Steel plate for enamel and its manufacturing method

A steel plate with controlled composition and manufacturing processes addresses fish scale and bubble defects, enhancing enamel adhesion and operational efficiency in enameling steel plates.

JP7588148B2Active Publication Date: 2024-11-21CLEANSOLUTION CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022538249
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-20
Filing Date
2020-12-17
Publication Date
2024-11-21
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Existing enameling steel plates face issues with fish scale defects, bubble defects, and poor enamel adhesion due to hydrogen absorption and surface defects, which are exacerbated by continuous annealing processes, leading to reduced productivity and increased costs.

Method used

A steel plate composition with controlled carbon, manganese, silicon, aluminum, phosphorus, sulfur, nitrogen, and oxygen levels, along with a thin oxidized layer and optimized manufacturing processes including hot rolling, cold rolling, and continuous annealing, to create a steel plate with excellent enamel adhesion and fish scale resistance.

Benefits of technology

The solution effectively suppresses fish scale and bubble defects, enhances enamel adhesion, and improves operational efficiency by utilizing low-temperature precipitates and controlled micropores, ensuring high-quality enameling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588148000004
    Figure 0007588148000004
  • Figure 0007588148000005
    Figure 0007588148000005
  • Figure 0007588148000001
    Figure 0007588148000001
Patent Text Reader

Abstract

A steel sheet for enamel according to one embodiment of the present invention contains, by weight, C: 0.01 to 0.05%, Mn: 0.46 to 0.80%, Si: 0.001 to 0.03%, Al: 0.01 to 0.08%, P: 0.001 to 0.02%, S: 0.001 to 0.02%, N: 0.004% or less (excluding 0%), and O: 0.003% or less (excluding 0%), with the remainder being Fe and unavoidable impurities. The steel sheet for enamel according to one embodiment of the present invention includes an oxide layer extending from the surface toward the inside, and the thickness of the oxide layer is 0.006 to 0.030 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] One embodiment of the present invention relates to a steel sheet for enamel and a manufacturing method thereof. More specifically, one embodiment of the present invention relates to a steel sheet for enamel of continuous annealing type for processing, which is free from bubble defects after enameling and has excellent enamel adhesion and fish scale resistance, and a manufacturing method thereof. [Background technology]

[0002] Enameled steel sheets are a type of surface-treated product in which a glassy glaze is applied to a base steel sheet such as a hot-rolled steel sheet or a cold-rolled steel sheet, and then the sheet is fired at high temperatures to improve corrosion resistance, weather resistance, heat resistance, etc. Such enameled steel sheets are used for building exteriors, home appliances, tableware, and various industrial materials.

[0003] Rimmed steel has been used for a long time as a steel plate for enamel, but in recent years, as continuous casting has been actively used to improve productivity, most materials are being continuously cast. In addition, fishscale defects, which are one of the most fatal defects in enamel steel plates in steel manufacturing, are a typical enamel defect that occurs when hydrogen dissolved in the steel becomes supersaturated in the steel during the sintering and cooling process during the enamel product manufacturing process, and is released to the steel surface, causing the enamel layer to fall off in the form of fish scales. If such fishscale defects occur, rust will form intensively at the defective area, greatly reducing the value of the enamel product, so it is necessary to suppress their occurrence. In order to prevent fishscale defects, it is necessary to form a large number of sites inside the steel that can adsorb hydrogen dissolved in the steel. Therefore, in order to prevent fish scale defects that reduce enamelability or to improve aging, open coil annealing (OCA), a type of box annealing method, has been applied. However, this method has problems such as reduced productivity, increased manufacturing costs, and large quality deviations due to long-term heat treatment. In addition, the open coil annealing method has problems such as difficulty in controlling the amount of decarburization, and if the amount of decarburization is excessive and the amount of carbon in the steel is excessively low, the grain boundaries of the steel sheet soften and cracks such as brittle fracture occur during product formation. In order to overcome the problems of poor productivity and increased manufacturing costs due to such long-term annealing, recently developed steel sheets for enamel actively use a continuous annealing process, and inclusions such as precipitates of titanium or inclusions made of undeoxidized steel are used as hydrogen storage sources. However, even in this case, a large amount of carbonitride-forming elements are added or undeoxidized compounds cause a high rate of surface defects, and the recrystallization temperature rises, reducing sheet threadability, which acts as a factor of various quality problems, reduced productivity, and increased costs.

[0004] In other words, enameled steel sheets that utilize titanium (Ti)-based precipitates have a large amount of titanium added to inhibit the hydrogen reaction that causes fish scale, which causes frequent nozzle clogging due to titanium nitride (TiN) and inclusions at the continuous casting stage of the steelmaking process, directly contributing to reduced workability and production loads. In addition, TiN mixed into the molten steel is present on the top of the steel sheet, causing blister defects, a typical bubble defect, and the addition of large amounts of titanium can also be a factor in impairing the adhesion between the steel sheet and the glaze layer.

[0005] On the other hand, high-oxygen enamel steel sheets, which increase the dissolved oxygen content inside the steel sheet and utilize inclusions such as oxides in the steel to absorb hydrogen and ensure fishscale resistance, also have fundamental problems in that the high oxygen content causes severe refractory corrosion, significantly reducing continuous casting productivity in the steelmaking process, and frequently causing surface defects. Summary of the Invention [Problem to be solved by the invention]

[0006] One embodiment of the present invention provides a steel sheet for enamel and a manufacturing method thereof. More specifically, one embodiment of the present invention provides a steel sheet for enamel of continuous annealing type for processing, which is free from bubble defects after enamel treatment and has excellent enamel adhesion and fish scale resistance, and a manufacturing method thereof. [Means for solving the problem]

[0007] The steel sheet for enamel according to one embodiment of the present invention contains, by weight, C: 0.01-0.05%, Mn: 0.46-0.80%, Si: 0.001-0.03%, Al: 0.01-0.08%, P: 0.001-0.02%, S: 0.001-0.02%, N: 0.004% or less (excluding 0%) and O: 0.003% or less (excluding 0%), with the remainder being Fe and unavoidable impurities.

