Heat seal paper
The heat-sealing paper with a PHBH layer and ethylene vinyl acetate copolymer or polyester resin layer addresses adhesion issues, ensuring strong heat-sealability and biodegradability, suitable for applications like paper cups and packaging.
Patent Information
- Application Number
- JP2024005759
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-01-18
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2044-01-18
AI Technical Summary
Heat-sealing papers containing PHBH on one side and paper base material on the other side exhibit poor heat-sealability and adhesion failure, leading to issues like poor adhesion when rolled and heat-sealed, which is critical for applications like paper cups.
A heat-sealing paper design with a PHBH-containing heat-sealing layer on one outermost surface and an auxiliary coating layer containing ethylene vinyl acetate copolymer or polyester resin on the other, optimized with specific glass transition temperatures and peel strengths to ensure firm adhesion.
The paper achieves robust heat-sealability, allowing easy formation into shapes like cylinders and bags, with high biodegradability and rapid environmental decomposition.
Smart Images

Figure 0007588258000001 
Figure 0007588258000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat seal paper having a heat seal layer containing PHBH. [Background technology]
[0002] In recent years, efforts have begun to prevent environmental destruction caused by plastic waste, and there is a demand to replace disposable plastic products with materials that have a smaller impact on the environment. Alternative materials to plastic include biodegradable plastics, wood, paper, etc. Aliphatic polyesters such as polylactic acid and polycaprolactone are known as biodegradable plastics. However, aliphatic polyesters have the problem that they take a long time to biodegrade at low temperatures and decompose slowly in natural environments such as the ocean.
[0003] Poly(3-hydroxybutyrate) resins are microbially produced thermoplastics that are highly degradable under aerobic and anaerobic conditions, and have the remarkable ability to be decomposed by microorganisms in a short period of time even in water such as the ocean. Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter also referred to as PHBH), a copolymer of 3-hydroxybutyrate and 3-hydroxyhexanoate, has attracted attention for its biodegradability and resin properties.
[0004] Patent Document 1 proposes a coated paper with few coating defects, which has a coating layer containing PHBH and an adhesive on at least one surface of a paper base material, and in which the solid mass ratio of PHBH to adhesive in the coating layer is 99.9 / 0.1 to 60.0 / 40.0, and describes that the coated paper can be used as heat seal paper, waterproof paper, oil-resistant paper, etc. Patent Document 2 proposes a heat seal paper with excellent adhesion, in which a heat seal layer made of a film mainly composed of PHBH is attached to at least one surface of a paper base material via an anchor layer, and the anchor layer is a coating layer containing a polyester-based resin having a glass transition temperature of -25 to 46°C. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2021 / 256381 [Patent Document 2] Patent No. 7285387 Summary of the Invention [Problem to be solved by the invention]
[0006] Heat seal paper with a heat seal layer containing PHBH can strongly heat seal the heat seal layers together. However, it has been found that when a heat seal paper having a heat seal layer containing PHBH on one side and a paper surface with an exposed paper base on the other side is heat sealed from one side to the other side, the heat sealability between the heat seal layer and the paper surface is poor, and adhesion failure is likely to occur. For example, when a heat seal paper is rolled and heat sealed from one side to the other side to make the body of a paper cup, such adhesion failure is fatal for the paper cup. The present invention has been developed based on the above background, and an object of the present invention is to provide a heat seal paper having a heat seal layer containing PHBH on one outermost surface and having excellent heat sealability with the other surface. [Means for solving the problem]
[0007] The means for solving the problems of the present invention are as follows. 1. A paper substrate and a heat seal layer containing PHBH on one outermost surface, A heat seal paper characterized in that it has an auxiliary coating layer containing an ethylene-vinyl acetate copolymer or a polyester resin on the outermost surface of the other side. 2. The heat sealable paper described in 1., characterized in that the glass transition temperature of the ethylene-vinyl acetate copolymer is -25°C or higher and 20°C or lower. 3. The heat sealable paper according to 1 or 2, wherein the ethylene-vinyl acetate copolymer has a molar ratio of ethylene to vinyl acetate (ethylene:vinyl acetate) of 30:70 to 1:99. 4.180℃, 0.2MPa (20.0N / cm 2 4. The heat sealable paper according to any one of 1. to 3., characterized in that the hot tack peel distance in 1 second is less than 300 mm. 5.160℃, 0.2MPa (20.0N / cm 2 5. The heat sealable paper according to any one of 1. to 4., characterized in that when heat sealed under conditions of 1000 psi (0.2 mm) and 1 sec, and peeled off at a peel speed of 200 mm / min using a T-shaped strip, the peel strength is 6.0 N / 15 mm or more. 6.0.2MPa (20.0N / cm 2 6. The heat sealable paper according to any one of 1. to 5., characterized in that when heat sealed under conditions of 100° C. for 1 second and peeled off using a T-shaped strip at a peel speed of 200 mm / min, the critical temperature for material fracture is 150° C. or lower. 7. A package having the heat seal paper described in any one of 1. to 6. Effect of the Invention
