Sinter manufacturing method
A divided granulation method using a 50-100% hematite-magnetite fine ore mix maintains sintered ore strength, addressing the limitations of magnetite-based fine ore distribution and enhancing production properties.
Patent Information
- Application Number
- JP2021028678
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-25
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2041-02-25
AI Technical Summary
The challenge is to replace magnetite-based fine ore with readily available hematite-based fine ore in sintered ore production without compromising the strength of the sintered ore, as magnetite-based fine ore is not widely distributed in the seaborne trade market and its combination with hematite-based fine ore has not been adequately studied.
A method involving a divided granulation process where magnetite-based and hematite-based fine ores are mixed in a ratio of 50% to 100% by mass, with the magnetite-based fine ore's particle size equal to or less than that of the hematite-based, and combined with a sub-granulation step using a mixture of hematite-based and magnetite-based fine ores to enhance strength.
This approach maintains the strength of sintered ore while allowing the use of hematite-based fine ore, improving handling properties and sinter strength during production.
Smart Images

Figure 0007587142000007 
Figure 0007587142000008 
Figure 0007587142000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for granulating a fine raw material in the production of sintered ore, and in particular to a method for granulating a fine raw material using a separate granulation method. [Background technology]
[0002] In recent years, the amount of gangue components (SiO2·Al2O3) in iron ore has increased due to the depletion and deterioration of iron ore resources. Therefore, it will be important in the future to increase the amount of finely powdered ore (also called concentrate or pellet feed (PF)) that has been artificially treated to have a high Fe content in the ore dressing process, and to maintain or reduce the amount of gangue components (SiO2·Al2O3) in iron ore in the production of sintered ore.
[0003] Therefore, technological development is being carried out to granulate fine ore using selective and separate granulation equipment to produce coarse granules with diameters of 5 to 15 mm, and then to feed these into a sintering machine together with raw materials processed using conventional granulation equipment in order to reduce the amount of ungranulated powder and avoid the deterioration of the air permeability of the raw material packed bed caused by the fine ore and the drop in productivity [Non-Patent Document 1].
[0004] Here, hematite-based (Fe2O3) fine ore and magnetite-based (Fe3O4(FeO·Fe2O3)) fine ore are known as types of fine ore. Patent Document 1 discloses a method of using magnetite-based fine ore alone.
[0005] Non-Patent Document 2 also indicates the finding that magnetite-based fine ore, even without the addition of CaO, has a post-sintering strength equivalent to that of hematite-based fine ore to which CaO has been added. Furthermore, Patent Document 2 shows that when granulating hematite-based fine ore, the strength of the granulated material is improved by adding core fine ore to the fine ore in a ratio (fine ore / fine ore) of 1.5 / 1 or more and less than 3 / 1. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-253281 A [Patent Document 2] JP 2016-191122 A [Non-patent literature]
[0007] [Non-Patent Document 1] TK Sandeep et al:Metallurgical and Materials Transaction B, Volume 46B, No 2(2015), 635 [Non-Patent Document 2] TK Sandeep et al.: Metallurgical and Materials Transaction B, Volume 47B, No 1(2016), 309 Summary of the Invention [Problem to be solved by the invention]
[0008] As will be described in detail later, when a large amount of magnetite-based fine ore is used, for example, the strength of sintered ore is increased. For this reason, there is a growing demand to produce sintered ore using as much magnetite-based fine ore as possible. However, magnetite-based fine ore is often processed into pellets at a pellet factory located near a mine or at a shipping port before being shipped. For this reason, the amount of magnetite-based fine ore circulating in the iron ore sea trade market is currently small. Therefore, as in the method described in Patent Document 1, it is not feasible to use magnetite-based fine ore as the entire amount of iron ore used as a raw material for sintered ore without using hematite-based fine ore. In addition, there has been no study to use hematite-based fine ore and magnetite-based fine ore in combination. In the method described in Patent Document 2, the addition of fine ore as a nucleus is considered, but there has been no study to use hematite-based fine ore and magnetite-based fine ore in combination while using such fine ore as a nucleus.