[0008] The steel sheet for enamel according to one embodiment of the present invention includes an oxide layer extending from the surface toward the inside, and the oxide layer has a thickness of 0.006 to 0.030 μm.

[0009] The oxide layer may contain 90% by weight or more of Fe oxide.

[0010] The steel sheet for enamel according to one embodiment of the present invention has an adhesion relationship index (I PEI ) may be 0.001 to 0.020. [Formula 1] I PEI = ([Mn] × [P] × [Si] × [Oxide layer thickness]) / ([Al] × [C]) (In the above formula 1, [Mn], [P], [Si], [Al], and [C] represent the content (weight%) of each element divided by the atomic weight of each element, and [oxide layer thickness] represents the thickness (nm) of the oxide layer.)

[0011] The steel sheet for enamel according to one embodiment of the present invention may have a micropore area ratio difference (MVv) in each region calculated by the following formula 3 of 0.07 to 0.16%. [Formula 3] MVv=MV 1 / 8t -MV Av (In the above formula 3, MV 1 / 8t and MV Av indicates the 1 / 8 site and average micropore fraction in the thickness direction, respectively.)

[0012] The steel sheet for enamel according to one embodiment of the present invention may further include one or more of Cu: 0.01 wt % or less and Ti: 0.005 wt % or less.

[0013] The steel sheet for enamel according to one embodiment of the present invention may have a cementite fraction difference (Cv) after annealing calculated by the following formula 2 of 0.8 to 2.5%. [Formula 2] Cv=C 1 / 2t -C 1 / 8t (In the above formula 2, C 1 / 2t and C. 1 / 8tindicate the cementite fraction at the center and 1 / 8 of the thickness of the steel plate, respectively.)

[0014] The steel sheet for enamel according to one embodiment of the present invention may have enamel adhesion of 95% or more.

[0015] The steel sheet for enamel according to one embodiment of the present invention has a hydrogen permeability of 600 sec / mm 2 It may be more than that.

[0016] A method for producing a steel sheet for enamel according to one embodiment of the present invention includes the steps of: hot rolling a slab containing, by weight, C: 0.02-0.08%, Mn: 0.45-0.80%, Si: 0.001-0.03%, Al: 0.01-0.08%, P: 0.001-0.02%, S: 0.001-0.02%, N: 0.004% or less (excluding 0%), and O: 0.003% or less (excluding 0%), with the balance being Fe and unavoidable impurities, to produce a hot-rolled steel sheet; cold rolling the hot-rolled steel sheet to produce a cold-rolled steel sheet; and annealing the cold-rolled steel sheet.

[0017] The annealing stage is the oxidation index (PH 2 O / PH 2 ) can be heat-treated for 30 to 180 seconds in a humid atmosphere where the thermal expansion coefficient is 0.51 to 0.65.

[0018] The slabs can be hot rolled at a finish rolling temperature of 850℃~910℃.

[0019] In the step of producing a hot-rolled steel sheet, the hot-rolled steel sheet can be coiled at 580°C to 720°C.

[0020] Cold rolling can be performed at a rolling reduction of 60 to 90% to produce cold rolled steel sheets.

[0021] In the stage of annealing the cold rolled steel sheet, annealing can be performed at 720°C to 850°C.

[0022] After the step of annealing the cold rolled steel sheet, the method may further include a step of temper rolling the cold rolled steel sheet at a rolling reduction of 3% or less. Effect of the Invention

[0023] The steel sheet for enamel having excellent fish scale resistance and enamel adhesion according to one embodiment of the present invention can be used for home appliances, chemical equipment, kitchen equipment, sanitary equipment, and building interior and exterior materials.

[0024] The steel sheet for enamel with excellent fish scale resistance and enamel adhesion according to one embodiment of the present invention has a chemical composition of the steel material within an appropriate range and an adhesion-related index controlled at the same time, so that the cold-rolled steel sheet produced can ensure high enamel adhesion. In addition, by controlling the carbide and micropore fractions in the surface layer and center, fish scale and bubble defects, which are fatal defects in enamel steel sheets, can be suppressed, and enamel properties are significantly improved.

[0025] According to one embodiment of the present invention, a steel sheet for enamel having excellent fish scale resistance and enamel adhesion improves productivity and operability by utilizing low carbon steel with excellent surface properties of C: 0.02 to 0.08 wt % at the steelmaking stage, and when a thin sheet after cold rolling is heat treated in a continuous annealing furnace, the atmosphere in the furnace is optimized to control the carbide fraction in the steel in the thickness direction, thereby significantly improving the enamel properties even during high-speed heat treatment operations.

[0026] According to an embodiment of the present invention, a steel sheet for enamel with excellent fishscale resistance and enamel adhesion uses cementite, which is a low-temperature precipitate, and promotes decarburization reaction by controlling the atmosphere during the continuous annealing process. Cementite is uniformly dispersed during hot rolling, and micropores formed by cold rolling and decarburization reaction act as a hydrogen storage source, preventing fishscale defects caused by hydrogen. Meanwhile, residual carbon in the inner surface layer of the steel sheet can act as a factor inducing bubble defects in enamel products due to a gasification reaction during enamel firing, so in the present invention, the distribution of carbides and micropores in the thickness direction of the cold-rolled steel sheet is controlled to prevent the occurrence of surface bubble defects as well as enamelability. [Brief description of the drawings]

[0027] [Figure 1] 1 is a schematic diagram of a cross section of a steel plate for enamel according to an embodiment of the present invention. FIG. [Diagram 2] 1 shows the results of GDS analysis by depth of a steel plate for enamel according to Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] In this specification, terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, the first part, component, region, layer or section described below can be referred to as the second part, component, region, layer or section without departing from the scope of the present invention.

[0029] As used herein, when a part "comprises" a certain element, this means that it can further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.

