Steel for carburizing, carburizing steel parts, and method for manufacturing carburizing steel parts

The carburizing steel with controlled cooling and specific compositions stabilizes deformation in complex shapes, enhancing machinability and fatigue strength by reducing hardness variations.

JP7587124B2Active Publication Date: 2024-11-20NIPPON STEEL CORPORATION
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020204375
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-09
Publication Date
2024-11-20
Estimated Expiration
2040-12-09

AI Technical Summary

Technical Problem

Existing carburizing and quenching processes for machine parts like gears and pulleys result in deformation and distortion, affecting fatigue properties and assembly accuracy, with existing techniques failing to effectively stabilize deformation for complex shapes.

Method used

A carburizing steel with specific chemical compositions and controlled cooling processes, including hot forging, softening heat treatment, and controlled cooling rates to achieve a martensitic structure with reduced hardness variations, suitable for complex shapes.

Benefits of technology

The solution significantly reduces hardness variations and deformation in carburized steel parts, improving machinability and dimensional accuracy, while maintaining high fatigue strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587124000003
    Figure 0007587124000003
  • Figure 0007587124000004
    Figure 0007587124000004
  • Figure 0007587124000001
    Figure 0007587124000001
Patent Text Reader

Abstract

To provide carburizing steel that has sufficiently lowered hardness after softening heat treatment, and reduces variation of a deformation amount of carburized steel components after a carburization treatment, and exhibits its effect even in a component having a complicated shape, a carburized steel component therewith and a manufacturing method of the carburized steel component.SOLUTION: Carburizing steel contains, by mass%, C: 0.06 to 0.25%, Si: 0.01 to 0.90%, Mn: 3.51 to 6.00%, P: 0.05% or less, S: 0.001-0.100%, Cr: 0.03 to 1.49%, Al: 0.001-0.050%, N: 0.0030 to 0.0250%, and the balance made of Fe and impurities, in which, when carburized, the following index Ms representing an Ms point (°C) of a depth 25 μm position from a carburized surface is 30°C or higher. Ms=219.2-1.3×Si-31.7×Mn-11.6×Cr In the formula representing the index Ms, each element mark shows a content (mass%) of each element.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel for carburizing, a carburized steel part, and a method for manufacturing a carburized steel part. [Background technology]

[0002] Mechanical parts such as gears, shafts, and pulleys (pulleys used in CVTs (Continuously Variable Transmissions)) used in automobiles, ships, industrial machinery, etc. require high bending fatigue strength and pitting strength, so carburized and quenched low-alloy steel is used. Carburizing and quenching produces a harder surface layer than induction hardening, another surface hardening heat treatment, and can form a deeper hardened layer than soft nitriding, so it can effectively improve fatigue properties.

[0003] However, the disadvantage is that the steel is quenched from the austenite region to transform into martensite, which causes distortion and deformation of the parts. These deformations can deteriorate the fatigue properties and assembly accuracy of the parts. Finishing processes to reduce the adverse effects of deformation lead to increased manufacturing costs.

[0004] As a means of reducing the adverse effects of deformation during carburizing, there is a method of designing parts on the assumption that a certain amount of deformation will occur. In order to design parts on the assumption that a certain amount of deformation will occur, it is necessary to reduce the variation so that the amount of deformation is always constant. Therefore, various techniques have been disclosed for reducing the variation in the amount of deformation of machine parts during carburizing.

[0005] For example, Patent Document 1 discloses a technique that finds that the hardenability of steel is correlated with the amount of deformation and the variation in the amount of deformation, and that optimizes the amount of alloy elements to stabilize the deformation at a low level. Patent Document 2 discloses a technology that optimizes the electromagnetic stirring conditions during continuous casting to reduce the variation in the equiaxed crystal ratio and C concentration, thereby making the amount of deformation constant when carburizing after molding into a hollow part. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 2-277744 [Patent Document 2] JP 2003-320439 A Summary of the Invention [Problem to be solved by the invention]

[0007] The technology described in Patent Document 1 stabilizes deformation at a low level by restricting the hardenability of the steel material within a certain range, but its main effect is to reduce the amount of deformation. In Patent Document 1, the variation in the amount of deformation of the invention example is about the same as that of the comparative example using chromium steel (SCr420), so the effect of reducing the variation in the amount of deformation is small.

[0008] In addition, the technology described in Patent Document 2 can make the amount of deformation constant when carburizing after molding into a hollow shaft-shaped part by optimizing the electromagnetic stirring conditions during continuous casting. However, there are restrictions on the shape of the part, and there is no mention of making the amount of deformation constant for parts with shapes other than a hollow shaft shape.

[0009] In addition, carburizing steel is cut before carburizing to obtain a carburized steel part of a desired shape, and therefore the carburizing steel is required to have high machinability and to have its hardness sufficiently reduced by softening heat treatment so that it can be cut using ordinary processing equipment.

