Polarizing film with pressure-sensitive adhesive layer, image display panel, method for producing image display panel, and pressure-sensitive adhesive layer

The polarizing film with a specialized adhesive composition addresses the challenge of reworkability and durability in high-temperature environments by using a compound with an acidic group and polyether compound, ensuring effective peeling and durability.

JP7587367B2Active Publication Date: 2024-11-20NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020130893
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-31
Publication Date
2024-11-20
Estimated Expiration
2040-07-31

AI Technical Summary

Technical Problem

The existing polarizing films with adhesive layers face issues of reduced reworkability and durability when attached to conductive layers in high-temperature environments, particularly due to the adhesive layer's improved adhesiveness during preheating, which compromises its ability to be peeled off from transparent substrates.

Method used

A polarizing film with an adhesive layer composed of a specific adhesive composition containing a compound with an acidic group or acid anhydride group and a polyether compound, ensuring adhesive strength within certain limits to maintain reworkability and durability, even when attached to conductive layers.

Benefits of technology

The adhesive layer maintains reworkability after preheating and exhibits durability in high-temperature environments, allowing for easy peeling from transparent substrates while maintaining optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587367000011
    Figure 0007587367000011
  • Figure 0007587367000012
    Figure 0007587367000012
  • Figure 0007587367000013
    Figure 0007587367000013
Patent Text Reader

Abstract

To provide a polarization film having an adhesive layer, equipped with an adhesive layer capable of maintaining reworkability after preheating even if adhered onto a conductive layer while having durability under a high temperature environment.SOLUTION: A polarization film having an adhesive layer includes a polarization film and an adhesive layer formed of an adhesive composition. The adhesive composition includes a compound (C) containing an acidic group or an acid anhydride group and a polyether compound (D). In the adhesive layer, an adhesive force P85 is 10.0 N / 25 mm or less and an adhesive force P105 is larger than 10.0 N / 25 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing film with a pressure-sensitive adhesive layer, an image display panel, a method for producing an image display panel, and a pressure-sensitive adhesive layer. [Background technology]

[0002] An image display panel included in an image display device such as a liquid crystal display device has a structure in which a polarizing film is attached to a transparent substrate via an adhesive layer, for example. A conductive layer containing a metal oxide such as indium tin oxide (ITO) may be provided on the surface of the transparent substrate in order to prevent the image display device from being charged. When a conductive layer is provided on the surface of the transparent substrate, the adhesive layer is usually in direct contact with the conductive layer in the image display panel.

[0003] When manufacturing an image display panel, for example, a polarizing film with an adhesive layer, which includes an adhesive layer and a polarizing film, is attached to a transparent substrate. At this time, problems may occur such as the attachment position of the polarizing film with an adhesive layer being shifted, or foreign matter being mixed between the polarizing film with an adhesive layer and the transparent substrate. In this case, in order to improve the productivity of the image display panel, it is desirable to peel the polarizing film with an adhesive layer from the transparent substrate and reuse the member. Therefore, it is required that the polarizing film with an adhesive layer can be easily peeled off from the transparent substrate. In this specification, the ease of peeling the polarizing film with an adhesive layer from the transparent substrate or the conductive layer may be expressed as "reworkability of the adhesive layer". [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6071459 Summary of the Invention [Problem to be solved by the invention]

[0005] When the moisture content of the polarizing film is large, the optical properties of the image display device tend to deteriorate when the image display device is used in a high-temperature environment (for example, in an environment with a temperature higher than 95°C) (for example, Patent Document 1). The deterioration of optical properties in a high-temperature environment is particularly noticeable when the polarizer in the polarizing film contains polyvinyl alcohol. Therefore, when it is expected that the image display device will be used in a high-temperature environment, for example, when the image display device is used as an in-vehicle display, it is necessary to heat-treat (preheat) the polarizing film with the adhesive layer at a temperature of about 70°C to 95°C at the stage when the polarizing film with the adhesive layer is attached to a transparent substrate, thereby reducing the moisture content of the polarizing film in advance.

[0006] However, this preheating may damage the polarizing film or the transparent substrate. Therefore, even after the preheating, it is required that the reworkability of the adhesive layer is maintained so that the polarizing film with the adhesive layer can be peeled off from the transparent substrate. However, the composition of the adhesive layer in the polarizing film with the adhesive layer is usually adjusted so that the adhesive layer improves in a high temperature environment. Therefore, when the above preheating is performed, the adhesive layer tends to improve and the reworkability of the adhesive layer tends to decrease. According to the study by the present inventors, the decrease in reworkability is remarkable when the adhesive layer is in direct contact with a conductive layer, particularly an ITO layer.

[0007] According to the study by the present inventors, if a compound that improves the reworkability of the adhesive layer is added in excess to the adhesive layer, it may be possible to suppress the deterioration of the reworkability of the adhesive layer due to preheating. However, in this case, the durability of the adhesive layer in a high-temperature environment tends to be significantly reduced.

[0008] Therefore, an object of the present invention is to provide a polarizing film with an adhesive layer, which has an adhesive layer that maintains reworkability after preheating even when attached to a conductive layer and has durability in high-temperature environments. [Means for solving the problem]

[0009] The present invention relates to A polarizing film with a pressure-sensitive adhesive layer, comprising a polarizing film and a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition, The pressure-sensitive adhesive composition contains a compound (C) having an acidic group or an acid anhydride group and a polyether compound (D), The adhesive strength P of the pressure-sensitive adhesive layer was determined by the following test 1. 85 is 10.0N / 25mm or less, and the adhesive strength P obtained by the following test 2 105 The present invention provides a polarizing film with an adhesive layer, the strength of which is greater than 10.0 N / 25 mm. Test 1: The adhesive layer attached to the indium tin oxide layer of the glass with an indium tin oxide layer is subjected to a heat treatment at 85° C. for 5 hours. The force required to peel the adhesive layer from the indium tin oxide layer at a peel speed of 300 mm / min and a peel angle of 90° (adhesion strength P 85 ) is measured. Test 2: The adhesive layer attached to the indium tin oxide layer of the glass with an indium tin oxide layer is subjected to a heat treatment at 105° C. for 24 hours. The force required to peel the adhesive layer from the indium tin oxide layer at a peel speed of 300 mm / min and a peel angle of 90° (adhesive strength P 105 ) is measured.

[0010] Further, the present invention relates to The above-mentioned polarizing film with a pressure-sensitive adhesive layer, A conductive layer including a metal oxide; A transparent substrate; Equipped with The pressure-sensitive adhesive layer is in direct contact with the conductive layer.

[0011] Further, the present invention relates to A method for manufacturing the image display panel, comprising the steps of: and performing a first heat treatment at 70° C. to 95° C. on the pressure-sensitive adhesive layer in a state in which the pressure-sensitive adhesive layer-attached polarizing film is attached to the conductive layer.

[0012] Further, the present invention relates to A pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition, The pressure-sensitive adhesive composition contains a compound (C) having an acidic group or an acid anhydride group and a polyether compound (D), Adhesive strength P obtained by the following test 1 85 is 10.0N / 25mm or less, and the adhesive strength P obtained by the following test 2 105 The adhesive layer has a strength greater than 10.0 N / 25 mm. Test 1: The adhesive layer attached to the indium tin oxide layer of the glass with an indium tin oxide layer is subjected to a heat treatment at 85° C. for 5 hours. The force required to peel the adhesive layer from the indium tin oxide layer at a peel speed of 300 mm / min and a peel angle of 90° (adhesion strength P 85 ) is measured. Test 2: The adhesive layer attached to the indium tin oxide layer of the glass with an indium tin oxide layer is subjected to a heat treatment at 105° C. for 24 hours. The force required to peel the adhesive layer from the indium tin oxide layer at a peel speed of 300 mm / min and a peel angle of 90° (adhesive strength P 105 ) is measured. Effect of the Invention

[0013] According to the present invention, a polarized film with an adhesive layer can be provided, which has an adhesive layer that maintains reworkability after preheating even when attached to a conductive layer and has durability in high-temperature environments. [Brief description of the drawings]

[0014] [Figure 1] 1 is a cross-sectional view of a polarizing film with a pressure-sensitive adhesive layer according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram for explaining the characteristics of a pressure-sensitive adhesive layer included in a pressure-sensitive adhesive layer-attached polarizing film. [Diagram 3] 1 is a cross-sectional view of an image display panel according to one embodiment of the present invention. [Figure 4] FIG. 11 is a cross-sectional view showing a modified example of the image display panel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will now be described in detail, but the following description is not intended to limit the present invention to a specific embodiment.

[0016] (Embodiment of Polarizing Film with Pressure-Sensitive Adhesive Layer) 1, the pressure-sensitive adhesive layer-attached polarizing film 10 of the present embodiment includes a pressure-sensitive adhesive layer 1 and a polarizing film 2. The pressure-sensitive adhesive layer 1 is in direct contact with the polarizing film 2, for example. The surface of the pressure-sensitive adhesive layer 1 is exposed to the outside of the pressure-sensitive adhesive layer-attached polarizing film 10, for example.

[0017] In the polarizing film 10 with the adhesive layer, the adhesive strength P 85 is 10.0N / 25mm or less, and the adhesive strength P obtained by test 2 105 is greater than 10.0N / 25mm.

[0018] Test 1 is performed by the following method. First, the polarizing film 10 with the adhesive layer is cut into a strip of 150 mm length x 25 mm width to prepare a test piece. Next, a glass with an indium tin oxide (ITO) layer is prepared. The glass with the ITO layer has, for example, an alkali-free glass and an ITO layer in contact with the alkali-free glass. The alkali-free glass is glass that does not substantially contain an alkali component (alkali metal oxide), and in detail, the weight ratio of the alkali component in the glass is, for example, 1000 ppm or less, and further 500 ppm or less. The alkali-free glass is, for example, plate-shaped and has a thickness of 0.5 mm or more. The ITO layer is, for example, made of only substantially non-crystalline (amorphous) ITO. However, the ITO layer may contain impurities other than ITO. The ITO layer can be formed on the surface of the alkali-free glass by a physical deposition method such as a sputtering method.

[0019] Next, the test piece is attached to the surface of the ITO layer of the ITO-layered glass by the adhesive layer 1. The test piece is attached to the ITO layer using, for example, a laminator, so that no air bubbles are mixed between the ITO layer and the adhesive layer 1. After the test piece is attached, it is placed in an autoclave at 50°C and 5 atm (absolute pressure) for 15 minutes to homogenize the bonding between the ITO layer and the adhesive layer 1, and the adhesive layer 1 is adhered to the ITO layer. Next, the test piece (adhesive layer 1) is subjected to a heat treatment for 5 hours under atmospheric pressure at 85°C. Next, the test piece is left in an atmosphere at room temperature (for example, 23°C) to reduce the temperature of the test piece to room temperature. The test piece is peeled off from the ITO layer at a peel speed of 300 mm / min and a peel angle of 90° (measurement length 80 mm). At this time, the force required to peel off the test piece from the ITO layer is measured once per 0.5 s interval. The average of the obtained measurements is taken as the adhesive strength P 85 Identify as:

[0020] Test 2 can be performed in the same manner as Test 1, except that the heat treatment after homogenizing the bond between the ITO layer and the adhesive layer 1 in an autoclave is performed in an atmospheric pressure atmosphere at 105°C for 24 hours.

[0021] According to the study by the present inventors, the adhesive strength P 85 When the adhesive strength P is 10.0 N / 25 mm or less, the reworkability of the adhesive layer 1 tends to be sufficiently maintained after preheating. 85 is preferably 9.0 N / 25 mm or less, more preferably 8.0 N / 25 mm or less, further preferably 7.0 N / 25 mm or less, and particularly preferably 6.0 N / 25 mm or less. 85 From a practical standpoint, the lower limit is, for example, 3.0 N / 25 mm.

[0022] According to the study by the present inventors, the adhesive strength P 105 When the adhesive strength P is greater than 10.0 N / 25 mm, the adhesive layer 1 tends to have sufficient durability in a high temperature environment. 105is preferably 11.0 N / 25 mm or more, more preferably 12.0 N / 25 mm or more, even more preferably 13.0 N / 25 mm or more, and particularly preferably 14.0 N / 25 mm or more. 105 The upper limit is not particularly limited, and is, for example, 30.0 N / 25 mm.

[0023] Furthermore, in the polarizing film 10 with the adhesive layer, the adhesive layer 1 may have an adhesive strength P0 of 10.0 N / 25 mm or less as determined by Test 3. Test 3 may be performed in the same manner as Test 1, except that the heat treatment is not performed after the ITO layer and the adhesive layer 1 are homogenized in an autoclave. The adhesive strength P0 is preferably 9.0 N / 25 mm or less, more preferably 8.0 N / 25 mm or less, even more preferably 7.0 N / 25 mm or less, and particularly preferably 6.0 N / 25 mm or less. From a practical standpoint, the lower limit of the adhesive strength P0 is, for example, 3.0 N / 25 mm.

[0024] [Adhesive layer] The pressure-sensitive adhesive layer 1 is formed from a pressure-sensitive adhesive composition. The pressure-sensitive adhesive composition contains a compound (C) having an acidic group or an acid anhydride group and a polyether compound (D), and further contains, for example, a base polymer. The "base polymer" is, for example, the polymer contained in the largest amount by weight in the pressure-sensitive adhesive composition, and functions as a component that contributes to the adhesiveness of the pressure-sensitive adhesive layer 1.

[0025] <Compound (C)> Compound (C) is, for example, a low molecular weight compound or an oligomer. The acidic group of compound (C) is, for example, a carboxyl group or a mercapto group, and is preferably a carboxyl group. The acidic group of compound (C) may be a group generated by hydrolysis of an acid anhydride group. Specific examples of the acid anhydride group include carboxylic anhydride groups such as succinic anhydride group, phthalic anhydride group, and maleic anhydride group, and is preferably a succinic anhydride group. The total value of the content of the acidic group and the content of the acid anhydride group in compound (C) is not particularly limited, and is, for example, 5.0 wt% to 50 wt%, and preferably 8.3 wt% to 40 wt%.

