Anticorrosion coating composition, corrosion prevention method for magnesium alloy molded article using said composition, and coated molded article
A coating composition of bisphenol and polymer type epoxy resins with an amine curing agent addresses the barrier and curing challenges of magnesium alloys, providing effective corrosion prevention at room temperature for large structures.
Patent Information
- Application Number
- JP2023120696
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-07-25
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2039-09-30
AI Technical Summary
Existing anticorrosive paints for magnesium alloys, particularly for large structural members like high-speed transportation vehicles, fail to provide sufficient barrier properties against water and oxygen penetration, leading to corrosion, and require high-temperature curing processes that are difficult to implement.
A coating composition comprising a blend of bisphenol type epoxy resin with a weight average molecular weight of 470 to 900 and a polymer type epoxy resin with a weight average molecular weight of 10,000 to 100,000, along with an amine curing agent, forms an anticorrosive coating film with sufficient adhesion and barrier properties, capable of drying at room temperature.
The composition effectively prevents corrosion by forming a strong adhesive coating film that withstands defects, ensuring corrosion resistance even at room temperature, suitable for large magnesium alloy structures.
Smart Images

Figure 0007588187000001 
Figure 0007588187000002 
Figure 0007588187000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an anticorrosive coating composition, and more specifically to an anticorrosive coating composition which can effectively protect magnesium alloy materials from corrosion, and which is excellent in drying properties, coating workability, and resistance to cleaning solutions, and which can be applied to large magnesium alloy materials, such as high-speed transport vehicles, construction machinery, and buses. [Background technology]
[0002] Magnesium alloys have the lowest density among practical structural metal materials, are lighter than aluminum alloys, have almost the same density as carbon fiber reinforced plastics (CFRP), and are also excellent in strength, highly recyclable, and are abundant resources, and therefore are applied to home appliances, office equipment, mobile devices, automobile parts, etc. In recent years, to address the problem of magnesium alloys' tendency to easily ignite, which was one of their shortcomings, flame-retardant magnesium alloys have been developed in which the ignition temperature is increased by adding calcium, and their use in large structural components, particularly components for high-speed transport vehicles such as the Shinkansen, is being considered (see, for example, Patent Documents 1-3 and Non-Patent Document 1).
[0003] When such flame-retardant magnesium alloys are deployed in transportation vehicles, it is necessary to address the issue of corrosion, which has been recognized as another issue for magnesium alloys. Magnesium alloys are more chemically active and less corrosion-resistant than other metals, and it has been revealed that the addition of calcium makes them more susceptible to corrosion. Therefore, surface treatment (chemical conversion coating, anodizing, painting, etc.) is required to ensure corrosion resistance. However, most of the past results have been for small products for indoor use, and when treating large components, it is difficult to apply the conventional chemical conversion treatment method using a complex treatment tank, and a painting method and a paint suitable for it are required. Since the conventional heat curing process is difficult due to equipment and work process reasons, a paint that can be dried and cured at a relatively low temperature, preferably at room temperature, is required.
[0004] Here, several paints for magnesium alloys and painting methods using them have been proposed, mainly for small items such as home appliances and car wheels, and in particular, a method of using an epoxy resin such as a bisphenol type together with a hardener has been proposed (Patent Documents 4 to 7). As disclosed in Patent Documents 4 to 7, it is said that the use of an epoxy resin of the bisphenol type in particular shows good results in salt spray and adhesion tests. However, as will be described later, according to the verification by the present inventors, even if the coating film has a barrier property that prevents the intrusion of water, oxygen, etc., if a defect such as a pinhole occurs in the coating film due to some unforeseen event, water, oxygen, etc. will penetrate between the coating film and the metal through such a defect, and rust will spread horizontally. In particular, it was found that magnesium alloys do not have a strong oxide film like aluminum alloys, so that the influence of the penetration of water and oxygen caused by defects in the coating film becomes large. In addition, the inventors of the present application have also confirmed that simply reducing the water permeability of the coating film will in fact make it easier for invading moisture to remain there, resulting in blisters and the like in the coating film.