[0010] Therefore, an object of the present invention is to provide a carburized steel that has a sufficiently reduced hardness after softening heat treatment and that reduces the variation in the amount of deformation of carburized steel parts after carburizing treatment, and that exerts this effect even in parts with complex shapes, a carburized steel part using the same, and a method for manufacturing a carburized steel part. [Means for solving the problem]

[0011] The means for solving the problems include the following aspects. <1> In mass%, C: 0.06 to 0.25%, Si: 0.01 to 0.90%, Mn: 3.51-6.00%, P: 0.05% or less, S: 0.001 to 0.100%, Cr: 0.03-1.49%, Al: 0.001 to 0.050%, N: Contains 0.0030 to 0.0250%; the balance being Fe and impurities, Carburizing steel that, when carburized, has a Ms point (℃) at a depth of 25μm from the carburized surface of 30℃ or higher. Ms=219.2-1.3×Si-31.7×Mn-11.6×Cr In the formula expressing the index Ms, each element symbol indicates the content (mass %) of each element. <2> In mass%, Ti: 0.05% or less, Nb: 0.05% or less Mo: 0.25% or less V: 0.15% or less, Cu: 0.50% or less, Ni: 0.50% or less and B: 0.005% or less, Contains one or more of the following: <1> The carburizing steel according to claim 1. <3> In mass%, C: 0.06 to 0.25%, Si: 0.01 to 0.90%, Mn: 3.51-6.00%, P: 0.05% or less, S: 0.001 to 0.100%, Cr: 0.03-1.49%, Al: 0.001 to 0.050%, N: Contains 0.0030 to 0.0250%; the balance being Fe and impurities, The following index Ms, which indicates the Ms point (℃) at a depth of 25 μm from the carburized surface, is 30℃ or higher, The amount of C at a depth of 25 μm from the carburized surface is 0.40 to 0.70% by mass. A carburized steel part with a hardness of 630HV or more at a depth of 25μm from the carburized surface. Ms=219.2-1.3×Si-31.7×Mn-11.6×Cr In the formula expressing the index Ms, each element symbol indicates the content (mass %) of each element. <4> In mass%, Ti: 0.05% or less, Nb: 0.05% or less Mo: 0.25%, V: 0.15% or less, Cu: 0.50% or less, Ni: 0.50% or less and B: 0.005% or less, Contains one or more of the following: <3> 2. The carburized steel part according to claim 1 . <5> <3> or <4> A method for manufacturing a carburized steel part according to the present invention, The carburizing steel is subjected to a hot forging forming process, a softening heat treatment process at 650-750°C for 30-640 minutes, and a cutting process in sequence to obtain a steel part. A method for manufacturing a carburized steel part, comprising carburizing the steel part so that the C content at a position 25 μm deep from the surface of the carburized steel part is 0.40 to 0.70% by mass, and then cooling from the carburizing temperature from 800°C to 200°C at a cooling rate of 0.01 to 2°C / s. Effect of the Invention

[0012] According to the present invention, it is possible to provide a carburized steel that has a sufficiently reduced hardness after softening heat treatment and that reduces the variation in the amount of deformation of carburized steel parts after carburizing treatment, and that exerts this effect even on parts with complex shapes, as well as a carburized steel part and a method for manufacturing a carburized steel part using the same. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a schematic diagram showing a rotating bending fatigue test piece and a test piece for measuring deformation amount, which were prepared in the examples. [Diagram 2] FIG. 2 is a schematic diagram showing how to hang a test piece. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described in detail. The "%" for the content of each element means "mass %." The content of each element in a chemical composition is sometimes expressed as the "element amount." For example, the carbon content is sometimes expressed as the carbon amount. A numerical range expressed using "~" means that the range includes the numerical values ​​before and after "~" as the lower and upper limits. When a numerical range is preceded by "to" and followed by "greater than" or "less than," it means that the numerical range does not include the numerical value as the lower limit or upper limit.

[0015] <Steel for carburizing> The carburizing steel according to this embodiment (hereinafter also simply referred to as "carburizing steel") has a specified chemical composition and, when carburized, has an index Ms, which indicates the Ms point (°C) at a depth of 25 μm from the carburized surface, of 30°C or higher. Ms=219.2-1.3×Si-31.7×Mn-11.6×Cr In the formula expressing the index Ms, each element symbol indicates the content (mass %) of each element.

[0016] The carburizing steel according to this embodiment has a sufficiently reduced hardness after softening heat treatment and reduces the variation in the amount of deformation of carburized steel parts after carburizing treatment, and can exert this effect even on parts with complex shapes. The carburizing steel according to this embodiment was discovered based on the following findings.

[0017] The inventors of the present invention have investigated the conditions under which the variation in the amount of deformation after carburizing treatment differs by changing the chemical composition of the steel and the cooling conditions after carburizing treatment in various ways. As a result, they have obtained the following findings (a) and (b). (a) The more complex the shape of a steel part, the greater the deformation. This is because the difference in cooling speed between different parts of a part with a complex shape becomes greater. (b) One of the main causes of differences in cooling speed is the variation in the cooling speed of each steel part when it is cooled after carburizing. This variation is caused by the difference in the boiling state of the oil depending on the position when quenching in oil after carburizing, and is caused by the fact that the positional relationship between the nozzle and each part is not constant when quenching with high-pressure gas such as helium or nitrogen.

[0018] Based on the above findings, the inventors of the present invention considered that cooling from the carburizing temperature could be reduced to suppress deformation by performing cooling in a vacuum, in air, or in an atmospheric gas at a cooling rate equivalent to air cooling or air cooling with a fan, instead of the conventional oil cooling or gas cooling, thereby reducing the temperature difference within the part. Hereinafter, the oil cooling, high-pressure gas cooling, or cooling at a rate equal to or higher than those performed in general carburizing treatments will be referred to as quenching, and the air cooling, air cooling with a fan, or cooling at a rate equal to or lower than those will be referred to as slow cooling. Therefore, the inventors further investigated the conditions for applying these steels as carburized steel parts by using steels with increased alloy component amounts so that martensitic transformation occurs even when cooling after carburizing treatment is slow. As a result, the following findings (c) and (d) were obtained. (c) It is known that by adding a large amount of Mn, martensitic transformation can be induced even if the steel is cooled slowly from a temperature equivalent to carburizing. However, when such steel is formed by hot forging and subsequent cutting, the structure after hot forging becomes martensite, and machinability deteriorates. (d) In order to soften the structure after hot forging, it is sufficient to carry out softening heat treatment in the ferrite region after hot forging. However, depending on the steel composition and the softening heat treatment conditions, the hardness of the carburized layer after subsequent vacuum carburization may vary. (e) The variation in hardness during vacuum carburization is due to the fact that alloying elements are concentrated in cementite during softening heat treatment, stabilizing it, and do not completely dissolve during the subsequent vacuum carburization. In order to suppress the stabilization of cementite during softening heat treatment, it is necessary to appropriately control the content of alloying elements with high carbide forming ability.