[0009] The object of the present invention is to provide a method for producing sintered ore that can replace magnetite-based fine ore with easily available hematite-based fine ore while suppressing a decrease in strength of the sintered ore after firing. That is, the present invention clarifies a replacement range in which a granulated product in which a part of magnetite-based fine ore is replaced with hematite-based fine ore is equivalent to a granulated product made of only magnetite-based fine ore in terms of handling during sintered ore production and sintered ore strength after firing. [Means for solving the problem]
[0010] First, the inventors conducted a basic experiment using an electric furnace to measure the strength of a mixture of magnetite-based fine ore and hematite-based fine ore after sintering. The inventors then clarified that if the mixture contains magnetite-based fine ore at a mixing ratio of 50% by mass or more, the sintered product of the mixture exhibits the same strength as that of a sintered product containing only magnetite-based fine ore. Next, the inventors conducted a sintering experiment under practical raw material blending conditions. As a result, the inventors confirmed that the strength of the sintered ore can be obtained by setting the mixing ratio of magnetite-based fine ore to the total mass of hematite-based fine ore and magnetite-based fine ore within the above range, as well as the strength of the sintered ore, that is, the strength of the sintered ore can be obtained by using only magnetite-based fine ore (i.e., using only magnetite-based fine ore as the fine ore of the iron-containing raw material). The present invention was devised based on the results of such investigations, and the gist of the present invention is as follows.
[0011] The gist of the present invention is as follows. According to one aspect of the present invention, there is provided a method for producing sintered ore, which comprises: dividing a sintering raw material into a main sintering raw material and a sub-sintering raw material containing fine ore; performing a main granulation process in which the main sintering raw material is mixed and granulated; and performing a sub-granulation process in which the sub-sintering raw material is mixed and granulated in parallel; combining the granulated products produced in the main granulation process and the sub-granulation process; and firing the combined granulated product to produce sintered ore. The method is characterized in that the fine ore used in the sub-granulation process is a mixture of magnetite-based fine ore and hematite-based fine ore, and the mixing ratio of the magnetite-based fine ore to the total mass of the magnetite-based fine ore and the hematite-based fine ore is 50% by mass or more and less than 100% by mass. Here, the particle size of the magnetite-based fine ore is preferably equal to or smaller than the particle size of the hematite-based fine ore. Furthermore, it is preferable that the auxiliary sintering raw material further contains fine ore, and the mass ratio of the fine ore to the fine ore is 1.5 / 1 or more and less than 3 / 1. Effect of the Invention
[0012] The magnetite-based fine ore powder can be replaced with the hematite-based fine ore powder while suppressing a decrease in the strength of the sintered ore after firing. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram of an apparatus used in a basic experiment using an electric furnace. [Diagram 2] FIG. 1 is a diagram showing the relationship between the mixing ratio (mass%) of magnetite-based fine ore and the average particle size (mm) after dropping. [Diagram 3] FIG. 2 is a diagram showing a schematic flow of a granulation processing system (granulation device). [Figure 4] FIG. 2 is a diagram showing a schematic configuration of an apparatus used in a sintering experiment (pot test). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] A preferred embodiment of the present invention will be described in detail below with reference to the accompanying drawings. Each raw material used in this embodiment is an aggregate of many particles. Unless otherwise specified, the name of each raw material refers to the aggregate of particles that constitute the raw material. A numerical range expressed using "~" means a range that includes the numerical values written before and after "~" as the lower and upper limits. A numerical value indicated as "greater than" or "less than" does not fall within the numerical range.
[0015] <Basic studies leading to the present invention> When hematite fine ore is mixed with magnetite fine ore, it is considered that the strength changes depending on the mixing ratio of magnetite fine ore due to the difference in the properties of hematite fine ore and magnetite fine ore. Therefore, the change in strength when hematite fine ore is mixed with magnetite fine ore was experimentally investigated.