[0030] The terminology used herein is for the purpose of referring to particular embodiments only and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the text clearly indicates otherwise. As used herein, the term "comprising" refers to the inclusion of particular features, regions, integers, steps, operations, elements, and / or components, and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.

[0031] As used herein, the term "combinations thereof" contained in a Markush-form expression means a mixture or combination of one or more elements selected from the group of elements set forth in the Markush-form expression, and is intended to include one or more elements selected from the group of elements.

[0032] As used herein, when a part is referred to as being "on" or "on" another part, it means that it is immediately on or above the other part, or there may be other parts between them. In contrast, when a part is referred to as being "directly on" another part, there are no other parts between them.

[0033] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the currently disclosed content, and are not interpreted in an ideal or very formal sense unless otherwise defined.

[0034] Moreover, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight.

[0035] In an embodiment of the present invention, the term "additionally contain an additional element" refers to the addition of an additional amount of the additional element in place of the remaining iron (Fe).

[0036] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art will be able to easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.

[0037] The steel sheet for enamel according to one embodiment of the present invention contains, by weight, C: 0.01-0.05%, Mn: 0.46-0.80%, Si: 0.001-0.03%, Al: 0.01-0.08%, P: 0.001-0.02%, S: 0.001-0.02%, N: 0.004% or less (excluding 0%) and O: 0.003% or less (excluding 0%), with the remainder being Fe and unavoidable impurities.

[0038] First, the reasons for limiting the components of the steel sheet will be explained.

[0039] C:0.01~0.05% by weight If carbon (C) is added in an excessive amount, the amount of carbon dissolved in the steel increases, increasing strength, but it also hinders the development of texture during annealing, making formability poor and inducing bubble defects due to bubble rings in the enamel layer.On the other hand, if the C content is too low, the proportion of carbides that act as sites for absorbing hydrogen in the steel decreases, making it vulnerable to fishscale defects.

[0040] The slab may contain 0.02 to 0.08% by weight of carbon. More specifically, the slab may contain 0.024 to 0.076% by weight of carbon.

[0041] In relation to the manufacturing process described below, since decarburization is performed in a high oxidation index atmosphere during the final annealing process, the C content in the slab and the C content in the final steel sheet may be different from each other. Since decarburization is performed at about 0.01 to 0.05 wt%, the C content in the final steel sheet may be 0.01 to 0.05 wt%. The C content in the final steel sheet may have a concentration gradient in the thickness direction, and the above C content indicates the average C content in the entire steel sheet 100 including the oxide layer 20. More specifically, the C content in the final steel sheet may be 0.015 to 0.045 wt%.

[0042] Mn:0.46~0.80wt% Manganese (Mn) is a representative solid solution strengthening element, and it prevents hot shortness by precipitating sulfur dissolved in steel in the form of manganese sulfide (MnS) and promotes the precipitation of carbides. If too little Mn is added, it is difficult to obtain the above-mentioned effects sufficiently. On the other hand, if the Mn content is too high, problems may occur such as poor formability, a lowering of the Ar3 transformation temperature, and deformation occurring due to transformation during enamel firing. Therefore, Mn may be contained in an amount of 0.46 to 0.80 wt%. More specifically, Mn may be contained in an amount of 0.48 to 0.78 wt%.

[0043] Si:0.001~0.03wt% Silicon (Si) is an element that promotes the formation of carbides that act as a hydrogen storage source. If too little Si is added, it is difficult to obtain the above-mentioned effects sufficiently. On the other hand, if too much Si is added, a problem may occur in which an oxide film is formed on the steel sheet surface, reducing enamel adhesion. Therefore, the Si content may be 0.001 to 0.030 wt %. More specifically, the Si content may be 0.002 to 0.027 wt %.

[0044] Al:0.01~0.08wt% Aluminum (Al) is used as a powerful deoxidizer to remove oxygen from molten steel during steelmaking, and is an element that fixes dissolved nitrogen and improves aging resistance. If too little Al is added, it is difficult to fully obtain the above-mentioned effects. On the other hand, if too much Al is added, aluminum oxide remains in the steel or on the steel surface, which can cause problems such as blister defects during the enamel treatment process. Therefore, Al can be contained in the range of 0.01 to 0.08 wt %. More specifically, it can be contained in the range of 0.014 to 0.077 wt %.

[0045] P:0.001~0.020wt% Phosphorus (P) is a representative material strengthening element. If too little P is added, it is difficult to obtain the above-mentioned effects sufficiently. On the other hand, if too much P is added, a segregation layer is formed inside the steel sheet, which not only reduces formability but also deteriorates the pickling properties of the steel and can have a negative effect on enamel adhesion. Therefore, P can be contained in the range of 0.001 to 0.020 wt %. More specifically, it can be contained in the range of 0.002 to 0.018 wt %.

[0046] S:0.001~0.020wt% Sulfur (S) is an element that combines with manganese to cause red shortness. If too little S is added, problems such as poor weldability may occur. If too much S is added, not only does it significantly reduce softness and impair workability, but it may also have a negative effect on the fishscale properties of the product due to excessive precipitation of manganese sulfides. Therefore, S may be contained in an amount of 0.001 to 0.020 wt %. More specifically, S may be contained in an amount of 0.002 to 0.018 wt %.

[0047] N: 0.004% by weight or less Nitrogen (N) is a typical hardening element, but if the amount added is increased, problems such as frequent aging defects, poor formability, and the generation of air bubble defects during the enamel treatment process may occur. Therefore, the upper limit of N is limited to 0.004 wt.%. More specifically, N can be contained in an amount of 0.0005 to 0.0037 wt.%.

[0048] O: 0.003% by weight or less Oxygen (O) is an essential element for forming oxides, and such oxides not only cause refractory corrosion during steelmaking, but also act as a factor inducing oxide-induced surface defects on the surface during steel plate production. Therefore, the amount of O added in the slab may be 0.003 wt% or less. More specifically, the slab may contain O in an amount of 0.0001 to 0.0019 wt%.

