Forging die and spline forming method
The forging die and spline forming method maintain consistent back pressure to prevent underfilling and defects by applying back pressure from the front side and extruding from the rear side, ensuring precise spline formation.
Patent Information
- Application Number
- JP2020201131
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-19
- Filing Date
- 2020-12-03
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-12-03
AI Technical Summary
Existing spline forming methods face issues with underfilling due to decreasing back pressure during the forming process, leading to molding defects such as underfilling of the spline tooth pattern.
A forging die and spline forming method that applies back pressure from the front side and extrudes the workpiece from the rear side, using a pin and biasing member to maintain consistent back pressure throughout the spline forming process.
The method ensures consistent back pressure application, preventing underfilling and reducing molding defects like underfilling, while allowing for precise and efficient spline formation.
Smart Images

Figure 0007587121000002 
Figure 0007587121000003 
Figure 0007587121000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a forging die used for forming a spline in a workpiece and a spline forming method. [Background technology]
[0002] Patent Document 1 discloses a forging die in which a punch is inserted from above into a hole to be formed in a workpiece, and a spline is formed on the outer peripheral surface of the workpiece while the hole to be formed, i.e., the workpiece, is stretched downward. A step that decreases in diameter from above to below is arranged on the outer peripheral surface of the punch. According to the forging die of Patent Document 1, the step is utilized to expand the diameter of the hole to be formed, thereby pressing the outer peripheral surface of the workpiece against a spline tooth mold, and forming a spline on the outer peripheral surface of the workpiece.
[0003] However, in the case of the forging die of Patent Document 1, the workpiece is not supported from below during spline forming. Therefore, the pressing force of the punch applied to the workpiece from above is likely to be consumed in elongating the workpiece. On the other hand, the pressing force of the punch is not likely to be consumed in expanding the diameter of the workpiece, i.e., in forming the spline.
[0004] In this regard, Patent Document 2 discloses a spline forming method in which a spline is formed while applying back pressure to a workpiece. According to the spline forming method of Patent Document 2, the pressing force of the punch is likely to be consumed in forming the spline. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-177182 A [Patent Document 2] Japanese Patent Application Publication No. 6-126369 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the spline forming method of Patent Document 2, the back pressure is set to be highest at the start of spline forming. Therefore, the back pressure gradually decreases as spline forming progresses. If the back pressure decreases as spline forming progresses, the filling ability of the workpiece into the spline tooth shape decreases. As a result, underfill is likely to occur in the spline after forming. Therefore, an object of the present invention is to provide a forging die and a spline forming method that are less likely to cause underfill. [Means for solving the problem]
[0007] In order to solve the above problems, the forging die of the present invention is characterized by comprising: a punch that pushes out a workpiece from the rear side; a die having spline teeth that form a spline in the workpiece; a back pressure pin that applies back pressure to the workpiece from the front side; and a biasing member that biases the back pressure pin so that the back pressure does not decrease while the spline is being formed.
[0008] In order to solve the above problems, the spline forming method of the present invention is a spline forming method in which a spline is formed in a workpiece by applying back pressure to the workpiece from the front side while pushing the workpiece from the rear side and pressing the workpiece against a spline tooth mold, and is characterized in that the back pressure does not decrease during the forming of the spline.