[0019] In addition, by increasing the Mn content and decreasing the Cr content, the hardness of the steel material after softening heat treatment is sufficiently reduced, and the machinability can be improved.

[0020] Based on the above findings, it has been discovered that the carburizing steel according to this embodiment has a sufficiently reduced hardness after softening heat treatment, reduces the variation in the amount of deformation of carburized steel parts after carburizing treatment, and can exert this effect even on parts with complex shapes. Furthermore, since the carburizing steel according to this embodiment can significantly reduce the variation in the amount of deformation of carburized steel parts after carburizing treatment, by performing a design assuming a certain amount of deformation, it is possible to improve the dimensional accuracy of the finished product or omit finishing processing. In addition, the carburizing steel according to this embodiment has a sufficiently reduced hardness after softening heat treatment, so that it has high machinability and improves the degree of freedom in the shape of the resulting carburized steel part. Furthermore, carburized steel parts obtained from the carburizing steel according to this embodiment are suitable for use as machine parts for automobiles, industrial machinery, construction machinery, and the like.

[0021] The carburizing steel according to this embodiment will be described in detail below.

[0022] [Chemical composition (essential elements)] The chemical composition of the carburizing steel according to this embodiment contains the following elements.

[0023] C: 0.06 to 0.25% C increases the hardness of martensite formed during cooling after carburizing. The C content of the carburized layer is determined by the carburizing conditions, so the C content of the core does not have a significant effect on the C content of the carburized layer. Therefore, increasing the C content of the core does not promote the formation of retained austenite in the carburized layer. On the other hand, if the C content is too high, the hardness does not decrease sufficiently even with softening heat treatment, and the cutting resistance increases, resulting in poor machinability. Therefore, the C content is 0.06-0.25%. The lower limit of the C content is preferably 0.08%, more preferably 0.10%, and even more preferably 0.12%. The upper limit of the C content is preferably 0.23%, and more preferably 0.20%.

[0024] Silicon: 0.01 to 0.90% Silicon increases the hardness of martensite through solid solution strengthening, improving fatigue properties. On the other hand, if the amount of silicon is too high, oxides are formed on the surface layer depending on the cooling atmosphere, deteriorating machinability. Therefore, the amount of silicon is 0.01 to 0.90%. The lower limit of the Si content is preferably 0.03%, and more preferably 0.05%. The upper limit of the Si content is preferably 0.50%, more preferably 0.35%, and further preferably 0.25%.

[0025] Mn: 3.51-6.00% Mn is an important element for transforming the structure into martensite, even if the cooling after carburizing is equivalent to natural cooling. Mn also forms MnS in the steel, which improves the machinability of the steel after softening heat treatment. On the other hand, if the Mn content is too high, a large amount of retained austenite is generated, even if the C concentration during carburizing is appropriately controlled, which reduces hardness and deteriorates fatigue properties. Therefore, the Mn content is 3.51 to 6.00%. The lower limit of the Mn content is preferably 3.80%, and more preferably 4.00%. The upper limit of the Mn content is preferably 5.80%, and more preferably 5.65%.

[0026] P:0.05% or less P is an impurity. P segregates at grain boundaries and causes grain boundary embrittlement cracking. Therefore, it is preferable that the P content is as low as possible. Therefore, the upper limit of the P content is 0.05% or less, and the preferred upper limit of the P content is 0.02% or less. The lower limit of the P content is preferably 0% (that is, it is preferable that the P content is not contained), but from the viewpoint of reducing the dephosphorization cost, it is preferable that the P content is more than 0% (or 0.0001% or more).

[0027] S: 0.001 to 0.100% S combines with Mn in steel to form MnS, which improves the machinability of the steel. On the other hand, if the S content is too high, coarse MnS is formed, which reduces the fatigue strength of the steel. Therefore, the S content is 0.001 to 0.100%. The lower limit of the S content is preferably 0.003%, more preferably 0.005%, and even more preferably 0.010%. The upper limit of the S content is preferably 0.080%, more preferably 0.060%, and even more preferably 0.050%.

[0028] Cr: 0.03~1.49% Cr has the effect of transforming the structure into martensite even if the cooling after carburizing is equivalent to natural cooling. On the other hand, Cr has a very high affinity with carbon, so when steel containing Cr is subjected to softening heat treatment, Cr is concentrated in the cementite. Cementite with concentrated Cr becomes very stable, and it may take time to dissolve if carburized afterwards. In particular, when the type of carburizing treatment is vacuum carburizing, cementite is difficult to dissolve, and depending on the conditions, cementite may remain after the treatment. Even if the cementite dissolves, the concentrated Cr remains unevenly distributed even after the cementite dissolves, which can cause variations in the structure and properties after cooling. In addition, if the Cr content is large, the temper softening resistance increases, so that the hardness of the steel material after softening heat treatment is unlikely to decrease sufficiently, and the machinability cannot be sufficiently improved. Therefore, the Cr content is 0.03 to 1.49%. The lower limit of Cr is preferably 0.10%, and more preferably 0.30%. The upper limit of Cr is preferably 1.00%, more preferably 0.60%, and further preferably 0.45%.

