth)acrylic acid-based thickener, which is an O / W type emulsion in which a poly(meth)acrylic acid-based polymer is dispersed in water, is added to iron ore containing moisture, thereby agglomerating iron ore particles in the iron ore.
[0017] The iron ore processing method according to the present embodiment is a method for processing iron ore that has a high effect of suppressing the formation of a slurry of the iron ore, for the following reasons.
[0018] When a poly(meth)acrylic acid-based thickener is applied to iron ore, the polyacrylic acid-based polymer is adsorbed onto the surface of the iron ore particles or released when the iron ore is hydrated, and the polyacrylic acid-based polymer associates with the iron ore particles under neutral to alkaline conditions, causing the iron ore particles to aggregate. In other words, since the pH of the water contained in the iron ore is neutral to weakly alkaline, the iron ore particles aggregate simply by applying a poly(meth)acrylic acid-based thickener to the iron ore. The aggregation of the iron ore particles causes the iron ore to thicken, suppressing the formation of a slurry.
[0019] Moreover, since the poly(meth)acrylic acid-based thickener is an O / W type emulsion, it is unlikely to gel even when it comes into contact with the water contained in the iron ore. Even if the poly(meth)acrylic acid-based thickener is diluted with water to reduce the viscosity, it is unlikely to gel. Therefore, the poly(meth)acrylic acid-based thickener can be easily applied uniformly to the iron ore.
[0020] From the above, the iron ore processing method according to this embodiment has a high effect of suppressing the slurrying of the iron ore. By suppressing the formation of a slurry in the iron ore, the iron ore is prevented from collapsing even if it rains after it is piled up in a yard, and the belt conveyor is also prevented from becoming difficult to transport.
[0021] In addition, polyacrylamide-based flocculants have a short lifetime (gelling in about 1 to 6 months) and contain nitrogen, which causes NOx emissions when iron ore is sintered, whereas poly(meth)acrylic acid-based thickeners have a long lifetime (about 2 years) and do not contain nitrogen, so no NOx emissions are generated when iron ore is sintered. Furthermore, while the polyacrylamide-based flocculant is a W / O type emulsion, the poly(meth)acrylic acid-based thickener is an O / W type emulsion, and the solvent is water. Therefore, the iron ore processing method according to this embodiment is an environmentally friendly processing method.
[0022] In addition, since poly(meth)acrylic acid-based thickeners are O / W type emulsions, they have a lower viscosity than W / O type emulsions. Specifically, for example, W / O emulsions usually have a viscosity of 500 to 2000 mPa·s, whereas O / W emulsions have a viscosity of 500 mPa·s or less. In addition, since poly(meth)acrylic acid-based thickeners exhibit thixotropic viscosity, their viscosity tends to decrease when diluted with water, and they are easily mixed uniformly with water. Therefore, even if the poly(meth)acrylic acid-based thickener contains a small amount of poly(meth)acrylic acid-based polymer, the slurry formation suppression effect is high, which is advantageous in terms of cost.
[0023] Hereinafter, the iron ore processing method according to this embodiment will be described in detail.
[0024] (Iron Ore) The iron ore to which the thickener is applied is iron ore containing moisture. Examples of the iron ore include PFFT (Brazilian fine ore), Minas Rio, AMMC (Canadian fine ore), San Marco, Metalloinvest, Northland, and other fine ores; Carajas, and other ores. These iron ores have a small specific surface area, so they have low water retention and are prone to forming a slurry due to the impregnated water.
[0025] Here, the iron ore containing moisture is, for example, iron ore containing 10 to 20% by mass of moisture relative to the iron ore. When the (meth)acrylic acid-based thickener is applied to iron ore containing more than 20% by mass of water, the iron ore may not be sufficiently aggregated, and sufficient effects may not be obtained. Therefore, it is more preferable to apply the thickener to iron ore containing 12 to 18% by mass of water.
[0026] (Poly(meth)acrylic acid-based thickener) Poly(meth)acrylic acid-based thickeners are O / W type emulsions in which poly(meth)acrylic acid-based polymers are dispersed in water.
[0027] A poly(meth)acrylic acid polymer is a copolymer containing structural units derived from (meth)acrylic acid and / or (meth)acrylic acid ester monomers, where (meth)acrylic acid refers to acrylic acid and / or methacrylic acid. Examples of the (meth)acrylic acid ester include (meth)acrylic acid esters having a linear, branched, or cyclic alkyl group having 1 to 24 carbon atoms. Specific examples of (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, icosyl (meth)acrylate, henicosyl (meth)acrylate, docosyl (meth)acrylate, octadecenyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, and benzyl (meth)acrylate. Among these, from the viewpoint of suppressing the formation of a slurry of iron ore, the (meth)acrylic acid ester is preferably a (meth)acrylic acid ester having a linear or branched alkyl group having 1 to 12 carbon atoms (e.g., ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, butyl methacrylate, etc.), and particularly preferably ethyl acrylate.