[0008] The heat seal paper of the present invention has a heat seal layer containing PHBH on one outermost surface, and this heat seal layer can be firmly heat sealed to the other surface. Since the heat seal paper of the present invention does not require heat fusion between the heat seal surfaces, it can be easily processed into a tube, bag, etc. The heat seal paper of the present invention contains a high proportion of biodegradable materials and will decompose quickly even if it is released into the environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The heat seal paper of the present invention has a paper base material, a heat seal layer containing PHBH on one outermost surface, and an auxiliary coating layer containing an ethylene-vinyl acetate copolymer or a polyester resin on the other outermost surface. The heat seal paper of the present invention only needs to have a heat seal layer on one outermost surface and an auxiliary coating layer on the other outermost surface, and may have other layers such as an anchor layer, a water vapor barrier layer, a gas barrier layer, an ink receiving layer, etc. between the paper substrate and the heat seal layer, and between the paper substrate and the auxiliary coating layer. In this specification, the expression "A to B" (A and B are numerical values or ratios) means a numerical range including A and B.
[0010] (Paper base material) The paper base material is a sheet mainly made of pulp, and is obtained by papermaking a paper stock containing fillers, various auxiliaries, etc. Examples of pulp include chemical pulps such as bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), unbleached hardwood kraft pulp (LUKP), unbleached softwood pulp (NUKP), sulfite pulp, and other mechanical pulps, stone-ground pulp, thermomechanical pulp, and other wood fibers such as deinked pulp and waste paper pulp, and non-wood fibers obtained from kenaf, bamboo, hemp, and the like, and one or more of these can be used in appropriate combination. Among these, it is preferable to use chemical pulp of wood fiber or mechanical pulp of wood fiber, and it is more preferable to use chemical pulp of wood fiber, for reasons such as the fact that foreign matter is unlikely to be mixed into the paper base material, that discoloration is unlikely to occur over time when recycled as waste paper raw material, that the surface texture is good when printed due to its high whiteness, and that its value in use is particularly high when used as a packaging material. Specifically, the blending amount of wood fiber chemical pulp such as LBKP or NBKP relative to the total pulp is preferably 80 mass % or more, more preferably 90 mass % or more, even more preferably 95 mass % or more, and most preferably 100 mass %.
[0011] Examples of fillers that can be used include inorganic fillers such as talc, kaolin, calcined kaolin, clay, heavy calcium carbonate, light calcium carbonate, white carbon, zeolite, magnesium carbonate, barium carbonate, titanium dioxide, zinc oxide, silicon oxide, amorphous silica, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, barium sulfate, and calcium sulfate, and organic fillers such as urea-formalin resin, polystyrene resin, phenolic resin, and hollow microparticles. Note that fillers are not essential materials and may not be used.
[0012] Examples of various auxiliary agents include sizing agents such as rosin, alkyl ketene dimer (AKD), alkenyl succinic anhydride (ASA), polyacrylamide polymers, polyvinyl alcohol polymers, cationic starch, various modified starches, urea-formaldehyde resin, melamine-formaldehyde resin, and other dry strength agents, wet strength agents, retention agents, drainage improvers, coagulants, aluminum sulfate, bulking agents, dyes, fluorescent brighteners, pH adjusters, defoamers, UV inhibitors, anti-fading agents, pitch control agents, slime control agents, and the like, and can be selected and used as appropriate as needed.
[0013] The surface of the paper substrate may be treated with various chemicals. Examples of chemicals include oxidized starch, hydroxyethyl etherified starch, enzyme-modified starch, polyacrylamide, polyvinyl alcohol, surface sizing agents, water-resistant agents, water retention agents, thickeners, and lubricants, and these may be used alone or in combination of two or more. Furthermore, these various chemicals may be used in combination with pigments. Examples of pigments include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, and satin white, and organic pigments such as solid, hollow, and core-shell types may be used alone or in combination of two or more.