[0029] Al: 0.001 to 0.050% Al combines with N to form AlN, and the pinning effect of this suppresses the formation of coarse grains. Al is also used for deoxidation during steel manufacturing. On the other hand, if the Al content is too high, coarse oxides are more likely to form, and fatigue properties deteriorate. Therefore, the Al content is 0.001 to 0.050%. The lower limit of the Al content is preferably 0.005%, and more preferably 0.010%. The upper limit of the Al content is preferably 0.035%, and more preferably 0.030%.

[0030] N: 0.0030~0.0250% N combines with Al to form AlN, and the pinning effect of this inhibits the generation of coarse grains. On the other hand, if the N content is too high, bubbles are generated in the steel material. Since bubbles become defects, it is preferable to inhibit the generation of bubbles. Therefore, the N content is 0.0030 to 0.0250%. The preferred lower limit of the N content is 0.0050. The preferred upper limit of the N content is 0.0200%, more preferably 0.0180%, and even more preferably 0.0170%.

[0031] In the chemical composition of the carburizing steel according to this embodiment, the balance consists of Fe and impurities. Here, impurities refer to substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of steel, and are acceptable within a range that does not adversely affect the carburizing steel of this embodiment.

[0032] [Chemical composition (arbitrary elements)] The carburizing steel according to this embodiment may contain optional elements, the lower limit of which is 0%.

[0033] In the carburizing steel according to this embodiment, among the optional elements, the group consisting of Ti, Nb, Mo, V, Cu and Ni has the effect of improving fatigue properties, and the carburizing steel may contain one or more of these elements.

[0034] Ti: 0.050% or less Ti combines with N to form TiN, which suppresses the coarsening of crystal grains during hot forging and carburizing, thereby improving fatigue properties. However, if the Ti content is too high, TiC is generated in the core during carburizing, reducing the amount of solute C. A reduction in the amount of solute C can deteriorate hardness and fatigue properties. Therefore, if Ti is included, the Ti content is 0.050% or less. The lower limit of the Ti content is preferably 0.005%, and more preferably 0.010%. The upper limit of the Ti content is preferably 0.040%, and more preferably 0.030%.

[0035] Nb: 0.050% or less Nb combines with N to form NbN, which suppresses the coarsening of crystal grains during hot forging and carburizing, thereby improving fatigue properties. However, if the Nb content is too high, NbC is generated in the core during carburizing, reducing the amount of solute C. A reduction in the amount of solute C can deteriorate hardness and fatigue properties. Therefore, if Nb is included, the Nb content is 0.050% or less. The lower limit of the Nb content is preferably 0.005%, and more preferably 0.010%. The upper limit of the Nb content is preferably 0.040%, and more preferably 0.030%.

[0036] Mo: 0.25% or less Mo has the effect of transforming the structure into martensite even if the cooling rate after carburizing is slowed down. On the other hand, Mo stabilizes cementite, so if steel with too much Mo is softened by heat treatment, cementite may remain during the subsequent vacuum carburizing, causing fatigue properties to deteriorate. Mo is expensive, and adding a large amount of it increases manufacturing costs. Therefore, if Mo is added, the Mo content is 0.25% or less. The lower limit of the Mo content is preferably 0.05%. The upper limit of the Mo content is preferably 0.20%, and more preferably 0.15%.

[0037] V: 0.15% or less V has the effect of transforming the structure into martensite even if the cooling rate after carburizing is slowed down. On the other hand, V stabilizes cementite, so if steel with too much V is softened by heat treatment, cementite may remain during the subsequent vacuum carburizing, causing fatigue properties to deteriorate. Therefore, if V is included, the V content should be 0.15% or less. The lower limit of the V content is preferably 0.05%. The upper limit of the V content is preferably 0.13%, and more preferably 0.10%.

[0038] Cu: 0.50% or less Cu has the effect of transforming the structure into martensite even if the cooling rate after carburizing is slow. On the other hand, if the amount of Cu is excessively large, it segregates at the grain boundaries of the steel during hot forging and induces hot cracking. Therefore, if Cu is included, the amount of Cu should be 0.50% or less. The lower limit of the Cu content is preferably 0.05%, and more preferably 0.10%. The upper limit of the Cu content is preferably 0.40%, and more preferably 0.30%.

[0039] Ni: 0.50% or less Ni has the effect of transforming the structure into martensite even if the cooling rate after carburizing is slow. However, Ni is expensive, and adding a large amount of Ni increases the manufacturing cost. Therefore, when Ni is added, the Ni content is 0.50% or less. The lower limit of the Ni content is preferably 0.05%, and more preferably 0.10%. The upper limit of the Ni content is preferably 0.40%, and more preferably 0.30%.

[0040] In the carburizing steel according to this embodiment, of the optional elements, B has the effect of improving fatigue properties, and the carburizing steel may contain B.

[0041] B: 0.0050% or less B has the effect of stabilizing grain boundaries and converting the structure to martensite even if the cooling rate after carburizing is slow. On the other hand, if the B content is excessively high, it will form coarse carboborides with other elements, deteriorating fatigue properties. Therefore, the B content is 0.0050% or less. In order to stably obtain the above effect, the preferred lower limit of the B content is 0.0005%. The preferred upper limit of the B content is 0.0040% or less.

[0042] [Ms point (℃) at a depth of 25 μm from the carburized surface: 30℃ or higher] When the carburizing steel according to this embodiment is carburized, the index Ms, which indicates the Ms point (°C) at a depth of 25 µm from the carburized surface, is 30°C or higher. Details of the index Ms representing the Ms point (° C.) will be explained later in relation to the carburized steel part according to this embodiment. Here, carburizing treatment means that the steel is carburized so that the C content at a depth of 25 μm from the surface of the carburized steel part is 0.40 to 0.70% by mass, and then cooled from the carburizing temperature from 800°C to 200°C at a cooling rate of 0.01 to 2°C / s.