[0049] In relation to the manufacturing process described below, during the final annealing process, decarburization occurs in an atmosphere with a high oxidation potential index, and some oxygen penetrates, forming an oxide layer 20. However, since the thickness of the oxide layer 20 is very thin compared to the entire steel sheet 100, there is substantially no variation in the amount of oxygen in the entire steel sheet 100. The oxide layer 20 contains 5 wt % or more of oxygen. More specifically, the oxide layer 20 may contain 10 to 50 wt % of O. The oxygen content in the oxide layer 20 refers to the average content in the oxide layer 20.

[0050] In addition to the above components, the present invention includes Fe and inevitable impurities. The addition of effective components other than the above components is not excluded. Inevitable impurities include Cu, Ti, etc. In one embodiment of the present invention, Cu and Ti are not intentionally added, and Cu can be contained at 0.01 wt% or less and Ti at 0.005 wt% or less.

[0051] The reasons for limiting the volume fraction of microvoids in the steel sheet and carbides in the hot rolling stage of the present invention will now be described. The carbides used in the steel of the present invention are not only crushed during the cold rolling process due to the difference in softness with the base material, or form microvoids during the subsequent decarburization heat treatment, but also serve as a hydrogen storage source that fixes hydrogen in the steel. Therefore, the carbide fraction affects the enameling properties not only alone but also depending on the interrelationship with added elements. The steel sheet for enameling proposed in the present invention adjusts the steel composition to mainly use Fe as a hydrogen storage site. 3The company aims to provide a steel sheet for enamel that is free of surface defects and has excellent enamel adhesion and fishscale resistance by actively utilizing not only carbides such as C (cementite) but also micropores caused by decarburization, and by controlling the components and processes that affect enamel adhesion and surface defects among the steel components. The cementite that is uniformly dispersed and precipitated during hot rolling is crushed during cold rolling, and by controlling the atmosphere during the annealing process, it acts as a decarburization reaction source and forms micropores that are a hydrogen storage source, which effectively fixes hydrogen in the steel and suppresses fishscale defects. Continuous annealing and decarburization work controls the carbide and micropore fraction in the thickness direction, and also controls the behavior of the oxides in the steel sheet surface layer, which has a significant effect on enamel adhesion and suppression of bubble defects. Meanwhile, unlike the high-temperature precipitate / inclusion system that precipitates during the high-temperature solidification process, the present invention utilizes carbides that are stable at low temperatures, which can prevent problems with existing enamel steels, such as refractory meltdown and clogging of continuous casting nozzles, as well as surface defects such as black lines. The carbide fraction is not only closely related to the total carbon content in the steel, but is also greatly affected by the operating conditions. Meanwhile, in the case of the steel of the present invention, elements such as titanium (Ti), which is more oxidizable than iron (Fe), are not added, and the enamel adhesion between the steel sheet and the glaze can be greatly improved by controlling the surface oxide layer.

[0052] FIG 1 shows a schematic diagram of a cross section of a steel sheet for enamel according to an embodiment of the present invention. As shown in FIG 1, the steel sheet includes an oxide layer 20 extending from the surface to the inside. The oxide layer 20 contains 5% or more by weight of oxygen (O) and is therefore distinguished from the steel sheet substrate 10 containing less than 5% by weight of oxygen (O). Specifically, when the oxygen concentration is analyzed from the surface to the inside of the steel sheet cross section, the oxide layer 20 and the substrate 10 are distinguished based on the point containing 5% by weight of oxygen. When there are multiple points containing 5% by weight of oxygen, the distinction is made based on the innermost point.

[0053] The oxide layer 20 may contain 90% by weight or more of Fe oxide.

[0054] Since enamel products are made by applying an organic glaze to a steel plate, it is very important to ensure the adhesion between the steel plate and the glaze. In general, the main component of the glaze is silicon oxide (SiO 2 ) system, and in order to prevent a decrease in adhesion to the steel sheet, expensive glazes containing large amounts of NiO and other ingredients are often used.

[0055] In one embodiment of the present invention, a method for improving enamel adhesion by controlling the thickness of the oxide layer on the surface of the steel sheet was confirmed through repeated experiments. By controlling the thickness of the oxide layer, which is mainly composed of FeO, within a certain range, covalent bonding with silicon (Si) atoms of the glaze layer is promoted, improving enamel adhesion, and for this purpose, it is necessary to control the thickness of the oxide layer to 0.006 to 0.030 μm. If the oxide layer is too thin, the bonding force between the glaze layer and the steel sheet is reduced, making it difficult to ensure enamel adhesion, and on the other hand, if the oxide layer is too thick, it is advantageous in terms of adhesion, but there is a problem that the surface characteristics of the steel sheet are deteriorated. Therefore, the thickness of the oxide layer 20 on the steel sheet surface is limited to 0.006 to 0.030 μm. More specifically, the thickness of the oxide layer 20 may be 0.007 to 0.028 μm. The thickness of the oxide layer 20 may vary throughout the steel sheet 100, and in one embodiment of the present invention, the thickness of the oxide layer 20 means the average thickness over the entire steel sheet 100.

[0056] Specifically, the adhesion relationship index (I PEI ) may be 0.001 to 0.020.

[0057] [Formula 1] I PEI = ([Mn] × [P] × [Si] × [Oxide layer thickness]) / ([Al] × [C])

[0058] In the above formula 1, [Mn], [P], [Si], [Al], and [C] represent the content of each element (weight %) divided by the atomic weight of each element, and [oxide layer thickness] represents the thickness of the oxide layer (nm).

[0059] I PEI If the value is too low, the thickness of the oxide layer that is advantageous for ensuring adhesion is thin, and the amount of aluminum oxide formed increases, causing problems such as a decrease in adhesion between the enamel glaze layer and the base iron. PEI If the value is too high, the amount of gas generated on the steel sheet surface during enamel firing heat treatment increases, causing air bubble defects. Therefore, the adhesion relationship index (I PEI ) values ​​were limited to 0.001 to 0.020. More specifically, I PEI The value may be between 0.001 and 0.019.