[0009] Here, "front side" refers to the front side in the direction of travel of the punch when the spline is formed. Similarly, "rear side" refers to the rear side in the direction of travel of the punch when the spline is formed. In addition, the form in which "the back pressure does not decrease during the molding of the spline" includes a form in which the back pressure increases during the molding of the spline, a form in which the back pressure is kept constant during the molding of the spline, and a combination of these forms. Effect of the Invention
[0010] According to the forging die and the spline forming method of the present invention, back pressure can be applied to the workpiece until the formation of the spline is completed. Therefore, the filling of the workpiece into the spline tooth shape is not easily reduced. Therefore, molding defects such as underfill are not easily caused. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a vertical cross-sectional view of a forging die according to one embodiment of the present invention in an open state. [Diagram 2] FIG. 2 is a vertical cross-sectional view of the forging die in a closed state. [Diagram 3] FIG. 3 is a composite enlarged view of the area within frame IIIA in FIG. 1 and the area within frame IIIB in FIG. [Figure 4] Fig. 4(A) is an enlarged vertical cross-sectional view of the spline forming method (first stage) of the forging die of this embodiment, and Fig. 4(B) is an enlarged vertical cross-sectional view of the spline forming method (second stage) of the same forging die. [Diagram 5] Fig. 5(A) is a front view of the workpiece before and after the spline forming method is performed, and Fig. 5(B) is a front view of the workpiece after the spline forming method is performed. [Figure 6] FIG. 6 is a schematic diagram showing the relationship between the amount of descent of the back pressure pin and the biasing force of the spring member. [Figure 7] FIG. 7 is an axial cross-sectional view of the workpiece after the spline forming method has been performed. [Figure 8] FIG. 8 is a graph showing the relationship between the wall thickness and the minimum back pressure of each model in the CAE analysis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, embodiments of the forging die and spline forming method of the present invention will be described.
[0013] <Forging die configuration> First, the configuration of the forging die of this embodiment will be described. In the following figures, the upper side corresponds to the "rear side" of the present invention, and the lower side corresponds to the "front side" of the present invention. FIG. 1 shows a vertical cross-sectional view of the forging die of this embodiment in a die-open state. FIG. 2 shows a vertical cross-sectional view of the same forging die in a die-closed state. FIG. 3 shows a composite enlarged view of the inside of frame IIIA in FIG. 1 and the inside of frame IIIB in FIG. 2. As shown in FIGS. 1 to 3, the forging die 1 includes an upper die 2 and a lower die 3. The forging die 1 is for warm forging.
[0014] (upper mold 2) As shown in Figs. 1 to 3, the upper die 2 is a movable die that can move in the vertical direction (uniaxial direction). The upper die 2 includes an upper die holder 20, an upper die sleeve 21, and a punch 22. The upper die sleeve 21 is disposed on the lower surface of the upper die holder 20. The upper die sleeve 21 has a cylindrical shape extending in the vertical direction. A large diameter portion 240 (upper portion) of a shaft portion 24 of a punch 22 (described later) is disposed radially inside the upper die sleeve 21. The shape of the lower end portion of the upper die sleeve 21 is transferred to the upper end portion of the workpiece 9 (described later). That is, the upper die sleeve 21 functions as an upper end forming punch that forms the upper end portion of the workpiece 9.
[0015] The punch 22 includes a head 23 and a shaft 24. The head 23 is embedded in the lower surface of the upper die holder 20. The shaft 24 is press-fitted into a forming hole 90 of the work 9 described later. The shaft 24 includes, from the upper side to the lower side, a large diameter portion 240, a tapered portion 241, and a small diameter portion 242. The large diameter portion 240 protrudes downward from the head 23. The large diameter portion 240 has a coaxial cylindrical shape extending in the vertical direction. The tapered portion 241 has a diameter that decreases from the upper side to the lower side. The small diameter portion 242 has a coaxial cylindrical shape extending in the vertical direction. The small diameter portion 242 has a smaller diameter than the large diameter portion 240. The lower end surface of the small diameter portion 242 has a curved shape that bulges downward.
[0016] (Lower mold 3) The lower die 3 is disposed below the upper die 2. The lower die 3 is a fixed die. The lower die 3 includes a lower die holder 30, a lower die sleeve 31, a sleeve support 32, a die 33, a die support 34, a spring seat 35, a spring member 36, a lifting member 37, a pin seat 38, and a back pressure pin 39.
[0017] The lower die holder 30 has an accommodation hole 300. The accommodation hole 300 penetrates the lower die holder 30 in the up-down direction. The accommodation hole 300 has, from the bottom to the top, a large diameter portion 303, a tapered portion 302, and a small diameter portion 301. The large diameter portion 303 opens at the bottom surface of the lower die holder 30. The tapered portion 302 reduces in diameter from the bottom to the top. The small diameter portion 301 opens at the top surface of the lower die holder 30.
[0018] The spring seat 35 is disposed on the lower surface of the lower die holder 30. The spring seat 35 covers the large diameter portion 303 of the accommodation hole 300 from below. The spring seat 35 has a pin insertion hole 350 formed therein.