[0005] That is, as disclosed in Patent Documents 4 to 7, even if the barrier properties of the coating film against water, oxygen, etc. are improved by using a bisphenol-type epoxy resin, it is difficult to say that the corrosion resistance is sufficient. In particular, in order to improve the corrosion resistance of magnesium alloys, which do not have a strong oxide film and are prone to corrosion, it has been found that it is necessary to deal with unexpected coating film defects and the like and to provide adhesion between the coating film and the metal that can prevent the progression of corrosion from the defective parts. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-78184 A [Patent Document 2] JP 2017-159345 A [Patent Document 3] JP 2017-159346 A [Patent Document 4] Japanese Patent Application Publication No. 7-204577 [Patent Document 5] JP 2001-11672 A [Patent Document 6] JP 2003-82277 A [Patent Document 7] JP 2017-105221 A [Non-patent literature]
[0007] [Non-Patent Document 1] ISMA REPORT No.3, "Taking on the Challenge of Producing High-Speed Trains with a New Flame-Retardant Magnesium Alloy," June 2016, published by the New Structural Materials Technology Research Association (ISMA) Summary of the Invention [Problem to be solved by the invention]
[0008] Under these circumstances, the inventors of the present application have conducted intensive research into an anticorrosive paint which can provide a sufficient anticorrosive effect for magnesium alloy materials by ensuring a barrier property against factors that induce rust, such as water and oxygen, while ensuring adhesion between the paint film and the metal even if unexpected paint film defects occur, so as to prevent corrosion from spreading, and which can be dried and cured at room temperature and has good paint workability even for large structural members such as those of high-speed transportation vehicles that will be developed in the future.As a result, they unexpectedly discovered that an anticorrosive paint which can solve these problems can be obtained by blending a specific polymer-type modified epoxy resin in a specific ratio with the bisphenol-type epoxy resin that has been used until now, and have completed the present invention.
[0009] Therefore, an object of the present invention is to provide an anticorrosive coating composition which has sufficient barrier properties, particularly for magnesium alloy metals which are susceptible to corrosion, and which can form an anticorrosive coating film having sufficient adhesion to prevent corrosion from progressing between the coating film and the metal even in the event of an unexpected defect, and which can be dried at room temperature and has excellent coating workability. [Means for solving the problem]
[0010] That is, the present invention is an anticorrosive coating composition containing an epoxy resin and a curing agent, The composition comprises a bisphenol-type epoxy resin (A-1) having a weight-average molecular weight of 470 to 900 and an epoxy equivalent of 180 to 1000 g / eq., a polymer-type epoxy resin (A-2) having a weight-average molecular weight of 10,000 to 100,000, and an amine-based curing agent (B), This is an anticorrosive coating composition characterized in that the mass ratio of the components (A-1) and (A-2) is (A-1):(A-2)=10:90 to 90:10 calculated as solid contents.
[0011] The present invention also provides a method for protecting a magnesium alloy molded article from corrosion, comprising coating at least the above-mentioned anticorrosive coating composition on the surface of the magnesium alloy molded article to form a coating film on the surface of the molded article.
[0012] Furthermore, the present invention relates to a coated molding comprising a magnesium-containing molding, the surface of which is coated with at least the above-mentioned anticorrosive coating composition. Effect of the Invention
[0013] According to the present invention, it is possible to provide an anticorrosive coating composition which can form an anticorrosive coating film having sufficient barrier properties even for a substrate susceptible to corrosion, particularly a magnesium alloy, and which has sufficient adhesion to prevent corrosion from progressing between the coating film and the metal even if an unexpected defect occurs, and which can be dried at room temperature and has excellent coating workability. Such an anticorrosive coating composition of the present invention is particularly useful as an undercoat coating for large magnesium alloy materials such as high-speed transportation vehicles, construction machines, and buses. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described in detail below, but the scope of the present invention is not limited to these descriptions, and other than the following examples, modifications and variations can be made as appropriate without departing from the spirit of the present invention.