[0028] The structural units of the poly(meth)acrylic acid polymer may contain structural units derived from copolymerizable monomers such as vinyl carboxylate monomers, styrene monomers, hydroxyl group-containing monomers, amide group-containing monomers, and cyano group-containing monomers, in addition to structural units derived from (meth)acrylic acid and / or (meth)acrylic acid ester monomers. However, it is preferable that the poly(meth)acrylic acid-based polymer contains 70 mass % (80 mass % or more, or 90 mass % or more) of structural units derived from (meth)acrylic acid and / or (meth)acrylic acid ester monomers.
[0029] The weight average molecular weight of the poly(meth)acrylic acid polymer is preferably from 500,000 to 10,000,000, and more preferably from 1,000,000 to 500, from the viewpoint of suppressing the formation of a slurry of iron ore. The weight average molecular weight is a value measured by gel permeation chromatography (GPC).
[0030] The viscosity of the poly(meth)acrylic acid-based thickener is preferably from 1 to 500 mPa·s, and more preferably from 1 to 100 mPa·s, from the viewpoint of suppressing the formation of a slurry of the iron ore. The viscosity is a value measured at 25°C.
[0031] (Position of poly(meth)acrylic acid-based thickener) The location where the poly(meth)acrylic acid-based thickener is applied is not particularly limited, but examples include raw material yards for iron ore, storage sites (loading points, etc.), during transportation by ship or truck, when unloading from a ship, and during transport on a conveyor belt. In particular, in order to further suppress the slurrying of iron ore, it is more effective to add the thickener at a loading port overseas, for example, during belt conveyor transport at a mine or port, during loading or unloading, before loading onto a ship, rather than adding the thickener at the time of domestic unloading. In other words, it is preferable to add the poly(meth)acrylic acid-based thickener to the iron ore before loading onto a ship. The reasons are as follows.
[0032] When iron ore contains moisture, the moisture moves toward the bottom of the ship during sea transport and accumulates, turning it into a slurry. When unloading, the water must be pumped up to extract the slurried iron ore, which reduces work efficiency (i.e., impedes unloading). Slurried iron ore is also likely to fall off the conveyor belt during transportation. For this reason, it is more advantageous to apply a thickening agent to the ore at the loading port in advance to prevent the iron ore from turning into a slurry. In addition, slurried iron ore on board the ship is prone to flow and tends to accumulate on one side of the ship's hold, causing the ship to lose its balance and, in the worst case, capsize. By applying a thickening agent to the iron ore at the loading port to prevent the iron ore from turning into a slurry, such situations can be avoided.
[0033] (Method of adding poly(meth)acrylic acid-based thickener) The method of applying the poly(meth)acrylic acid-based thickener is not particularly limited, but examples thereof include a method of spraying the thickener in a shower-like manner on a belt conveyor or at a junction of a belt conveyor when loading at a loading port or unloading at a discharging port, or a method of pouring the thickener in a straight rod-like manner from a faucet. If possible, it is desirable to mix the thickener with the iron ore while mechanically stirring the iron ore during storage or preservation.
[0034] (Amount of poly(meth)acrylic acid-based thickener added) From the viewpoint of suppressing the slurrying of the iron ore, the amount of the poly(meth)acrylic acid-based thickener added is preferably 0.0005 to 0.04 parts by mass, and more preferably 0.002 to 0.02 parts by mass, of the poly(meth)acrylic acid-based polymer per 100 parts by mass of the iron ore.
[0035] Here, the poly(meth)acrylic acid-based thickener can also be used as is in the form of a stock solution having a solids concentration (that is, poly(meth)acrylic acid-based polymer concentration) of 20 to 40% by mass. However, from the viewpoint of uniformly applying the thickener to the iron ore, it is preferable to dilute with water so that the mass ratio of water to the poly(meth)acrylic acid-based polymer (water / poly(meth)acrylic acid-based thickener) is 5 or more and less than 20 (preferably 5 or more and 10 or less). If the mass ratio is 20 or more, the iron ore may contain too much water, which may reduce the effect of suppressing the slurrying of the iron ore. EXAMPLES
[0036] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0037] Example 1 The cohesiveness was evaluated by a method simulating a slump flow test for evaluating the fluidity of concrete, etc. (hereinafter, referred to as the crumbling property confirmation test). The iron ore used was PFFT, a finely powdered ore, and the chemical used was an O / W type emulsion thickener (Acryset, manufactured by Nippon Shokubai Co., Ltd.), in which a polyacrylic acid polymer is dispersed in water. The solids concentration of the chemical (polyacrylic acid polymer concentration) was 30% by mass (water / polyacrylic acid polymer (solids) mass ratio was 2.33).