[0019] The lifting member 37 includes, from the bottom to the top, a cup portion 370, a flange portion 371, and a tapered portion 372. The cup portion 370 is accommodated in the large diameter portion 303 of the accommodation hole 300. The cup portion 370 has a bottomed cylindrical shape that opens downward. The flange portion 371 is accommodated in the large diameter portion 303 of the accommodation hole 300. The flange portion 371 protrudes radially outward from the upper edge of the cup portion 370. The tapered portion 372 is accommodated in the tapered portion 302 of the accommodation hole 300. The tapered portion 372 is reduced in diameter from the bottom to the top. A pin insertion hole 373 is opened in the tapered portion 372. The pin insertion hole 373 extends in the vertical direction from the upper surface of the tapered portion 372 to the upper bottom surface of the cup portion 370.
[0020] The spring member 36 is a so-called disc spring. The spring member 36 is housed in the large diameter portion 303. The spring member 36 is annularly mounted in the cup portion 370. The spring member 36 is disposed between the spring seat 35 and the flange portion 371. A total of six spring members 36 are stacked in the vertical direction. The upper three spring members 36 and the lower three spring members 36 are arranged in the vertically opposite directions. In the mold open state shown in FIG. 1, an initial load is set to the spring members 36. That is, the spring members 36 are set in a state in which they are contracted in the vertical direction by a predetermined amount (a state in which a biasing force (elastic restoring force) is accumulated) with respect to a natural state (a state in which no load is applied to the spring members 36).
[0021] The pin seat 38 is accommodated in the small diameter portion 301. The pin seat 38 is ring-shaped. The pin seat 38 is disposed on the upper surface of the tapered portion 372. A tapered surface 380 that expands in diameter from the bottom to the top is disposed on the inner peripheral surface of the pin seat 38.
[0022] The die support 34 is disposed on the upper surface of the lower die holder 30. The die support 34 has a cylindrical shape. The die support 34 is disposed above the small diameter portion 301 of the accommodation hole 300, i.e., above the pin seat 38.
[0023] The die 33 is disposed on the upper surface of the die support 34. The die 33 has a cylindrical shape. A plurality of spline teeth 330 are disposed all around the inner peripheral surface of the die 33. The spline teeth 330 extend in the up-down direction.
[0024] The sleeve support 32 is disposed on the upper surface of the lower die holder 30. The sleeve support 32 has a cylindrical shape. The sleeve support 32 is disposed radially outward of the die support .
[0025] The lower sleeve 31 is disposed on the upper surface of the sleeve support 32. The lower sleeve 31 has a cylindrical shape. Inside the lower sleeve 31, from the bottom to the top, a die accommodating section 310 and a forming section 311 are disposed. A die 33 is accommodated in the die accommodating section 310. The forming section 311 has a stepped inner peripheral surface that expands in diameter from the bottom to the top. The inner peripheral surface of the forming section 311 forms the outer peripheral surface of the workpiece 9, which will be described later.
[0026] The back pressure pin 39 is a so-called knockout pin. The back pressure pin 39 includes, from the bottom to the top, a small diameter portion 392, a tapered portion 391, and a large diameter portion 390. The small diameter portion 392 is disposed radially inside the pin insertion hole 350, the pin insertion hole 373, and the cup portion 370. The small diameter portion 392 has a coaxial cylindrical shape extending in the vertical direction. The tapered portion 391 is disposed radially inside the pin seat 38. The tapered portion 391 abuts against the tapered surface 380 of the pin seat 38. The tapered portion 391 expands in diameter from the bottom to the top. The large diameter portion 390 is disposed radially inside the die support 34. The large diameter portion 390 has a coaxial cylindrical shape extending in the vertical direction. The large diameter portion 390 has a larger diameter than the small diameter portion 392.
[0027] The lifting member 37, the pin seat 38, and the back pressure pin 39 are movable up and down relative to the lower die holder 30. The lifting member 37, the pin seat 38, and the back pressure pin 39 are biased upward by the biasing force of the spring member 36.
