Mold powder for continuous casting of high titanium steel and its manufacturing method
A specialized mold powder composition for high titanium steel casting stabilizes performance by reducing titanium oxide formation, ensuring defect-free continuous casting and extended operation, addressing issues of melting point and viscosity control.
Patent Information
- Application Number
- JP2023519714
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-11-02
- Filing Date
- 2022-07-20
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2042-07-20
AI Technical Summary
High titanium steel casting is hindered by titanium oxide formation in mold powder, leading to increased melting point, viscosity, and performance deterioration, which causes defects like subcutaneous slag, cracks, and limited applicability due to rapid mold powder melting and thick sintered layers.
A mold powder composition comprising specific proportions of CaO, SiO2, Al2O3, Li2O, BaO, and C, along with controlled impurities, stabilizes performance by reducing titanium reactivity and maintaining structural integrity, with a melting point of 850°C to 1150°C and viscosity of 0.08 to 0.28Pa·S, allowing continuous casting up to 120 minutes.
The mold powder ensures stable lubrication and heat transfer, prevents defects, and maintains continuous casting performance for high titanium steel, with no surface or internal cracks, and extended continuous life.
Smart Images

Figure 0007588221000001
Abstract
Description
[Technical field]
[0001] The present invention belongs to the technical field of metallurgy, and in particular to a mold powder for continuous casting of high titanium steel and a method for producing the same. [Background technology]
[0002] High titanium steel Casting In the process, because the titanium content in the molten steel is high, the titanium in the steel Casting In the process, titanium oxide not only reacts with oxygen in the steel and air to produce titanium oxide, but also undergoes a series of complex chemical reactions with oxides such as SiO2, Fe2O3, Al2O3, Na2O, and B2O3 in the mold powder to produce titanium oxide. This high melting point titanium oxide enters the mold powder, causing an increase in the melting point and viscosity of the mold powder and deterioration of its performance. TiO2 further combines with CaO in the mold powder to precipitate high melting point perovskite, which adversely affects the lubrication and heat transfer between the cast piece and the mold, and ultimately causes defects such as subcutaneous slag, cracks, and dents in the cast piece. Conventional mold powders for titanium-containing steels lower the melting point of the mold powder by adding a large amount of aggregates such as Na2O, B2O3, and K2O, but if the content of these low melting point material phases is too high, the mold powder will melt too quickly, and these liquid mold powders cannot penetrate the mold powder layer, resulting in a thick sintered layer. Therefore, this method is also effective in the continuous sintering of high titanium steels. Casting Therefore, the current production of high titanium steel generally adopts the mold injection method, which limits the application field of high titanium steel and makes it difficult to realize large-scale and low-cost production. Summary of the Invention [Means for solving the problem]
[0003] In view of this, an object of the present invention is to provide a mold powder for continuous casting of high titanium steel and a manufacturing method thereof, and the mold powder for continuous casting of high titanium steel provided by the present invention has high performance.
[0004] The present invention provides a mold powder for continuous casting of high titanium steel, 0-6wt% CaO; 20-30wt% SiO2, 0~10wt% Al 2 O 3 and 5-14 wt% F, 3 to 10 wt% Li2O, 35-50 wt% BaO; 3 to 15 wt% C, The remainder is impurities.
[0005] Preferably, the mass content of CaO is 1 to 5%.
[0006] Preferably, the mass content of the SiO2 is 23 to 27%.
[0007] Preferably, Al 2 O The mass content of 3 is 2 to 8%.
[0008] Preferably, the mass content of F is 6 to 12%.
[0009] The mass content of Li2O is preferably 4 to 8%.
[0010] Preferably, the mass content of BaO is 40 to 45%.
[0011] Preferably, the mass content of C is 5 to 12%.
[0012] Preferably, the high titanium steel continuous casting mold powder has a melting point of 850°C to 1150°C and a viscosity of 0.08 to 0.28 Pa·S; Crystallization rate is 82-100%.