[0026] The compound (C) may contain a silicon atom, and may further contain a hydrolyzable group (h1) bonded to the silicon atom. The hydrolyzable group (h1) can form a siloxane bond, for example, by hydrolysis and / or condensation. Examples of the hydrolyzable group (h1) include a halogen atom, an alkoxy group, an acyloxy group, an alkenyloxy group, a carbamoyl group, an amino group, an aminooxy group, and a ketoximate group. When the hydrolyzable group (h1) has a carbon atom, the number of carbon atoms is, for example, 10 or less, preferably 6 or less, and more preferably 4 or less. In particular, an alkoxy group or an alkenyloxy group having 4 or less carbon atoms is preferable, and a methoxy group or an ethoxy group is particularly preferable. The content of the hydrolyzable group (h1) in the compound (C) is, for example, 10 wt% or more, preferably 13 wt% to 50 wt%, and more preferably 13 wt% to 49 wt%.

[0027] The compound (C) may contain functional groups other than the acidic group, the acid anhydride group, and the hydrolyzable group (h1), but it is preferable that the compound (C) does not contain any other functional groups. For example, the compound (C) does not contain any polyether group.

[0028] The compound (C) includes, for example, at least one selected from the group consisting of an alkoxysilane compound (S1) having an acidic group or an acid anhydride group, an organopolysiloxane compound (S2) having an acidic group or an acid anhydride group, and a hydrolysis condensate thereof, and preferably includes an organopolysiloxane compound (S2).

[0029] The alkoxysilane compound (S1) is represented, for example, by the following formula (1). R 1 R 2 a Si(OR 3 ) 3-a (1)

[0030] In formula (1), R 1R is an organic group having 1 to 20 carbon atoms and having an acidic group or an acid anhydride group. This organic group may be linear, branched, or cyclic. 2 R are each independently a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom. 3 are each independently an alkyl group having 1 to 10 carbon atoms, and preferably a methyl group or an ethyl group.

[0031] R 1 From the viewpoint of easy availability of the alkoxysilane compound (S1), is preferably an organic group represented by the following formula (2). [ka]

[0032] In formula (2), A is a linear or branched alkylene or alkenylene group having 2 to 10 carbon atoms, and is preferably a linear or branched alkylene group having 2 to 6 carbon atoms. Specific examples of A include an ethylene group and a propane-1,3-diyl group.

[0033] Examples of the alkoxysilane compound (S1) include 2-trimethoxysilylethylsuccinic anhydride, 3-trimethoxysilylpropylsuccinic anhydride (manufactured by Shin-Etsu Chemical Co., Ltd., product name "X-12-967C"), 3-triethoxysilylpropylsuccinic anhydride, 3-methyldiethoxysilylpropylsuccinic anhydride, and 1-carboxy-3-triethoxysilylpropylsuccinic anhydride.

[0034] The organopolysiloxane compound (S2) is a compound having a siloxane bond, and contains, for example, a siloxane unit (U1) represented by the following formula (3). The organopolysiloxane compound (S2) may further contain a siloxane unit (U2) represented by the following formula (4). [ka] [ka]

[0035] In formula (3), X is an organic group having an acidic group or an acid anhydride group, and is preferably an organic group represented by formula (2). 4 R are each independently a hydrogen atom, an alkoxy group having 1 to 10 carbon atoms, or a monovalent hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom. 4 The alkoxy group in R is preferably a methoxy group or an ethoxy group. 4 The hydrocarbon group is, for example, a methyl group.

[0036] The number of siloxane units (U1) contained in the organopolysiloxane compound (S2) is not particularly limited and is, for example, 1 to 100, preferably 1 to 50, and more preferably 1 to 20. The number of siloxane units (U2) contained in the organopolysiloxane compound (S2) is not particularly limited and is, for example, 0 to 100, preferably 0 to 50, and more preferably 0 to 20. The organopolysiloxane compound (S2) preferably contains at least one siloxane unit (U2).

[0037] The organopolysiloxane compound (S2) may have a structure in which at least one siloxane unit (U1) is inserted between the O-Si bonds contained in an alkoxysilane represented by the following formula (5) or a partial hydrolysis condensate thereof. Both the siloxane unit (U1) and the siloxane unit (U2) may be inserted between the O-Si bonds. Of the multiple O-Si bonds, the siloxane unit (U1) may be inserted between some of the O-Si bonds, and the siloxane unit (U2) may be inserted between the other O-Si bonds. R 5 n Si(OR 6 ) 3-n (5)

[0038] In formula (5), R 5R are each independently a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom. 6 are each independently an alkyl group having 1 to 10 carbon atoms. n is 0 or 1.

[0039] Examples of the alkoxysilane represented by formula (5) or a partial hydrolysis condensation product thereof include tetramethoxysilane, methyltrimethoxysilane, tetraethoxysilane, methyltriethoxysilane, and compounds obtained by partial hydrolysis condensation of one or more of these alkoxysilanes.

[0040] The organopolysiloxane compound (S2) can be produced by a known production method described in, for example, JP-A-2013-129809, JP-A-2013-129691, and the like.

[0041] The compound (C) is not limited to the above alkoxysilane compound (S1) and organopolysiloxane compound (S2) as long as it has an acidic group or an acid anhydride group. The compound (C) may contain a (meth)acrylic oligomer (B) having an acidic group or an acid anhydride group. The (meth)acrylic oligomer (B) contains, for example, a structural unit derived from an alkyl (meth)acrylate as a main component, and also contains a structural unit derived from a (meth)acrylate having an acidic group or an acid anhydride group. In this specification, "(meth)acrylate" means acrylate and / or methacrylate. "Main component" means the structural unit contained most in the polymer by weight.

[0042] Examples of the alkyl (meth)acrylate constituting the (meth)acrylic oligomer (B) include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, and dodecyl (meth)acrylate. Examples of the (meth)acrylate having an acidic group include (meth)acrylic acid, carboxyl group-containing (meth)acrylates such as carboxyethyl (meth)acrylate and carboxypentyl (meth)acrylate.

[0043] Examples of other monomers constituting the (meth)acrylic oligomer (B) include esters of (meth)acrylic acid and alicyclic alcohols such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; aryl (meth)acrylates such as phenyl (meth)acrylate and benzyl (meth)acrylate; (meth)acrylates obtained from terpene compound derivative alcohols; and alkyl (meth)acrylates containing ether bonds such as methoxyethyl (meth)acrylate and phenoxyethyl (meth)acrylate. These (meth)acrylates can be used alone or in combination of two or more kinds. As a monomer constituting the (meth)acrylic oligomer (B), a monomer constituting the (meth)acrylic polymer (A) described later can also be used.

[0044] As with the (meth)acrylic polymer (A) described later, the polymerization method for the (meth)acrylic oligomer (B) may be solution polymerization, emulsion polymerization, bulk polymerization, emulsion polymerization, polymerization by heat or active energy ray irradiation (thermal polymerization, active energy ray polymerization), etc. Among them, solution polymerization and active energy ray polymerization are preferred in terms of transparency, water resistance, cost, etc. The obtained (meth)acrylic oligomer (B) may be any of a random copolymer, a block copolymer, a graft copolymer, etc.

[0045] From the viewpoint of improving the durability, corrosion resistance and reworkability of the pressure-sensitive adhesive layer 1, the content of the compound (C) in the pressure-sensitive adhesive composition is preferably 0.05 to 10 parts by weight, more preferably 3 parts by weight or less, even more preferably 2 parts by weight or less, particularly preferably 1 part by weight or less, and most preferably 0.6 parts by weight or less, relative to 100 parts by weight of the base polymer described below. The content of the compound (C) is more preferably 0.1 parts by weight or more, even more preferably 0.2 parts by weight or more, and particularly preferably 0.4 parts by weight or more, relative to 100 parts by weight of the base polymer.

[0046] The weight average molecular weight of the compound (C) is not particularly limited and is, for example, 10000 or less, preferably 8000 or less, more preferably 5000 or less, further preferably 3000 or less, and particularly preferably 1500 or less. The lower limit of the weight average molecular weight of the compound (C) is not particularly limited and is, for example, 100.

[0047] Compound (C) may have a low acid dissociation constant pKa due to the acidic group. The pKa (particularly the first acid dissociation constant) of compound (C) is, for example, 12 or less, preferably 11 or less, more preferably 8 or less, further preferably 6 or less, and particularly preferably 5 or less. The lower limit of pKa of compound (C) is not particularly limited, and is, for example, 1. In this specification, pKa is a value in water at 25°C.

[0048] <Polyether Compound (D)> The polyether compound (D) is a compound having a polyether skeleton. The polyether skeleton may be linear or branched. The polyether skeleton of the polyether compound (D) contains, for example, an oxyalkylene unit (U3) represented by the following formula (6). [ka]

[0049] In formula (6), R 7 R is a linear or branched alkylene group having 1 to 10 carbon atoms. 7 The number of carbon atoms is preferably 2 to 6, and more preferably 3. The polyether compound (D) may contain one or more types of oxyalkylene units (U3). The polyether compound (D) may be a random copolymer or a block copolymer. Specific examples of the oxyalkylene unit (U3) include an oxyethylene group, an oxypropylene group, and an oxybutylene group. The oxyalkylene unit (U3) is preferably an oxypropylene group (particularly -CH2CH(CH3)O-) in terms of ease of production of the material and stability of the material.

[0050] The polyether compound (D) may contain a silicon atom, and may further contain a hydrolyzable group (h2) bonded to the silicon atom. The hydrolyzable group (h2) can form a siloxane bond, for example, by hydrolysis and / or condensation. Examples of the hydrolyzable group (h2) include a halogen atom, an alkoxy group, an acyloxy group, an alkenyloxy group, a carbamoyl group, an amino group, an aminooxy group, and a ketoximate group. When the hydrolyzable group (h2) has a carbon atom, the number of carbon atoms is, for example, 10 or less, preferably 6 or less, and more preferably 4 or less. In particular, an alkoxy group or an alkenyloxy group having 4 or less carbon atoms is preferred, and a methoxy group or an ethoxy group is particularly preferred. The content of the hydrolyzable group (h2) in the polyether compound (D) is, for example, 14 wt% or less, preferably less than 13 wt%, and more preferably less than 10 wt%. The lower limit of the content of the hydrolyzable group (h2) is not particularly limited, and may be, for example, 2.0 wt%, 2.5 wt%, or 3.0 wt%. In some cases, the content of the hydrolyzable group (h2) may be 2.0 wt% or less.

[0051] The hydrolyzable group (h2) bonded to a silicon atom is located, for example, at an end of the polyether compound (D). As an example, the polyether compound (D) has a reactive silyl group (b) represented by the following formula (7) at at least one end. -SiR 8 a M 3-a (7)

[0052] In formula (7), R 8 R are each independently a monovalent organic group having 1 to 20 carbon atoms which may have a substituent. 8 is preferably a linear or branched alkyl group having 1 to 8 carbon atoms, a fluoroalkyl group having 1 to 8 carbon atoms, or a phenyl group, more preferably an alkyl group having 1 to 6 carbon atoms, and particularly preferably a methyl group. 8 If there are multiple R 8may be the same as or different from each other. M is, independently of each other, a hydroxyl group or a hydrolyzable group (h2). When a plurality of M's are present in the polyether compound (D), the plurality of M's may be the same as or different from each other. a is an integer of 0 to 2.

[0053] The polyether compound (D) has, for example, at least one reactive silyl group (b) per molecule at its end. When the polyether compound (D) is linear, the polyether compound (D) may have one or two reactive silyl groups (b) at its end, and preferably has two reactive silyl groups (b). When the polyether compound (D) is branched, the polyether compound (D) has at least one reactive silyl group (b) at the main chain end or the side chain end. The number of reactive silyl groups (b) can be appropriately adjusted according to the number of ends of the polyether compound (D), and is preferably 2 or more, and may be 3 or more.

[0054] It is preferable that the polyether compound (D) has a reactive silyl group (b) on at least a part of its molecular terminals and has at least one, preferably 1.1 to 5, and more preferably 1.1 to 3 reactive silyl groups (b) in its molecule.

[0055] The reactive silyl group (b) is preferably an alkoxysilyl group (b1) represented by the following formula (8) or an alkoxysilyl group (b2) represented by the following formula (9). [ka] [ka]

[0056] In formula (8) and formula (9), R 9 , R 10 and R 11are each independently a monovalent hydrocarbon group having 1 to 6 carbon atoms, and examples thereof include a linear or branched alkyl group having 1 to 6 carbon atoms, a linear or branched alkenyl group having 2 to 6 carbon atoms, a cycloalkyl group having 5 to 6 carbon atoms, and a phenyl group. 9 , -OR 10 -OR 11 Specific examples of the aryl group include a methoxy group, an ethoxy group, a propoxy group, a propenyloxy group, and a phenoxy group. Of these, a methoxy group and an ethoxy group are preferred, and a methoxy group is particularly preferred.

[0057] The polyether compound (D) preferably has a main chain substantially composed of a polyether skeleton, except for the reactive silyl group (b). However, the main chain of the polyether compound (D) may contain a small amount of other chemical structures. Examples of the other chemical structures include a chemical structure derived from an initiator for forming the oxyalkylene unit (U3) and a linking group between the polyether skeleton and the reactive silyl group (b). The content of the oxyalkylene unit (U3) in the polyether compound (D) is preferably 50% by weight or more, more preferably 80% by weight or more.

[0058] The polyether compound (D) is represented, for example, by the following formula (10). R 12 a M 3-a Si-XY-(AO) n -Z (10)

[0059] In formula (10), R 12are each independently a monovalent organic group having 1 to 20 carbon atoms which may have a substituent. Each M is independently a hydroxyl group or a hydrolyzable group (h2). a is an integer of 0 to 2. AO is a linear or branched oxyalkylene group having 1 to 10 carbon atoms. n represents the average number of moles added of the oxyalkylene group and is 1 to 1700. X is a linear or branched alkylene group having 1 to 20 carbon atoms. Y is an ether bond, an ester bond, a urethane bond, or a carbonate bond. Z is a hydrogen atom, a monovalent hydrocarbon group having 1 to 10 carbon atoms, a group represented by the following formula (11), or a group represented by the following formula (12). -Y 1 -X-SiR 12 a M 3-a (11) -Q{-(OA) n -YX-SiR 12 a M 3-a} m (12)

[0060] In formula (11), R 12 , M and X are the same as in formula (10). 1 is a single bond, a -CO- bond, a -CONH- bond or a -COO- bond. 12 M, X, Y, and n are the same as in formula (10). OA is the same as AO in formula (10). Q is a divalent or higher hydrocarbon group having 1 to 10 carbon atoms. m is a value obtained by subtracting 1 from the valence of the hydrocarbon group of Q.

[0061] X in the formula (10) is a linear or branched alkylene group having 1 to 20 carbon atoms. The alkylene group preferably has 2 to 10 carbon atoms, and more preferably has 3 carbon atoms.