[0015] In the present invention, the material (substrate) to be painted is not limited as long as it is within the scope of the present invention, that is, the material is intended to be anticorrosive, but in particular, the present invention targets magnesium alloys. The composition of the magnesium alloy is not particularly limited, but it may be one containing 85 mass% or more of magnesium for reasons of lightness and strength. As other elements, it may contain 1 mass% or more and 10 mass% or less of aluminum (denoted by "A"), 1 mass% or more and 5 mass% or less of zinc (denoted by "Z"), and also, for the purpose of imparting flame retardancy, it may contain 0.5 mass% or more and 2.5 mass% or less of calcium (denoted by "X"). As other elements, for example, zirconium, manganese (denoted by "M"), yttrium, rare earths, etc. may be contained. Specific examples include AZ61, which contains magnesium as the main component and is blended with approximately 6% by mass of aluminum (A) and approximately 1% by mass of zinc (Z); AZ91, which contains approximately 9% by mass of aluminum (A) and approximately 1% by mass of zinc (Z); AZX311, which contains approximately 3% by mass of aluminum (A), approximately 1% by mass of zinc (Z), and approximately 1% by mass of calcium (X); AZX312, which is AZX311 with the calcium content changed to approximately 2% by mass; and AZX312, which contains approximately 6% by mass of aluminum (A), approximately 1% by mass of zinc (Z), and approximately 1% by mass of calcium (X). Examples of the magnesium alloys include AZX611, AZX612, AZX611 with about 2% by mass of calcium, AZX911 with about 9% by mass of aluminum (A), about 1% by mass of zinc (Z), and about 1% by mass of calcium (X), AZX912, AZX911 with about 2% by mass of calcium, AMX601, AMX602, AMX601 with about 6% by mass of aluminum (A) and about 1% by mass of calcium (X), and AMX602, AMX601 with about 2% by mass of calcium, and the like. The magnesium alloys may be used in the form of a cast material having the above composition, or in a molded product such as a wrought material processed by rolling or forging the cast material. These may be used, for example, as small parts such as home appliances and mobile devices, or as large parts such as the bodies of automobiles, high-speed transport vehicles, and aircraft, or as industrial and construction machinery.The anticorrosive coating composition of the present invention can also be used for relatively large members having a cross-sectional diameter of more than 3 m, such as high-speed transportation vehicles, which have not been used in the past.
[0016] The anticorrosive coating composition of the present invention contains at least each of the epoxy resins A-1 and A-2 described below, and an amine-based curing agent (B). Each of these will be described in detail below.
[0017] <Bisphenol-type epoxy resin (A-1)> The A-1 component used in the anticorrosive coating composition of the present invention can be a general bisphenol-type epoxy resin, such as bisphenol A type or bisphenol F type, which is used as the base agent for the amine-based curing agent (B) described below.
[0018] From the viewpoint of the viscosity of the solution being suitable for coating, such a bisphenol type epoxy resin should have a weight average molecular weight of 470 to 900. From the viewpoint of adhesion to a substrate and corrosion resistance, the epoxy equivalent should be 180 to 1,000 g / eq., preferably 230 to 600 g / eq.
[0019] From the viewpoints of adhesion to substrates and the physical properties of the dried coating film, the content of the epoxy resin of component A-1 is preferably 2 to 19 mass %, more preferably 5 to 15 mass %, calculated as solid content in the composition.
[0020] As the bisphenol type epoxy resin in the present invention, for example, bisphenol A type epoxy resin is available from Mitsubishi Chemical Corporation. j ER834, jER834X90 (90% solution product), jER1001, jER1001X70 (70% solution product), jER1001X75 (75% solution product) 、Examples of the bisphenol F type epoxy resin include jER806, jER806H, jER807, etc., manufactured by Mitsubishi Chemical Corporation, and EPICLON830 and EPICLON835, etc., manufactured by DIC Corporation. These bisphenol A type epoxy resins and bisphenol F type epoxy resins may be used alone or in combination of two or more. When using in combination of two or more, a plurality of bisphenol A type epoxy resins or bisphenol F type epoxy resins having different molecular chains (repeating units) per molecule may be mixed, or a plurality of bisphenol A type epoxy resins and a plurality of bisphenol F type epoxy resins may be mixed as desired within the scope of the object of the present invention.