[0016] (Experimental method and conditions) Hematite-based fine ore (sometimes referred to as H in this experiment) and magnetite-based fine ore (sometimes referred to as M in this experiment) were used as samples (Table 1). In order to examine the effects of the mixing ratio and particle size combination of magnetite-based fine ore, each ore was sieved into 20-45 μm and 63-125 μm. Here, in the particle size range by sieve classification, "A-B μm" indicates the particle size range of the ore that remained on the sieve with mesh size A (μm) and fell through the sieve with mesh size B (μm). In sieve classification, "A-B μm" indicates A or more and less than B. Hereafter, hematite fine ore with a size of 20 to 45 μm will be referred to as H-fine, and 63 to 125 μm as H-coarse. Similarly, magnetite fine ore with a size of 20 to 45 μm will be referred to as M-fine, and 63 to 125 μm as M-coarse. Table 1 also shows the compositions of H-fine, H-coarse, M-fine, and M-coarse. The compositions were determined by chemical analysis.
[0017] A total of 29 samples were prepared by changing the mixing ratio from 7 to 9 levels under four combination conditions (2 levels of ore type and 2 levels of particle size).The effects of the mixing ratio and particle size combination of magnetite fine ore were examined using these samples.
[0018] Specifically, first, about 3.6% water was added to about 1.6 g of a mixture of two types of fine ore (two types from among H fine, H coarse, M fine, and M coarse) mixed at a specified mixing ratio, and the mixture was filled into a die and subjected to a pressure of 4.8 MPa for 30 seconds. This produced a cylindrical tablet with a diameter of 8 mm and a height of about 10 mm.
[0019] [Table 1]
[0020] The molded tablets were then sintered in an electric furnace with a heat pattern simulating that of an actual sintering machine (heating rate 200°C / min, maximum temperature reached 1300°C, maximum temperature holding time 0 seconds, cooling rate 67°C / min). The equipment used for sintering is shown in Figure 1. A drop weight test was conducted in which a 300g load was dropped from a height of 30cm three times on the sintered tablets. After the drop weight test, the samples were sieved to calculate the average particle size (average particle diameter) and evaluate their strength. (Hereinafter, this is referred to as the average particle size after dropping.) Specifically, sieves with openings of 4.75 mm, 2.8 mm, 2.0 mm, 1.0 mm, 0.5 mm, 0.25 mm, and 0.125 mm were stacked to perform sieving, and the average value of each sieve and the next upper sieve was taken as the representative particle size (for example, 2.4 mm for 2.0 to 2.8 mm), and the weighted average value was calculated by the sum of the products of the representative particle size and the weight ratio. From the viewpoint of the strength of the actual sintered ore, it is considered necessary for the average particle size after dropping to be 1.5 mm or more in order to ensure the minimum sintered ore strength without forming localized brittle parts. It is more preferable for the average particle size after dropping to be 2.5 mm or more because a sufficiently high strength can be obtained.
[0021] Four tablets were fired for each level, three were subjected to a drop weight test, and one was embedded in resin and polished for cross-sectional structure observation and image analysis. In addition, one tablet each with a mixing ratio of magnetite-based fine powder ore of 25 mass%, 50 mass%, and 75 mass% was molded, and then embedded in resin without firing, polished, and subjected to cross-sectional structure observation and image analysis.
[0022] (Experimental Results) The change in the average particle size after dropping is shown in Figure 2. Under all different particle size combination conditions, the average particle size after dropping, i.e., the strength after sintering, increased with an increase in the mixing ratio of magnetite-based fine ore (here, M fine or M coarse). However, the increase in strength was not constant; when the mixing ratio of magnetite-based fine ore was less than 25 mass%, there was almost no increase, and when the mixing ratio was 25 to 50 mass%, the increase was particularly large, and after 50 mass%, the slope became gentle again, and when the mixing ratio was 75 mass% to 80 mass%, the strength value was roughly equivalent to that of magnetite-based fine ore alone (100%). It was also found that the tablets had higher strength in combinations that included M fine.
[0023] (action) There are three bonding mechanisms for granulated products of magnetite-based fine ore and hematite-based fine ore: (1) bonding between magnetite particles, (2) bonding between magnetite particles and hematite particles, and (3) bonding between hematite particles. Of these, (1) has a stronger bonding strength than (2) and (3). This is thought to be because magnetite particles are oxidized by the temperature rise accompanying the sintering reaction and change into hematite particles, and the changes in crystal structure and volume at that time promote diffusion bonding between particles. Therefore, the strength is improved by increasing the amount of magnetite-based fine ore.