[0062] Y in formula (10) is a bond formed by reaction with a hydroxyl group of an oxyalkylene group at the end of the polyether skeleton, and is preferably an ether bond or a urethane bond, and more preferably a urethane bond.

[0063] Z is derived from a hydroxy compound that is an initiator for synthesizing an oxyalkylene polymer used in preparing the polyether compound (D) represented by formula (10). Z is, for example, a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms. In this case, the polyether compound (D) represented by formula (10) has one reactive silyl group (b) at its terminal. When Z is a hydrogen atom, this corresponds to the case where a structural unit similar to that of the oxyalkylene polymer is used as the hydroxy compound. When Z is a monovalent hydrocarbon group having 1 to 10 carbon atoms, this corresponds to the case where a hydroxy compound having one hydroxyl group is used.

[0064] On the other hand, when Z is represented by formula (11) or formula (12), the polyether compound (D) has a plurality of reactive silyl groups (b) at its terminals. When Z is represented by formula (11), it corresponds to the case where the same structural unit as the oxyalkylene polymer is used as the hydroxy compound. When Z is represented by formula (12), it corresponds to the case where a hydroxy compound having two hydroxyl groups and different from the structural unit of the oxyalkylene polymer is used. Note that, Y in formula (11) 1 is a bond formed by reaction with the hydroxyl group of the oxyalkylene group at the end of the polyether skeleton, similar to Y in formula (10).

[0065] From the viewpoint of reworkability, the polyether compound (D) is preferably represented by the following formula (13), formula (14) or formula (15). Z 0 -A 2 -O-(A 1 O) n -Z 1 (13) Z 0 -A 2 -NHCOO-(A 1 O) n -Z 2 (14) Z 3 -O-(A 1 O) n -CH{-CH2-(A 1 O) n -Z 3}2(15)

[0066] In formulas (13) to (15), Z 0 A is an alkoxysilyl group represented by formula (8) or formula (9). 1 O is an oxyalkylene group having 2 to 6 carbon atoms, and is preferably an oxypropylene group. 1 The oxyalkylene group of O may be linear or branched. 1 The average number of moles of O added is 1 to 1700. A in formula (13) and formula (14) 2 A is an alkylene group having 2 to 6 carbon atoms, and is preferably a propylene group. 2 The alkylene group of formula (13) may be linear or branched. 1 is a hydrogen atom or -A 2 -Z 0 In equation (14), Z 2 is a hydrogen atom or -CONH-A 2 -Z 0 In equation (15), Z 3 is a hydrogen atom or -A 2 -Z 0 and there is at least one Z 3 Ga-A 2 -Z 0 It is.

[0067] As the compound represented by formula (14), for example, a compound represented by the following formula (16) is preferable. [ka]

[0068] In formula (16), R 9 , R 10 and R 11 are each independently a monovalent hydrocarbon group having 1 to 6 carbon atoms. n represents the average number of moles of oxypropylene groups added and is 1 to 1,700. 21 is a hydrogen atom or a trialkoxysilyl group represented by the following formula (17). [ka]

[0069] In formula (17), R 9 , R 10 and R 11 is the same as equation (16).

[0070] The number average molecular weight of the polyether compound (D) is preferably 300 to 100,000 from the viewpoint of reworkability. The number average molecular weight is preferably 500 or more, more preferably 1,000 or more, more preferably 2,000 or more, more preferably 3,000 or more, more preferably 4,000 or more, and even more preferably 5,000 or more, and is preferably 50,000 or less, more preferably 40,000 or less, more preferably 30,000 or less, more preferably 20,000 or less, and even more preferably 10,000 or less. n (average number of moles of oxyalkylene groups added in the polyether skeleton) in the above formulas (10) to (16) is appropriately adjusted, for example, so that the number average molecular weight of the polyether compound (D) is in the above range. When the number average molecular weight of the polyether compound (D) is 1,000 or more, the above n is usually 10 to 1,700.

[0071] The Mw (weight average molecular weight) / Mn (number average molecular weight) of the polyether compound (D) is preferably 3.0 or less, more preferably 1.6 or less, and particularly preferably 1.5 or less. In order to obtain a polyether compound (D) having a small Mw / Mn, it is preferable to use a method in which a reactive silyl group is introduced into an oxyalkylene polymer obtained by polymerizing a cyclic ether in the presence of an initiator using the composite metal cyanide complex described below as a catalyst.

[0072] The polyether compound (D) can be produced, for example, by using an oxyalkylene polymer having a functional group at the molecular end as a raw material and bonding a reactive silyl group to the molecular end via an organic group such as an alkylene group. The oxyalkylene polymer used as the raw material is preferably a polymer having a hydroxyl group at the end obtained by ring-opening polymerization of a cyclic ether in the presence of a catalyst and an initiator.

[0073] As the initiator, a compound having one or more active hydrogen atoms per molecule, for example, a hydroxy compound having one or more hydroxyl groups per molecule, can be used. Examples of the initiator include ethylene glycol, propylene glycol, dipropylene glycol, butanediol, hexamethylene glycol, hydrogenated bisphenol A, neopentyl glycol, polybutadiene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, allyl alcohol, methallyl alcohol, glycerin, trimethylolmethane, trimethylolpropane, pentaerythritol, and hydroxy compounds such as alkylene oxide adducts thereof. The initiator may be one or more kinds.

[0074] When the cyclic ether is subjected to ring-opening polymerization in the presence of an initiator, a polymerization catalyst can be used. Examples of the polymerization catalyst include alkali metal compounds such as potassium hydroxide, potassium methoxide, and cesium compounds such as cesium hydroxide; composite metal cyanide complexes; metal porphyrin complexes; and compounds having a P=N bond.

[0075] The polyether skeleton (polyoxyalkylene chain) in the polyether compound (D) is preferably composed of oxyalkylene units formed by ring-opening polymerization of an alkylene oxide having 2 to 6 carbon atoms, more preferably composed of oxyalkylene units formed by ring-opening polymerization of at least one alkylene oxide selected from the group consisting of ethylene oxide, propylene oxide, and butylene oxide, and particularly preferably composed of oxyalkylene units formed by ring-opening polymerization of propylene oxide. When the polyoxyalkylene chain is composed of two or more kinds of oxyalkylene units, the arrangement of the two or more kinds of oxyalkylene units may be in a block form or a random form.

[0076] The polyether compound (D) represented by the above formula (14) can be obtained, for example, by subjecting a polymer having a polyoxyalkylene chain and a hydroxyl group to a urethane reaction using a compound having a reactive silyl group (b) and an isocyanate group. The polyether compound (D) represented by the formula (14) can also be obtained by adding hydrosilane or mercaptosilane to the unsaturated group of an oxyalkylene polymer having an unsaturated group, for example, an allyl-terminated polyoxypropylene monol obtained by polymerizing an alkylene oxide using allyl alcohol as an initiator, to introduce a reactive silyl group (b) into the molecular end.

[0077] The method for introducing the reactive silyl group (b) into the end group of the hydroxyl-terminated oxyalkylene polymer obtained by ring-opening polymerization of a cyclic ether in the presence of an initiator is not particularly limited, and usually, the following methods (a) to (c) in which a reactive silyl group is further linked to the end group via an organic group are preferred.

[0078] (a) A method in which an unsaturated group is introduced at the end of an oxyalkylene polymer having a hydroxyl group, and then a reactive silyl group (b) is bonded to this unsaturated group. As this method, the following two methods (a-1) and (a-2) can be further exemplified: (a-1) A method using a so-called hydrosilylation reaction in which a hydrosilyl compound is reacted with the unsaturated group in the presence of a catalyst such as a platinum compound. (a-2) A method of reacting an unsaturated group with a mercaptosilane compound.

[0079] Examples of the mercaptosilane compound (a-2) include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyltriisopropenyloxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyldimethylmonomethoxysilane, and 3-mercaptopropylmethyldiethoxysilane.

[0080] When reacting an unsaturated group with a mercapto group, a compound such as a radical generator used as a radical polymerization initiator may be used, or the reaction may be carried out by radiation or heat without using a radical polymerization initiator if desired. Examples of the radical polymerization initiator include peroxide-based, azo-based and redox-based polymerization initiators, as well as metal compound catalysts, and specific examples include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, benzoyl peroxide, tert-alkyl peroxy ester, acetyl peroxide and diisopropyl peroxycarbonate. The reaction conditions when reacting an unsaturated group with a mercapto group using a radical polymerization initiator vary depending on the decomposition temperature (half-life temperature) of the polymerization initiator, but it is preferable to carry out the reaction for several hours to several tens of hours at a reaction temperature of 20 to 200°C, preferably 50 to 150°C.

[0081] The method of introducing an unsaturated group into the terminal of an oxyalkylene polymer includes a method of reacting an oxyalkylene polymer with a functional group capable of linking the terminal hydroxyl group of the oxyalkylene polymer with an ether bond, an ester bond, a urethane bond, a carbonate bond, or the like, and a reactant having an unsaturated group. A method of introducing an unsaturated group into at least a part of the terminal of an oxyalkylene polymer by copolymerizing an unsaturated group-containing epoxy compound such as allyl glycidyl ether when polymerizing a cyclic ether in the presence of an initiator can also be used.

[0082] The hydrosilylation reaction is preferably carried out at a temperature of 60 to 120° C. In general, the hydrosilylation reaction proceeds sufficiently within a reaction time of several hours.

[0083] (b) A method of reacting an oxyalkylene polymer having a hydroxyl group at its terminal with an isocyanate silane compound having a reactive silyl group (b). Examples of the isocyanate silane compound include isocyanate silane compounds such as 1-isocyanate methyl trimethoxysilane, 1-isocyanate methyl triethoxysilane, 1-isocyanate propyl trimethoxysilane, 1-isocyanate propyl triethoxysilane, 3-isocyanate propyl trimethoxysilane, 3-isocyanate propyl triethoxysilane, 1-isocyanate methyl methyl dimethoxysilane, 1-isocyanate methyl dimethyl monomethoxysilane, 1-isocyanate methyl methyl diethoxysilane, 1-isocyanate propyl methyl dimethoxysilane, 1-isocyanate propyl dimethyl monomethoxysilane, 1-isocyanate propyl methyl diethoxysilane, 3-isocyanate propyl methyl dimethoxysilane, 3-isocyanate propyl dimethyl monomethoxysilane, and 3-isocyanate propyl methyl diethoxysilane. Of these, 3-isocyanatepropyltrimethoxysilane and 1-isocyanatemethyldimethoxysilane are more preferred, and 3-isocyanatepropyltrimethoxysilane is particularly preferred.

[0084] The reaction between the oxyalkylene polymer and the isocyanate silane compound is preferably carried out so that the molar ratio of the isocyanate group (NCO) of the isocyanate silane compound to the hydroxyl group (OH) of the oxyalkylene polymer is NCO / OH=0.80-1.05. This method can significantly shorten the process time because of the small number of manufacturing steps, and does not require complicated operations such as purification because there are few impurities produced as by-products during the manufacturing process. A more preferable molar ratio of NCO group to OH group is NCO / OH=0.85-1.00. When the ratio of NCO is low, the remaining OH group reacts with the reactive silyl group, etc., and the storage stability may decrease. In this case, it is preferable to adjust the silylation rate to a predetermined level by newly reacting with the isocyanate silane compound or monoisocyanate compound and consuming the excess OH group.

[0085] When the hydroxyl group of the oxyalkylene polymer is reacted with the above-mentioned isocyanate silane compound, a known urethanization catalyst may be used. The reaction temperature and the reaction time required for the reaction to be completed vary depending on the presence or absence of the urethanization catalyst and the amount of the catalyst used, but the reaction between the oxyalkylene polymer and the isocyanate silane compound is preferably carried out at a temperature of, for example, 20 to 200°C, preferably 50 to 150°C, for several hours.

[0086] (c) A method in which an oxyalkylene polymer having a hydroxyl group at the molecular terminal is reacted with a polyisocyanate compound under conditions of an excess of isocyanate groups to produce an oxyalkylene polymer having an isocyanate group at at least a portion of the terminals, and then the isocyanate group is reacted with a silicon compound having a functional group. The functional group of the silicon compound is at least one active hydrogen-containing group selected from the group consisting of hydroxyl, carboxyl, mercapto, primary amino and secondary amino groups. Examples of silicon compounds include aminosilane-based compounds such as N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldimethoxysilane and 3-aminopropylmethyldiethoxysilane; and mercaptosilane-based compounds such as 3-mercaptopropyltrimethoxysilane and 3-mercaptopropylmethyldimethoxysilane. When reacting the oxyalkylene polymer with the silicon compound, a known urethanization catalyst may be used. The reaction temperature and the reaction time required to complete the reaction vary depending on the presence or absence of the urethanization catalyst and the amount of the catalyst used, but the reaction is preferably carried out at a temperature of, for example, 20 to 200°C, preferably 50 to 150°C for several hours.

[0087] Specific examples of the polyether compound (D) include MS Polymer S203, S303, S810; SILYL EST250, EST280; SAT10, SAT200, SAT220, SAT350, SAT400 manufactured by Kaneka Corporation; and EXCESTAR S2410, S2420, S3430 manufactured by Asahi Glass Co., Ltd.

[0088] The content of the polyether compound (D) in the pressure-sensitive adhesive composition is preferably 0.001 to 20 parts by weight relative to 100 parts by weight of the base polymer. When the content is 0.001 parts by weight or more, the reworkability of the pressure-sensitive adhesive layer 1 tends to be sufficiently improved. The content of the polyether compound (D) is preferably 0.01 parts by weight or more, more preferably 0.02 parts by weight or more, even more preferably 0.1 parts by weight or more, and even more preferably 0.5 parts by weight or more. When the content of the polyether compound (D) is 20 parts by weight or less, the pressure-sensitive adhesive layer 1 has sufficient moisture resistance and is unlikely to peel off in a reliability test or the like. The content of the polyether compound (D) is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and even more preferably 3 parts by weight or less. The content of the polyether compound (D) may be 1 part by weight or less, or even 0.5 parts by weight or less.

[0089] <Adhesive> Examples of the adhesive contained in the adhesive composition include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinylpyrrolidone-based adhesives, polyacrylamide-based adhesives, cellulose-based adhesives, etc. As the adhesive, acrylic-based adhesives are preferred because they have excellent optical transparency, appropriate adhesive properties such as wettability, cohesiveness, and adhesion, and excellent weather resistance, heat resistance, etc.