[0021] <High polymer epoxy resin (A-2)> In the anticorrosive coating composition of the present invention, in addition to the above-mentioned A-1 component, a polymeric epoxy resin is further blended in order to impart adhesion when the coating is formed (adhesion that can suppress the progress of corrosion between the coating and the metal even if unexpected defects or the like occur in the coating). Specifically, this polymeric epoxy resin is a resin obtained by increasing the molecular weight of a bisphenol A type epoxy resin with a modifier and imparting a specific functional group resulting from the modifier. Unlike the above-mentioned A-1 component, this A-2 component is a type of resin that can increase the coating hardness and exhibit film properties in one liquid only by lacquer drying (volatilization of the solvent) without using a curing agent, and can be blended as a main agent together with the above-mentioned A-1 component, or it can be blended separately from the A-1 component and the amine-based curing agent (B) described later as a third component, and then finally mixed with the A-1 component and the amine-based curing agent (B) to form the anticorrosive coating composition of the present invention. For reasons of product management and user convenience, it is preferable to use it as a main component by blending it with component A-1.
[0022] Here, in order to realize the adhesive properties specific to the component A-2, the weight average molecular weight must be 10,000 to 100,000, and is preferably 20,000 to 60,000.
[0023] The modifier in component A-2 may be, for example, an alkyl glycidyl ether, a glycidyl ester of a t-alkanecarboxylic acid, ε-caprolactone, an acid anhydride, propionyl chloride, or an acyl chloride.
[0024] The hydroxyl value of the A-2 component is preferably 100 to 500 mgKOH / g, more preferably 100 to 350 mgKOH / g, which is preferable because it improves the adhesion between the formed coating film and the substrate (metal).
[0025] Furthermore, from the viewpoint of ensuring sufficient adhesion to the substrate, the content of the epoxy resin of component A-2 is preferably 3 to 20 mass %, and more preferably 5 to 15 mass %, calculated as solid content in the composition.
[0026] Specific examples of such A-2 components include EPICLON H304-40, H-401-45, H403-45, H408-40 (all from DIC Corporation), MODEPIX 401, 402, etc., ARAQIDE 9201N, 9203N, 9205, 9208, KA-1439A (all from Arakawa Chemical Industries, Ltd.), EPOKY 813, 814, 818, 863 (all from Mitsui Chemicals, Inc.), etc. Within the scope of the object of the present invention, only one of these may be used, or two or more of them may be mixed and used.
[0027] Here, the blending ratio of the epoxy resin of the A-1 component and the epoxy resin of the A-2 component needs to be A-1:A-2=10:90 to 90:10 in terms of solid content based on mass, preferably A-1:A-2=30:70 to 70:30, more preferably A-1:A-2=40:60 to 60:40. When the A-1 component is less than 10 (A-2 component is more than 90), problems such as swelling of the coating film in high temperature and high humidity environments may occur, while when the A-1 component is more than 90 (A-2 component is less than 10), problems such as poor adhesion to the substrate may occur. Regarding such components A-1 and A-2, the epoxy resins A-1 and A-2 are preferably blended in the composition in a total amount of 5 to 25 mass %, more preferably 10 to 20 mass %, calculated as solid content.
[0028] In addition, in the anticorrosive coating composition of the present invention, in addition to the epoxy resins which are the above-mentioned components A-1 and A-2, other resin components may be contained within the scope of the object of the present invention, particularly within the scope of the object of application to flame-retardant magnesium alloy materials. The anticorrosive coating composition of the present invention may contain resin components which are not reactive with the components A-1 and A-2 of the present invention, such as fluororesins, acrylic resins, soluble cellulose resins, and polyester resins.