[0014] The basis weight of the paper base material can be selected appropriately depending on the desired quality and its application, but is usually 20 g / m 2 More than 600g / m 2 Less than 25 g / m is preferred. 2 More than 600g / m 2 The following is more preferable: When used for packaging materials such as wrapping paper, paper bags, lid materials, lining paper, liquid paper containers such as milk cartons, and posters to be used outdoors, the basis weight of the paper base material is 20 g / m 2 More than 350g / m 2 When used as a flexible packaging material, the paper base material preferably has a basis weight of 20 g / m 2 More than 100g / m 2 Less than 20 g / m is preferable. 2 More than 80g / m 2 The following is more preferable. The soft packaging material is, among the packaging materials, particularly, a material having a density of 20 g / m 2 From 100g / m 2 It is a flexible packaging material made of thin paper of about 150g / m2. When used for paper cups, paper containers, paper boxes, paper plates, paper trays, etc., the basis weight of the paper base material is 150g / m2. 2 More than 300g / m 2 The following is preferred: The density of the paper base material can be appropriately selected depending on the desired qualities and ease of handling, but is usually 0.5 g / cm 3 More than 1.0g / cm 3 The following are preferred:
[0015] The method of manufacturing (papermaking) the paper base material is not particularly limited, and known manufacturing (papermaking) methods and papermaking machines can be selected, such as a Fourdrinier papermaking machine, a cylinder papermaking machine, a short wire papermaking machine, a twin-wire papermaking machine such as a gap former type or a hybrid former type (on-top former type). The pH during papermaking may be in the acidic range (acidic papermaking), pseudo-neutral range (pseudo-neutral papermaking), neutral range (neutral papermaking), or alkaline range (alkaline papermaking), and after papermaking in the acidic range, an alkaline agent may be applied to the surface of the paper layer. The paper base material may be one layer, or may be composed of two or more layers. Furthermore, when treating the surface of a paper substrate with a chemical, the method of surface treatment is not particularly limited, and known coating devices such as a rod metering size press, a pond type size press, a gate roll coater, a spray coater, a blade coater, or a curtain coater can be used.
[0016] (auxiliary coating layer) The heat seal paper of the present invention has an auxiliary coating layer on the other outermost surface opposite to the heat seal layer. The auxiliary coating layer contains an ethylene-vinyl acetate copolymer or a polyester resin. The ethylene-vinyl acetate copolymer and the polyester resin may be used in combination.
[0017] <Ethylene vinyl acetate copolymer> Ethylene vinyl acetate copolymer (hereinafter also referred to as EVA) is a copolymer having ethylene and vinyl acetate as monomers, and may further have other monomers as monomers. When EVA has other monomers as monomers, the content of structural units derived from other monomers in the whole EVA is preferably 30% by mass or less. This content is not particularly limited as long as it does not impair the effects of the present invention, and can be, for example, 20% by mass or less, 10% by mass or less, 5% by mass or less, 3% by mass or less, 1% by mass or less, etc.
[0018] From the viewpoint of heat seal strength, the glass transition temperature of EVA is preferably −25 to 20° C. This glass transition temperature is more preferably −23° C. or higher, even more preferably −20° C. or higher, and more preferably 16° C. or lower, even more preferably 12° C. or lower. In this specification, the glass transition temperature means the midpoint glass transition temperature measured in accordance with JIS K 7121-1987. The molar ratio of ethylene to vinyl acetate in the EVA (structural units derived from ethylene:structural units derived from vinyl acetate, also expressed as ethylene:vinyl acetate, the total being 100) is preferably 30:70 to 1:99 from the viewpoint of heat seal strength, more preferably 25:75 to 5:95, and further preferably 20:80 to 10:90.
[0019] <Polyester resin> As the polyester-based resin, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), etc. can be used. However, because they are biodegradable, aliphatic polyester-based resins such as polycaprolactone, polybutylene succinate adipate, polybutylene succinate, and polylactic acid, and aliphatic aromatic polyester-based resins such as polybutylene adipate terephthalate and polybutylene azelate terephthalate are preferred, with polylactic acid being more preferred.