[0028] <Spline forming method> Next, the spline forming method of this embodiment will be described. FIG. 4(A) shows an enlarged vertical cross-sectional view of the spline forming method (first stage) of the forging die of this embodiment. FIG. 4(B) shows an enlarged vertical cross-sectional view of the spline forming method (second stage) of the same forging die. FIG. 5(A) shows a front view of the work before the spline forming method is performed. FIG. 5(B) shows a front view of the work after the spline forming method is performed. FIG. 6 shows a schematic diagram of the relationship between the lowering amount of the back pressure pin and the biasing force of the spring member. Note that FIG. 4(A) and FIG. 4(B) correspond to frame IIIB (right side part) of FIG. 3. Also, in FIG. 5(A) and FIG. 5(B), the right half of the work 9 is shown in an external view, and the left half is shown in a cross-sectional view.
[0029] By the spline forming method, the workpiece 9 shown in FIG. 5(A) is formed into the workpiece 9 (a rough material of a hollow shaft part with a spline) shown in FIG. 5(B). In the spline forming method, first, the workpiece 9 shown in FIG. 5(A) is set in the lower die 3 shown in FIG. 1. The workpiece 9 is disposed radially inside the lower die sleeve 31, the die 33, and the die support 34. As shown in FIG. 5(A), a hole to be formed 90 is recessed in the upper end surface of the workpiece 9. The hole to be formed 90 extends in the vertical direction. A spline-intended portion 91 is set in the outer peripheral surface of the workpiece 9. As shown in the frame IIIA (left part) of FIG. 3, the spline-intended portion 91 of the workpiece 9 is disposed radially inside the spline tooth die 330. The upper end of the spline-intended portion 91 is disposed below the bottom surface of the hole to be formed 90.
[0030] Next, the upper die 2 is lowered. That is, the forging die 1 is switched from the die open state shown in FIG. 1 to the die closed state shown in FIG. 2. As shown in FIG. 4(A), first, the shaft portion 24 of the punch 22 is inserted into the hole 90 to be formed in the work 9 and descends inside the hole 90 to be formed. The shaft portion 24 reaches the bottom surface of the hole 90 to be formed. As shown in FIG. 4(B), the shaft portion 24 then pushes the hole 90 to be formed, i.e., the work 9, radially outward while extending it downward. Specifically, the curved lower end surface of the small diameter portion 242 expands the diameter of the bottom surface of the hole 90 to be formed while extending it downward. Also, the tapered portion 241 expands the diameter of the inner peripheral surface of the hole 90 to be formed. The work 9 extended downward abuts against the large diameter portion 390 of the back pressure pin 39.
[0031] At the time when the workpiece 9 comes into contact with the back pressure pin 39, the shaft portion 24 of the punch 22 is disposed above the pre-spline portion 91. On the other hand, the back pressure pin 39 is disposed below the pre-spline portion 91. In addition, even before the spline forming method is performed, an upward biasing force is applied to the back pressure pin 39 from the spring member 36 via the lifting member 37 and the pin seat 38. Therefore, the pressing force of the shaft portion 24 of the punch 22 is applied to the pre-spline portion 91 from above, and the back pressure of the back pressure pin 39 (the biasing force of the spring member 36) is applied to the pre-spline portion 91 from below.
[0032] As the shaft portion 24 further descends, the spline portion 91 is compressed in the vertical direction between the shaft portion 24 and the backpressure pin 39. As the shaft portion 24 descends, the pressing force that the shaft portion 24 applies to the spline portion 91 increases. As a result, the backpressure pin 39 descends to a position where it balances with the pressing force. At this time, the spring member 36 is compressed. Therefore, as shown by line L1 in Figure 6, the biasing force of the spring member 36, i.e., the backpressure that the backpressure pin 39 applies to the spline portion 91, gradually increases as the backpressure pin 39 descends.
[0033] As the pressing force and back pressure increase, the material of the spline portion 91 flows radially outward. Thus, as shown in frame IIIB of FIG. 3, the shape of the spline tooth mold 330 is transferred to the spline portion 91. That is, the spline 92 shown in FIG. 5(B) is formed in the spline portion 91 shown in FIG. 5(A). Also, the shape of the lower end of the upper sleeve 21 is transferred to the upper end of the work 9. The shape of the inner peripheral surface of the forming portion 311 of the lower sleeve 31 is transferred to the outer peripheral surface of the work 9. In this way, the work 9 of FIG. 5(A) is formed into the work 9 of FIG. 5(B).