[0024] In addition, when the mixing ratio of magnetite-based fine ore is 50% by mass or more, the bonds of (1) form a network throughout the entire granulated material. Once this network is formed throughout the entire granulated material, the strength improvement thereafter becomes gradual. Therefore, when the mixing ratio of magnetite-based fine ore is 50% by mass or more, the strength of the tablet becomes approximately equal to the strength value of a tablet made from magnetite-based fine ore alone.
[0025] Here, it is thought that the combination of raw materials with different particle sizes affects network formation. In the case of a combination of H coarse and M fine, fine magnetite particles fill the voids around and between the hematite particles, and a network of type (1) with high bonding strength is formed as easily as in the combination of H fine and M fine. On the other hand, in the case of a combination of H fine and M coarse, fine hematite particles, which have weak bonding strength, fill the voids around and between the magnetite particles, and the formation of a network of type (1) with high bonding strength is inhibited. In the case of the combination of H coarse and M coarse, the number of particles and therefore the number of contact points between the particles are small, so the strength is also low. However, in any combination of particle sizes, if the mixing ratio of magnetite fine ore is 50 mass% or more, the average particle size after dropping is 1.5 mm or more.
[0026] <Embodiment> The present invention was devised based on the above-mentioned fundamental studies, and is a method for producing sintered ore having a secondary granulation process for selectively strengthening the granulation of fine raw materials, characterized in that the fine raw materials are a mixture of hematite-based fine ore and magnetite-based fine ore, and the mixing ratio of the magnetite-based fine ore to the total mass of both is 50 mass% or more and less than 100 mass%. Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings.
[0027] (Overall composition) FIG. 3 shows the flow of the granulation process system in this embodiment. This granulation process is a raw material processing method known as selective granulation or divided granulation. As shown in FIG. 3, in this granulation process, the sintering raw material is divided into a main sintering raw material group 11 and a sub-sintering raw material group 21, which are mixed and granulated. Specifically, in this granulation process, a main granulation process 1 for granulating the main sintering raw material group 11 and a sub-granulation process 2 for granulating the sub-sintering raw material group 21 are performed in parallel. After that, the granulated products 3 produced in the main granulation process 1 and the sub-granulation process 2 are combined, and the combined granulated products 3 are fired in a sintering machine 4.
[0028] (Main granulation process) In the main granulation process 1, a predetermined amount of the main sintering raw material group 11 is supplied from a hopper 111 to a conveyor 112, and the main sintering raw material group 11 is blended on the conveyor 112. The conveyor 112 supplies the blended raw materials of the main sintering raw material group 11 to a drum mixer 12. The blended raw materials of the main sintering raw material group 11 are mixed and granulated in the drum mixer 12 to produce pseudo-particle granules 13. The main sintering raw material group 11 includes an iron-containing raw material, an auxiliary raw material, return ore, dust, and carbonaceous material. The main sintering raw material group 11 is the remaining raw materials excluding the raw materials selected as the auxiliary sintering raw material group 21 described below.
[0029] In FIG. 3, a connected tandem type drum mixer is arranged, but a plurality of drum mixers may be arranged in series, or mixing and granulation may be performed by a single drum mixer.
[0030] (Sub-granulation process) In the secondary granulation process 2, a predetermined amount of the secondary sintering raw material group 21 is supplied from a hopper 2111 to a conveyor 2112, and the secondary sintering raw material group 21 is blended on the conveyor 2112. The conveyor 2112 supplies the blended raw material of the secondary sintering raw material group 21 to a granulator. The blended raw material of the secondary sintering raw material 11 is then mixed and granulated in the granulator to produce granulated pseudo-particles 24. The granulator is preferably, for example, a combination of a high-speed stirring mixer 22 and a dish-type pelletizer 23 in this order. The granulator is not limited to the above example, as long as the former has a high mixing and stirring function and the latter has a high granulation function.
[0031] Table 2 shows an example of the composition of the auxiliary sintering raw material group 21. The mixing ratio of the auxiliary sintering raw material group 21 is preferably in the range of 15% by mass to 30% by mass with respect to the total mass of the entire blended raw materials (the blended raw materials of the main sintering raw material 11 and the auxiliary sintering raw material 21). If it is less than 15% by mass, the effect of improving productivity is low, and if it exceeds 30% by mass, there is a possibility that processing cannot be performed due to insufficient equipment capacity.