[0038] First, water was added to the dried PFFT so that the moisture content was 15% by mass and mixed. 200 g of iron ore after moisture adjustment was placed in a 250 cc plastic bottle. After adding 0.008% by mass of thickener as a solid concentration (polyacrylic acid-based polymer concentration) to 100 parts by mass of iron ore, the bottle was covered and mixed by rotating up and down 5 times. An acrylic tube with an inner diameter of 25 mm and a height of 50 mm was placed on a stainless steel flat plate, and the mixed sample was filled to the top, and then the tube was removed. After leaving it for 1 minute, the height of the sample was measured. The higher the height after the tube was removed, the higher the cohesiveness and the better the agent was evaluated to be in terms of its ability to retain its original shape. As a result of this test, even when the acrylic tube was removed, there was only a slight deformation of the shape, and the height was 49 mm, which was a good result.
[0039] Comparative Example 1 A W / O emulsion type flocculant (Rockmaster manufactured by Hymo Co., Ltd.), in which a polyacrylamide polymer is dispersed in a hydrocarbon solvent, was used as the chemical agent, and a crumbling confirmation test was conducted in the same manner as in Example 1. The solids concentration (polyacrylamide polymer concentration) of the flocculant was 40 mass%, and the flocculant was added at a solids concentration (polyacrylamide polymer concentration) of 0.008 mass% per 100 mass parts of iron ore. After the tube was pulled out, the shape collapsed, the height decreased to 35 mm, and the flocculation properties were weak.
[0040] (Examples 2 to 12, Comparative Examples 2 to 10) The iron ore used was PFFT, and the chemical used was the O / W emulsion thickener used in Example 1 (Acryset manufactured by Nippon Shokubai Co., Ltd., solids concentration (polyacrylic acid-based polymer concentration) 30% by mass) or the W / O emulsion flocculant used in Comparative Example 1 (Lockmaster manufactured by Hymo Co., Ltd., solids concentration (polyacrylamide-based polymer concentration) 40% by mass). Then, the moisture content in the iron ore and the solids concentration of the agent were changed, and a crumbling confirmation test was carried out in the same manner as in Example 1 and Comparative Example 1, and the height was measured. The results are shown in Table 1 for Examples 2 to 12 and Comparative Examples 2 to 10. In the table, the type of chemical is recorded as "thickener" for the O / W emulsion thickener (Acryset, manufactured by Nippon Shokubai Co., Ltd.) and "flocculant" for the W / O emulsion flocculant (Lockmaster, manufactured by Hymo Co., Ltd.). The evaluation was as follows: ◯ (excellent) for heights of 47 mm or more, △ (passable) for heights of less than 47 mm or 42 mm or more, and × (unacceptable) for heights of less than 42 mm. In Examples 2 to 12, which used poly(meth)acrylic acid-based thickeners, evaluation results of △ or ◯ were obtained even with relatively small amounts of agent applied, whereas in Comparative Examples 2, 3, and 5 to 10, which did not apply the agent or used a polyacrylamide-based flocculant, the coagulation of the iron ore particles was weak, the shape was distorted, and the evaluation was ×. In addition, in order to obtain good results using a polyacrylamide-based flocculant, it is necessary to significantly increase the amount of agent applied, as exemplified in Comparative Example 4, which increases costs and also causes environmental problems such as an increase in the amount of organic solvent.
[0041] [Table 1]
[0042] (Examples 13 to 15, Comparative Examples 16 to 19) Carajas iron ore was used as the iron ore, and after sieving to reduce the particle size to 5 mm or less, water was added to adjust the moisture content to 14%, and a test was conducted to confirm the ease of crumbling. The chemicals used were the O / W emulsion thickener used in Example 1 (Acryset, manufactured by Nippon Shokubai Co., Ltd., solids concentration (polyacrylic acid-based polymer concentration) 30% by mass) or the W / O emulsion flocculant used in Comparative Example 1 (Lockmaster, manufactured by Hymo Co., Ltd., solids concentration (polyacrylamide-based polymer concentration) 40% by mass).