[0020] The auxiliary coating layer may contain other water-soluble resins or water-dispersible resins in addition to EVA or polyester-based resins, and may further contain various auxiliaries that are blended into coating solutions in the papermaking field, such as dispersants, viscosity improvers, water retention agents, defoamers, water resistance agents, pH adjusters, cationic resins, anionic resins, UV absorbers, metal salts, lubricants, coloring dyes, pigments, etc. However, the auxiliary coating layer preferably contains EVA or polyester-based resin as the main component, and the total amount of EVA and polyester-based resin relative to the entire auxiliary coating layer (solid content) is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0021] (Heat seal layer) The heat seal layer is located on one outermost surface of the heat seal paper, and may be a coating layer or a laminate layer. The heat seal layer contains PHBH as a thermoplastic resin. The heat seal layer may contain other thermoplastic resins, but the ratio of PHBH to the total thermoplastic resins contained in the heat seal layer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, even more preferably 99% by mass or more, and most preferably 100% by mass. When the heat seal layer contains other thermoplastic resins, the other thermoplastic resins are preferably biodegradable resins such as aliphatic polyester resins such as polycaprolactone, polybutylene succinate adipate, polybutylene succinate, and polylactic acid, and aliphatic aromatic polyester resins such as polybutylene adipate terephthalate and polybutylene azelate terephthalate.
[0022] <phbh> PHBH is a copolymer of 3-hydroxybutyrate (hereinafter also referred to as 3HB) and 3-hydroxyhexanoate (hereinafter also referred to as 3HH), and is a biodegradable resin known to be produced by microorganisms. In the present invention, the PHBH used may be derived from microorganisms or petroleum resources, but it is preferable to use the PHBH derived from microorganisms in terms of reducing the environmental load.
[0023] Microorganisms that produce PHBH are not particularly limited as long as they accumulate PHBH intracellularly, and examples of such microorganisms include bacteria of the genus Alcaligenes, such as A. lipolytica, A. eutrophus, and A. latus, as well as bacteria of the genus Pseudomonas, Bacillus, Azotobacter, Nocardia, and Aeromonas. Among them, in terms of productivity of PHBH, strains such as Aeromonas caviae, and Alcaligenes eutrophus AC32 into which genes of PHA synthase group have been introduced (Accession No. FERM BP-6038, Date of deposit on August 7, 1997, National Institute of Advanced Industrial Science and Technology, International Patent Organism Depositary, Address: Central 6, 1-1-1 Higashi, Tsukuba-shi, Ibaraki-ken, Japan) (J. Bacteriol., 179, pp. 4821-4830 (1997)) are particularly preferred. A method for obtaining PHBH from Aeromonas caviae, a microorganism of the Aeromonas genus, is disclosed, for example, in Japanese Patent Application Laid-Open No. 05-093049. These microorganisms are used by culturing them under appropriate conditions to accumulate PHBH in the cells. The carbon source and culture conditions used in the culture can be obtained according to the methods described in JP-A-05-093049, JP-A-2001-340078, etc., but are not limited thereto.
[0024] The composition ratio (mol%) of PHBH is preferably 3HB:3HH=97:3 to 75:25, more preferably 95:5 to 85:15. If the composition of 3HH is less than 3 mol%, the properties of PHBH become similar to those of 3HB homopolymer, resulting in loss of flexibility and an excessively high film-forming processing temperature, which is undesirable. If the composition of 3HH exceeds 25 mol%, the crystallization rate becomes too slow to be suitable for film-forming processing, and the degree of crystallization decreases, making the resin flexible and decreasing the bending modulus. The composition ratio of PHBH can be measured by centrifuging the aqueous dispersion and then drying the powder obtained by NMR analysis. Microbial PHBH is a random copolymer. To adjust the molar ratio of the copolymer, there are several methods, such as selecting the bacterial cells, selecting the carbon source as the raw material, blending with PHBH of different molar ratios, and blending with 3HB homopolymer.
[0025] The mass average molecular weight of PHBH is preferably 50,000 to 1,500,000. When the mass average molecular weight of PHBH is within this range, a film can be formed at a low temperature when PHBH is applied, and a film with excellent mechanical properties can be obtained when PHBH is laminated. The mass average molecular weight of PHBH is more preferably 100,000 to 500,000, and even more preferably 150,000 to 450,000. The mass average molecular weight of PHBH can be determined by gel permeation chromatography (GPC, such as "Shodex GPC-101" manufactured by Showa Denko K.K.) using polystyrene gel (such as "Shodex K-804" manufactured by Showa Denko K.K.) in a column, using chloroform as the mobile phase, and converting it into a polystyrene-equivalent molecular weight. The measurement sample is a powder obtained by centrifuging an aqueous dispersion containing PHBH and then drying it.