[0043] [Hardness at a depth of 8.75 μm from the softening heat-treated surface: 400 HV or less] When the carburizing steel according to this embodiment is subjected to softening heat treatment, the hardness at a depth of 8.75 mm from the softening heat treated surface (hereinafter also referred to as "hardness of the steel after softening heat treatment") is preferably 400 HV or less. If the hardness of the steel after softening heat treatment is 400HV or less, it can be cut using normal processing equipment. The hardness of the steel material after the softening heat treatment is more preferably 350 HV or less. However, from the viewpoint of ensuring strength, the lower limit of the hardness of the steel material after the softening heat treatment is, for example, 120 HV or more.

[0044] Here, the hardness of the steel material after softening heat treatment is the hardness of the steel material after softening heat treatment is performed on the carburizing steel (i.e., the carburizing steel part raw material) formed by hot forging and before the carburizing treatment. The softening heat treatment means a heat treatment at 650 to 750° C. for 30 to 640 minutes.

[0045] The hardness of the steel material after the softening heat treatment is a Vickers hardness, which is measured by the method described in the examples below.

[0046] <Carburized steel parts> The carburized steel part according to this embodiment (hereinafter also simply referred to as "carburized steel part") has a chemical composition at a position deeper than 3 mm from the surface, which is not affected by carburization, that is the chemical composition of the carburized steel according to this embodiment, and satisfies the following characteristics. Carburized steel parts are parts that are carburized but not subsequently quenched. (1) The index Ms, which indicates the Ms point (°C) at a depth of 25 μm from the carburized surface (hereinafter also referred to as the "surface layer"), is 30°C or higher. (2) The carbon content at a depth of 25 μm from the carburized surface (hereinafter also referred to as the "surface layer") is 0.40 to 0.70% by mass. (3) The hardness at a depth of 25 μm from the carburized surface (hereinafter also referred to as the "surface layer") is 630 HV or more.

[0047] The carburized steel part according to this embodiment will be described in detail below.

[0048] [Ms point (℃) at a depth of 25 μm from the carburized surface: 30℃ or higher] When steel with a high Mn and Cr content is carburized, a larger amount of retained austenite is produced than when a typical case-hardened chrome steel (such as SCr420) is carburized, resulting in a decrease in hardness. In order to suppress the production of retained austenite, even if the carbon content of the surface layer (i.e., the carburized layer) becomes 0.70% after carburizing the steel, it is sufficient that the index Ms, which indicates the Ms point (℃) of the surface layer (i.e., the carburized layer), is 30℃ or higher. The index Ms representing the Ms point (°C) of the surface layer portion is preferably 50°C or higher, and more preferably 60°C or higher. However, the upper limit of the index Ms representing the Ms point (°C) of the surface layer portion is set to, for example, 300°C or lower from the viewpoint of suppressing the generation of pro-eutectoid ferrite. The index Ms indicating the Ms point (°C) is defined as the Ms point of a steel when the C content at a depth of 25 µm from the carburized surface is 0.70%.

[0049] Ms=219.2-1.3×Si-31.7×Mn-11.6×Cr In the formula expressing the index Ms, each element symbol indicates the content (mass %) of each element.

[0050] The index Ms, which indicates the Ms point (° C.) of the surface layer (at a depth of 25 μm from the carburized surface), is calculated by a method which will be described in the examples below.

[0051] [C content at a depth of 25 μm from the carburized surface: 0.40 to 0.70%] Even if a steel can be made into martensite without significantly lowering the Ms point of the surface layer, if that steel is carburized to have the same carbon content in the surface layer as a typical case-hardened part, the amount of retained austenite produced may increase, resulting in a decrease in hardness. To sufficiently harden the surface layer of carburizing steel, the C content in the surface layer must be 0.70% or less. On the other hand, if the C content in the surface layer is too low, the hardness of the martensite decreases and the fatigue properties deteriorate, so the C content in the surface layer must be 0.40% or more. The lower limit of the surface layer C content is preferably 0.45% or more, more preferably 0.50% or more, and even more preferably 0.55% or more. The upper limit of the surface layer C content is preferably 0.65% or less, and more preferably 0.62% or less.

[0052] The amount of C in the surface layer (at a depth of 25 μm from the carburized surface) is measured by the method described in the examples below.

[0053] [Hardness at a depth of 25 μm from the carburized surface: 630 HV or more] In order to impart high fatigue properties to carburized steel parts, the hardness of the surface layer must be 630HV or more. The lower limit of the hardness of the surface layer is preferably 650HV or more. Although there is no particular upper limit to the hardness of the surface layer, the hardness obtained when the steel is carburized is usually 1000 HV or less. In addition, when the possibility that the mating material may be worn when the parts slide, the upper limit of the hardness may be 900 HV or less, 850 HV or less, or 800 HV or less.

[0054] The hardness of the surface layer (at a depth of 25 μm from the carburized surface) is a Vickers hardness, and is measured by the method described in the examples below.

[0055] The structure of the surface layer (25 μm deep from the carburized surface) is mainly martensite, and is a mixture of retained austenite, non-metallic inclusions such as oxides and carbides, and incompletely hardened structure. As long as the hardness of the surface layer meets the regulations, there are no restrictions on the ratio of the mixed structure, but to achieve high surface hardness, the area rate on the cross section at the same depth must be less than 30% for retained austenite, less than 5% for non-metallic inclusions, and less than 15% for incompletely hardened structure. The incompletely hardened structure is a mixed structure of bainite and pearlite.