[0060] The steel sheet for enamel according to one embodiment of the present invention may have a cementite fraction difference (Cv) calculated by the following formula 2 of 0.8 to 2.5%.

[0061] [Formula 2] Cv=C 1 / 2t -C 1 / 8t

[0062] In the above formula 2, C 1 / 2t and C. 1 / 8t indicate the cementite fraction at the center and 1 / 8 region in the thickness direction of the steel sheet, respectively.

[0063] Carbon in metal alloys combines with metal atoms to form carbides, and cementite is one of the carbides formed at relatively low temperatures when iron combines with carbon. Cementite is usually formed in carbon steel between 250 and 700°C, and at higher temperatures it coarsens into spherical particles. Cementite formed during the hot rolling stage is crushed during the cold rolling process and decomposed during the decarburization process, acting as a source for absorbing hydrogen. However, if this cementite is concentrated on the surface of the steel, it can become a source that promotes the gasification reaction of carbon during the enamel firing process, causing bubble defects. Therefore, in order to suppress fish scale and bubble defects in enamel products, it is necessary to strictly control the volume fraction of carbide objects in the thickness direction. That is, if the difference in cementite fraction in the thickness direction of the cold-rolled steel sheet, Cv, is too small, the decarburization reaction does not proceed smoothly, and the carbide fraction in the surface layer increases, which acts as a factor inducing bubble defects after enamel firing. On the other hand, if Cv is too large, there is a problem that the supply of sites capable of absorbing hydrogen in the steel is insufficient, making it difficult to suppress the occurrence of fishscale defects. Therefore, the difference in cementite fraction in the thickness direction, Cv, can be 0.8 to 2.5%. More preferably, Cv may be 0.85 to 2.45%.

[0064] The steel sheet for enamel according to one embodiment of the present invention may have a micropore area ratio difference (MVv) in each region calculated by the following formula 3 of 0.07 to 0.16%.

[0065] [Formula 3] MVv=MV 1 / 8t -MV Av

[0066] In the above formula 3, MV 1 / 8t and MV Av indicates the 1 / 8 site and average micropore fraction in the thickness direction, respectively.

[0067] The cementite precipitated during hot rolling is crushed during cold rolling and decarburization heat treatment, forming micropores around the cementite. The formed micropores act as hydrogen storage sources to suppress the generation of fishscale defects. The micropores in the cold-rolled steel sheet were measured by taking 10 photographs at a magnification of 1000 times using a scanning electron microscope on a surface parallel to the rolled surface (ND surface), and then measuring the area fraction of the micropores in the area using an image analyzer. In one embodiment of the present invention, it was confirmed that there is a region in which fishscale and bubble defects can be simultaneously suppressed by controlling the area fraction distribution of these micropores by region. In order to secure such an effect, it was necessary to control the micropore area fraction difference, MVv, to 0.07 to 0.16%. If the micropore area fraction difference, MVv, is excessively small, it is advantageous in terms of fishscale resistance, but problems such as deterioration of workability and frequent occurrence of surface defects such as bubble defects may occur. On the other hand, if MVv is too large, there are few sites that can act as hydrogen storage sources to fix hydrogen in the steel, which may cause a problem that the fishscale defect rate of the product increases. Therefore, the micropore area rate difference, MVv, is limited to 0.070 to 0.160%. More specifically, MVv may be 0.075 to 0.155%.

[0068] The enamel adhesion of the steel sheet for enamel according to one embodiment of the present invention may be 95% or more. By satisfying these physical properties, it can be used as an enamel material even if a relatively inexpensive glaze is used. If the enamel adhesion is excessively reduced, the glaze layer will fall off during distribution or handling after enamel processing, reducing the marketability of the enamel material. In consideration of stability, the company applies expensive glazes with large amounts of NiO and other components added, which acts as a factor in increasing costs, so it is making efforts to provide a method for ensuring enamel adhesion even with low-priced glazes. Normally, if the enamel adhesion is 90% or more, it is classified as the best enamel product, but in one embodiment of the present invention, a method for ensuring enamel adhesion of 95% or more is proposed. In addition, if the enamel adhesion is reduced, the rate of fish scale generation due to hydrogen in the steel increases, so it is preferable to ensure as high adhesion as possible, and in the present invention, an excellent enamel adhesion of 95% or more is ensured in terms of adhesion characteristics and fish scale control. More specifically, the enamel adhesion may be 96% or more. The adhesion of enamel is defined in the American Society for Testing and Materials standard, ASTM C313-78, by applying a certain load to the enamel layer with a steel ball and evaluating the degree of electrical conductivity at this point, and expressing the degree of peeling of the enamel glaze layer as an index.

[0069] The steel sheet for enamel according to one embodiment of the present invention has a hydrogen permeability of 600 sec / mm 2 The hydrogen permeability ratio is a representative index for evaluating fishscale resistance, which indicates resistance to fishscale defects, which are fatal defects, when enamel steel manufactured using the cold rolled steel sheet according to one embodiment of the present invention is applied, and evaluates the ability to fix hydrogen in the steel sheet by the method described in the European standard (EN10209). It is the time (t s , unit: seconds) and dividing it by the square of the material thickness (t, unit: mm), t s / t 2 (Unit: seconds / mm 2If the hydrogen permeability ratio is too low, when the resistance to fishscale defects is evaluated by accelerated heat treatment at 200°C for 24 hours after enamel treatment, the defect rate will be 50% or more, which is problematic for use as a stable enamel product. Therefore, in order to secure a steel sheet with excellent fishscale resistance, the hydrogen permeability ratio must be 600 sec / mm 2 More specifically, the hydrogen permeability must be controlled to 610 sec / mm 2 It may be more than that.