[0034] As shown in box IIIB of Fig. 3, during the execution of the spline forming method, the back pressure pin 39 descends by an amount ΔA from the top dead center A0 to the bottom dead center A1. During the descent of the back pressure pin 39, as shown by line L1 in Fig. 6, the biasing force of the spring member 36 increases from an initial load F0 to a maximum load F1.
[0035] The back pressure pin 39 can move up and down as a knockout pin, independent of the lifting member 37, the pin seat 38, and the spring member 36. The molded work 9 is ejected from the lower die 3 by the back pressure pin 39. Thereafter, the work 9 is subjected to appropriate processes such as sizing (processing for smoothing the tooth surface of the spline 92) and drilling (processing for vertically penetrating the molded hole 90), thereby completing a hollow shaft part.
[0036] <Action and effect> Next, the effects of the forging die and the spline forming method of this embodiment will be described. As shown in FIG. 3, according to the forging die 1 and the spline forming method of this embodiment, the back pressure pin 39 can continuously apply back pressure to the workpiece 9 during spline forming (from the start of forming the spline 92 to the completion of forming). Therefore, the filling property of the workpiece 9 into the spline tooth shape 330 is unlikely to decrease. Therefore, as shown in FIG. 5(B), forming defects (underfill, insufficient strength, poor appearance, etc.) are unlikely to occur in the spline 92 after forming. Similarly, forming defects are unlikely to occur in the flange portion 93 after forming. Moreover, according to the forging die 1 and the spline forming method of this embodiment, the spline 92 and the flange portion 93 can be formed in the workpiece 9 in the same process.
[0037] 6, the biasing force of the spring member 36, i.e., the back pressure applied to the workpiece 9, increases as the forming of the spline 92 progresses. Therefore, the filling of the material of the workpiece 9 into the lower portion of the spline tooth die 330 (the portion formed in the later stage of the spline forming method) is less likely to decrease.
[0038] Assume that the initial load F0 shown in Fig. 6 is not set on the spring member 36 in the mold open state shown in Fig. 1 (obviously, this case is also within the technical scope of the present invention). In this case, in order to achieve the maximum load F1 required to improve the forming accuracy of the spline 92 at the bottom dead center A1 shown in Fig. 3, a method of increasing the spring constant of the spring member 36 as shown by line L2 in Fig. 6 is conceivable. However, in this case, the back pressure load is affected to be low in the first half of spline forming.
[0039] In this regard, according to the forging die 1 and spline forming method of this embodiment, in the die open state shown in Fig. 1, an initial load F0 shown in Fig. 6 is set on the spring member 36. By appropriately setting this initial load F0, it becomes possible to appropriately adjust the back pressure in the first half of the spline forming, and even if the spring constant of the spring member 36 is made small, as shown by line L1 in Fig. 6, it is possible to achieve the maximum load F1 at the bottom dead center A1 shown in Fig. 3. Thus, in this embodiment, the forming accuracy of the workpiece 9 can be improved by appropriately selecting the spring constant, spring height, etc. of the spring member 36 so that the initial load F0 and the maximum load F1 are appropriate values (including the case where the initial load F0 is 0).
[0040] As shown in Fig. 1, of the six spring members 36, the upper three (a part) spring members 36 and the lower three (the remaining part) spring members 36 are arranged in vertically opposite directions. This allows the spring members 36 to have a large amount of elastic deformation (amount of strain) in the vertical direction. This allows the spring constant of the spring members 36 to be small.
[0041] As shown in FIG. 1 and FIG. 2, the forging die 1 of this embodiment is provided with a spring member 36 as the biasing member of the present invention. Therefore, compared to the case where a hydraulic cylinder is used as the biasing member, the spline 92 can be formed quickly because hydraulic control is not required. Therefore, the time required for the spline forming method can be shortened. In addition, even if the workpiece 9 is at a high temperature (in the case of warm forging or hot forging), the forging die 1 is not easily affected by the heat of the workpiece 9. In addition, as shown in FIG. 3, the punch 22 has a tapered portion 241. Therefore, the workpiece 9 can be easily deformed by expanding its diameter. According to the forging die 1 of this embodiment, a knockout pin is used as the back pressure pin 39. Therefore, compared to the case where the back pressure pin 39 and the knockout pin are separately arranged, the number of parts of the forging die 1 can be reduced.