[0043] 500g of iron ore with adjusted moisture content was placed in a 500cc plastic bottle. After adding the prescribed amount of the agent, the bottle was closed and mixed by rotating the bottle upside down 5 times. An acrylic tube with an inner diameter of 60mm and a height of 100mm was placed on a stainless steel flat plate and filled to the brim with the mixed sample, after which the tube was removed. After leaving it for 1 minute, the height of the sample was measured. The lower the height of the tube after it was removed, the better the agent, with higher cohesiveness and ability to retain its original shape. The results are shown in Table 2 for Examples 13 to 15 and Comparative Examples 16 to 19. In the table, the type of chemical is recorded as "thickener" for the O / W emulsion thickener (Acryset, manufactured by Nippon Shokubai Co., Ltd.) and "flocculant" for the W / O emulsion flocculant (Lockmaster, manufactured by Hymo Co., Ltd.). The evaluation was made as follows: ◯ (excellent) for a height of 90 mm or more, △ (passable) for a height of less than 90 mm or 80 mm or more, and × (unacceptable) for a height of less than 80 mm. In Examples 13 to 15, in which a polyacrylic acid-based thickener was used, an evaluation result of △ or ◯ was obtained even with a relatively small amount of agent applied, whereas in Comparative Examples 16 to 19, in which no agent was applied or a polyacrylamide-based flocculant was used, the agent was not mixed uniformly, the particle aggregation was weakened, and the shape was lost, resulting in an evaluation of ×.
[0044] [Table 2]
[0045] (Examples 16 to 20, Comparative Examples 20 to 25) Carajas ore that had been sieved to a particle size of 5 mm or less and had a moisture content adjusted to 14 mass % was used as the iron ore, and a crumbling test similar to that in Example 14 was conducted. The agent used was the O / W emulsion thickener used in Example 1 (Acryset, manufactured by Nippon Shokubai Co., Ltd., solids concentration (polyacrylic acid polymer concentration) 30% by mass). In order to further improve the diffusibility of the thickener, the thickener was diluted with water and then added to the iron ore so that the mass ratio of water to polyacrylic acid polymer (water / polyacrylic acid polymer=solids mass ratio (water / solids)) was a predetermined ratio. The results are shown in Examples 16 to 20 in Table 3. The evaluation was made as follows: a height of 90 mm or more was ◯ (excellent), a height of less than 90 mm or 80 mm or more was △ (passable), and a height of less than 80 mm was × (unacceptable). By diluting the thickener, it was possible to mix the thickener more uniformly and reduce deformation, but if the dilution rate was too high, the moisture content in the iron ore increased, causing some deformation and a decrease in height. For comparison, the W / O emulsion type flocculant used in Comparative Example 1 (Lockmaster manufactured by Hymo Co., Ltd., solids concentration (polyacrylamide polymer concentration) 40% by mass) was used and was diluted with water before being added to the iron ore so that the mass ratio of water to polyacrylamide polymer (water / polyacrylamide polymer=solids mass ratio (water / solids)) became a specified ratio. The results are shown in Comparative Examples 20 to 25 in Table 3. In Comparative Examples 20 to 24, when water was added to the flocculant, the flocculant gelled, and it was not possible to mix uniformly, resulting in poor flocculation. In Comparative Example 25, the agent became fluid, but the viscosity was high, and the non-uniformity of the mixed state was not improved. In addition, the water content in the iron ore increased, causing significant deformation and a small height, which was unsuitable.
[0046] [Table 3]
Claims
1. A method for treating iron ore, comprising the steps of: adding a polyacrylic acid-based thickener, which is an O / W emulsion in which a polyacrylic acid-based polymer having a weight-average molecular weight of 500,000 to 10,000,000 is dispersed in water and which does not contain a polymethacrylic acid-based polymer, to iron ore containing moisture, thereby flocculating iron ore particles in the iron ore.
2. 2. The method of claim 1, wherein the polyacrylic thickener is applied to the iron ore before the iron ore is loaded onto a ship.
3. The method for treating iron ore according to claim 1 or 2, wherein the amount of the polyacrylic acid-based thickener applied is an amount such that the polyacrylic acid-based polymer is 0.002 to 0.02 parts by mass per 100 parts by mass of the iron ore.
4. The method for treating iron ore according to any one of claims 1 to 3, wherein in the polyacrylic acid-based thickener, a mass ratio of the water to the polyacrylic acid-based polymer (water / polyacrylic acid-based polymer) is 5 or more and less than 20.
Citation Information
Patent Citations
Timing detector for diesel engine
JP1984010810A
cosmetic
JP1984027807A
Pelletizing agent for iron-making and pelletizing method using the agent
JP2002088418A
Pelletizing agent for iron-making raw material and pelletization method using the same
JP2009280849A
Adhesion and jamming prevention method of mineral material
JP2018058017A