[0013] The present invention provides a method for producing a molding powder for continuous casting of high titanium steel as described in the above technical solution, It involves producing bauxite, aluminum oxide, barium carbonate, barium fluoride, fluorspar, quartz sand, lithium carbonate and carbonaceous materials to obtain mould powder for continuous casting of high titanium steel.
[0014] The present invention is a continuous casting method for high titanium steel, especially for steels with Ti of 0.3 to 2.0 wt%. Casting The present invention provides a mold powder that can be used in molds that are suitable for the following applications: The mold powder provided by the present invention effectively reduces the reactivity of Fe2O3, Al2O3, Na2O, B2O3 and other substances with titanium in steel, thereby stabilizing the performance of the mold powder. In addition, the present invention provides a mold powder that can significantly reduce the CaO content in the powder, effectively preventing the formation of high melting point perovskite, and stabilizing the performance of high titanium steel. Casting To ensure the stability of performance during the process. After using the molding powder provided by the present invention, Cast in High titanium steel slabs have no cracks on the surface, good internal quality, no center or intermediate cracks, and can be continuously heated for 120 minutes or more. Casting To achieve this.
[0015] The content of CaO in the mold powder provided by the present invention is very low, so as to avoid TiO2 entering the mold powder to generate high melting point perovskite and deteriorate the performance of the mold powder. No aggregates that react with titanium, such as Na2O, K2O, B2O3, Fe2O3, are added, so as to prevent the problem of large changes in mold powder performance due to the reaction of these aggregates with titanium. At the same time, the problem of the sintered layer becoming thicker, the consumption of liquid slag decreasing, and the stop of continuous casting caused by the content of these low melting point phases in the mold powder being too high is prevented. SiO2 is the main network former, and the appropriate content of SiO2 can effectively maintain the stability of the structure and performance of the mold powder. 3-10wt% Li2O component is added, and the addition of Li2O can effectively and stably adjust the performance of the mold powder, and Li2O does not react with [Ti] in the molten steel, and its function of adjusting the mold powder performance is obvious, so Li2O is a good choice of welding flux for high titanium steel mold powder. The molding powder provided by the present invention has physicochemical properties of a melting point of 850°C to 1150°C and a viscosity of 0.08 to 0.28 Pa·S. Crystallization rate The content of the powder is 82-100%, which not only effectively controls the lubrication and heat transfer properties, but also has a very strong ability to absorb TiO2 inclusions. Continuously poured After that, the mold powder performance can be stabilized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The technical solutions in the embodiments of the present invention are described below clearly and completely, and obviously, the described embodiments are only some of the embodiments of the present invention, not all of the embodiments, and all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative labor are all within the scope of protection of the present invention.
[0017] The present invention provides a mold powder for continuous casting of high titanium steel, 0-6wt% CaO; 20-30wt% SiO2, 0-10wt% Fe2O3, 5-14 wt% F, 3 to 10 wt% Li2O, 35-50 wt% BaO; 3 to 15 wt% C, The remainder is impurities.
[0018] In the present invention, the mass content of the CaO is preferably 1 to 5%, more preferably 2 to 4%, and most preferably 3%. The mass content of the SiO2 is preferably 23 to 27%, and more preferably 25%. Al 2 O The mass content of 3 is preferably 2 to 8%, more preferably 3 to 6%, and most preferably 4 to 5%. The mass content of F is preferably 6 to 12%, more preferably 8 to 10%, and most preferably 9%. The mass content of Li2O is preferably 4 to 8%, more preferably 5 to 7%, and most preferably 6%. The mass content of BaO is preferably 40 to 45%, more preferably 42 to 43%. The mass content of C is preferably 5 to 12%, more preferably 8 to 10%, and most preferably 9%.
[0019] In the present invention, the total mass content of Na2O+K2O+B2O3+Fe2O3 in the impurities is preferably ≦3%.
[0020] The mold powder for continuous casting of high titanium steel provided by the present invention has a melting point of preferably 850°C to 1150°C and a viscosity of preferably 0.08 to 0.28 Pa·S; Crystallization rate is preferably 82 to 100%.