[0070] A method for producing a steel sheet for enamel according to one embodiment of the present invention includes the steps of: hot rolling a slab containing, by weight, C: 0.02-0.08%, Mn: 0.45-0.80%, Si: 0.001-0.03%, Al: 0.01-0.08%, P: 0.001-0.02%, S: 0.001-0.02%, N: 0.004% or less (excluding 0%), and O: 0.003% or less (excluding 0%), with the balance being Fe and unavoidable impurities, to produce a hot-rolled steel sheet; cold rolling the hot-rolled steel sheet to produce a cold-rolled steel sheet; and annealing the cold-rolled steel sheet.

[0071] First, a slab satisfying the above-mentioned composition is prepared. In the steelmaking step, molten steel with the above-mentioned composition can be produced as a slab through continuous casting. As mentioned above, the C and O contents are partially changed during the process of annealing the cold-rolled steel sheet, and the other alloying components are substantially the same as those of the above-mentioned steel sheet for enamel. The alloying components have been described above, so a duplicated description will be omitted.

[0072] The manufactured slab is then heated. By heating, the subsequent hot rolling process can be smoothly performed and the slab can be homogenized. More specifically, heating can mean reheating.

[0073] At this time, the slab heating temperature may be 1150 to 1280°C. If the slab heating temperature is too low, the rolling load in the subsequent hot rolling process may increase rapidly, which may lead to poor workability. On the other hand, if the slab heating temperature is too high, not only the energy cost but also the amount of surface scale may increase, which may lead to material loss. More specifically, the slab heating temperature may be 1180 to 1260°C.

[0074] The heated slab is then hot rolled to produce a hot rolled steel sheet.

[0075] At this time, the finish rolling temperature of the hot rolling may be 850 to 910°C. If the finish hot rolling temperature is too low, the rolling is finished in a low temperature region, so that the grains are rapidly mixed, which may lead to a decrease in rollability and workability. On the other hand, if the finish hot rolling temperature is too high, the peelability of the surface scale decreases, and the hot rolling is not uniform throughout the thickness, which may result in a decrease in impact toughness due to grain growth. More specifically, the finish hot rolling temperature may be 860 to 900°C.

[0076] Thereafter, the hot-rolled steel sheet produced after the hot rolling is subjected to a coiling process. More specifically, the hot-rolling coiling process may be used.

[0077] At this time, the coiling temperature may be 580 to 720°C. The hot-rolled steel sheet may be cooled on a run-out table (ROT) before coiling. If the hot-rolling coiling temperature is too low, temperature non-uniformity in the width direction occurs during the cooling and maintaining process, and the formation of low-temperature precipitates changes, resulting in material deviation and a negative effect on enameling. On the other hand, if the coiling temperature is too high, the agglomeration of carbides is promoted, resulting in a decrease in corrosion resistance and a decrease in cold rolling ability due to the promotion of grain boundary segregation of P, as well as a problem of poor workability due to the coarsening of the structure in the final product. More specifically, the coiling temperature may be 590 to 710°C.

[0078] The coiled hot-rolled steel sheet may additionally include a step of pickling the steel sheet before cold rolling.

[0079] The coiled hot-rolled steel sheet is then cold-rolled to produce a cold-rolled steel sheet.

[0080] At this time, the cold reduction may be 60-90%. If the cold reduction is too low, the driving force for recrystallization in the subsequent heat treatment process is not secured, and unrecrystallized grains remain locally, increasing the strength, but significantly reducing the workability. In addition, the crushing ability of carbides formed in the hot rolling stage is reduced, reducing the number of sites capable of absorbing hydrogen, making it difficult to ensure fishscale resistance, and the thickness of the hot-rolled sheet must be reduced in consideration of the thickness of the final product, which also reduces rolling workability. On the other hand, if the cold reduction is too high, the material hardens, reducing workability, and increasing the load on the rolling machine, reducing operability. More specifically, the cold reduction may be 63-88%.

[0081] The cold-rolled steel sheet is then subjected to continuous annealing heat treatment to be manufactured into a steel sheet for enamel. Cold-rolled steel has high strength but very poor workability due to the high deformation caused by cold rolling, so atmospheric heat treatment is performed in the subsequent process to ensure workability and decarburization reaction.

[0082] In one embodiment of the present invention, in the step of heat treating the cold-rolled steel sheet, the oxidation ability (PH 2 O / PH 2 ) conditions to promote the external diffusion of carbon atoms in the material and improve the decarburization. For this purpose, the decarburization temperature was set in the range of 720 to 850°C as the optimization control standard for the decarburization annealing process, and the oxidation ability (PH 2 O / PH 2 ) is heat-treated in a humidity atmosphere of 0.51 to 0.65, and the appropriate maintenance time is 20 to 180 seconds.

[0083] At this time, the heat treatment temperature may be 720 to 850°C. If the decarburization annealing temperature is too low, not only does the deformation formed by cold rolling not get sufficiently removed, resulting in a significant decrease in workability, but also the decarburization rate by the atmospheric heat treatment is too low, making it impossible to ensure the desired properties of the cold-rolled steel sheet for enamel. On the other hand, if the heat treatment temperature is too high, not only does the annealing passability decrease due to sheet breakage caused by softening due to a decrease in high-temperature strength, but also the thickness of the surface oxide layer increases, resulting in the opposite effect of suppressing the decarburization reaction, so the heat treatment temperature is limited to 720 to 850°C. More preferably, the annealing temperature may be 730 to 840°C.

[0084] At this time, the oxidation capacity (PH 2 O / PH 2 ) may be 0.51 to 0.65. If the oxidizing ability is too low, it takes a long time to decarburize, and the decarburization performance during continuous annealing decarburization deteriorates, making it difficult to ensure enamel properties. On the other hand, if the oxidizing ability is too high, there is a problem that the occurrence rate of surface defects due to the surface film formed by overoxidation is high. Therefore, the oxidizing ability of the atmospheric gas is limited to 0.51 to 0.65. More specifically, the oxidizing ability may be 0.52 to 0.64.