[0056] [Manufacturing method] An example of a method for manufacturing the carburized steel and the carburized steel part according to this embodiment will be described.

[0057] The carburized steel part according to this embodiment is manufactured by sequentially carrying out a forming process by hot forging, a softening heat treatment process at 650-750°C for 30-640 minutes, and a cutting process on a carburized steel to obtain a steel part, carburizing the steel part so that the C content at a depth of 25 μm from the surface of the carburized steel part is 0.40-0.70% by mass, and then cooling from the carburizing temperature from 800°C to 200°C at a cooling rate of 0.01-2°C / s. The specific process is as follows.

[0058] The manufacturing method of the carburized steel part according to this embodiment includes, for example, a steel material preparation step, a molding step, a softening heat treatment step, a cutting step, and a carburizing treatment step, and also includes a heat treatment step for adjusting the structure as required. Each step will be described below.

[0059] [Steel material preparation process] Molten steel satisfying the chemical composition of the carburizing steel according to the present embodiment is manufactured. The manufactured molten steel is made into a slab (or bloom) by a general continuous casting method. Alternatively, the molten steel is made into an ingot by an ingot casting method. The slab or ingot is hot worked to manufacture a billet. The hot working may be hot rolling or hot forging. The billet is then heated, rolled, and cooled under general conditions to manufacture a steel bar. The manufactured steel bar is used as the steel material for the carburizing steel part.

[0060] [Molding process] The produced steel bar is formed into a carburized steel part raw material by hot forging. If the heating temperature of the hot forging is too low, an excessive load is applied to the forging device. On the other hand, if the heating temperature is too high, there is a large scale loss. Therefore, the preferable heating temperature is 1000 to 1300°C. The preferred finishing temperature for hot forging is 900°C or higher. If the finishing temperature is too low, the burden on the die increases. On the other hand, the preferred upper limit of the finishing temperature is 1250°C. To facilitate subsequent machining, the cooling rate after hot forging may be slow to reduce hardness.

[0061] [Softening heat treatment process] The carburized steel part raw material is subjected to heat treatment to soften it. Specifically, the raw material after hot forging is heated at 650 to 750°C for 30 to 640 minutes to reduce the hardness to a level where sufficient machinability is obtained. Cooling after heating may be performed by any method, including cooling in the air or water cooling.

[0062] [Cutting process] The carburized steel part blank after the soft heat treatment is cut to form a desired carburized steel part shape. In addition to the cutting, grinding may also be performed.

[0063] [Carburizing process] The machined steel parts are subjected to a carburizing treatment, after which they are cooled at a specified cooling rate.

[0064] The carburizing treatment is carried out so that the carbon content at a depth of 25 μm from the surface of the carburized steel part is 0.40 to 0.70% by mass. The carburizing process may be gas carburizing or vacuum carburizing. Any type of process may be used as long as the carburizing temperature and time are within the specified ranges for the amount of carbon (the amount of carbon at a depth of 25 μm from the carburized surface) and the cooling rate from the carburizing temperature, which will be described later, is within the specified ranges. For example, when obtaining a carburized steel part according to this embodiment containing 0.15% C and 5.0% Mn, gas carburizing with a surface carbon potential of 0.6 may be performed at 920°C for 3 hours, or vacuum carburizing may be performed at 950°C with acetylene flowing for 22 minutes, followed by holding for 148 minutes.

[0065] After the carburizing treatment, the steel part is cooled from the carburizing temperature of 800°C to 200°C at a cooling rate of 0.01 to 2°C / s. In general carburizing, the steel is cooled from the holding temperature by oil cooling or forced air cooling. The average cooling rate during this type of quenching is 5°C / s or more, which increases the temperature gradient in the steel part and the amount of deformation. In order to reduce the temperature gradient in the steel part and the amount of deformation, the cooling rate must be 2°C / s or less. On the other hand, if the cooling rate is slower than 0.01°C / s, an incompletely quenched structure is formed, which reduces the hardness and deteriorates the fatigue properties. Therefore, the cooling rate from 800°C to 200°C must be 0.01 to 2°C / s. The lower limit of the cooling rate is preferably 0.05° C. / s or more, more preferably 0.10° C. / s or more, and even more preferably 0.20° C. / s or more. The upper limit of the cooling rate is preferably 1.5° C. / s or less, more preferably 1.2° C. / s or less, and even more preferably 1.0° C. / s or less. Here, the average cooling rate is the time required for the surface temperature of the steel part to cool from 800°C to 200°C divided by the temperature difference of 600°C.

[0066] [Post-carburizing process] Steel parts after carburizing may be subjected to various post-treatments in the same way as general carburized and quenched parts. Specifically, they may be subjected to low-temperature tempering at 200°C or less to increase toughness, sub-zero treatment to reduce retained austenite, shot peening to increase hardness and compressive residual stress, or a combination of multiple post-treatments. EXAMPLES

[0067] The present invention will be described in detail below with reference to examples, although the present invention is not limited to these examples.

[0068] First, 50 kg ingots of steels B to O, and S, and 150 kg ingots of steels A, P to R, each having the chemical composition shown in Table 1, were produced using a vacuum melting furnace. Each ingot was heated to 1250°C, and then hot forged into a steel bar with a diameter of φ35 mm. In order to soften the forged steel bar, it was subjected to a softening heat treatment in which it was heated at 700°C for 2 hours and then allowed to cool.