[0090] The pressure-sensitive adhesive composition containing an acrylic pressure-sensitive adhesive contains a (meth)acrylic polymer (A) as a base polymer. The (meth)acrylic polymer (A) contains, for example, a structural unit derived from an alkyl (meth)acrylate as a main component.

[0091] <(Meth)acrylic polymer (A)> The number of carbon atoms of the alkyl group contained in the alkyl (meth)acrylate for forming the main skeleton of the (meth)acrylic polymer (A) is not particularly limited, and is, for example, 1 to 18. The alkyl group may be linear, branched, or cyclic. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, an amyl group, a hexyl group, a cyclohexyl group, a heptyl group, a 2-ethylhexyl group, an isooctyl group, a nonyl group, a decyl group, an isodecyl group, a dodecyl group, an isomyristyl group, a lauryl group, a tridecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, and an octadecyl group. The alkyl (meth)acrylates can be used alone or in combination. The average number of carbon atoms of the alkyl group is preferably 3 to 9.

[0092] Examples of monomers constituting the (meth)acrylic polymer (A) include, in addition to alkyl (meth)acrylates, one or more copolymerizable monomers selected from the group consisting of aromatic ring-containing (meth)acrylates, amide group-containing monomers, carboxyl group-containing monomers, and hydroxyl group-containing monomers. The copolymerizable monomers can be used alone or in combination. The (meth)acrylic polymer (A) preferably has an acidic group resulting from a copolymerizable monomer such as a carboxyl group-containing monomer. The (meth)acrylic polymer (A) having an acidic group is suitable for maintaining the reworkability of the pressure-sensitive adhesive layer 1 after preheating.

[0093] The aromatic ring-containing (meth)acrylate is a compound that contains an aromatic ring structure in its structure and also contains a (meth)acryloyl group. Examples of aromatic rings include a benzene ring, a naphthalene ring, and a biphenyl ring. The aromatic ring-containing (meth)acrylate has an effect of adjusting the phase difference that occurs when stress is applied to the pressure-sensitive adhesive layer 1 due to the shrinkage of an optical film such as the polarizing film 2, and can suppress light leakage caused by the shrinkage of the optical film.

[0094] Examples of aromatic ring-containing (meth)acrylates include benzyl (meth)acrylate, phenyl (meth)acrylate, o-phenylphenol (meth)acrylate, phenoxy (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, ethylene oxide-modified cresol (meth)acrylate, phenol ethylene oxide-modified (meth)acrylate, 2-hydroxy- Examples of the acrylate include those having a benzene ring, such as 3-phenoxypropyl (meth)acrylate, methoxybenzyl (meth)acrylate, chlorobenzyl (meth)acrylate, cresyl (meth)acrylate, and polystyryl (meth)acrylate; those having a naphthalene ring, such as hydroxyethylated β-naphthol acrylate, 2-naphthoethyl (meth)acrylate, 2-naphthoxyethyl acrylate, and 2-(4-methoxy-1-naphthoxy)ethyl (meth)acrylate; and those having a biphenyl ring, such as biphenyl (meth)acrylate. Among these, benzyl (meth)acrylate and phenoxyethyl (meth)acrylate are preferred from the viewpoint of improving the adhesive properties and durability of the adhesive layer 1.

[0095] The amide group-containing monomer is a compound that contains an amide group in its structure and also contains a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the amide group-containing monomer include acrylamide-based monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropylacrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylol-N-propane(meth)acrylamide, aminomethyl(meth)acrylamide, aminoethyl(meth)acrylamide, mercaptomethyl(meth)acrylamide, and mercaptoethyl(meth)acrylamide; N-acryloyl heterocyclic monomers such as N-(meth)acryloylmorpholine, N-(meth)acryloylpiperidine, and N-(meth)acryloylpyrrolidine; and N-vinyl group-containing lactam-based monomers such as N-vinylpyrrolidone and N-vinyl-ε-caprolactam. Among these, from the viewpoint of improving the durability of the pressure-sensitive adhesive layer 1 relative to the conductive layer, N-vinyl group-containing lactam monomers are preferred.

[0096] The carboxyl group-containing monomer is a compound that contains a carboxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Among these, acrylic acid is preferred from the viewpoints of copolymerizability, cost, and improving the adhesive properties of the adhesive layer 1.

[0097] The hydroxyl group-containing monomer is a compound that contains a hydroxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate; (4-hydroxymethylcyclohexyl)-methyl acrylate, etc. Among these, from the viewpoint of improving the durability of the adhesive layer 1, 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are preferred, and 4-hydroxybutyl (meth)acrylate is more preferred.

[0098] The copolymerization monomer serves as a reaction site with the crosslinking agent. Carboxyl group-containing monomers and hydroxyl group-containing monomers are highly reactive with the intermolecular crosslinking agent, and are therefore preferably used to improve the cohesiveness and heat resistance of the pressure-sensitive adhesive layer 1. Carboxyl group-containing monomers are preferred in terms of achieving both durability and reworkability, and hydroxyl group-containing monomers are preferred in terms of improving reworkability.

[0099] From the viewpoint of improving the adhesiveness of the pressure-sensitive adhesive layer 1, the ratio of alkyl (meth)acrylate to all monomer components forming the (meth)acrylic polymer (A) is preferably 50% by weight or more.

[0100] When an aromatic ring-containing (meth)acrylate is used as a monomer component, the ratio of the aromatic ring-containing (meth)acrylate to all monomer components forming the (meth)acrylic polymer (A) is preferably 3 to 25% by weight, more preferably 22% by weight or less, and even more preferably 20% by weight or less, from the viewpoint of improving the durability of the pressure-sensitive adhesive layer 1. This ratio is more preferably 8% by weight or more, and even more preferably 12% by weight or more. By adjusting the copolymerization rate of the aromatic ring-containing (meth)acrylate within the above range, light leakage due to shrinkage of the optical film can be suppressed, and the reworkability of the pressure-sensitive adhesive layer 1 tends to be improved.

[0101] When a hydroxyl group-containing monomer is used as the monomer component, the ratio of the hydroxyl group-containing monomer to the total monomer components forming the (meth)acrylic polymer (A) is preferably 0.01 to 10% by weight, more preferably 5% by weight or less, even more preferably 2% by weight or less, and particularly preferably 1% by weight or less, from the viewpoint of improving the adhesive properties and durability of the adhesive layer 1. This ratio is more preferably 0.03% by weight or more, and even more preferably 0.05% by weight or more. By adjusting the copolymerization rate of the hydroxyl group-containing monomer within the above range, the adhesive in the adhesive layer 1 can be sufficiently crosslinked while preventing the adhesive from hardening, which tends to improve the durability of the adhesive layer 1.

[0102] As the monomer component, in addition to the alkyl (meth)acrylate and the above-mentioned copolymerizable monomers, other copolymerizable monomers having a polymerizable functional group containing an unsaturated double bond, such as a (meth)acryloyl group or a vinyl group, can be used for the purpose of improving the adhesive property and heat resistance of the pressure-sensitive adhesive layer 1. The other copolymerizable monomers can be used alone or in combination.

[0103] Examples of other copolymerizable monomers include acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride; caprolactone adducts of acrylic acid; sulfonic acid group-containing monomers such as allylsulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, and sulfopropyl (meth)acrylate; phosphoric acid group-containing monomers such as 2-hydroxyethyl acryloyl phosphate; aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and the like. alkylaminoalkyl (meth)acrylates such as t-butylaminoethyl (meth)acrylate; alkoxyalkyl (meth)acrylates such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; succinimide monomers such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyoctamethylene succinimide; N-cyclohexylmaleimide, N-isopropyl ... maleimide monomers such as N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide; vinyl monomers such as vinyl acetate and vinyl propionate; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate; glycol (meth)acrylates such as polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate; tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, silicone (meth)acrylate, and 2-methoxyethyl acrylate (meth)acrylate monomers;Examples of silane-based monomers containing silicon atoms include 3-acryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 4-vinylbutyltrimethoxysilane, 4-vinylbutyltriethoxysilane, 8-vinyloctyltrimethoxysilane, 8-vinyloctyltriethoxysilane, 10-methacryloyloxydecyltrimethoxysilane, 10-acryloyloxydecyltrimethoxysilane, 10-methacryloyloxydecyltriethoxysilane, and 10-acryloyloxydecyltriethoxysilane.

[0104] Further, examples of other copolymerizable monomers include polyfunctional monomers having two or more unsaturated double bonds, such as tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and caprolactone-modified dipentaerythritol hexa(meth)acrylate.

[0105] When other copolymerizable monomers are used as monomer components, the ratio of the other copolymerizable monomers to the total monomer components forming the (meth)acrylic polymer (A) is preferably 10% by weight or less, more preferably 7% by weight or less, and even more preferably 5% by weight or less.

[0106] <Method for producing (meth)acrylic polymer (A)> The (meth)acrylic polymer (A) can be prepared by a known polymerization method such as solution polymerization, radiation polymerization using electron beams or UV rays, or various radical polymerizations such as bulk polymerization and emulsion polymerization. The obtained (meth)acrylic polymer (A) may be any of a random copolymer, a block copolymer, a graft copolymer, and the like.

[0107] In the solution polymerization, for example, ethyl acetate, toluene, etc. are used as a polymerization solvent. The solution polymerization is usually carried out under reaction conditions of about 50 to 70° C. for about 5 to 30 hours by adding a polymerization initiator under a stream of an inert gas such as nitrogen.

[0108] The polymerization initiator, chain transfer agent, emulsifier, etc. used in the radical polymerization are not particularly limited and can be appropriately selected and used. The weight average molecular weight of the (meth)acrylic polymer (A) can be controlled by the amount of the polymerization initiator and the chain transfer agent used, the reaction conditions, etc. Therefore, the amount of the polymerization initiator and the chain transfer agent used is appropriately adjusted depending on the composition.

[0109] Examples of the polymerization initiator include azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-amidinopropane)dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis(2-methylpropionamidine)disulfate, 2,2'-azobis(N,N'-dimethyleneisobutylamidine), and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate (VA-057, manufactured by Wako Pure Chemical Industries, Ltd.); persulfates such as potassium persulfate and ammonium persulfate; di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butyl ... Examples of the initiator include, but are not limited to, peroxide initiators such as dicarbonate, t-butyl peroxyneodecanoate, t-hexyl peroxypivalate, t-butyl peroxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, dibenzoyl peroxide, t-butyl peroxyisobutyrate, 1,1-di(t-hexylperoxy)cyclohexane, t-butyl hydroperoxide, and hydrogen peroxide; and redox initiators that combine a peroxide and a reducing agent, such as a combination of a persulfate and sodium hydrogen sulfite, or a combination of a peroxide and sodium ascorbate.

[0110] The polymerization initiators can be used alone or in combination, but the total amount used is preferably about 0.005 to 1 part by weight, and more preferably about 0.01 to 0.5 part by weight, per 100 parts by weight of the monomer components.

[0111] Examples of the chain transfer agent include lauryl mercaptan, glycidyl mercaptan, mercaptoacetic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethylhexyl thioglycolate, 2,3-dimercapto-1-propanol, etc. The chain transfer agent may be used alone or in combination of two or more kinds, but the total amount used is about 0.1 part by weight or less per 100 parts by weight of the monomer component.

[0112] Examples of emulsifiers used in emulsion polymerization include anionic emulsifiers such as sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzenesulfonate, ammonium polyoxyethylene alkyl ether sulfate, and sodium polyoxyethylene alkyl phenyl ether sulfate; and nonionic emulsifiers such as polyoxyethylene alkyl ether, polyoxyethylene alkyl phenyl ether, polyoxyethylene fatty acid ester, and polyoxyethylene-polyoxypropylene block polymer. The emulsifiers can be used alone or in combination.

[0113] Examples of the reactive emulsifier include emulsifiers having radical polymerizable functional groups such as propenyl and allyl ether groups. Specific examples of this emulsifier include Aqualon HS-10, HS-20, KH-10, BC-05, BC-10, and BC-20 (all manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and Adeka Reasoap SE10N (manufactured by ADEKA Corporation). Reactive emulsifiers are preferred because they are incorporated into the polymer chain after polymerization and improve water resistance. The amount of emulsifier used is preferably 0.3 to 5 parts by weight based on 100 parts by weight of the total amount of monomer components, and more preferably 0.5 to 1 part by weight in terms of polymerization stability and mechanical stability.

[0114] In radiation polymerization, the monomer components are polymerized by irradiating them with radiation such as electron beams or UV rays to produce a (meth)acrylic polymer (A). When radiation polymerization is performed with electron beams, it is not particularly necessary to include a photopolymerization initiator in the monomer components. When radiation polymerization is performed with UV rays, a photopolymerization initiator may be included in the monomer components due to the advantage that the polymerization time can be shortened. The photopolymerization initiators can be used alone or in combination.

[0115] The photopolymerization initiator is not particularly limited as long as it initiates photopolymerization, and a commonly used photopolymerization initiator can be used. As the photopolymerization initiator, for example, benzoin ether type, acetophenone type, α-ketol type, photoactive oxime type, benzoin type, benzyl type, benzophenone type, ketal type, thioxanthone type, etc. can be used. The amount of the photopolymerization initiator used is 0.05 to 1.5 parts by weight, preferably 0.1 to 1 part by weight, based on 100 parts by weight of the monomer component. The photopolymerization initiator can be used alone or in combination.

[0116] The weight average molecular weight of the (meth)acrylic polymer (A) is usually 1 million to 2.5 million. Considering durability, particularly heat resistance, the weight average molecular weight of the (meth)acrylic polymer (A) is preferably 1.2 million to 2 million. A weight average molecular weight of 1 million or more is preferable in terms of heat resistance. If the weight average molecular weight is 2.5 million or less, the adhesive is less likely to harden and peeling is less likely to occur. The weight average molecular weight (Mw) / number average molecular weight (Mn), which means the molecular weight distribution, is preferably 1.8 to 10, more preferably 1.8 to 7, and even more preferably 1.8 to 5. A molecular weight distribution (Mw / Mn) of 10 or less is preferable in terms of durability. The weight average molecular weight and the molecular weight distribution (Mw / Mn) are measured by GPC (gel permeation chromatography) and calculated based on polystyrene standards.