[0021] The present invention provides a method for producing a molding powder for continuous casting of high titanium steel as described in the above technical solution, It involves producing bauxite, aluminum oxide, barium carbonate, barium fluoride, fluorspar, quartz sand, lithium carbonate and carbonaceous materials to obtain mould powder for continuous casting of high titanium steel.
[0022] In accordance with the present invention, the mass content of Al2O3 in the bauxite is preferably >77%.
[0023] In the present invention, the aluminum oxide is preferably aluminum oxide for electrolytic aluminum. The mass content of Al2O3 in the aluminum oxide is preferably >77%.
[0024] In the present invention, the mass content of BaCO3 in the barium carbonate is preferably >96%, the mass content of BaF2 in the barium fluoride is preferably >96%, the mass content of CaF2 in the fluorite is preferably >86%, the mass content of SiO2 in the quartz sand is preferably >92%, the mass content of Li2CO3 in the lithium carbonate is preferably >97%, and the mass content of C in the carbonaceous material is preferably >95%.
[0025] In the present invention, the method for producing a mold powder for continuous casting of high titanium steel comprises the steps of: Bauxite, aluminum oxide, barium carbonate, barium fluoride, fluorite, quartz sand, lithium carbonate and carbonaceous material are mixed, then pelletized and dried, melted and smelted, cooled and dried to obtain a mold powder pre-melted material; The method preferably includes manufacturing said mold powder pre-melt material into a mold powder for continuous casting of high titanium steel.
[0026] In the present invention, grinding is preferably carried out in the mixing process. The particle size of the mixture obtained after the mixing is preferably 1 mm to 5 mm, more preferably 2 to 4 mm, and most preferably 3 mm.
[0027] In the present invention, after the mixing, preferably, The method further includes mixing the resulting mixture with water and forming the mixture into spheres.
[0028] In the present invention, the mass of the water is preferably 10 to 20% of the mass of the mixture, more preferably 13 to 17%, and most preferably 15%.
[0029] The present invention is not particularly limited to the method of forming the pellets and drying them, and the methods of forming the pellets and drying them may be performed by any method known to those skilled in the art.
[0030] In the present invention, the smelting is preferably carried out in an induction furnace or other smelting equipment. The smelting is preferably carried out by melting the dried pellets in a liquid.
[0031] The present invention does not particularly limit the cooling, drying and crushing methods, and any cooling, drying and crushing methods known to those skilled in the art may be adopted. In the present invention, the particle size of the product after crushing is preferably less than 5 mm.
[0032] The present invention does not particularly limit the method for producing the mold powder from the pre-melted material, and any method for producing the mold powder known to those skilled in the art may be adopted.
[0033] In the present invention, the method for producing the mold powder includes: The mold powder pre-melted material is crushed and then mixed with a carbonaceous material to obtain a mixture; The mixture is mixed with water and an adhesive to obtain a slurry, The method preferably includes granulating the slurry and then drying it to obtain a mold powder for continuous casting of high titanium steel.
[0034] In the present invention, the crushing is preferably performed to a size of 200 mesh or less.
[0035] In the present invention, the mixing is preferably carried out in a refiner roll mill.
[0036] In the present invention, the mass of the water is preferably 0.7 to 1.1 times the mass of the mold powder pre-melted material, more preferably 0.8 to 1 time, and most preferably 0.9 times.
[0037] In the present invention, the adhesive is preferably a cellulose adhesive.
[0038] In the present invention, the mass of the adhesive is preferably 1.5 to 1.8% of the mass of the mold powder pre-melted material, and more preferably 1.6 to 1.7%.
[0039] In the present invention, the mixing is preferably fine grinding. The time for the fine grinding is preferably 40 to 70 minutes, more preferably 50 to 60 minutes, and most preferably 55 minutes.
[0040] In the present invention, the granulation method is preferably spraying to produce hollow particles.
[0041] In the present invention, the drying is preferably performed using a drying tower.
[0042] In the present invention, the mold powder for continuous casting of high titanium steel preferably has a moisture content of <0.6 wt%, and a particle size of preferably 0.01 to 1.5 mm, more preferably 0.05 to 1 mm, more preferably 0.1 to 0.8 mm, even more preferably 0.2 to 0.6 mm, and most preferably 0.3 to 0.5 mm.