[0026] The average particle size of PHBH is preferably 0.1 to 50 μm. PHBH with an average particle size of less than 0.1 μm is difficult to produce by microbial production, and even when obtained by chemical synthesis, a microparticulation operation is required. If the average particle size exceeds 50 μm, uneven coating may occur on the surface when a coating liquid containing PHBH is applied. The average particle size of PHBH is more preferably 0.5 to 10 μm. The average particle size of PHBH refers to the particle size corresponding to 50% accumulation of all particles in a normal distribution when a water suspension of PHBH is adjusted to a predetermined concentration using a general-purpose particle sizer such as a Microtrack particle sizer (manufactured by Nikkiso, FRA).
[0027] (Coating layer) When the heat seal layer is a coating layer, the heat seal layer preferably contains an inorganic pigment and an adhesive. The coating layer may be one layer or multiple layers. When the coating layer is composed of multiple layers, the number of layers is preferably three or less, and more preferably two layers. When the coating layer is composed of multiple layers, it is preferable that the coating layer located on the paper layer side contains an inorganic pigment from the viewpoint of improving the heat seal strength, while the coating layer located farther from the paper layer preferably does not contain an inorganic pigment or contains a smaller amount of inorganic pigment than the coating layer located on the paper layer side from the viewpoint of achieving both water resistance and oil resistance.
[0028] <Inorganic pigments> As the inorganic pigment, those used for coating on paper can be used without any particular limitation, and examples thereof include kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, bentonite, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, satin white, etc., and one or more of these can be used. Among these, one or more of kaolin, heavy calcium carbonate, light calcium carbonate, mica, talc, and bentonite are preferred.
[0029] From the viewpoint of the fixation of the coating layer, the inorganic pigment preferably has a volume 50% average particle size (D50) (hereinafter also referred to as "average particle size") of 6.0 μm or less, measured by a laser diffraction / scattering method. Examples of measuring devices for the laser diffraction / scattering method include a particle size distribution measuring device "Partica" from Horiba, Ltd. and a particle size distribution measuring device "MASTER SIZER S" from Malvern Instruments. From the viewpoint of the fixation of the coating layer, the average particle size of the inorganic pigment is more preferably 5.0 μm or less, even more preferably 4.0 μm or less, even more preferably 3.0 μm or less, and even more preferably 2.0 μm or less. There is no particular lower limit for the average particle size of the inorganic pigment, but from the viewpoint of dispersibility, for example, it is preferably 0.1 μm or more, and more preferably 0.2 μm or more. When two or more inorganic pigments are contained, it is preferable that the average particle size of at least one of the inorganic pigments is within the above-mentioned numerical range, and the proportion of the inorganic pigments satisfying this average particle size relative to the total inorganic pigments is preferably 50 mass % or more, and more preferably 70 mass % or more.
[0030] In addition, from the viewpoint of oil resistance and water resistance when a second coating layer is provided on the coating layer, the average particle size of the inorganic pigment contained in the coating layer is preferably 8.0 μm or less. From the viewpoint of oil resistance and water resistance when a second coating layer is provided, the average particle size of the inorganic pigment contained in the coating layer is more preferably 7.0 μm or less, even more preferably 6.0 μm or less, even more preferably 5.0 μm or less, even more preferably 4.0 μm or less, even more preferably 3.0 μm or less, and even more preferably 2.0 μm or less. The lower limit of the average particle size of the inorganic pigment contained in the coating layer is not particularly limited, but from the viewpoint of dispersibility, for example, it is preferably 0.1 μm or more, and more preferably 0.2 μm or more. When the coating layer contains two or more inorganic pigments, it is preferable that the average particle size of at least one of them is in the above-mentioned numerical range, and the ratio of the inorganic pigment satisfying this average particle size to the total inorganic pigments contained in the coating layer is preferably 50 mass% or more, and more preferably 70 mass% or more.
[0031] The inorganic pigment preferably has an aspect ratio of 60 or less in terms of oil resistance and water resistance when a second coating layer is provided on the coating layer. The aspect ratio can be calculated using measurements from a particle size measuring device by the calculation method described in "Basic Research on the Relationship between Coating Pigment Properties and Coated Paper Quality" in Vol. 65, No. 12 of the Paper and Pulp Technical Association. The aspect ratio of the inorganic pigment contained in the coating layer is more preferably 40 or less, even more preferably 30 or less, even more preferably 25 or less, and even more preferably 20 or less. There is no particular lower limit for the aspect ratio of the inorganic pigment contained in the coating layer. When the coating layer contains two or more inorganic pigments, it is preferable that the aspect ratio of at least one of them is within the above-mentioned numerical range, and the ratio of the inorganic pigment satisfying this aspect ratio to the total inorganic pigments contained in the coating layer is preferably 50% by mass or more, and more preferably 70% by mass or more.