[0117] <Silane coupling agent> The pressure-sensitive adhesive composition may further contain a silane coupling agent (E) in addition to the compound (C) and the polyether compound (D). The silane coupling agent (E) may have a reactive functional group other than an acidic group and an acid anhydride group. The reactive functional group is preferably at least one selected from the group consisting of an epoxy group, an amino group, an isocyanate group, an isocyanurate group, a vinyl group, a styryl group, an acetoacetyl group, a ureido group, a thiourea group, a (meth)acrylic group, and a heterocyclic group. The silane coupling agent (E) may be used alone or in combination.

[0118] Examples of the silane coupling agent (E) include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-γ Examples of the silane coupling agents include amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane, vinyl group-containing silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane, styryl group-containing silane coupling agents such as p-styryltrimethoxysilane, and (meth)acrylic group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane. Among these, epoxy group-containing silane coupling agents are preferred.

[0119] As the silane coupling agent (E), one having a plurality of alkoxysilyl groups in the molecule (oligomeric silane coupling agent) can also be used. Specific examples of oligomeric silane coupling agents include epoxy group-containing oligomeric silane coupling agents manufactured by Shin-Etsu Chemical Co., Ltd., trade names of "X-41-1053", "X-41-1059A", "X-41-1056", and "X-40-2651". Oligomeric silane coupling agents are preferred because they are less likely to volatilize and have a plurality of alkoxysilyl groups, and therefore can effectively improve the durability of the adhesive layer 1.

[0120] When the pressure-sensitive adhesive composition contains a silane coupling agent (E), the content of the silane coupling agent (E) in the pressure-sensitive adhesive composition is preferably 0.001 to 5 parts by weight, more preferably 1 part by weight or less, and even more preferably 0.6 parts by weight or less, based on 100 parts by weight of the base polymer. The content of the silane coupling agent (E) is more preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, and particularly preferably 0.1 parts by weight or more, based on 100 parts by weight of the base polymer. By appropriately adjusting the content of the silane coupling agent (E), the durability of the pressure-sensitive adhesive layer 1 tends to be improved.

[0121] When the adhesive composition contains a silane coupling agent (E), the weight ratio of compound (C) to silane coupling agent (E) (compound (C) / silane coupling agent (E)) is, from the viewpoint of improving the durability of the adhesive layer 1, preferably 0.1 or more, more preferably 0.5 or more, and even more preferably 1 or more; and is preferably 50 or less, more preferably 15 or less, and even more preferably 5 or less.

[0122] <Crosslinking agent> The adhesive composition may further contain a crosslinking agent. As the crosslinking agent, an organic crosslinking agent, a polyfunctional metal chelate, etc. can be used. As the organic crosslinking agent, for example, an isocyanate crosslinking agent, a peroxide crosslinking agent, an epoxy crosslinking agent, an imine crosslinking agent, etc. can be mentioned. In the polyfunctional metal chelate, a polyvalent metal atom is covalently bonded or coordinately bonded to an organic compound. As the polyvalent metal atom, Al, Cr, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Sr, Ba, Mo, La, Sn, Ti, etc. can be mentioned. The organic compound that is covalently bonded or coordinately bonded contains, for example, an oxygen atom, etc., and preferably includes an alkyl ester, an alcohol compound, a carboxylic acid compound, an ether compound, a ketone compound, etc. The crosslinking agent can be used alone or in combination.

[0123] As the crosslinking agent, an isocyanate-based crosslinking agent and / or a peroxide-based crosslinking agent is preferred, and it is more preferred to use an isocyanate-based crosslinking agent and a peroxide-based crosslinking agent in combination.

[0124] As the isocyanate-based crosslinking agent, a compound having at least two isocyanate groups (including an isocyanate regenerating functional group in which the isocyanate group is temporarily protected by a blocking agent or oligomerization, etc.) can be used. For example, known aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates, etc., which are generally used in urethanization reactions, can be used.

[0125] Examples of the aliphatic polyisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.

[0126] Examples of alicyclic isocyanates include 1,3-cyclopentene diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, and hydrogenated tetramethylxylylene diisocyanate.

[0127] Examples of aromatic diisocyanates include phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-toluidine diisocyanate, 4,4'-diphenylether diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, and xylylene diisocyanate.

[0128] Examples of the isocyanate-based crosslinking agent include polymers (dimers, trimers, pentamers, etc.) of the above diisocyanates, urethane-modified products reacted with polyhydric alcohols such as trimethylolpropane, urea-modified products, biuret-modified products, alphanate-modified products, isocyanurate-modified products, and carbodiimide-modified products.

[0129] Examples of commercially available isocyanate crosslinking agents include those manufactured by Tosoh Corporation under the trade names "Millionate MT," "Millionate MTL," "Millionate MR-200," "Millionate MR-400," "Coronate L," "Coronate HL," and "Coronate HX," and those manufactured by Mitsui Chemicals, Inc. under the trade names "Takenate D-110N," "Takenate D-120N," "Takenate D-140N," "Takenate D-160N," "Takenate D-165N," "Takenate D-170HN," "Takenate D-178N," "Takenate 500," and "Takenate 600."

[0130] As the isocyanate-based crosslinking agent, aromatic polyisocyanate and its modified aromatic polyisocyanate compounds, and aliphatic polyisocyanate and its modified aliphatic polyisocyanate compounds are preferred. Aromatic polyisocyanate compounds are preferably used because they have a good balance between crosslinking speed and pot life. As the aromatic polyisocyanate compound, tolylene diisocyanate and its modified compounds are particularly preferred.

[0131] Any peroxide can be used as long as it generates radical active species upon heating or exposure to light and promotes crosslinking of the base polymer of the pressure-sensitive adhesive composition (e.g., the (meth)acrylic polymer (A)). Taking into consideration workability and stability, it is preferable to use a peroxide having a 1-minute half-life temperature of 80°C to 160°C, and it is more preferable to use a peroxide having a 1-minute half-life temperature of 90°C to 140°C.

[0132] Examples of peroxides include di(2-ethylhexyl)peroxydicarbonate (1-minute half-life temperature: 90.6° C.), di(4-t-butylcyclohexyl)peroxydicarbonate (1-minute half-life temperature: 92.1° C.), di-sec-butylperoxydicarbonate (1-minute half-life temperature: 92.4° C.), t-butylperoxyneodecanoate (1-minute half-life temperature: 103.5° C.), t-hexylperoxypivalate (1-minute half-life temperature: 109.1° C.), t-butylperoxypivalate (1-minute half-life temperature: 110.3° C.), dilauroylperoxide (1 1-minute half-life temperature: 116.4°C), di-n-octanoyl peroxide (1-minute half-life temperature: 117.4°C), 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (1-minute half-life temperature: 124.3°C), di(4-methylbenzoyl)peroxide (1-minute half-life temperature: 128.2°C), dibenzoyl peroxide (1-minute half-life temperature: 130.0°C), t-butylperoxyisobutyrate (1-minute half-life temperature: 136.1°C), 1,1-di(t-hexylperoxy)cyclohexane (1-minute half-life temperature: 149.2°C), and the like. Among these, di(4-t-butylcyclohexyl) peroxydicarbonate (1-minute half-life temperature: 92.1°C), dilauroyl peroxide (1-minute half-life temperature: 116.4°C), dibenzoyl peroxide (1-minute half-life temperature: 130.0°C), etc. are particularly preferred because of their excellent crosslinking reaction efficiency.

[0133] The half-life of a peroxide is an index showing the decomposition rate of the peroxide, and refers to the time it takes for the remaining amount of the peroxide to be reduced to half. The decomposition temperature for obtaining the half-life at any time and the half-life time at any temperature are listed in manufacturer catalogs, for example, NOF Corporation's "Organic Peroxide Catalog 9th Edition (May 2003)."

[0134] When a crosslinking agent is blended in the pressure-sensitive adhesive composition, the blending amount of the crosslinking agent is preferably 0.01 to 3 parts by weight, more preferably 0.02 to 2 parts by weight, and even more preferably 0.03 to 1 part by weight, relative to 100 parts by weight of the base polymer. When the blending amount of the crosslinking agent is 0.01 part by weight or more, the pressure-sensitive adhesive layer 1 is sufficiently crosslinked, and the durability and adhesive properties tend to be improved. On the other hand, when the blending amount of the crosslinking agent is 3 parts by weight or less, the pressure-sensitive adhesive layer 1 tends to become hard, and a decrease in durability tends to be suppressed.

[0135] When an isocyanate crosslinking agent is blended in the pressure-sensitive adhesive composition, the blending amount of the isocyanate crosslinking agent is preferably 0.01 to 2 parts by weight, more preferably 0.02 to 2 parts by weight, and even more preferably 0.05 to 1.5 parts by weight, relative to 100 parts by weight of the base polymer. When the blending amount of the isocyanate crosslinking agent is within the above range, the cohesive strength of the pressure-sensitive adhesive layer 1 is improved, and peeling in a durability test tends to be suppressed.

[0136] When a peroxide is blended in the pressure-sensitive adhesive composition, the blending amount of the peroxide is preferably 0.01 to 2 parts by weight, more preferably 0.04 to 1.5 parts by weight, and even more preferably 0.05 to 1 part by weight, relative to 100 parts by weight of the base polymer. When the blending amount of the peroxide is within the above range, the processability, crosslinking stability, etc. of the pressure-sensitive adhesive layer 1 can be easily adjusted.

[0137] <Other ingredients> The adhesive composition may further contain an ionic compound. The ionic compound is not particularly limited, and those used in this field can be suitably used. Examples of the ionic compound include those described in JP 2015-4861 A, and among them, (perfluoroalkylsulfonyl)imide lithium salt is preferable, and bis(trifluoromethanesulfonylimide)lithium is more preferable. The amount of the ionic compound is not particularly limited, and can be within a range that does not impair the effects of the present invention, but for example, it is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, even more preferably 3 parts by weight or less, and particularly preferably 1 part by weight or less, relative to 100 parts by weight of the base polymer.

[0138] The adhesive composition may contain other known additives, such as colorants, powders such as pigments, dyes, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, softeners, antioxidants, antiaging agents, light stabilizers, UV absorbers, polymerization inhibitors, inorganic or organic fillers, metal powders, particles, and foils, which can be added appropriately depending on the application. Furthermore, a redox system containing a reducing agent may be used within a controllable range. These additives are preferably used in an amount of 5 parts by weight or less, more preferably 3 parts by weight or less, and even more preferably 1 part by weight or less, per 100 parts by weight of the base polymer.

[0139] <Method of manufacturing pressure-sensitive adhesive layer> When forming the pressure-sensitive adhesive layer 1 from the pressure-sensitive adhesive composition, it is preferable to adjust the total amount of crosslinking agent added to the pressure-sensitive adhesive composition and to fully consider the effects of the crosslinking temperature and crosslinking time.

[0140] The crosslinking temperature and time can be adjusted as appropriate depending on the crosslinking agent used. The crosslinking temperature is preferably 170° C. or less. Such crosslinking may be performed at the temperature during the drying process of the pressure-sensitive adhesive layer 1, or may be performed in a separate crosslinking process after the drying process. The crosslinking time can be set in consideration of productivity and workability, but is usually about 0.2 to 20 minutes, and preferably about 0.5 to 10 minutes.

[0141] The method for forming the adhesive layer 1 is not particularly limited, and may be a method in which an adhesive composition is applied onto various substrates, dried in a dryer such as a heat oven to volatilize the solvent, and if necessary, crosslinked to form the adhesive layer 1, and then the adhesive layer 1 is transferred onto the polarizing film 2; or a method in which the adhesive composition is applied directly onto the polarizing film 2 to form the adhesive layer 1.

[0142] The substrate is not particularly limited, and examples thereof include various substrates such as release films and transparent resin film substrates.

[0143] Various methods can be used to apply the pressure-sensitive adhesive composition to the substrate or the polarizing film 2. Specific examples include extrusion coating using a fountain coater, roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and a die coater.

[0144] The drying conditions (temperature, time) are not particularly limited and can be appropriately set depending on the composition and concentration of the pressure-sensitive adhesive composition, for example, at about 80 to 170° C., preferably 90 to 200° C., for 1 to 60 minutes, preferably 2 to 30 minutes. After drying, a crosslinking treatment can be carried out as necessary, and the conditions are as described above.

[0145] The thickness of the pressure-sensitive adhesive layer 1 (after drying) is, for example, preferably 5 to 100 μm, more preferably 7 to 70 μm, and even more preferably 10 to 50 μm. When the thickness of the pressure-sensitive adhesive layer 1 is 5 μm or more, the adhesive layer 1 tends to have improved adhesion to an adherend and sufficient durability under humid conditions. On the other hand, when the thickness of the pressure-sensitive adhesive layer is 100 μm or less, the pressure-sensitive adhesive layer 1 can be sufficiently dried when the pressure-sensitive adhesive composition is dried to form the pressure-sensitive adhesive layer 1, and the occurrence of residual air bubbles and uneven thickness of the pressure-sensitive adhesive layer 1 can be suppressed, so that problems in appearance tend not to occur.

[0146] Examples of the material of the release film include resin films such as polyethylene, polypropylene, polyethylene terephthalate, and polyester films, porous materials such as paper, cloth, and nonwoven fabric, nets, foam sheets, metal foils, and laminates thereof. As the release film, resin films are preferably used because of their excellent surface smoothness. Examples of the resin film include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polybutylene terephthalate films, polyurethane films, and ethylene-vinyl acetate copolymer films.

[0147] The thickness of the release film is usually 5 to 200 μm, and preferably about 5 to 100 μm. The release film may be subjected to a release treatment and an antifouling treatment using a release agent such as a silicone-based, fluorine-based, long-chain alkyl-based, or fatty acid amide-based agent, or silica powder, or an antistatic treatment such as a coating type, kneading type, or deposition type. In particular, by appropriately performing a release treatment such as a silicone treatment, a long-chain alkyl treatment, or a fluorine treatment on the surface of the release film, the releasability from the pressure-sensitive adhesive layer 1 can be further improved.

[0148] The transparent resin film substrate is not particularly limited, but various resin films having transparency are used. The resin film is formed of a single layer film. For example, the material thereof may be polyester-based resins such as polyethylene terephthalate and polyethylene naphthalate, acetate-based resins, polyethersulfone-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyolefin-based resins, (meth)acrylic-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, polyarylate-based resins, polyphenylene sulfide-based resins, etc. Among these, polyester-based resins, polyimide-based resins, and polyethersulfone-based resins are particularly preferred. The thickness of the film substrate is preferably 15 to 200 μm.