[0032] [Table 2]
[0033] The auxiliary sintering raw material group 21 mainly contains fine raw material powder 211 which is the target of enhanced granulation. The fine raw material powder 211 is selectively enhanced in granulation in the auxiliary granulation process 2. This is because the drum mixer 12 used as a granulator in the main granulation process 1 is not suitable for granulating the fine raw material powder 211.
[0034] The feature of the present invention is that the fine raw material powder 211 is a mixture of hematite-based fine ore 211a and magnetite-based fine ore 211b. Furthermore, the mixing ratio of the magnetite-based fine ore 211b is 50 mass% or more and less than 100 mass% with respect to the total mass of the magnetite-based fine ore 211b and the hematite-based fine ore 211a. As explained in Fig. 2, by making the mixing ratio of the magnetite-based fine ore 211b 50 mass% or more, the strength after firing equivalent to that in the case where the magnetite-based fine ore is used alone can be obtained.
[0035] The first embodiment in Table 2 is an example in which the mixing ratio of magnetite-based fine ore and hematite-based fine ore is 50 mass%. Examples of the hematite-based fine ore include concentrates from Brazil and Canada. Examples of the magnetite-based fine ore include concentrates from North America, South America, Europe, Australia, and Africa.
[0036] Since fine raw materials are shipped after being dressed at each iron ore mine, they have a certain particle size distribution according to their mineralogical characteristics and processing process. Methods for measuring particle size distribution include sieve passing weight rate and laser diffraction / scattering method, and evaluation indices include median diameter (cumulative 50 mass% diameter) and average particle size.
[0037] In the above-mentioned basic study, the strength after firing was low in the case of the combination of H-coarse + M-coarse in which both the hematite-based fine ore and the magnetite-based fine ore were 63 to 125 μm, but sufficient strength was obtained in other combinations. In addition, the strength after firing was particularly high in the combination of H-fine and M-fine, and in the combination of H-fine and M-coarse. Therefore, in the method according to the present invention, the particle size of the magnetite-based fine ore is preferably equal to or smaller than the particle size of the hematite-based fine ore. In addition, the preferred particle size of the hematite-based fine ore is less than 125 μm, and the preferred particle size of the magnetite-based fine ore is less than 45 μm. More preferably, the particle sizes of both the hematite-based fine ore and the magnetite-based fine ore are less than 45 μm. The smaller the particle size of the magnetite-based fine ore, the more the productivity and the like tend to improve. The more preferred particle size of the magnetite-based fine ore is 15 μm or less. Furthermore, there is no particular lower limit for the particle size of any of the fine ores.
[0038] In order to promote the granulation of the fine raw material in the secondary granulation step 2, fine ore (core ore) 212 as the nucleus of granulation may be used together. When the mass ratio of the fine ore to the fine ore (core ore) is 1.5 / 1 or more and less than 3 / 1 (fine ore / fine ore), the strength of the granulated product after granulation is the highest. As the nucleus ore, sinter feed (hereinafter referred to as SF) that is usually used in the production of sintered ore may be used. Specifically, limonite-based ore is preferable in that the fine raw material has strong adhesion when the ore is used as a granulation nucleus. The embodiment 2 shown in Table 2 is an example in which 1 / 3 mass% (mass% relative to the total mass of the fine ore and the fine ore) of Australian limonite is used as the nucleus ore.
[0039] In order to promote the granulation of the fine powder raw material, a binder such as quicklime can be appropriately used. In the case of quicklime, it is preferable to use 5 mass% or less of the total mass of the auxiliary sintering raw material. In the third embodiment, in addition to the second embodiment, quicklime is used in an amount of 0.5 mass% of the total mass of the entire blended raw material (2.2 mass% of the total mass of the auxiliary sintering raw material).