[0042] <Other> The forging die and the spline forming method according to the present invention have been described above. However, the embodiments are not limited to the above. Various modifications and improvements that can be made by those skilled in the art are also possible.
[0043] As shown in FIG. 6, the application pattern of the biasing force of the spring member 36 is not particularly limited. Since the appropriate magnitude of the back pressure differs for each part, such as the part dimensions and the dimensions of the spline 92, an initial load F0 exceeding 0 may be set as in line L1. The initial load may be 0 as in lines L2, L4, and L5. The biasing force may be constant from the top dead center A0 to the bottom dead center A1 as in line L3. That is, the increasing speed of the biasing force (biasing force / amount of descent of the back pressure pin 39) may be 0. The biasing force may be applied in a curved shape that bulges downward as in line L4. The biasing force may be applied in a curved shape that bulges upward as in line L5. That is, the increasing speed of the biasing force may change midway. In addition, when the biasing force is constant as in line L3, a hydraulic cylinder may be provided instead of the spring member 36, and the hydraulic pressure may be controlled so that the biasing force is constant.
[0044] The timing at which the workpiece 9 comes into contact with the large diameter portion 390 of the back pressure pin 39 is not particularly limited (see FIG. 4(B)). It may come into contact before the formation of the spline 92 begins or during the formation of the spline 92. Also, the back pressure may decrease before the formation of the spline 92 is completed. Even in this case, the remaining back pressure can be used to fill the spline tooth mold 330 with the material of the workpiece 9.
[0045] In the above embodiment, a disc spring is used as the spring member 36, but the type of the spring member 36 is not particularly limited. A coil spring, a leaf spring, or the like may be used. In the above embodiment, the spring member 36 is used as the urging member, but the type of the urging member is not particularly limited. A hydraulic cylinder, an air cylinder, rubber, or the like may be used. A plurality of spring members with different spring constants may be stacked in the vertical direction.
[0046] 4, a step that decreases in diameter from the top to the bottom may be provided on the shaft portion 24. The arrangement direction of the upper die 2 and the lower die 3 is not particularly limited. The upper die 2 may be a fixed die, and the lower die 3 may be a movable die. The forging die 1 may be used for any of cold forging, warm forging, and hot forging.
[0047] Particularly in the case of steel, the workpiece 9 after hot forging or warm forging may be subjected to cold forging in order to correct the tooth surface accuracy of the spline 92. In this case, the workpiece 9 after hot forging or warm forging but before cold forging is usually subjected to annealing treatment in order to improve ductility. However, when the forging die 1 is used for warm forging and the forging temperature is set to 900°C or higher and 1000°C or lower, the ductility is improved compared to the case of hot forging, so that the annealing treatment may be omitted.
[0048] The type of hollow shaft part manufactured using the forging die 1 and the spline forming method is not particularly limited. For example, it may be an automobile transmission part (drive pinion gear, reduction drive gear, rotor shaft, etc.). The material of the workpiece 9 is not particularly limited. It may be steel (carbon steel for machine construction, etc.), alloy steel for machine construction (chromium molybdenum steel, etc.), stainless steel, aluminum alloy, etc. EXAMPLES
[0049] Below, we will explain experiments conducted using the forging die 1 of the above-mentioned embodiment (however, a hydraulic device equipped with a hydraulic cylinder is provided instead of the spring member 36) and the spline forming method, as well as CAE (Computer Aided Engineering) analysis.
[0050] <Experiment> First, an experiment was conducted. Specifically, spline forming was actually performed on six workpieces 9. Fig. 7 shows an axial cross-sectional view of the workpiece after the spline forming method was performed.