[0149] [Polarizing film] The polarizing film 2 is a laminate including a polarizer and a transparent protective film. The transparent protective film is disposed, for example, in contact with the main surface (the surface having the largest area) of the layered polarizer. The polarizer may be disposed between two transparent protective films.

[0150] The polarizer is not particularly limited, and various polarizers can be used. Examples of the polarizer include a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or an ethylene-vinyl acetate copolymer partially saponified film, which is uniaxially stretched after adsorbing a dichroic substance such as iodine or a dichroic dye; a polyene-based oriented film such as a dehydrated polyvinyl alcohol or a dehydrochlorinated polyvinyl chloride; and the like. Among these, a polarizer made of a polyvinyl alcohol film and a dichroic substance such as iodine is preferred, and an iodine-based polarizer containing iodine and / or iodine ions is more preferred. The thickness of the polarizer is not particularly limited, but is generally about 5 to 80 μm.

[0151] In polyvinyl alcohol-based films, the optical properties of the film may deteriorate due to polyenization caused by a dehydration reaction of polyvinyl alcohol in a high-temperature environment. Polyenization tends to occur more significantly when the polarizing film 2 has a high water content. Therefore, when a polyvinyl alcohol-based film is used as a polarizer, preheating to reduce the water content of the polarizing film 2 in advance is particularly important.

[0152] A polarizer obtained by dyeing a polyvinyl alcohol-based film with iodine and stretching it uniaxially can be produced, for example, by dyeing the polyvinyl alcohol by immersing it in an aqueous solution of iodine and stretching it to 3 to 7 times its original length. If necessary, the polyvinyl alcohol can also be immersed in an aqueous solution of potassium iodide containing boric acid, zinc sulfate, zinc chloride, or the like. Furthermore, if necessary, the polyvinyl alcohol-based film may be immersed in water and washed before dyeing. Washing the polyvinyl alcohol-based film with water not only makes it possible to wash off dirt and antiblocking agents on the surface of the polyvinyl alcohol-based film, but also has the effect of suppressing the occurrence of uneven dyeing by swelling the polyvinyl alcohol-based film. The stretching of the polyvinyl alcohol-based film may be performed after dyeing with iodine, may be performed while dyeing, or may be performed before dyeing with iodine. The stretching may be performed in an aqueous solution of boric acid, potassium iodide, or the like, or in a water bath.

[0153] As the polarizer, a thin polarizer having a thickness of 10 μm or less can also be used. From the viewpoint of thinning, the thickness of the polarizer is preferably 1 to 7 μm. Such a thin polarizer is preferable in that it has less thickness unevenness, excellent visibility, and excellent durability due to less dimensional change, and further allows the polarizing film 2 to be thinned.

[0154] Representative examples of thin polarizers include thin polarizing films described in JP-A-51-069644, JP-A-2000-338329, WO-A-2010 / 100917, Japanese Patent No. 4751481, and JP-A-2012-073563. These thin polarizing films can be obtained by a manufacturing method including a step of stretching a polyvinyl alcohol-based resin (hereinafter also referred to as PVA-based resin) layer and a resin substrate for stretching in a laminated state, and a step of dyeing. With this manufacturing method, since the PVA-based resin layer is supported by the resin substrate for stretching, defects such as breakage due to stretching can be suppressed even if the PVA-based resin layer is thin.

[0155] Among the manufacturing methods including a step of stretching the laminate and a step of dyeing it, the manufacturing methods including a step of stretching in an aqueous boric acid solution described in WO 2010 / 100917, Japanese Patent No. 4751481, and JP 2012-073563 A are preferred because they enable stretching at a high ratio and improve polarization performance, and in particular, the manufacturing methods including a step of auxiliary air-stretching before stretching in an aqueous boric acid solution described in Japanese Patent No. 4751481 and JP 2012-073563 A are preferred.

[0156] As a material for forming the transparent protective film provided on one or both sides of the polarizer, for example, a thermoplastic resin excellent in transparency, mechanical strength, thermal stability, moisture blocking property, isotropy, etc. is used. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material of the transparent protective film may be a thermosetting resin or an ultraviolet-curing resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film 2 has two transparent protective films, the materials of the two transparent protective films may be the same or different from each other. For example, a transparent protective film made of a thermoplastic resin may be attached to one main surface of the polarizer via an adhesive, and a transparent protective film made of a thermosetting resin or an ultraviolet-curable resin may be attached to the other main surface of the polarizer. The transparent protective film may contain one or more types of optional additives. Examples of additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, coloring inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants. The content of the thermoplastic resin in the transparent protective film is preferably 50 to 100% by weight, more preferably 50 to 99% by weight, even more preferably 60 to 98% by weight, and particularly preferably 70 to 97% by weight. When the content of the thermoplastic resin in the transparent protective film is 50% by weight or more, the inherent high transparency of the thermoplastic resin tends to be fully exhibited.

[0157] The thickness of the transparent protective film can be determined appropriately, but is generally about 10 to 200 μm in terms of strength, workability such as handleability, thinness, and the like.

[0158] At least one transparent protective film included in the polarizing film 2 has a moisture permeability of 300 g / m 2- 24h or more is preferable, 500g / m 2 24h or more is preferable, 800g / m 2 24 hours or more is even more preferable. If the transparent protective film has high moisture permeability, the moisture content of the polarizing film 2 can be easily reduced by preheating. On the other hand, if the transparent protective film has an excessively high moisture permeability, the moisture durability of the polarizing film 2 may decrease. Therefore, the moisture permeability of the transparent protective film should be 1600 g / m 2 - 24h or less is preferable, 1300g / m 2 The moisture permeability is a value measured in accordance with the moisture permeability test (cup method) of JIS Z0208, and is measured at 40°C, with a relative humidity difference of 90%, over an area of ​​1 m 2 is the weight of water vapor that permeates a sample in 24 hours.

[0159] The polarizer and the transparent protective film are usually adhered to each other via a water-based adhesive. Examples of the water-based adhesive include an isocyanate-based adhesive, a polyvinyl alcohol-based adhesive, a gelatin-based adhesive, a vinyl-based latex-based adhesive, a water-based polyurethane, and a water-based polyester. Examples of adhesives other than the above-mentioned adhesives include an ultraviolet-curable adhesive and an electron beam-curable adhesive. The electron beam-curable polarizing film adhesive exhibits suitable adhesion to various transparent protective films. The adhesive may contain a metal compound filler.

[0160] In the polarizing film 2, a retardation film or the like can be formed on the polarizer instead of the transparent protective film. Another transparent protective film or a retardation film or the like can be further provided on the transparent protective film.

[0161] The transparent protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for the purposes of anti-reflection, anti-sticking, diffusion, anti-glare, etc.

[0162] [Other parts] The pressure-sensitive adhesive layer-attached polarizing film 10 may further include other optical films other than the polarizing film 2. Examples of the other optical films include films used in liquid crystal display devices, such as a reflector, a translucent plate, a retardation film, a viewing angle compensation film, and a brightness improvement film. Retardation films include, for example, a 1 / 2 wavelength plate and a 1 / 4 wavelength plate. The pressure-sensitive adhesive layer-attached polarizing film 10 may include one or more of these other optical films.

[0163] The polarizing film 10 with the pressure-sensitive adhesive layer may further include an anchor layer located between the polarizing film 2 and the pressure-sensitive adhesive layer 1. The material forming the anchor layer is not particularly limited, and examples thereof include various polymers, metal oxide sol, silica sol, and the like. Among these, polymers are particularly preferably used. The form of the polymer used may be any of a solvent-soluble type, a water-dispersed type, and a water-soluble type.

[0164] Examples of the polymers include polyurethane resins, polyester resins, acrylic resins, polyether resins, cellulose resins, polyvinyl alcohol resins, polyvinylpyrrolidone, and polystyrene resins.

[0165] When the pressure-sensitive adhesive layer 1 of the pressure-sensitive adhesive layer-attached polarizing film 10 is exposed, the pressure-sensitive adhesive layer 1 may be protected with a release film (separator) until it is put to practical use. Examples of the release film include those mentioned above. When a release film is used as a substrate in producing the pressure-sensitive adhesive layer 1, the release film can be used as a release film for the pressure-sensitive adhesive layer 1 of the pressure-sensitive adhesive layer-attached polarizing film 10 by laminating the pressure-sensitive adhesive layer 1 on the release film and the polarizing film 2, which allows simplification in terms of the process.

[0166] [Characteristics of adhesive layer] Next, we will explain the possible mechanism why the adhesive layer 1 of the adhesive layer-attached polarizing film 10 can maintain reworkability after preheating and has durability in high-temperature environments even when attached to a conductive layer.

[0167] After forming the adhesive layer 1 from the adhesive composition, the acid anhydride group of the compound (C) in the adhesive layer 1 is hydrolyzed by moisture in the air and converted into an acidic group. On the other hand, on the surface of the conductive layer containing a metal oxide such as ITO, not only hydroxyl groups but also metal cations generated by the hydroxyl groups being released as hydroxide ions are present. As shown in FIG. 2, when the polarizing film 10 with the adhesive layer is attached to the conductive layer 3 by the adhesive layer 1, the acidic group of the compound (C) is deprotonated by a neutralization reaction with the hydroxide ions present in the vicinity of the surface of the conductive layer 3. The anion thus generated forms an ionic bond with the metal cation on the surface of the conductive layer 3. That is, an acid-base reaction occurs between the acidic group of the compound (C) and the conductive layer 3. As a result, the compound (C) is segregated on the surface of the conductive layer 3, and it is presumed that a first layer 11 containing the compound (C) is formed in the adhesive layer 1.

[0168] After the first layer 11 is formed, the polyether compound (D) tends to segregate on the surface of the first layer 11. Therefore, in the pressure-sensitive adhesive layer 1, a second layer 12 containing the polyether compound (D) is formed on the first layer 11. When the pressure-sensitive adhesive layer 1 does not contain the compound (C), the polyether compound (D) hardly segregates on the surface of the conductive layer 3. Therefore, the first layer 11 can be regarded as a surface-modifying layer that modifies the surface of the conductive layer 3 so that the polyether compound (D) easily segregates.

[0169] In this manner, it is presumed that a first layer 11 and a second layer 12 are formed in the adhesive layer 1 by attaching the adhesive layer-attached polarizing film 10 to the conductive layer 3 with the adhesive layer 1. By forming the first layer 11 and the second layer 12, for example, a third layer 13 mainly containing an adhesive is further formed in the adhesive layer 1. The first layer 11, the second layer 12, and the third layer 13 are arranged in this order in the stacking direction.

[0170] Before preheating, the first layer 11 and the second layer 12 have a smaller cohesive force than the third layer 13. Therefore, before preheating, the pressure-sensitive adhesive layer-attached polarizing film 10 can be easily peeled off from the conductive layer 3 due to cohesive failure in the first layer 11 or the second layer 12.

[0171] For example, when preheating is performed at a temperature of about 70°C to 95°C, the cohesive strength of the first layer 11 tends to increase significantly due to the reaction of the compound (C). The increase in the cohesive strength of the first layer 11 is particularly remarkable when the compound (C) contains a hydrolyzable group (h1). On the other hand, the cohesive strength of the second layer 12 is less likely to increase than that of the first layer 11. Therefore, after preheating, the pressure-sensitive adhesive layer-attached polarizing film 10 can be easily peeled off from the conductive layer 3 due to cohesive failure in the second layer 12 or at the interface between the first layer 11 and the second layer 12. That is, the second layer 12 functions as a layer that ensures the reworkability of the pressure-sensitive adhesive layer 1 after preheating.

[0172] Furthermore, when the pressure-sensitive adhesive layer 1 is placed in an environment with a temperature higher than 95° C., the cohesive strength of the second layer 12 tends to increase significantly due to the reaction of the polyether compound (D) or the like. The increase in the cohesive strength of the second layer 12 is particularly remarkable when the polyether compound (D) contains a hydrolyzable group (h2). This tends to increase the adhesive strength between the pressure-sensitive adhesive layer 1 and the conductive layer 3 significantly, and improve the durability of the pressure-sensitive adhesive layer 1.

[0173] According to another aspect of the present invention, A pressure-sensitive adhesive layer 1 formed from a pressure-sensitive adhesive composition, The pressure-sensitive adhesive composition contains a compound (C) having an acidic group or an acid anhydride group and a polyether compound (D), Adhesive strength P obtained by test 1 85 is 10.0N / 25mm or less, and the adhesive strength P obtained by test 2 105 The adhesive layer 1 has a compressibility of greater than 10.0 N / 25 mm.

[0174] (Embodiment of Image Display Panel) As shown in Fig. 3, the image display panel 100 of this embodiment includes a polarizing film 10 with an adhesive layer, a conductive layer 3, and a transparent substrate 4. The conductive layer 3 and the transparent substrate 4 are, for example, members that constitute a liquid crystal cell 20. That is, the image display panel 100 is a liquid crystal display panel that includes the polarizing film 10 with an adhesive layer and the liquid crystal cell 20. However, the image display panel 100 may include an organic EL cell instead of the liquid crystal cell 20. In the image display panel 100, the polarizing film 10 with an adhesive layer is, for example, located closer to the viewing side than the liquid crystal cell 20.

[0175] The adhesive layer-attached polarizing film 10, the conductive layer 3, and the transparent substrate 4 are arranged, for example, in this order in the stacking direction, and the adhesive layer 1 of the adhesive layer-attached polarizing film 10 is in direct contact with the conductive layer 3. In other words, the adhesive layer-attached polarizing film 10 is attached to the conductive layer 3 by the adhesive layer 1. The conductive layer 3 is in direct contact with, for example, the transparent substrate 4. If necessary, other layers such as an undercoat layer or an oligomer prevention layer may be disposed between the conductive layer 3 and the transparent substrate 4.

[0176] [Adhesive layer] As described above, when the pressure-sensitive adhesive layer-attached polarizing film 10 is attached to the conductive layer 3 by the pressure-sensitive adhesive layer 1, a first layer 11, a second layer 12, and a third layer 13 are formed in the pressure-sensitive adhesive layer 1. The conductive layer 3, the first layer 11, the second layer 12, and the third layer 13 are arranged in this order in the stacking direction, and the third layer 13 is located between the second layer 12 and the polarizing film 2.

[0177] The first layer 11 contains, for example, a compound (C) or a reactant (R1) thereof. When the compound (C) contains a hydrolyzable group (h1), the reactant (R1) is, for example, a hydrolysis condensate of a plurality of compounds (C), or a reaction product of the compound (C) and a hydroxyl group on the surface of the conductive layer 3. The first layer 11 may contain the compound (C) or the reactant (R1) thereof as a main component.