[0040] In addition, the raw materials blended in the secondary granulation step 2 may contain any sintering raw materials as long as they do not inhibit the granulation of the fine powder raw materials. EXAMPLES
[0041] In order to confirm the feasibility and effects of the present invention, the influence of the ratio of fine ore used in the secondary granulation process on sinter productivity and sinter strength in the granulation process shown in FIG. 3 was investigated by a sinter pot test. The results are described below as an example. The present invention is not limited to this one example. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0042] (Experimental Equipment) The main specifications of the experimental equipment used in the sintering experiment are listed in Table 3, and the configuration of the experimental equipment is shown in Figure 4. The sintering pot consists of the pot body and a wind box located below it. A thermocouple is inserted in the wind box, and the sintering completion point is determined based on the point at which the temperature reaches its maximum. A pressure gauge is inserted in the wind box to measure the negative pressure under the pot. The wind box is connected to the suction blower by piping. The piping is equipped with a gas sampling probe (pump for component analysis) connected to a gas component analyzer (component analysis device), and an orifice flow meter for measuring the flow rate. The ignition furnace is installed above the sintering pot during ignition and can be moved to a retreat position during sintering. A drum-type granulator (not shown) was used to granulate the raw materials for the main line, and an Eirich-type and pan-type batch-type granulator was used for the side line.
[0043] [Table 3]
[0044] (Experimental methods and conditions) (Raw material blend) In this embodiment, the hematite-based fine ore 211a was made of ore H1 produced in Brazil, and the magnetite-based fine ore 211b was made of ore M1 produced in Sweden. The particle sizes were measured by a laser diffraction / scattering method, and the average particle sizes were calculated to be 26 μm and 19 μm, respectively.
[0045] Furthermore, as a verification example of the case where finer magnetite-based fine ore is used, Australian magnetite-based fine ore M2 was used. The average particle size was 14 μm.
[0046] Tables 4 and 5 show the raw material blending in the main granulation process and the secondary granulation process. The raw material blending in the main granulation process was all constant. The mixing ratio of magnetite-based fine ore and hematite-based fine ore in the secondary granulation process was set to 15.0 mass% in total (relative to the total mass of the blended raw materials of the main sintering raw material and the secondary sintering raw material), and tests were conducted in which the mixing ratio of magnetite-based fine ore (mass% relative to the total mass of the hematite-based fine ore and the magnetite-based fine ore) was changed to 0 mass%, 25 mass%, 50 mass%, 75 mass%, and 100 mass%. In addition, fine ore (core ore) that serves as the nucleus of granulation was also used. The core ore was limonite (fine ore) produced in Australia. The mixing ratio of the core ore was set to a constant 7.5 mass% (relative to the total mass of the blended raw materials of the main sintering raw material and the secondary sintering raw material).
[0047] [Table 4]
[0048] [Table 5]
[0049] Here, in the sintering process, it is customary to include return ore, which is generated as a by-product during sintering and recycled as a raw material, and carbonaceous materials such as coke fines that are burned and lost during sintering. The total of so-called new raw materials excluding these is 100% by mass, and the total raw materials including return ore and carbonaceous materials is 119.7% by mass.
[0050] (granulation) In the main granulation process, the main sinter raw materials, return ore and fine coke were put into a drum mixer and rolled for 2 minutes to mix the raw materials. After that, the raw materials were rolled for another 3 minutes and 45 seconds while pouring a specified amount of water into the mixer so that the moisture content was 7.0%, and granulation was performed.
[0051] In the secondary granulation process, the secondary sintering raw materials were put into a high-speed agitating mixer, water was added, and the mixture was mixed and stirred for 1 minute.Then, the mixture was put into a pan pelletizer at 1 wet-kg, and the discharged granules were collected one by one.
[0052] Next, the granules produced in the main granulation process and the sub-granulation process were lightly mixed for 15 seconds in the drum mixer to combine these granules.