[0051] As shown in Fig. 7, the axial length L of the spline 92 of the workpiece 9 is 33 mm. The inner diameter (diameter) D1 of the spline portion 94 (the portion where the spline 92 is formed) is 20.0 mm. Note that the inner diameter D1 corresponds to the outer diameter of the small-diameter portion 242 of the punch 22 shown in Fig. 2. The small diameter D2 (the diameter of the circle (root circle) passing through the radially inner end of the spline 92) is 36.6 mm. The large diameter D3 (the diameter of the circle (tooth tip circle) passing through the radially outer end of the spline 92) is 40 mm. The wall thickness T of the spline portion 94 is 8.3 mm. Note that the wall thickness T corresponds to (small diameter D2 - inner diameter D1) / 2, that is, the radial width of the gap between the small-diameter portion 242 of the punch 22 shown in Fig. 2 and the radially inner end of the spline tooth profile 330 (however, the width on one side in the radial direction). The module is 1.25. The pressure angle is 38°. The tooth depth is 1.4 mm. The material of the workpiece 9 is SCM420.
[0052] In the experiment, six levels of back pressure (back pressure load) of 0 t, 10 t, 30 t, 50 t, 70 t, and 90 t were set, and spline forming was performed on the workpiece 9 for each level. Also, the meat filling property of the formed spline 92 (the filling property of the meat of the workpiece 9 with respect to the spline tooth profile 330), forming defects (such as burrs), etc. were observed. Note that the back pressure during forming was kept constant by a hydraulic device. For example, when conducting the experiment at the back pressure level of 30 t, as shown by the line L3 in Fig. 6, the back pressure during forming was kept at 30 t. As a result of the experiment, it was found that the back pressure range in which no forming defects occurred and good meat filling property was obtained was 30 t or more and 70 t or less.
[0053] <CAE Analysis> Next, CAE analysis was performed. In the CAE analysis, seven models #1 to #7 of the workpiece 9 with different dimensions were adopted. Also, a forging die having substantially the same shape as the forging die 1 used in the above experiment (however, there are shape differences due to the dimensional differences of the models #1 to #7) was used. Table 1 shows the axial length L of the spline 92, the inner diameter D1, small diameter D2, large diameter D3, wall thickness T of the spline portion 94, module, pressure angle, tooth depth, surface pressure threshold, and minimum back pressure of the seven models #1 to #7. The surface pressure threshold and the minimum back pressure will be described later.
Table 1
[0054] The smaller the back pressure, the smaller the adverse effect on the forging die 1 and the workpiece 9. In addition, the surface pressure applied to the spline 92 corresponds to the thickness (the greater the surface pressure, the better the thickness). Therefore, in each of the models #1 to #7, the surface pressure applied to the spline 92 at the back pressure of 30t (the minimum back pressure at which good thickness can be obtained) in the above-mentioned experiment was set as the surface pressure threshold value Pth. In addition, in each of the models #1 to #7, the back pressure (the minimum back pressure at which good thickness can be obtained) M corresponding to the surface pressure threshold value Pth was obtained.
[0055] The relationship between the wall thickness and the minimum back pressure of each model is shown in Figure 8. When the data of seven points (models #1 to #7) in Figure 8 was approximated with a quadratic function using the least squares method, the following formula (1) was obtained, where T (mm) is the wall thickness and M (t) is the minimum back pressure. M=0.66T 2 -2.06T+1.28...Equation (1)
[0056] The minimum value M of the back pressure shown in Table 1 is the calculated value using formula (1). As shown in FIG. 8, Table 1, and formula (1), the smaller the thickness T, the smaller the minimum value M. Also, for a given thickness T, when the back pressure is equal to or greater than the minimum value M, that is, the curve of formula (1), the thickness of the spline 92 is good. Conversely, for a given thickness T, when the back pressure is less than the minimum value M, that is, the curve of formula (1), the thickness of the spline 92 is poor.
[0057] As an example, looking at the data for model #4 in Table 1 in Fig. 8, the wall thickness T is 7.8 mm, and the minimum value M is 25t according to formula (1). Therefore, as shown by the arrow in Fig. 8, if the back pressure applied to the workpiece 9 is 25t or more, the wall thickness of the spline 92 will be good.