[0043] The content of CaO in the mold powder provided by the present invention is very low, which avoids TiO2 entering the mold powder to generate high melting point perovskite and deteriorate the performance of the mold powder. No aggregates that react with titanium, such as Na2O, K2O, B2O3, Fe2O3, are added, which prevents the problem of large changes in mold powder performance due to the reaction of these aggregates with titanium. At the same time, it prevents the problem that the content of these low melting point phases in the mold powder is too high, which causes the sintered layer to become thick, the consumption of liquid slag to decrease, and the stop of continuous casting. SiO2 is the main network former, and the appropriate content of SiO2 can effectively maintain the stability of the structure and performance of the mold powder. Add 3-10wt% Li2O component, the addition of Li2O can effectively and stably adjust the performance of the mold powder, and Li2O does not react with [Ti] in the molten steel, and its function of adjusting the mold powder performance is obvious, so Li2O is a good choice of welding flux for high titanium steel mold powder. The molding powder provided by the present invention has physicochemical properties of a melting point of 850°C to 1150°C and a viscosity of 0.08 to 0.28 Pa·S. Crystallization rate The content of the powder is 82-100%, which not only effectively controls the lubrication and heat transfer properties, but also has a very strong ability to absorb TiO2 inclusions. Continuously poured After that, the mold powder performance can be stabilized.
[0044] The above contents of the present invention will be described in more detail below through specific embodiments in the form of examples. In view of the fact that those skilled in the art have carried out a large amount of research work on the design of mold powder and continuous casting process in the field of continuous casting, they have accumulated a large amount of rich experience in both theory and practice. After carefully reading this example and its corresponding analysis, they must select a number of sets of powder material composition components such as mold powder that specifically meet other conditions within the range of the process technology or powder material components and their corresponding ratios provided by the present invention (at most by conducting a few limited general tests), based on other specific conditions, so that the above technical effects of the present invention can be realized. Therefore, only some examples are given below. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and any technology realized based on the above content of the present invention belongs to the scope of the present invention. EXAMPLES
[0045] Examples 1 to 4 Bauxite and electrolytic aluminum are mixed with aluminum oxide, barium carbonate, barium fluoride, fluorite, quartz sand, lithium carbonate and carbonaceous material, and then ground to obtain powder with a particle size of 1mm to 5mm. After uniform stirring, 10 to 20% water is further added, stirred until uniform, then pelletized and dried, the dried pellets are put into an induction furnace and smelted until the pellets are completely melted into liquid, then cooled, dried and crushed (particle size after crushing is less than 5mm) to obtain mold powder pre-melted material. Further produced according to the normal process of mold powder, the pre-melted material is crushed to 200 mesh or less, and after adding the carbonaceous material, both are put into a refining roll machine, 1 time water (the mass of water is 1 time the mass of the pre-melted material), 1.6% cellulose adhesive (the mass of the cellulose adhesive is 1.6% of the mass of the pre-melted material) are added, and fine grinding is performed for 50 minutes to obtain a slurry. The slurry is sprayed to produce hollow particles, which are then put into a drying tower and dried to obtain mold powder. The mold powder is placed in a sealed bag so that the moisture content is less than 0.6 wt% and the particle size is 0.01 to 1.5 mm.
[0046] Test the viscosity and melting point of the mold powder using a viscometer and hemispherical melting point test method; Crystallization rate The detection method is to observe the cut surface of the mold powder using image software to obtain the crystal ratio, and then detect and analyze the components of the mold powder using fluorescence analysis method. The high titanium steel continuous casting mold powder produced in the embodiment is detected, and the detection result is shown in Table 1.
[0047] [Table 1]
[0048] Continuous casting mold powder produced according to the embodiment of the present invention Casting Among the steels, a steel type with a Ti content of 0.3 to 2.0% is used, and Casting When the time is ≧120 minutes, the resulting slab has no transverse or longitudinal cracks on the surface and no porosity or cracks inside.