[0085] In addition, the cracking maintenance time in the atmosphere continuous annealing process may be 20 to 180 seconds. If the cracking time at the maintenance temperature is too short, not only will unrecrystallized grains remain, significantly impairing formability, but also the decarburization reaction in the thickness direction will not proceed smoothly, which will act as a factor in impairing enamelability, and on the other hand, if the maintenance time is too long, abnormal crystal grain growth will occur due to the decarburization reaction, resulting in a problem of reduced workability due to non-uniform material properties and deterioration of fish scale properties, so the maintenance time at the cracking temperature may be 20 to 180 seconds, and more preferably 25 to 160 seconds.

[0086] In addition, the step of temper rolling the heat-treated steel sheet after the step of annealing the cold-rolled steel sheet may further include a step of temper rolling. Although the shape of the material can be controlled to obtain a desired surface roughness through temper rolling, if the temper rolling reduction is too high, the material hardens due to work hardening, resulting in poor workability. Therefore, the temper rolling may be applied with a reduction of 3% or less. Specifically, the reduction of the temper rolling may be 0.3 to 2.5%.

[0087] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are merely for illustrating and explaining the present invention in more detail, and are not intended to limit the scope of the present invention, since the scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred from the claims. EXAMPLES

[0088] Working Example Slabs were manufactured through the converter, secondary refining and continuous casting processes with the composition in Table 1 below by weight, with the balance being iron (Fe) and alloy components including unavoidable impurities. The slabs were maintained in a 1200°C heating furnace for 1 hour and then hot-rolled. The final thickness of the hot-rolled steel sheet was 4.0 mm. The hot-rolled specimens were pickled to remove the oxide film on the surface, and then cold-rolled at a rolling reduction. The cold-rolled specimens were processed and heat-treated into enameled specimens to investigate the enameling properties and specimens for mechanical property analysis. The finish hot-rolling temperature, coiling temperature, cold reduction, annealing temperature, maintenance time and oxidation ability are summarized in Table 2 below.

[0089] The operability, enamelability, and texture characteristics of the material obtained through the above process according to the manufacturing conditions are shown in Table 3 below.

[0090] In the case of threading ability, an "O" was given if the operability in the continuous casting, hot rolling and cold rolling processes was 90% or more of the productivity of normal material, and an "X" was given if the productivity was below 90% or the defect rate was 10% or more.

[0091] The carbide fraction was determined by obtaining images of 20 fields of view at 500x magnification using an optical microscope, and then calculating the carbide fraction relative to the total field of view area using an image analyzer.

[0092] The enamel-treated specimens were cut to the appropriate size for each purpose depending on the test purpose, and after heat treatment, the enamel-treated specimens were completely degreased and a relatively weak standard glaze (check frit) was applied to the fishscale defects and maintained at 300℃ for 10 minutes to remove moisture. After drying, the specimens were fired at a relatively low temperature of 800℃ for 20 minutes to highlight the differences in enamel properties such as adhesion, and then cooled to room temperature, with the atmospheric conditions of the firing furnace being set at a dew point of 30℃, a harsh condition that is likely to cause fishscale defects. After enameling, the specimens were subjected to an accelerated fishscale experiment by maintaining them in an oven at 200℃ for 24 hours.

[0093] After the accelerated fishscale treatment, the occurrence of fishscale defects was visually observed. If no fishscale defects were observed, they were marked with "O", and if they were observed, they were marked with "X".

[0094] Enamel adhesion, which evaluates the adhesion between the steel sheet and the glaze, is expressed as an index of the degree of enamel glaze layer loss by applying a certain load to the enamel layer with a steel ball and evaluating the degree of current flow at this point, as defined in the American Society for Testing and Materials standard, ASTM C313-78. In the case of enamel adhesion in this invention, the target was set at 95% or more to ensure application stability with relatively low-priced glazes.

[0095] The porosity defects were evaluated by visually observing the enamel surface of the test pieces that had been kept in an oven at 200°C for 24 hours after the enamel treatment, and were rated into three grades: "O" excellent, "△" average, and "X" poor.

[0096] The hydrogen permeability ratio is an index used to evaluate the resistance of enamel to fish scale, a fatal defect. It is measured by the experimental method described in the European standard (EN10209-2013), in which hydrogen is generated in one direction of the steel plate, and the time it takes for the hydrogen to permeate and escape from the other side (t s , unit seconds) and dividing it by the material thickness (t, unit mm) squared. s / t 2 (Unit: mm 2 ) is indicated.

[0097] [Table 1]

[0098] [Table 2]

[0099] [Table 3]

[0100] As can be seen from Tables 1 to 3, Examples 1 to 9 of the present invention, which satisfy all of the component compositions, manufacturing conditions, and oxide layer thicknesses of the present invention, not only have good sheet passing properties, but also the carbide and micropore fractions and correlation indices satisfy the limited ranges of the present invention. Even under harsh processing conditions, enamel defects such as fish scale and air bubble defects do not occur. In addition, the enamel adhesion is 95% or more, and the hydrogen permeability ratio is 600 sec / mm 2 The above is the adhesion-related index I PEI The value was in the range of 0.001 to 0.020, and the characteristics targeted by the present invention were ensured.

[0101] On the other hand, in Comparative Examples 1 to 4, which satisfied the chemical composition proposed by the present invention but did not satisfy the oxidation capacity and time range during final annealing, it can be seen that the oxide layer was not properly formed and the target properties could not be secured. As can be seen from Table 3, it was confirmed that the hydrogen permeability ratio was lower than the target (Comparative Examples 1 to 4) due to deviation from the micropore distribution control standard, the enamel adhesion was less than 95% (Comparative Examples 1 to 4), and enamel defects such as air bubbles or fish scales were generated after enamel treatment, and overall the target properties could not be secured.

[0102] Comparative Examples 5 to 9 are cases in which the manufacturing conditions proposed by the present invention were satisfied but the alloy composition was not satisfied. Most of Comparative Examples 5 to 9 did not satisfy the management criteria of the present invention for the area fraction of cementite and micropores in the thickness direction, the thickness of the surface oxide layer, the adhesion index, the hydrogen permeability ratio, and the enamel adhesion, and also had problems with applicability, such as the occurrence of fish scales and void defects when observed with the naked eye after enamel treatment.