[0032] The solid mass ratio of PHBH to inorganic pigment in the coating layer (PHBH:inorganic pigment, total 100) is preferably 90:10 to 0.01:99.99. By further blending an inorganic pigment into a coating liquid containing PHBH and an adhesive, the fixation of the resulting coating layer is improved. Although the mechanism is unclear, the present inventors speculate that this is because inorganic pigments have better thermal conductivity than organic PHBH and adhesive, so that the inorganic pigments quickly rise in temperature when heated, and this heat is transferred from the inorganic pigment to PHBH, thereby heating the PHBH sufficiently.
[0033] The solid content mass ratio of PHBH to inorganic pigment (PHBH:inorganic pigment, total 100) is more preferably 70:30 to 1:99, further preferably 60:40 to 2:98, and even further preferably 50:50 to 3:97, from the viewpoint of fixation of the coating layer. In addition, from the viewpoint of heat seal strength when a second coating layer is provided on the coating layer, the solid content mass ratio of PHBH to inorganic pigment in the coating layer (PHBH: inorganic pigment, total 100) is more preferably 90:10 to 5:95, more preferably 80:20 to 10:90, even more preferably 70:30 to 10:90, even more preferably 65:35 to 10:90, even more preferably 60:40 to 15:85, and even more preferably 50:50 to 25:75. In particular, when the average particle size of the inorganic pigment contained in the coating layer exceeds 8.0 μm, from the viewpoint of oil resistance and water resistance, the solid content mass ratio of PHBH to inorganic pigment (PHBH: inorganic pigment, total 100) is more preferably 90:10 to 40:60, and even more preferably 90:10 to 50:50. The total proportion of PHBH and the inorganic pigment to the total solid content of the coating layer is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more.
[0034] <Adhesive> The adhesive bonds PHBH, inorganic pigments, paper substrates, etc. By including an adhesive in the heat seal layer, it becomes easy to obtain a uniform heat seal layer in which coating defects such as cracks and pinholes are suppressed. The adhesive can be any adhesive that can be dissolved or dispersed in water and can bond PHBH, inorganic pigments, paper substrates, and the like. For example, fully saponified polyvinyl alcohol, partially saponified polyvinyl alcohol, acetoacetylated polyvinyl alcohol, carboxy-modified polyvinyl alcohol, amide-modified polyvinyl alcohol, sulfonic acid-modified polyvinyl alcohol, butyral-modified polyvinyl alcohol, olefin-modified polyvinyl alcohol, nitrile-modified polyvinyl alcohol, pyrrolidone-modified polyvinyl alcohol, silicone-modified polyvinyl alcohol, other modified polyvinyl alcohols, polyvinyl alcohols such as ethylene-vinyl alcohol copolymers, starches such as oxidized starch, etherified starch, and esterified starch, cellulose derivatives such as hydroxymethyl cellulose, hydroxyethyl cellulose, methyl cellulose, ethyl cellulose, carboxymethyl cellulose, acetyl cellulose, and nanocellulose, partially saponified ethylene-vinyl acetate copolymers, styrene-butadiene copolymer latex, conjugated diene polymer latex of methyl methacrylate-butadiene copolymer, acrylic polymer latex, styrene-maleic anhydride copolymer latex, polyvinyl chloride latex, polyvinyl acetate latex, and the like can be mentioned, and one or more of these can be appropriately selected and used.
[0035] Among these, it is preferable to include at least one selected from the group consisting of polyvinyl alcohols, starches, cellulose derivatives, partially saponified ethylene-vinyl acetate copolymers, styrene-butadiene copolymer latexes, conjugated diene polymer latexes of methyl methacrylate-butadiene copolymers, and acrylic polymer latexes, and more preferably to include at least one selected from this group. In addition, since it is biodegradable, it is more preferable to include at least one selected from the group consisting of polyvinyl alcohols, starches, cellulose derivatives, and partially saponified ethylene-vinyl acetate copolymers, and even more preferable to include at least one selected from the group consisting of fully saponified polyvinyl alcohols, partially saponified polyvinyl alcohols, and partially saponified ethylene-vinyl acetate copolymers.