[0069] A test piece was prepared from a part of the steel bar after softening heat treatment, with the cross section (i.e., a plane perpendicular to the length direction of the steel bar) as the test surface. The Vickers hardness of the test piece was measured based on JIS Z 2244 (2009). Specifically, the test force was set to 9.8 N, and the Vickers hardness was measured at five arbitrary points 8.75 mm deep from the surface of the steel bar on the test surface of the test piece. The average of the five Vickers hardness values ​​obtained was defined as the Vickers hardness of the steel after softening treatment. When the Vickers hardness of the steel after softening heat treatment was 400 HV or less, it was considered that the Vickers hardness of the steel after softening heat treatment was sufficiently low and the machinability was high. Furthermore, a rotating bending fatigue test specimen as shown in FIG. 1 and a test specimen for measuring deformation amount were prepared from another part of the steel bar after softening heat treatment. In the chemical compositions shown in Table 1, the notations "<0.01" and "-" indicate that the corresponding element is not intentionally added or is present at an impurity level.

[0070] The prepared test specimens were subjected to carburizing treatment while suspended by wire in a steel basket. At this time, the rotating bending fatigue test specimens were hung vertically with the axial direction facing vertically. Of the test specimens used to measure deformation, three of each test number were hung horizontally with the keyway facing vertically upwards (Fig. 2(a)). Three of each test number were hung horizontally with the keyway facing vertically downwards (Fig. 2(b)). Three of each test number were hung vertically with the keyway extending vertically (Fig. 2(c)). An overview of how the test specimens were hung is shown in Fig. 2.

[0071] These test pieces were vacuum carburized using acetylene at a carburizing temperature of 950° C. The carburizing conditions for the test pieces of each test number were as follows: For test pieces Nos. 1, 2, 5-11, 13, 14, 17, and 26, acetylene was introduced for 22 minutes and then the specimens were held in a vacuum state for 148 minutes. For test pieces Nos. 3 and 4, acetylene was introduced for 18 minutes and then the specimens were held in a vacuum state for 1,528 minutes. For test pieces Nos. 12, 15, and 16, acetylene was introduced for 16 minutes and then the specimens were held under vacuum for 154 minutes. For the test pieces of test numbers 18 to 24, acetylene was introduced for 53 minutes, and then the specimens were held in a vacuum state for 127 minutes. For the test piece of test number 25, acetylene was introduced for 10 minutes and then the specimen was held in a vacuum state for 170 minutes.

[0072] After the carburizing treatment, the test pieces of test numbers 1 to 9, 11 to 17, and 21 to 25 were taken out of the furnace and allowed to cool to 50°C or less in a nitrogen atmosphere. The average cooling rate from 800°C to 200°C during cooling from the carburizing temperature was 0.4°C / sec. The test pieces of test numbers 18 to 20 were carburized, removed from the furnace, and then placed in oil to cool. The average cooling rate from the carburizing temperature of 800°C to 200°C was about 10°C / sec. The test piece of test number 10 was carburized, removed from the furnace, and then cooled by blowing air on it with a fan. The average cooling rate from the carburizing temperature of 800°C to 200°C was about 1.0°C / sec. The test piece of test number 26 was carburized, removed from the furnace, and then transferred to an electric furnace heated to 800°C. At this time, the test piece was hung on a small hanger so that the top and bottom directions of the test piece were the same as those at the time of carburization. The atmosphere in the furnace was Ar. After the temperature of the test piece reached 820°C, the furnace temperature was controlled to decrease at a rate of 0.005°C / sec while cooling to 200°C. When the temperature of the test piece reached 200°C, the electric furnace was turned off and the test piece was allowed to cool in the furnace. The average cooling rate from 800°C to 200°C was 0.005°C / sec, the same as the rate of decrease in the furnace temperature.

[0073] [Hardness measurement, carbon content measurement, index Ms calculation] Using a part of the rotary bending fatigue test piece after carburization, hardness measurement, C amount measurement, and index Ms calculation were performed on the surface layer (position 25 μm deep from the carburized surface) as follows. First, a sample was prepared with the vertical cross section of the notch bottom of the test piece as the test surface, embedded in resin and polished. The Vickers hardness was measured based on JIS Z 2244 (2009) at five arbitrary points on the test surface at a depth of 25 μm from the surface near the notch bottom. The test force was 2.9 N. The average of the five Vickers hardness values ​​obtained was defined as the Vickers hardness of the surface layer. If the Vickers hardness of the surface layer was 630 HV or higher, the Vickers hardness of the surface layer was deemed to be sufficiently high.

[0074] Next, the test piece after hardness measurement was polished again and then indexed from the resin and subjected to carbon content analysis by EPMA. Starting from an arbitrary position 25 μm deep from the surface, line analysis was performed in a direction parallel to the surface. The measurement step was 2 μm, the measurement time for each measurement point was 2.0 seconds, and the measurement line length was 50 μm. Although the surface of the test piece on the cross section is strictly arc-shaped, the measurement line length is sufficiently short compared to the radius of the arc, so the surface of the test piece was considered to be a straight line, and the measurement line was considered to be a straight line. Such line analysis was performed twice at different positions, and the average value was considered to be the C content of the surface layer of the test piece of each test number.

[0075] Since the diffusion distance of substitutional alloying elements during carburization is extremely short, the Si, Mn and Cr contents in the surface layer were considered to be equal to the values ​​in the bulk, and the index Ms, which represents the Ms point (°C), was calculated.

[0076] [Rotary bending fatigue test] The rotating bending fatigue test specimens after carburizing were subjected to fatigue testing after the gripping portion was machined from φ12.4 mm to φ12.0 mm in order to align the axis. The rotating bending fatigue test was carried out in the air at room temperature (25°C) in accordance with JIS Z2274 (1978). The rotation speed during the test was 3000 rpm, and the number of repetitions was 1.0 x 10 7 The highest stress among the test pieces that did not break up to 1000 ps was defined as the fatigue strength (MPa) of that test number. A fatigue strength of 500 MPa or more was determined to be excellent.