[0058] In this way, from formula (1), a back pressure that provides good thickness tightening of the spline 92 can be set according to the thickness T of the workpiece 9, i.e., the radial width of the gap between the small diameter portion 242 of the punch 22 shown in Figure 2 and the radial inner end of the spline tooth die 330.
[0059] The back pressure during spline molding may be a constant value (maintaining a minimum value M) as shown by line L3 in Fig. 6. Alternatively, the back pressure may be increased from the minimum value M to a predetermined maximum value as shown by lines L1-L2 and L4-L5 in Fig. 6.
[0060] In addition to formula (1), the thickness T and back pressure conditions (maximum and minimum values) may be determined by the strength (e.g., torsional strength) required for the workpiece 9 and the configuration of the forging die 1. In this case, by adding these conditions to formula (1), it is possible to set a back pressure range that provides good thickness.
[0061] For example, if the back pressure is excessively large, the wall of the work 9 is likely to enter the gap for degassing in the lower die 3 during spline forming. This may cause burrs to occur on the work 9 after forming. In this case, the maximum value of the back pressure may be set to a value that can prevent burrs from occurring (which may vary depending on the configuration of the forging die 1, etc.). In the case of the above-mentioned experiment, if the back pressure exceeds 70t, burrs will occur on the work 9, so the maximum value of the back pressure may be set to 70t. In other words, the back pressure may be set to a range between the minimum value M and 70t. Also, if the wall thickness T is excessively small, the torsional strength of the work 9 after forming will be small. In this case, the minimum value of the wall thickness T may be set to a value that can ensure torsional strength (for example, 4mm, which may vary depending on the application of the work 9, etc.). [Explanation of symbols]
[0062] 1: forging die, 2: upper die, 20: upper die holder, 21: upper die sleeve, 22: punch, 23: head, 24: shaft, 240: large diameter portion, 241: tapered portion, 242: small diameter portion, 3: lower die, 30: lower die holder, 300: accommodation hole, 301: small diameter portion, 302: tapered portion, 303: large diameter portion, 31: lower die sleeve, 310: die accommodation portion, 311: forming portion, 32: sleeve support, 33: die, 330: spline tooth type, 3 4: die support, 35: spring seat, 350: pin insertion hole, 36: spring member, 37: lifting member, 370: cup portion, 371: flange portion, 372: tapered portion, 373: pin insertion hole, 38: pin seat, 380: tapered surface, 39: back pressure pin, 390: large diameter portion, 391: tapered portion, 392: small diameter portion, 9: workpiece, 90: hole to be formed, 91: splined portion, 92: spline, 93: flange portion, 94: spline portion
Claims
1. A punch that pushes the workpiece from the rear, a die having a spline tooth form for forming a spline in the workpiece; A back pressure pin that applies back pressure to the workpiece from the front side; a biasing member that biases the back pressure pin so that the back pressure does not decrease during molding of the spline; A forging die comprising: The workpiece has a forming hole that opens to a rear side, The punch is inserted into the hole to be formed, A forging die for forming the spline in the workpiece with the spline tooth die while extending the formed hole forward with the punch.
2. The forging die according to claim 1 , wherein the biasing member is a spring member.
3. A forging die as described in claim 1 or claim 2, wherein the spline is molded on the outer peripheral surface of the workpiece.
4. 4. The forging die according to claim 1, wherein a radial width of a gap between the punch and a radial inner end of the spline tooth die is T (mm), and a minimum value of the back pressure is M(t), and M is set according to T so as to satisfy the following formula (1). M=0.66T 2 -2.06T+1.28...Formula (1)
5. A spline forming method for forming a spline in a workpiece by applying back pressure to the workpiece from the front side while pushing the workpiece from the rear side and pressing the workpiece against a spline tooth mold, comprising: The workpiece has a forming hole that opens to a rear side, The spline is formed in the workpiece by the spline tooth die while the formed hole is extended forward; The spline forming method, wherein the back pressure is not reduced during forming of the spline.
Citation Information
Patent Citations
JP1975123557A
Method of molding cup-shaped product with internal teeth
JP1989317653A
Apparatus for forming inner and outer splines
JP1992081242A
Method for forming spline
JP1994126369A
Method for molding cylindrical gear
JP2010131626A