[0053] (Pot roasting) The granules (combined granules) produced in the granulation process were charged into a sintering pot to form a raw material packed bed. Next, the surface of the raw material packed bed was ignited and time measurement was started. Here, the ignition was performed with a constant air flow (1.5 Nm 3 The surface of the raw material packed bed was heated to 1300°C for 1 minute in an ignition furnace while continuing downward suction at a rate of 100 / min. After ignition, the raw material packed bed was sintered at a constant negative pressure below the pot of 9.8 kPa. The end of sintering was determined as the time when the exhaust gas temperature (measured with a thermocouple installed in the wind box) reached its maximum value, and the sintering time was defined as the time from the start of ignition to the end of sintering. Three minutes after the end of sintering, the blower was stopped and the sintered cake was collected from the pot. Thermocouples were also placed in the middle and bottom layers and below the sintering pot to measure the temperature changes in each layer.
[0054] The sintered cake obtained after the firing was dropped four times from a height of 2 m, and then classified using a square sieve with a diameter of 5 mm. The sieve-surface was regarded as the product sintered ore, and the product yield of +5 mm was evaluated. The productivity was also calculated from the firing time and the product yield.
[0055] (Experimental Results) The test results are shown in Table 6. The productivity did not change between Comparative Example 1, in which the fine powder raw material in the secondary granulation process was only hematite fine powder, and Comparative Example 2, in which the mixing ratio of magnetite-based fine ore was 25 mass%, but an improvement was observed from Example 1, in which the mixing ratio was 50 mass%, and Example 2, in which the mixing ratio was 75 mass%, obtained a value roughly close to that of the reference example, in which only magnetite fine powder was used.
[0056] Regarding particle size, in Example 3 in which the mixing ratio of magnetite-based fine ore was 50 mass % and finer magnetite-based fine ore M2 was used, a higher productivity was obtained than in Example 1.
[0057] [Table 6]
[0058] (Conclusion) The results of the basic test mentioned above were also confirmed in the sintering experiment. That is, it was confirmed that by mixing magnetite-based fine ore at a mixing ratio of 50 mass% or more and by mixing magnetite-based fine ore with finer particles than hematite-based fine ore, higher productivity can be obtained than by using hematite-based fine ore alone.
[0059] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or amended examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally fall within the technical scope of the present invention. [Industrial Applicability]
[0060] The present invention can be used in a method for producing sintered ore that can replace magnetite-based fine ore powder with easily available hematite-based fine ore powder while suppressing a decrease in strength of the sintered ore after firing. [Explanation of symbols]
[0061] 1: Main granulation process 11: Main sintering material 12: Drum mixer Granules produced at 13:12 2: Sub-granulation process 21: Sub-sintering materials group 211: Fine powder raw material to be granulated 211a: Hematite ore fines 211b: Magnetite ore fines 212: Nuclear ore 22: High-speed mixing mixer 23: Dish-type pelletizer 24: Granules produced in 22 and 23 3: Granules produced in the main granulation process and the secondary granulation process 4: Sintering machine
Claims
1. A method for producing sintered ore, comprising the steps of: dividing a sintering raw material into a main sintering raw material and a secondary sintering raw material containing fine iron ore; carrying out a main granulation process in which the main sintering raw material is mixed and granulated; and a secondary granulation process in which fine iron ore, fine iron ore, and a binder are mixed and granulated as the secondary sintering raw material in parallel; combining the granules produced in the main granulation process and the secondary granulation process; and firing the combined granules, The fine ore used in the secondary granulation step is a mixture of magnetite-based fine ore and hematite-based fine ore, and a mixing ratio of the magnetite-based fine ore to the total mass of the magnetite-based fine ore and the hematite-based fine ore is 50 mass% or more and less than 100 mass%.
2. A method for producing sintered ore as described in claim 1, characterized in that the fine ore is limonite.
3. 3. The method for producing sintered ore according to claim 1, wherein the particle size of the magnetite-based fine ore is equal to or smaller than that of the hematite-based fine ore.
4. A method for producing sintered ore as described in claim 3, characterized in that the particle size of the magnetite-based fine ore is 19 μm or less.
5. 5. The method for producing sintered ore according to claim 1, wherein the auxiliary sintering raw material further contains fine ore, and a mass ratio of the fine ore to the fine ore is 1.5 / 1 or more and less than 3 / 1.
Citation Information
Patent Citations
Method for producing sintered ore
JP2013253281A
Pseudo particles for sintered ore production
JP2016176122A
Method for producing sintered ore
JP2016191122A
Method of granulating sintering material for iron manufacturing