[0029] <Amine-based hardener (B)> In the anticorrosive coating composition of the present invention, the B component used as a curing agent for the A-1 component is an amine-based curing agent, i.e., one that contains at least an amino group, and undergoes an addition reaction with the epoxy group of the A-1 component to promote curing. It is preferable to select an amine-based curing agent whose ratio to the epoxy equivalent of the A-1 component (active hydrogen equivalent / epoxy equivalent) is preferably 1 / 0.8 to 1 / 1.2.
[0030] Examples of such amine-based curing agents include polyamine compounds such as aliphatic polyamines, alicyclic polyamines, aromatic polyamines, and polyamidoamines, and modified products thereof. However, since they can be used at room temperature and from the viewpoint of curing drying property and coating workability, aliphatic polyamines and polyamidoamines are preferable, and these can be used alone or in combination of two or more. In addition, amine-based resins of epoxy adduct modified products obtained by reacting these aliphatic polyamines or polyamidoamines with epoxy resins can also be used. It is presumed that aliphatic polyamines have excellent light resistance, and polyamidoamines have the effect of preventing rust from spreading horizontally at the interface between the substrate and the coating film. These amine-based resins may be used alone or in combination of two or more.
[0031] Examples of aliphatic polyamines include ethylenediamine, propylenediamine, butylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, pentaethylenehexamine, and modified polyamines thereof. Examples of aromatic polyamines include phenylenediamine, xylylenediamine, and modified polyamines thereof. Examples of polyamidoamines include products such as polyamidoamine obtained by reacting dimer acid (polymerization product of unsaturated fatty acid) or other polycarboxylic acids with polyamines, and modified polyamidoamines thereof.
[0032] <Rust inhibitor (C)> In the anticorrosive coating composition of the present invention, it is preferable to further include a rust inhibitor (C) mainly for the purpose of effectively suppressing the spread of corrosion. As the rust inhibitor (C), a wide variety of known ones can be used as long as they are within the scope of the object of the present invention, particularly within the scope of the object of application to flame-retardant magnesium alloy materials. For example, phosphates such as magnesium phosphate, aluminum phosphate, zinc phosphate, zirconium phosphate, manganese phosphate, calcium phosphate, aluminum pyrophosphate, calcium pyrophosphate, aluminum dihydrogen triphosphate, aluminum metaphosphate, calcium metaphosphate, etc., silicates such as strontium silicate, potassium silicate, calcium silicate, barium silicate, titanium silicate, aluminum silicate, magnesium silicate, etc., magnesium ion-exchanged silica, calcium ion-exchanged silica, colloidal silica, fumed silica, etc. can be used. In particular, magnesium phosphate, strontium silicate, aluminum phosphate, and calcium ion-exchanged silica can be preferably used because of their excellent corrosion prevention properties. Among them, magnesium phosphate is more preferable, and specifically, Pigmenthan 465M and Pigmenthan E of BannerChemicals can be mentioned. The content of the rust inhibitor (C) in the composition is preferably 1 to 10 mass %, more preferably 3 to 5 mass %. As for the blending form, it can be used together with the A-1, A-2 and the amine-based curing agent (B), or can be blended as a third component separately from them, but it is preferable to blend it together with the A-1 and A-2 in advance for the reason of shortening the mixing process.
[0033] In addition, in the anticorrosive coating composition of the present invention, it is preferable to further include a silane coupling agent (D) in order to prevent water, which is a cause of corrosion, from being drawn into the coating film and to maintain the adhesion of the coating film to the material. As such a silane coupling agent (D), a known one can be used within the scope of the purpose of the present invention, particularly within the scope of the purpose of application to flame-retardant magnesium alloy materials, but in particular, it is preferable to use a silane coupling agent having an amino group such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride, in terms of improving adhesion to the material. The content of the silane coupling agent (D) in the composition is preferably 0.1 to 5.0% by mass, more preferably 0.3 to 2.0% by mass. As for the blending form, it can be used together with the A-1, A-2 and amine-based curing agent (B) as in the case of the C component, or can be blended as a third component separately from these, but it is preferable to blend it together with the amine-based curing agent (B) in advance in order to shorten the mixing process.