[0049] The content of CaO in the mold powder provided by the present invention is very low, which avoids TiO2 entering the mold powder to generate high melting point perovskite and deteriorate the performance of the mold powder. No aggregates that react with titanium, such as Na2O, K2O, B2O3, Fe2O3, are added, which prevents the problem of large changes in mold powder performance due to the reaction of these aggregates with titanium. At the same time, it prevents the problem that the content of these low melting point phases in the mold powder is too high, which causes the sintered layer to become thick, the consumption of liquid slag to decrease, and the stop of continuous casting. SiO2 is the main network former, and an appropriate content of SiO2 can effectively maintain the stability of the structure and performance of the mold powder. Add 3-10wt% Li2O component, and the addition of Li2O can effectively and stably adjust the performance of the mold powder. Li2O does not react with [Ti] in the molten steel, and its function of adjusting the mold powder performance is obvious, so Li2O is a good choice of welding flux for high titanium steel mold powder. The molding powder provided by the present invention has physicochemical properties of a melting point of 850°C to 1150°C and a viscosity of 0.08 to 0.28 Pa·S. Crystallization rate The content of the powder is 82-100%, which not only effectively controls the lubrication and heat transfer properties, but also has a very strong ability to absorb TiO2 inclusions. Continuously poured After that, the mold powder performance can be stabilized.
[0050] Although the present invention has been described with reference to specific embodiments thereof, these descriptions and illustrations are not intended to limit the present invention. Those skilled in the art will recognize that various modifications may be made to adapt a particular situation, material, composition of matter, substance, method or process to the objective, spirit and scope of the present application without departing from the true spirit and scope of the present invention as defined by the appended claims. All such modifications are intended to be within the scope of the claims appended hereto. Although the methods disclosed herein have been described with reference to certain operations performed according to a particular order, it should be understood that these operations can be combined, sub-divided or re-sorted to form equivalent methods without departing from the teachings of the present invention. Thus, unless otherwise indicated herein, the order and grouping of operations is not intended to limit the present invention.
Claims
1. A mold powder for continuous casting of high titanium steel, which is a steel type containing 0.3 to 2.0 wt% Ti, 0 to 6 wt. % CaO; 20 to 30 wt% SiO 2 and, 0-10 wt% Al2O3; 5 to 14 wt% F; 3 to 10 wt% Li 2 O. and 35 to 50 wt % BaO; 3 to 15 wt % C, The remainder is impurities. Mold powder for continuous casting of high titanium steel.
2. The mass content of the CaO is 1 to 5%; 2. The mold powder for continuous casting of high titanium steel according to claim 1 .
3. The SiO 2 The mass content of is 23 to 27%.
2. The mold powder for continuous casting of high titanium steel according to claim 1 .
4. The mass content of the Al 2 O 3 is 2 to 8%; 2. The mold powder for continuous casting of high titanium steel according to claim 1 .
5. The mass content of F is 6 to 12%.
2. The mold powder for continuous casting of high titanium steel according to claim 1 .
6. The Li 2 The mass content of O is 4 to 8%.
2. The mold powder for continuous casting of high titanium steel according to claim 1 .
7. The mass content of the BaO is 40 to 45%.
2. The mold powder for continuous casting of high titanium steel according to claim 1 .
8. The mass content of the C is 5 to 12%.
2. The mold powder for continuous casting of high titanium steel according to claim 1 .
9. The high titanium steel continuous casting mold powder has a melting point of 850°C to 1150°C, a viscosity of 0.08 to 0.28 Pa·S, and a crystallization rate of 82 to 100%.
2. The mold powder for continuous casting of high titanium steel according to claim 1 .
10. The method includes producing bauxite, aluminum oxide, barium carbonate, barium fluoride, fluorite, quartz sand, lithium carbonate and carbonaceous material to obtain mold powder for continuous casting of high titanium steel. A method for producing the mold powder for continuous casting of high titanium steel according to claim 1.
Citation Information
Patent Citations
Powder for casting ti-containing powder
JP1982142762A
Powder for casting of ti-containing steel
JP1986176451A
Powder for casting al-containing steel
JP1986186155A
Mold powder for continuous casting
JP1993185195A
Mold powder for continuous casting
JP2003033849A