[0178] The second layer 12 contains, for example, a polyether compound (D) or a reactant (R2) thereof. When the polyether compound (D) contains a hydrolyzable group (h2), the reactant (R2) is, for example, a hydrolysis condensate of a plurality of polyether compounds (D). The second layer 12 may contain the polyether compound (D) or the reactant (R2) thereof as a main component.

[0179] The third layer 13 contains a base polymer such as a (meth)acrylic polymer (A) or a reactant thereof (R3). When the pressure-sensitive adhesive composition forming the pressure-sensitive adhesive layer 1 contains a crosslinking agent, the reactant (R3) is, for example, a crosslinked product of the (meth)acrylic polymer (A). The third layer 13 may contain the (meth)acrylic polymer (A) or the reactant thereof (R3) as a main component.

[0180] The presence of the first layer 11, the second layer 12, and the third layer 13 in the adhesive layer 1 may be confirmed by a method such as time-of-flight secondary ion mass spectrometry (TOF-SIMS). For example, an adhesive composition for forming the adhesive layer 1 is prepared. This adhesive composition is applied to the conductive layer 3 to prepare a coating film having a thickness of about 1 μm after drying. The coating film is dried to obtain a film, which is analyzed by TOF-SIMS from its surface to the thickness direction of the film. This makes it possible to confirm that the adhesive layer 1 has the first layer 11, the second layer 12, and the third layer 13.

[0181] [Conductive layer] The conductive layer 3 is not particularly limited as long as it contains a metal oxide. Examples of the metal oxide include oxides containing at least one metal selected from the group consisting of indium, tin, zinc, gallium, antimony, titanium, silicon, zirconium, magnesium, aluminum, gold, silver, copper, palladium, and tungsten. The conductive layer 3 may contain not only a metal oxide but also a metal listed in the above group, if necessary. The material of the conductive layer 3 is preferably indium tin oxide, tin oxide containing antimony, or the like. Indium tin oxide means indium oxide containing tin oxide, and is called indium-tin composite oxide or ITO. The conductive layer 3 preferably contains ITO, and more preferably is substantially made of ITO.

[0182] The ITO contained in the conductive layer 3 preferably has an indium oxide content of 80 to 99% by weight. The ITO preferably has a tin oxide content of 1 to 20% by weight. The ITO may be crystalline or non-crystalline (amorphous).

[0183] The thickness of the conductive layer 3 is not particularly limited, and is preferably 10 nm or more, more preferably 15 to 40 nm, and further preferably 20 to 30 nm.

[0184] The method for forming the conductive layer 3 is not particularly limited, and any conventionally known method can be used. Specifically, the conductive layer 3 can be produced by a vacuum deposition method, a sputtering method, an ion plating method, or the like. These methods can be appropriately selected depending on the required film thickness of the conductive layer 3.

[0185] [Transparent substrate] The transparent substrate 4 may be made of any material as long as it is transparent. Examples of the transparent substrate 4 include glass and transparent resin film substrates. Examples of the transparent resin film substrate include those mentioned above.

[0186] [Liquid crystal cell] The liquid crystal cell 20 further includes, for example, a liquid crystal layer 5 and a transparent substrate 6 in addition to the conductive layer 3 and the transparent substrate 4. In the liquid crystal cell 20, the conductive layer 3, the transparent substrate 4, the liquid crystal layer 5 and the transparent substrate 6 are arranged in this order in the stacking direction.

[0187] The liquid crystal layer 5 is not particularly limited, and any type such as TN type, STN type, π type, VA type, IPS type, etc. can be used. The transparent substrate 6 is only required to be a transparent substrate, and the material thereof is not particularly limited. Examples of the transparent substrate 6 include glass and transparent resin film substrates. Examples of the transparent resin film substrates include those mentioned above.

[0188] [Other parts] In addition to the pressure-sensitive adhesive layer-attached polarizing film 10 and the liquid crystal cell 20, the image display panel 100 may further include optical films such as a retardation film, a viewing angle compensation film, and a brightness enhancement film.

[0189] [Manufacturing method of image display panel] The method for producing the image display panel 100 is not particularly limited, and includes, for example, performing a first heat treatment at 70°C to 95°C on the adhesive layer 1 in a state where the adhesive layer-attached polarizing film 10 is attached to the conductive layer 3.

[0190] The first heat treatment corresponds to preheating for reducing the moisture content of the polarizing film 2. The temperature of the first heat treatment is preferably 80° C. to 95° C. The time of the first heat treatment is not particularly limited and is, for example, 1 hour to 5 hours, and preferably 3 hours to 5 hours.

[0191] The moisture content of the polarizing film 2 after the first heat treatment is not particularly limited, and may be, for example, 7 g / m 2 The moisture content of the polarizing film 2 can be measured by the method described in Patent Document 1.

[0192] The method for producing the image display panel 100 may further include performing a second heat treatment on the adhesive layer 1 at a temperature higher than 95° C. after the first heat treatment. The second heat treatment tends to significantly increase the adhesive strength of the adhesive layer 1 and improve the durability of the adhesive layer 1. The temperature of the second heat treatment may be 100° C. to 150° C. The time of the second heat treatment is not particularly limited and is, for example, 1 hour to 1000 hours, and is preferably 24 hours or more.

[0193] (Modification of Image Display Panel) The image display panel 100 may include two polarizing films 10 with an adhesive layer. As shown in Fig. 4, the image display panel 110 according to this modification includes two polarizing films 10a and 10b with an adhesive layer. Except for the polarizing film 10b with an adhesive layer, the structure of the image display panel 110 is the same as the structure of the image display panel 100. Therefore, elements common to the image display panel 100 and the image display panel 110 of the modification are given the same reference symbols, and their descriptions may be omitted.

[0194] The pressure-sensitive adhesive layer-attached polarizing film 10b is attached to the transparent substrate 6 of the liquid crystal cell 20 by the pressure-sensitive adhesive layer 1b. In the image display panel 110, the liquid crystal cell 20 is located between the pressure-sensitive adhesive layer-attached polarizing films 10a and 10b, and is located on the viewing side of the pressure-sensitive adhesive layer-attached polarizing film 10b.

[0195] The pressure-sensitive adhesive layer 1b and the polarizing film 2b of the pressure-sensitive adhesive layer-attached polarizing film 10b may be the same as or different from the pressure-sensitive adhesive layer 1a and the polarizing film 2a of the pressure-sensitive adhesive layer-attached polarizing film 10a. The pressure-sensitive adhesive layer 1b and the polarizing film 2b may be conventionally used in this field.

[0196] (Embodiment of Image Display Device) The image display device of this embodiment includes, for example, an image display panel 100 and an illumination system. In the image display device, an image display panel 110 can be used instead of the image display panel 100. In the image display device, the image display panel 100 is disposed, for example, on the viewing side of the illumination system. The illumination system includes, for example, a backlight or a reflector, and irradiates the image display panel 100 with light.

[0197] Examples of image display devices include liquid crystal display devices, electroluminescence (EL) displays, plasma displays (PDs), field emission displays (FEDs), etc. These image display devices can be used for home appliances, in-vehicle applications, public information displays (PIDs), etc., and are particularly preferably used for in-vehicle applications. EXAMPLES

[0198] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the examples shown below. In the following, unless otherwise specified, "%" indicates "weight %", "parts" indicates "weight parts", and "thickness" indicates "physical film thickness". Unless otherwise specified, the indoor temperature and humidity are 23°C and 65% RH.

[0199] (Acrylic polymer (A1)) A monomer mixture containing 100 parts by weight of butyl acrylate (BA), 0.075 parts by weight of 4-hydroxybutyl acrylate (HBA), and 5 parts by weight of acrylic acid (AA) was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) was charged as a polymerization initiator together with 100 parts of ethyl acetate for 100 parts by weight of the monomer mixture, and nitrogen gas was introduced while gently stirring to replace the atmosphere with nitrogen. The liquid temperature in the flask was kept at around 55°C and the polymerization reaction was carried out for 6 hours. As a result, a solution of an acrylic polymer (A1) with a weight average molecular weight of 2.4 million and Mw / Mn=4.5 was prepared.

[0200] (Acrylic polymer (A2)) A solution of the acrylic polymer (A2) was prepared in the same manner as for the acrylic polymer (A1), except that the monomers used were changed as shown in Table 1.

[0201] (Acrylic Oligomer (B1)) In a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser, 85 parts by weight of butyl acrylate (BA), 15 parts by weight of acrylic acid (AA), 0.1 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator, 100 parts by weight of toluene, and 3.5 parts by weight of α-thioglycerol were charged, and nitrogen gas was introduced while gently stirring to sufficiently replace the atmosphere with nitrogen. The liquid temperature in the flask was kept at around 60°C, and a polymerization reaction was carried out for 4 hours to prepare a solution of acrylic oligomer (B1). The weight average molecular weight of the acrylic oligomer (B1) was 6700.

[0202] (Acrylic Oligomer (B2)) Acrylic oligomer (B2) was prepared in the same manner as acrylic oligomer (B1), except that the monomers used were changed as shown in Table 1.

[0203] [Table 1]

[0204] The abbreviations in Table 1 are as follows. BA: n-butyl acrylate HBA: 4-hydroxybutyl acrylate AA: Acrylic acid PEA: Phenoxyethyl acrylate NVP: N-vinyl-2-pyrrolidone MEA: 2-Methoxyethyl acrylate

[0205] (Compound (C1)) Compound (C1) was prepared according to the method described in Example 1 of JP 2013-129809 A. Compound (C1) was an organopolysiloxane compound and contained the above-mentioned siloxane units (U1) and (U2). In the siloxane unit (U1), X is a propylsuccinic anhydride group, R 4 was a methyl group. In the siloxane unit (U2), two R 4 were all methoxy groups. The content of siloxane units (U1) in compound (C1) was 27 mol%. The content of siloxane units (U2) in compound (C1) was 73 mol%. The weight average molecular weight of compound (C1) was about 1000.

[0206] (Polarizing film) [TAC film with HC] First, a resin solution (manufactured by DIC Corporation, product name: Unidic 17-806, solid content concentration: 80%) in which an ultraviolet-curable resin monomer or oligomer mainly composed of urethane acrylate was dissolved in butyl acetate was prepared. Next, 5 parts of a photopolymerization initiator (manufactured by BASF Corporation, product name: IRGACURE907) and 0.1 parts of a leveling agent (manufactured by DIC Corporation, product name: GRANDIC PC4100) were added to the resin solution per 100 parts of solid content of the resin solution. Next, a material for forming a hard coat layer was prepared by adding cyclopentanone and propylene glycol monomethyl ether in a ratio of 45:55 to the solution so that the solid content concentration of the obtained solution was 36%. Next, this material was applied onto a TAC film (manufactured by Fuji Film Corporation, TJ40UL, raw material: triacetyl cellulose polymer, thickness: 40 μm) so that the thickness of the hard coat layer after curing was 7 μm to form a coating film. Next, the coating was dried at 90°C for 1 minute and then irradiated with a high-pressure mercury lamp at an integrated light intensity of 300 mJ / cm 2 The coating film was cured by irradiating it with ultraviolet light, forming a hard coat layer (HC). This produced a TAC film with HC.

[0207] [Acrylic film] A 30L kettle reactor equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen inlet tube was charged with 8,000g of methyl methacrylate (MMA), 2,000g of 2-(hydroxymethyl)methyl acrylate (MHMA), 10,000g of 4-methyl-2-pentanone (methyl isobutyl ketone, MIBK), and 5g of n-dodecyl mercaptan, and the temperature was raised to 105°C while nitrogen was passed through the reactor. When reflux started, 5.0g of t-butylperoxyisopropyl carbonate (Kayacarvon BIC-7, manufactured by Kayaku Akzo Co., Ltd.) was added as a polymerization initiator, and a solution consisting of 10.0g of t-butylperoxyisopropyl carbonate and 230g of MIBK was added dropwise over 4 hours, while solution polymerization was carried out at about 105 to 120°C under reflux, and maturation was carried out over another 4 hours.

[0208] To the obtained polymer solution, 30 g of a stearyl phosphate / distearyl phosphate mixture (PhoslexA-18, Sakai Chemical Industry Co., Ltd.) was added, and the cyclization condensation reaction was carried out at about 90 to 120 ° C. for 5 hours under reflux. Next, the obtained polymer solution was introduced into a vent-type screw twin-screw extruder (φ = 29.75 mm, L / D = 30) with a barrel temperature of 260 ° C., a rotation speed of 100 rpm, a vacuum degree of 13.3 to 400 hPa (10 to 300 mmHg), one rear vent, and four fore vents at a processing rate of 2.0 kg / h in terms of resin amount. In this extruder, further cyclization condensation reaction and devolatilization proceeded. As a result, transparent pellets of lactone ring-containing polymer were obtained.

[0209] The lactone ring-containing polymer thus obtained was subjected to dynamic TG measurement, and a mass loss of 0.17% by mass was detected. The lactone ring-containing polymer had a weight average molecular weight of 133,000, a melt flow rate of 6.5 g / 10 min, and a glass transition temperature of 131° C.

[0210] The pellets obtained were mixed and extruded with an acrylonitrile-styrene (AS) resin (Toyo ASAS20, manufactured by Toyo Styrene Co., Ltd.) in a mass ratio of 90 / 10 using a single-screw extruder (screw 30 mmφ) to obtain transparent pellets. The glass transition temperature of the pellets obtained was 127°C.

[0211] The pellets were melt-extruded from a 400 mm wide coat hanger type T-die using a 50 mmφ single screw extruder to produce a film with a thickness of 120 μm. The film thus produced was stretched 2.0 times in the vertical direction and 2.0 times in the horizontal direction at a temperature of 150° C. using a biaxial stretching device to obtain a stretched film (acrylic film) with a thickness of 30 μm. The optical properties of the stretched film were measured to find that the total light transmittance was 93%, the in-plane retardation Δnd was 0.8 nm, and the thickness direction retardation Rth was 1.5 nm.