[0036] From the viewpoint of fixation to the paper substrate, it is preferable to include at least one of fully saponified polyvinyl alcohol and partially saponified polyvinyl alcohol as an adhesive, and more preferably to include partially saponified polyvinyl alcohol having a saponification degree of 70 mol% to 95 mol% in order to provide excellent coating layer strength. The saponification degree of the partially saponified polyvinyl alcohol is preferably 75 mol% or more, more preferably 78 mol% or more, even more preferably 85 mol% or more, and is preferably 93 mol% or less, more preferably 90 mol% or less. Here, PHBH is water dispersible, but fully saponified polyvinyl alcohol and partially saponified polyvinyl alcohol are water soluble. Therefore, when fully saponified polyvinyl alcohol or partially saponified polyvinyl alcohol is used as an adhesive, the coating liquid may thicken as the degree of polymerization increases, and the handling and coating properties may decrease. Therefore, the degree of polymerization of fully saponified polyvinyl alcohol and partially saponified polyvinyl alcohol is preferably 2000 or less, more preferably 1500 or less, and even more preferably 1000 or less.
[0037] From the viewpoint of water resistance of the coating layer, the adhesive preferably contains a partially saponified ethylene-vinyl acetate copolymer, and more preferably consists of a partially saponified ethylene-vinyl acetate copolymer.
[0038] The ratio of the adhesive to the total solid content of the coating layer is preferably 0.1 to 40% by mass. If the adhesive is less than 0.1% by mass, the adhesive cannot be expected to have any significant effect on improving fixation, and if it exceeds 40% by mass, the adhesive becomes too much and the performance derived from PHBH may not be fully exhibited, and water resistance decreases, which is not preferable depending on the application of the coated paper. The ratio of the adhesive to the total solid content of the coating layer is more preferably 1% by mass or more, even more preferably 3% by mass or more, even more preferably 5% by mass or more, and more preferably 30% by mass or less, even more preferably 25% by mass or less, and even more preferably 20% by mass or less.
[0039] (Second coating layer) In the coated paper of the present invention, a second coating layer containing PHBH can be formed on the coating layer. By forming the second coating layer on the coating layer containing an inorganic pigment, the heat seal strength is improved. Although the mechanism is unclear, the inventors speculate that this is because the coating layer containing an inorganic pigment reaches a high temperature in a short time, and the second coating layer is exposed to a high temperature for a longer time during heat fusion processing.
[0040] The second coating layer may contain the same PHBH as above except for the range of the mass average molecular weight, and the PHBH of the second coating layer preferably has a mass average molecular weight of 50,000 to 1,500,000. The PHBH of the second coating layer is preferably larger in mass average molecular weight than the PHBH of the coating layer. The larger the molecular weight of PHBH, the smaller the MFR and the higher temperature required for heat sealing. However, if a coating layer containing an inorganic pigment is present between the second coating layer and the paper substrate on which it is coated, the coating layer can efficiently transmit the heat received by the paper substrate during the heat sealing process to the second coating layer due to the excellent thermal conductivity of the inorganic pigment. As a result, the second coating layer has excellent heat sealing properties, so that a high molecular weight PHBH can be suitably used. Furthermore, the second coating layer contains PHBH with a large mass average molecular weight, so that the properties such as oil resistance and water resistance derived from PHBH can be more effectively exhibited. From the viewpoint of oil resistance and water resistance, it is preferable that the second coating layer does not contain an inorganic pigment or contains a smaller amount of inorganic pigment than the coating layer, and the amount of inorganic pigment contained in the second coating layer relative to the total solid content is preferably 1% by mass or more less than the coating layer, more preferably 3% by mass or more less, and even more preferably 5% by mass or more less.
[0041] The second coating layer preferably contains 50% by mass or more of PHBH, more preferably 70% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. In addition to PHBH, the second coating layer may contain, as necessary, various auxiliaries that are blended in coating solutions in the papermaking field, such as other biodegradable resins such as polybutylene succinate, polycaprolactone, and polylactic acid, the adhesives described above, inorganic pigments, dispersants, viscosity improvers, water retention agents, defoamers, water resistance agents, fluorescent dyes, coloring dyes, coloring pigments, surfactants, pH adjusters, cationic resins, anionic resins, ultraviolet absorbers, and metal salts.