[0034] Incidentally, the components C to D may each be added singly or in combination of two or more, and it is preferable that each is appropriately selected and added within the scope of the object of the present invention.
[0035] <Additives> Furthermore, the anticorrosive composition of the present invention may further contain, as necessary, various additives generally used in paints, such as reactive diluents, non-reactive diluents, coloring pigments, extender pigments, thickeners, pH adjusters, dispersants, surface conditioners, anti-sagging agents, defoamers, anti-settling agents, mildew inhibitors, preservatives, ultraviolet absorbers, light stabilizers, organic solvents, etc., so long as it is within the scope of the object of the present invention, particularly within the scope of the object of application to flame-retardant magnesium alloy materials.
[0036] <Preparation and painting method> The anticorrosive coating composition of the present invention is prepared using such blending components, but it is preferable to prepare it through procedures such as rough stirring, pigment dispersion using a medium, and dissolving the mill base and resin. As described above, the prepared anticorrosive coating composition of the present invention can be used for metal substrates in general, but is particularly intended for large flame-retardant magnesium alloy molded products. As a coating method, a known coating method can be appropriately selected taking into consideration the size and shape of the target member, and examples thereof include spray coating, shower coating, electrostatic coating, electrodeposition coating, powder coating, immersion coating, roll coating, curtain flow coating, spin coating, and brush coating. In the case of large members such as the body of a high-speed transportation vehicle, methods using a drying oven or a treatment tank are subject to equipment restrictions, so spray coating and brush coating are preferably used for coating such large members. It is preferable to appropriately adjust the amount of coating to form a film so that the film thickness after drying is about 50 to 100 μm.
[0037] In view of the above-mentioned limitations of the coating method, the anticorrosive coating composition of the present invention is preferably cured by low-temperature baking, more preferably at 100° C. or less, and even more preferably capable of drying at room temperature. Here, room temperature varies depending on the atmospheric temperature of the environment in which coating is performed, but generally refers to 23° C., and refers to the absence of temperature manipulation such as forced heating or cooling.
[0038] The anticorrosive coating composition of the present invention may be directly applied to a target substrate (metal) depending on the purpose and application of the composition, or may be pretreated by providing a chemical conversion coating (e.g., a coating of zinc phosphate, zinc calcium phosphate, zirconium, etc.), for example, by immersing the composition in a strong acid such as phosphoric acid or hydrofluoric acid, or by shower coating the composition to treat a magnesium alloy. In addition, pretreatment such as degreasing or etching may be performed. The anticorrosive coating film formed by the anticorrosive coating composition of the present invention preferably has the physical properties of zinc phosphate, zinc calcium phosphate, zirconium, or iron phosphate.