[0103] 2 shows the GDS analysis results by thickness of the steel sheet for enamel according to Example 4. It can be seen that the innermost point where the oxygen content is 5 wt% is 0.015 μm, and that an oxide layer 20 with a thickness of 0.015 μm exists on the surface.

[0104] The present invention is not limited to the above-mentioned embodiments, and can be manufactured in various different forms, and a person having ordinary skill in the art to which the present invention pertains can understand that the present invention can be embodied in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above-described embodiments are illustrative and not limiting in all respects. [Explanation of symbols]

[0105] 100: Enamel steel plate 10: Steel plate base material 20: Oxide layer

Claims

1. The composition contains, by weight, C: 0.01-0.05%, Mn: 0.46-0.80%, Si: 0.001-0.03%, Al: 0.01-0.08%, P: 0.001-0.02%, S: 0.001-0.02%, N: 0.004% or less (excluding 0%), and O: 0.003% or less (excluding 0%), with the balance being Fe and inevitable impurities; The oxide layer includes an oxide layer from the surface toward the inside, and the oxide layer has a thickness of 0.006 to 0.030 μm; The difference in micropore area ratio (MVv) between different regions calculated by the following formula 3 is 0.07 to 0.16%, The cementite fraction difference (Cv) calculated by the following formula 2 is 0.8 to 2.5%, Steel plate for enamel. [Formula 3] MVv=MV 1 / 8t -MVAv (In the above formula 3, MV 1 / 8t and MV Av represent the 1 / 8 site and average micropore fraction in the thickness direction, respectively.) [Formula 2] Cv=C 1 / 2t - C 1 / 8t (In the above formula 2, C 1 / 2t and C 1 / 8t respectively represent the cementite fractions at the center and 1 / 8 portion in the thickness direction of the steel plate.)

2. The steel sheet for enamel according to claim 1 , wherein the oxide layer contains 90% by weight or more of Fe oxide.

3. The adhesion-related index (I PEI 3. The steel sheet for enamel according to claim 1 or 2, wherein the value of (a) is 0.001 to 0.

020. [Formula 1] I PEI = ([Mn] x [P] x [Si] x [Oxide layer thickness]) / ([Al] x [C]) (In the above formula 1, [Mn], [P], [Si], [Al], and [C] represent the content (wt%) of each element divided by the atomic weight of each element, and [Oxide layer thickness] represents the thickness (nm) of the oxide layer.)

4. The steel sheet for enamel according to any one of claims 1 to 3, further comprising one or more of Cu: 0.01 wt% or less and Ti: 0.005 wt% or less.

5. The steel sheet for enamel according to any one of claims 1 to 4, wherein the enamel adhesion is 95% or more.

6. Hydrogen permeability is 600 seconds / mm 2 The steel sheet for enamel according to any one of claims 1 to 5.

7. a step of producing a hot-rolled steel sheet by hot rolling a slab containing, by weight percent, C: 0.02-0.08%, Mn: 0.45-0.80%, Si: 0.001-0.03%, Al: 0.01-0.08%, P: 0.001-0.02%, S: 0.001-0.02%, N: 0.004% or less (except 0%), and O: 0.003% or less (except 0%), with the balance being Fe and unavoidable impurities; cold rolling the hot rolled steel sheet to produce a cold rolled steel sheet; and annealing the cold rolled steel sheet; Including, The annealing step is carried out by using an oxidation index (PH 2 O / P 2 ) is 0.51 to 0.65, and heat-treated for 30 to 180 seconds in a humid atmosphere; The produced steel sheet for enamel includes an oxide layer from the surface toward the inside, and the oxide layer has a thickness of 0.006 to 0.030 μm; The difference in micropore area ratio (MVv) between different regions calculated by the following formula 3 is 0.07 to 0.16%, A method for producing a steel sheet for enamel, wherein the cementite fraction difference (Cv) calculated by the following formula 2 is 0.8 to 2.5%. [Formula 3] MVv=MV 1 / 8t -MVAv (In the above formula 3, MV 1 / 8t and MV Av represent the 1 / 8 site and average micropore fraction in the thickness direction, respectively.) [Formula 2] Cv=C 1 / 2t - C 1 / 8t (In the above formula 2, C 1 / 2t and C 1 / 8t respectively represent the cementite fractions at the center and 1 / 8 portion in the thickness direction of the steel plate.)

8. The method for producing a steel sheet for enamel according to claim 7, wherein the slab is hot rolled at a finish rolling temperature of 850°C to 910°C.

9. The method for producing a steel sheet for enamel according to claim 7 or 8, wherein the hot-rolled steel sheet is coiled at 580 ° C. to 720 ° C. in the step of producing the hot-rolled steel sheet.

10. The method for producing a steel sheet for enamel according to any one of claims 7 to 9, wherein the cold-rolled steel sheet is cold-rolled at a step reduction rate of 60 to 90%.

11. The method for producing a steel sheet for enamel according to any one of claims 7 to 10, wherein the cold-rolled steel sheet is annealed at 720 ° C. to 850 ° C. in the step of annealing the cold-rolled steel sheet.

12. The method for producing a steel sheet for enamel according to any one of claims 7 to 11, further comprising a step of temper rolling the cold-rolled steel sheet at a rolling reduction of 3% or less after the step of annealing the cold-rolled steel sheet.

Citation Information

Patent Citations

  • JP1971002740Y1

  • Production of steel sheet for porcelain enameling by continuous decarburizing annealing

    JP1994116634A

  • Production of aluminum killed cold rolled steel sheet for enameling

    JP1994192727A

  • High tensile strength hot rolled steel plate excellent in stretch-flanging workability and material stability and its production

    JP2000273577A

  • Enamelized steel sheet and method for manufacturing the same

    JP2011530658A