[0077] [Investigation of variation in deformation amount] Among test numbers 1 to 26, the test pieces for measuring the amount of deformation after carburizing treatment (test pieces with test numbers 1 to 10, 12, 15, 16, and 18 to 20) had high hardness in the surface layer and therefore sufficient fatigue strength, and were used to investigate the variation in the amount of deformation during carburizing treatment. Specifically, a contact type roughness meter was used to measure the cross-sectional curve in the axial direction on the back side of the keyway of the test pieces. The measurement range was 95 mm, excluding 2.5 mm from both ends of the test pieces. The obtained cross-sectional profile was approximated by a circular arc to eliminate the effects of measurement error and surface defects, and the difference between the straight line connecting both ends of the arc and the circular arc at its maximum was defined as the amount of bending of the test piece. The average of the amounts of bending of three test pieces hung in a basket with the same orientation was taken as the amount of bending for each hanging direction. The absolute value of the difference between the maximum and minimum values ​​of the amount of bending for each of the three hanging directions was taken as the variation in the amount of deformation. When the variation in the amount of deformation was 20 μm or less, it was considered to be sufficiently small.

[0078] [Table 1]

[0079] [Table 2]

[0080] [Test Results] Test numbers 1 to 10 are examples within the scope of the present invention, with fatigue strengths of 500 MPa or more and deformation variations of 14 μm or less, which shows that the fatigue strength is increased while the deformation variations are reduced. It is also clear that the hardness of the steel material after softening heat treatment is low and the machinability is high.

[0081] In contrast, it is clear that the comparative examples of test numbers 11 to 26, which do not comply with the provisions of the present invention, do not achieve the targeted performance.

[0082] Specifically, in test numbers 11 and 13, the Mn content was high or the index Ms was low, so that retained austenite was formed, sufficient hardness was not obtained in the surface layer after carburizing treatment, and the fatigue strength was also low. Test No. 12 had a large C content, and therefore the steel material after softening heat treatment had high hardness and low machinability. In test numbers 14 and 17, the martensitic transformation was incomplete due to the small amount of Mn, so sufficient hardness was not obtained and the fatigue strength was also low. Test Nos. 15 and 16 have a large Cr content, and the steel material after softening heat treatment has high hardness and low machinability. Test numbers 18 to 20 were made using general JIS steel that had been carburized under general carburizing conditions and then oil-cooled, so the hardness and fatigue strength were sufficiently high, but the amount of deformation varied greatly depending on the hanging direction during carburization. Test numbers 21 to 23 are general JIS steels that have been carburized and then cooled in nitrogen. However, the chemical composition is not within the scope of the present invention and is not optimized. If the cooling after carburization is allowed to proceed naturally, martensitic transformation does not occur, and the hardness of the surface layer after carburization is extremely low. Therefore, the fatigue strength is also low. Test No. 24 has a chemical composition within the range of the present invention, but the surface layer has a high C content. This C content value is close to the carbon content of the surface layer of a typical carburized steel part. This test No. has a large amount of retained austenite, and the surface layer does not have sufficient hardness after carburizing, and the fatigue strength is also low. Test No. 25 has a chemical composition within the range specified by the present invention, but has a low carbon content in the surface layer, low hardness, and low fatigue strength. Test Example 26 has a chemical composition within the range specified by the present invention, but the hardness of the surface layer after carburizing is low, and the fatigue strength is also low.

Claims

1. In mass percent, C: 0.06-0.25%, Si: 0.01-0.90%, Mn: 3.51-6.00%, P: 0.05% or less, S: 0.001-0.100%, Cr: 0.03-1.49%, Al: 0.001-0.050%, N: 0.0030 to 0.0250%; The balance is Fe and impurities, The following index Ms, which indicates the Ms point (°C) at a depth of 25 μm from the carburized surface, is 30°C or higher, The amount of C at a depth of 25 μm from the carburized surface is 0.40 to 0.70% by mass, A carburized steel part having a hardness of 630 HV or more at a depth of 25 μm from the carburized surface. Ms=219.2-1.3×Si-31.7×Mn-11.6×Cr In the formula expressing the index Ms, each element symbol indicates the content (mass %) of each element.

2. In mass percent, Ti: 0.05% or less, Nb: 0.05% or less Mo: 0.25%, V: 0.15% or less, Cu: 0.50% or less, Ni: 0.50% or less; B: 0.005% or less, 2. The carburized steel part according to claim 1, further comprising one or more of the following:

3. A method for manufacturing a carburized steel part according to claim 1 or 2, comprising the steps of: The carburizing steel is subjected to a forming process by hot forging, a softening heat treatment process at 650 to 750°C for 30 to 640 minutes, and a cutting process in this order to obtain a steel part. A method for manufacturing a carburized steel part, comprising carburizing the steel part so that the amount of C at a position 25 μm deep from the surface of the carburized steel part is 0.40 to 0.70% by mass, and then cooling from the carburizing temperature from 800°C to 200°C at a cooling rate of 0.01 to 2°C / s.

Citation Information

Patent Citations

  • Carburizing manganese steel

    CN104294178A

  • Manufacture of parts for mechanical structure

    JP1987196322A

  • Case-hardening steel for carburizing and parts for machine structural use made therefrom

    JP1987196360A

  • Bar steel for carburizing low in amount of heat treating strain and its variance

    JP1990277744A

  • Method of producing carburized and quenched member, and carburized and quenched member

    JP2003193128A