[0039] On the other hand, it is also possible to use the anticorrosive coating composition of the present invention as an undercoat, and further coat such as an intermediate coat or a top coat. When coating the composition of the present invention, the coating can be changed appropriately depending on the purpose and use. For example, polyester putty or urethane resin paint is used for vehicles, and it is preferable to form a coating film by coating at least one type selected from the group consisting of fluororesin paint, acrylic resin paint, nitrocellulose resin paint, and polyester resin paint, preferably 1 to 5 times. For the purpose of decoration, conventionally known topcoat paints such as various enamels or clear paints can also be used. In addition, it is not limited to the type that is appropriately selected depending on the purpose and use, but it is preferable that the total thickness of the coating film formed is 100 to 200 μm or more. EXAMPLES
[0040] <Preparation of undercoat paint> Undercoat paints, which are anticorrosive paint compositions, were prepared in Production Examples 1 to 17 by mixing various raw materials using a disperser based on the formulations shown in Tables 1 and 2. Among the components used in Tables 1 and 2, the physical properties of the epoxy resin (A-1), epoxy resin (A-2) and amine-based hardener (B) are as follows. *1 and *2 indicate analytical values, and the analytical methods are shown below. All other values are catalog values. <Epoxy resin (A-1)> jER834X90 [Solid content 90% by mass, weight average molecular weight 470, epoxy equivalent 230-270g / eq., manufactured by Mitsubishi Chemical Corporation] jER1001X70 [solid content 70% by mass, weight average molecular weight 900, epoxy equivalent 450-500g / eq., manufactured by Mitsubishi Chemical Corporation] <Epoxy resin (A-2)> Epicron H403-45 [Solid content 45% by mass, weight average molecular weight 22,000 (※1), hydroxyl value 200 mgKOH / g, manufactured by DIC Corporation] Epicron H304-45 [Solid content 45% by mass, weight average molecular weight 30,000, hydroxyl value 200 mgKOH / g, manufactured by DIC Corporation] Arakied 9201N [solid content 40% by mass, weight average molecular weight 50,000, hydroxyl value 245 mgKOH / g, manufactured by Arakawa Chemical Industries, Ltd.] Epoxy 863 [Solid content 45% by mass, weight average molecular weight 14,000 (※1), hydroxyl value 250 mgKOH / g (※2), manufactured by Mitsui Chemicals, Inc.] (Measurement of weight average molecular weight related to *1) Weight average molecular weight calculated as polystyrene measured by gel permeation chromatography (GPC). (Measurement of hydroxyl value related to *2) The free hydroxyl groups in 1 g of resin were completely acetylated with acetic anhydride, and the amount of potassium hydroxide required to neutralize them was then determined in mg, to determine the hydroxyl value of the resin solid content. <Amine-based hardener (B)> Daitoclar HD-Q [aliphatic polyamine, solid content 60% by mass, theoretical active hydrogen equivalent 415g / eq., amine value 125mgKOH / g, manufactured by Daito Sangyo Co., Ltd.] · TOMAID TXP-696 [Polyamidoamine, solid content 80% by mass, active hydrogen equivalent 95g / eq., amine value 330mgKOH / g, manufactured by T&K TOKA Corporation]
[0041] [Table 1]
[0042] [Table 2]
[0043] <Preparation of topcoat paint> Based on the formula shown in Table 3 below, various raw materials were mixed in a disperser to prepare the topcoat base resin. Based on the formula shown in Table 4, various raw materials were mixed in a disperser to prepare the topcoat hardener. After that, the hydroxyl groups derived from the varnish in the topcoat base resin and the isocyanate groups derived from the isocyanate resin in the topcoat hardener were mixed in an equivalent ratio of 1:1 to prepare the topcoat paint.
[0044] [Table 3]
[0045] [Table 4]
[0046] <Creating test pieces> A magnesium alloy (AZX611 manufactured by Sankyo Material Co., Ltd.) was cut to a size of 150 mm x 70 mm x 3 mm thick to prepare a substrate. The undercoat paint of each of the manufacturing examples prepared above was then applied by air spray to a dry film thickness of 50 μm, and dried at 23° C. for 16 hours to form an undercoat coating. Thereafter, the topcoat paint prepared above was applied to the formed undercoat film using an air spray so that the dry film thickness was 50 μm, and the film was dried at 23°C for 7 days to form a topcoat film, which was then used as each test specimen. Using each of the test pieces thus obtained, the adhesion and corrosion prevention properties of the coating film were evaluated by the methods described below.
[0047] <Adhesion> According to JIS K 5600-5-6 (cross-cut adhesion method), the initial adhesion immediately after painting and the adhesion after a 40°C hot water immersion test conducted under the conditions of JIS K 5600-6-2 (liquid resistance water immersion method) were evaluated according to the following criteria. ◎: The coating film did not peel off from the cut and / or the area of peeling was less than 5%. ○: The coating film has peeled off along the edges of the cuts. The area is 5% or more but less than 15%. △: The coating film has peeled off along the edges of the cuts. The area is 15% or more but less than 35%. ×: The coating film is peeled off along the edge of the cut. The peeling area is 35% or more.