[0212] Next, a polarizing film was produced by the following method. First, a 45 μm thick polyvinyl alcohol film was dyed in a 0.3% iodine solution (temperature 30° C.) for 1 minute between a plurality of rolls with different speed ratios, while being stretched to a stretching ratio of 3 times. Next, the obtained stretched film was stretched to a total stretching ratio of 6 times while being immersed in an aqueous solution (temperature 60° C.) containing 4% boric acid and 10% potassium iodide for 0.5 minutes. Next, the stretched film was washed by immersing it in an aqueous solution (temperature 30° C.) containing 1.5% potassium iodide for 10 seconds. Next, the stretched film was dried at 50° C. for 4 minutes to obtain a polarizer with a thickness of 18 μm. The above saponified HC-attached TAC film was attached to one main surface of the obtained polarizer via a polyvinyl alcohol-based adhesive. At this time, the triacetyl cellulose film was located on the polarizer side rather than the hard coat layer. The above-mentioned acrylic film was attached to the other main surface of the polarizer via a polyvinyl alcohol adhesive, thereby obtaining a polarizing film.

[0213] Example 1 A solution of an acrylic adhesive composition was prepared by mixing 0.4 parts of compound (C1), 0.4 parts of polyether compound (D) (Silyl SAT10 manufactured by Kaneka Corporation), 0.5 parts of lithium bis(trifluoromethanesulfonyl)imide, 1 part of an isocyanate crosslinking agent (Coronate L, trimethylolpropane tolylene diisocyanate manufactured by Tosoh Corporation), and 0.2 parts of benzoyl peroxide (Niper BMT manufactured by Nippon Oil & Fats Co., Ltd.) with respect to 100 parts of the solid content of the solution of the acrylic polymer (A1). Silyl SAT10 is a compound represented by the above formula (13), and A 1 is -CH2CH(CH3)-, and A 2 is -C3H6- and Z 1 Ga-C3H6-Z 0 and a reactive silyl group (Z 0 -) is a dimethoxymethylsilyl group. The number average molecular weight of Silyl SAT10 is 5,000.

[0214] Next, the obtained solution of the acrylic adhesive composition was applied to one side of a polyethylene terephthalate film (separator film: MRF38, manufactured by Mitsubishi Chemical Polyester Film Co., Ltd.) treated with a silicone-based release agent so that the thickness of the adhesive layer after drying was 20 μm. The applied film was dried at 155° C. for 1 minute to form an adhesive layer on the surface of the separator film. Next, the adhesive layer formed on the separator film was transferred to the acrylic film side of the polarizing film to produce the adhesive layer-attached polarizing film of Example 1.

[0215] (Examples 2 to 12, Comparative Examples 1 to 3) The pressure-sensitive adhesive layer-attached polarizing films of Examples 2 to 12 and Comparative Examples 1 to 3 were produced in the same manner as in Example 1, except that the components of the acrylic pressure-sensitive adhesive composition were changed as shown in Table 2.

[0216] [evaluation] <Weight average molecular weight (Mw) of acrylic polymers and acrylic oligomers> The weight average molecular weight (Mw) of the obtained acrylic polymer and acrylic oligomer was measured by GPC (gel permeation chromatography). Analytical equipment: Tosoh HLC-8120GPC Column: Tosoh G7000H XL +GMH XL +GMH XL Column size: 7.8mmφ×30cm each, total 90cm Column temperature: 40℃ ·Flow rate: 0.8ml / min ·Injection volume: 100μl Eluent: Tetrahydrofuran Detector: Differential refractometer (RI) Standard sample: polystyrene

[0217] <Adhesive strength> Adhesive strength P0, P 85 and P 105 The above-mentioned tests 1 to 3 were carried out. The ITO-layered glass was prepared by forming an ITO layer on a 7 mm thick non-alkali glass (manufactured by Corning, product name "EG-XG"). The ITO layer was prepared by a sputtering method. In the ITO layer, the ratio of the weight of Sn atoms to the total value of the weight of Sn atoms and the weight of In atoms (Sn ratio) was 3 wt%. The surface of the ITO layer was analyzed under the following measurement conditions using an atomic force microscope (AFM, manufactured by Bruker, Dimension3100+NanoscopeV). As a result, the average surface roughness Ra of the ITO layer was 0.2 nm, the root mean square roughness Rq was 0.3 nm, and the maximum height Rmax was 2.6 nm. The operation of peeling off the test piece from the ITO layer was performed using a tensile tester (autograph SHIMAZU AG-1 1OKN). (AFM measurement conditions) Measurement mode: Tapping mode Cantilever: Si single crystal ·Measurement area: 10μm square

[0218] <Initial reworkability> A rework test was carried out by the following method using the glass with the ITO layer used for measuring the adhesive force. First, the polarizing film with the adhesive layer was cut into a strip of 230 mm length x 120 mm width to prepare a test piece. Next, the test piece was attached to the surface of the ITO layer of the glass with the ITO layer by the adhesive layer. The test piece was attached to the ITO layer using a laminator. After the test piece was attached, it was placed in an autoclave at 50°C and 5 atm (absolute pressure) for 15 minutes to homogenize the bonding between the ITO layer and the adhesive layer, and the adhesive layer was adhered to the ITO layer. Next, the test piece was peeled off from the glass with the ITO layer by hand. The rework test was carried out three times using the above procedure, and the initial reworkability of the adhesive layer was evaluated according to the following criteria. (Evaluation Criteria) A: All three sheets were able to be peeled off easily without any adhesive residue or film breakage. B: Some of the three sheets had their films broken when peeled off, but could be peeled off by peeling again. C: All three films were broken when peeled off, but could be peeled off by peeling again. D: All three sheets had adhesive residue, or the film broke and could not be peeled off no matter how many times attempts were made to peel it off.

[0219] <Reworkability after preheating> In the rework test, the reworkability after preheating of the adhesive layer was evaluated in the same manner as in the evaluation of reworkability described above, except that after the bonding between the ITO layer and the adhesive layer was homogenized in an autoclave, heat treatment was performed for 5 hours under atmospheric pressure at 85°C, and after the heat treatment, the test piece was left in an atmosphere at room temperature to reduce the temperature of the test piece to room temperature.

[0220] <Durability> The durability test was carried out by the following method using the glass with the ITO layer used for measuring the adhesive force. First, the polarizing film with the adhesive layer was cut into a strip of 300 mm length x 220 mm width to prepare a test piece. Next, the test piece was attached to the surface of the ITO layer of the glass with the ITO layer by the adhesive layer. The test piece was attached to the ITO layer using a laminator. After the test piece was attached, it was placed in an autoclave at 50°C and 0.5 MPa for 15 minutes to homogenize the bonding between the ITO layer and the adhesive layer, and the adhesive layer was adhered to the ITO layer. Next, the test piece was subjected to a heat treatment for 500 hours under atmospheric pressure at 105°C. The appearance of the adhesive layer between the polarizing film and the ITO layer was visually observed, and the durability of the adhesive layer was evaluated according to the following criteria. (Evaluation Criteria) A: There was absolutely no change in appearance such as foaming or peeling. B: There is peeling or foaming at the edges, but it does not pose a problem in practical use unless it is for a special purpose. C: There is significant peeling at the edge, and it is problematic for practical use.

[0221] [Table 2]

[0222] The abbreviations in Table 2 are as follows. A1: Acrylic polymer (A1) A2: Acrylic polymer (A2) B1: Acrylic oligomer (B1) B2: Acrylic oligomer (B2) C1: Compound (C1) X- 12 -967C: 3-trimethoxysilylpropylsuccinic anhydride (Shin-Etsu Chemical Co., Ltd.) SAT10: Silyl SAT10 (Kaneka) X-41-1056: Epoxy group-containing oligomer type silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0223] As can be seen from Table 2, the adhesive layer of the polarizing film with the adhesive layer of this embodiment maintained reworkability after preheating even when attached to a conductive layer, and had durability in a high-temperature environment. In Comparative Examples 2 and 3 in which the compound (C) was not present, the adhesive strengths P0 and P 85 Under the conditions for measuring the adhesion strength P 105 It is estimated that, under the conditions for measuring the adhesive strength P 105 is the adhesive strength P 85 This is thought to be the reason for the poor durability after heat treatment at 105°C. [Industrial Applicability]

[0224] The pressure-sensitive adhesive layer-attached polarizing film of the present invention can be suitably used in image displays such as liquid crystal displays, electroluminescence (EL) displays, plasma displays (PD) and field emission displays (FED). [Explanation of symbols]

[0225] 1 Adhesive layer 2. Polarizing film 3 Conductive layer 4 Transparent substrate 10 Polarizing film with adhesive layer 11 1st layer 12 2nd layer 13 3rd layer 20 Liquid crystal cell 100,110 Image display panel

Claims

1. A polarizing film with a pressure-sensitive adhesive layer, comprising a polarizing film and a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition, The pressure-sensitive adhesive composition includes a base polymer, a compound (C) having an acidic group or an acid anhydride group, and a polyether compound (D), the content of the compound (C) in the pressure-sensitive adhesive composition is 0.4 parts by weight or more based on 100 parts by weight of the base polymer, The adhesive strength P of the pressure-sensitive adhesive layer was determined by the following test 1. 85 is 10.0 N / 25 mm or less, and the adhesive strength P obtained by the following test 2 105 A polarizing film with an adhesive layer, the strength of which is greater than 10.0 N / 25 mm. Test 1: The adhesive layer attached to the indium tin oxide layer of the glass with an indium tin oxide layer was subjected to a heat treatment at 85° C. for 5 hours. The force required to peel the adhesive layer from the indium tin oxide layer at a peel speed of 300 mm / min and a peel angle of 90° (adhesion force P 85 ) is measured. Test 2: The adhesive layer attached to the indium tin oxide layer of the glass with an indium tin oxide layer was subjected to a heat treatment at 105° C. for 24 hours. The force required to peel the adhesive layer from the indium tin oxide layer at a peel speed of 300 mm / min and a peel angle of 90° (adhesive strength P 105 ) is measured.

2. The adhesive strength P of the pressure-sensitive adhesive layer was determined by the following test 3. 0 The pressure-sensitive adhesive layer-attached polarizing film according to claim 1 , wherein the tension is 10.0 N / 25 mm or less. Test 3: The adhesive layer attached to the indium tin oxide layer of the glass with an indium tin oxide layer is peeled off from the indium tin oxide layer at a peeling speed of 300 mm / min and a peeling angle of 90°. The force required for this (adhesive strength P 0 ) is measured.

3. 3. The pressure-sensitive adhesive layer-attached polarizing film according to claim 1, wherein the compound (C) and the polyether compound (D) each have a weight average molecular weight of 10,000 or less.

4. The pressure-sensitive adhesive layer-attached polarizing film according to any one of claims 1 to 3, wherein the acid anhydride group is a carboxylic acid anhydride group.

5. The pressure-sensitive adhesive layer-attached polarizing film according to any one of claims 1 to 4, wherein the compound (C) further has a silicon atom and a hydrolyzable group bonded to the silicon atom.

6. The pressure-sensitive adhesive layer-attached polarizing film according to claim 5 , wherein the content of the hydrolyzable group in the compound (C) is 10 wt % or more.

7. The pressure-sensitive adhesive layer-attached polarizing film according to any one of claims 1 to 6, wherein the compound (C) has a siloxane bond.

8. The pressure-sensitive adhesive layer-attached polarizing film according to any one of claims 1 to 7, wherein the polyether compound (D) further has a silicon atom and a hydrolyzable group bonded to the silicon atom.

9. The pressure-sensitive adhesive layer-attached polarizing film according to claim 8 , wherein the content of the hydrolyzable group in the polyether compound (D) is 14 wt % or less.

10. The pressure-sensitive adhesive layer-attached polarizing film according to any one of claims 1 to 9, wherein the pressure-sensitive adhesive composition comprises a (meth)acrylic polymer (A) as the base polymer.

11. The pressure-sensitive adhesive layer-attached polarizing film according to claim 10 , wherein the (meth)acrylic polymer (A) has an acidic group.

12. A polarizing film with a pressure-sensitive adhesive layer according to any one of claims 1 to 11, A conductive layer including a metal oxide; A transparent substrate; Equipped with The pressure-sensitive adhesive layer is in direct contact with the conductive layer.

13. The image display panel according to claim 12 , wherein the metal oxide comprises indium tin oxide.

14. the pressure-sensitive adhesive layer has a first layer containing the compound (C) or a reactant thereof, and a second layer containing the polyether compound (D) or a reactant thereof, 14. The image display panel according to claim 12, wherein the conductive layer, the first layer, and the second layer are arranged in this order in a stacking direction.

15. the pressure-sensitive adhesive layer further has a third layer containing a (meth)acrylic polymer (A) or a reaction product thereof, The image display panel according to claim 14 , wherein the third layer is located between the second layer and the polarizing film.

16. A method for manufacturing the image display panel according to any one of claims 12 to 15, comprising the steps of: and performing a first heat treatment on the pressure-sensitive adhesive layer at 70° C. to 95° C. in a state in which the pressure-sensitive adhesive layer-attached polarizing film is attached to the conductive layer.

17. The method for manufacturing an image display panel according to claim 16, further comprising: performing a second heat treatment on the pressure-sensitive adhesive layer at a temperature higher than 95°C after the first heat treatment.

18. A pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition, The pressure-sensitive adhesive composition includes a base polymer, a compound (C) having an acidic group or an acid anhydride group, and a polyether compound (D), the content of the compound (C) in the pressure-sensitive adhesive composition is 0.4 parts by weight or more based on 100 parts by weight of the base polymer, The adhesive strength P obtained by the following test 1 85 is 10.0 N / 25 mm or less, and the adhesive strength P obtained by the following test 2 105 The adhesive layer has a strength greater than 10.0 N / 25 mm. Test 1: The adhesive layer attached to the indium tin oxide layer of the glass with an indium tin oxide layer was subjected to a heat treatment at 85° C. for 5 hours. The force required to peel the adhesive layer from the indium tin oxide layer at a peel speed of 300 mm / min and a peel angle of 90° (adhesion force P 85 ) is measured. Test 2: The adhesive layer attached to the indium tin oxide layer of the glass with an indium tin oxide layer was subjected to a heat treatment at 105° C. for 24 hours. The force required to peel the adhesive layer from the indium tin oxide layer at a peel speed of 300 mm / min and a peel angle of 90° (adhesive strength P 105 ) is measured.

Citation Information

Patent Citations

  • Directional control method of fold printed matter

    JP1985071459A

  • Liquid crystal display device and polarizing plate with pressure-sensitive adhesive to be used therein

    JP2008009122A

  • Polarizing plate

    JP2016062029A

  • Polarizing film laminate for power vehicle and optical display panel in which the polarizing film laminate is used

    JP2019152863A

  • One-side protection polarization film having adhesive layer, picture display unit and continuous manufacturing method thereof

    JP2020003576A