[0048] <Salt spray test> According to JIS K 5600-7-1 (neutral salt spray resistance), the condition of the coating surface after 480 hours was visually inspected. ◎: Paint film blistering or peeling from the cross cut is within 2 mm, and no thread rust has occurred. ○: Paint film blistering or peeling from the cross cut is within 2 mm, and the number of rust threads is 3 or less. △: Paint film blistering or peeling from the cross cut is within 5 mm, and the number of rust threads is 6 or less. ×: Significant swelling, peeling or thread rust of the coating film from the cross cuts.
[0049] <Moisture resistance test> According to JIS K 5600-7-2 (humidity resistance continuous condensation method), the condition of the coating surface after 480 hours was visually inspected. ◎: No abnormality on the coating surface. ◯: No blisters were observed on the coating surface, and slight loss of gloss occurred. △: Five or more blisters were observed on the coating surface, and gloss loss occurred. ×: Blisters occurred over the entire coating surface.
[0050] <Painting workability (room temperature curing)> The coating was applied to a specified thickness using an air spray, and the coating was dried at room temperature for 7 days and evaluated in accordance with JIS K 5600-3-6 (non-tacky drying properties). ○: After drying at room temperature, it hardens completely and does not soften at the temperature inside the moisture resistance test chamber (50°C). △: After drying at room temperature, the coating film does not remain sticky, but softens at the temperature inside the humidity resistance test chamber (50°C). ×: The coating film remains sticky after drying at room temperature.
[0051] <Evaluation Results> The evaluation results are shown in Tables 5 and 6.
[0052] [Table 5]
[0053] [Table 6]
Claims
1. An anticorrosive coating composition comprising an epoxy resin, a rust inhibitor and a curing agent, The composition contains a bisphenol type epoxy resin (A-1) having a weight average molecular weight of 470 to 900 and an epoxy equivalent of 180 to 1,000 g / eq., a polymer type epoxy resin (A-2) having a weight average molecular weight of 10,000 to 100,000, and an amine type curing agent (B), The bisphenol-type epoxy resin (A-1) is contained in the composition in an amount of 2 to 19 mass% in terms of solid content, The polymeric epoxy resin (A-2) is contained in the composition in an amount of 3 to 20 mass% in terms of solid content, The mass ratio of the components (A-1) and (A-2) is, in terms of solid content, (A-1):(A-2)=10:90 to 49.94:50.06, The anticorrosive coating composition, wherein the amine-based curing agent (B) contains an aliphatic polyamine and / or a polyamidoamine.
2. 2. The anticorrosive coating composition according to claim 1, wherein the component (A-2) has a hydroxyl value of 100 to 350 mgKOH / g.
3. 3. The anticorrosive coating composition according to claim 1, further comprising a silane coupling agent having an amino group.
4. The anticorrosive coating composition according to any one of claims 1 to 3, characterized in that the ratio of the active hydrogen equivalent in the amine curing agent (B) to the epoxy equivalent of the component (A-1) (active hydrogen equivalent / epoxy equivalent) is 1 / 0.8 to 1 / 1.
2.
5. 5. The anticorrosive coating composition according to claim 1, which is cured at a temperature of 100° C. or lower.
6. 6. The anticorrosive coating composition according to claim 1, which is used by applying it to a molded article containing a magnesium alloy.
7. A method for protecting a magnesium alloy molded article from corrosion, comprising coating at least the anticorrosive coating composition according to any one of claims 1 to 6 on a magnesium alloy-containing molded article to form a coating film on the surface of the molded article.
8. A coated molded article comprising a magnesium alloy, the surface of which is coated with at least the anticorrosive coating composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Formation of highly corrosion-resistant coating film on magnesium alloy material
JP1995204577A
Magnesium alloy coated object and its production
JP2001011672A
Coating method of magnesium alloy formed body
JP2003071378A
Coating composition for magnesium alloy molded body
JP2003082277A
Anticorrosive coating material for aerosol spray can and ordinary simple repair method using the same
JP2004035947A