[0042] (Laminate layer) When the heat seal layer is a laminate layer, the heat seal layer may contain, in addition to PHBH, other thermoplastic resins, lubricants, inorganic fillers, plasticizers, antiblocking agents, odor absorbers, fragrances, antioxidants, antioxidants, weather resistance improvers, ultraviolet absorbers, crystal nucleating agents, release agents, water repellents, antibacterial agents, sliding improvers, colorants such as pigments and dyes, etc. However, the ratio of PHBH to the entire heat seal layer, which is the laminate layer, is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0043] As the lubricant, known lubricants can be used, and examples thereof include aliphatic amide compounds such as saturated or unsaturated fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, oleic acid amide, and erucic acid amide, alkylene fatty acid amides such as methylene bisstearic acid amide and methylene bisstearic acid amide, and pentaerythritol. The amount of the lubricant to be added is preferably 0.1 to 2 parts by mass, and more preferably 0.2 to 1 part by mass, based on 100 parts by mass of PHBH.
[0044] Examples of inorganic fillers include talc, calcium carbonate, mica, silica, clay, kaolin, titanium oxide, alumina, and zeolite, all of which have an average particle size of 0.5 μm or more. The amount of the inorganic filler to be added is preferably 0.5 to 5 parts by mass, and more preferably 1 to 3 parts by mass, based on 100 parts by mass of PHBH.
[0045] (Anchor layer) When the heat seal layer is a laminate layer, it is preferable from the viewpoint of adhesion to have an anchor layer between the paper substrate and the heat seal layer. The anchor layer is preferably a coating layer containing one or more thermoplastic resins selected from the group consisting of polyethyleneimine, styrene acrylic, acrylic, polyester, and ethylene-vinyl acetate copolymer (EVA), and more preferably a coating layer containing a polyester resin having a glass transition temperature of -25 to 46°C or EVA having a glass transition temperature of -50 to 30°C.
[0046] The anchor layer may contain other water-soluble resins and water-dispersible resins in addition to the above-mentioned thermoplastic resins, and may further contain various auxiliaries that are blended into coating solutions in the papermaking field, such as dispersants, viscosity improvers, water retention agents, defoamers, water resistance agents, pH adjusters, cationic resins, anionic resins, UV absorbers, metal salts, lubricants, coloring dyes, pigments, etc., as necessary. However, the anchor layer is preferably composed mainly of a thermoplastic resin, and the ratio of the thermoplastic resin to the entire anchor layer (solid content) is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0047] (Manufacturing method) The heat seal layer of the present invention can be manufactured by a conventionally known coating method or lamination method. For example, the coating device can be a blade coater, a bar coater, a roll coater, an air knife coater, a reverse roll coater, a curtain coater, a spray coater, a size press coater, a gate roll coater, etc. In addition, the coating system can be an aqueous coating using a solvent such as water, a solvent coating using a solvent such as an organic solvent, etc., and the aqueous coating is preferable. In addition, the lamination method can be either dry lamination or extrusion lamination.
[0048] When the heat seal layer is a coating layer, the coating weight (when it consists of multiple coating layers or when a second coating layer is present, the total coating weight) is 1 g / m2 in terms of dry mass. 2 More than 50g / m 2 It is preferable that the coating amount is 1 g / m or less. 2 If the thickness is less than 50 g / m, it may be difficult to form a coating layer, and the heat sealability may not be exhibited. 2 If the amount is more than this, the drying load during coating will be large. The coating amount of the coating layer is 3g / m 2 More preferably, 5 g / m 2 More preferably, 40 g / m 2 Less than 30 g / m is more preferable. 2 The following is even more preferred:
[0049] When the heat seal layer is a laminate layer, its thickness is preferably 5 μm or more and 300 μm or less. If the thickness of the heat seal layer is less than 5 μm, the heat sealability may not be fully exhibited. If the thickness of the heat seal layer exceeds 300 μm, the heat seal layer becomes too rigid, which may reduce the processability as a heat seal paper and increase the cost. The thickness of the heat seal layer is preferably 10 μm or more, more preferably 20 μm or more, and preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 60 μm or less.
[0050] The coating weight of the auxiliary coating layer is 0.3 g / m2 in dry weight. 2 More than 20g / m 2 The coating weight of the auxiliary coating layer is preferably 0.3 g / m or less. 2 If the thickness is less than 20 g / m, the effect of improving the heat sealability due to the auxiliary coating layer may be almost nonexistent. 2 If the amount is more than this, the drying load during coating will be large. The coating amount of the auxiliary coating layer is 1g / m 2 More preferably, 3 g / m 2 More preferably, 15 g / m 2 Less than 10 g / m is more preferable. 2 More preferably, 5 g / m 2 Even more preferred is the following:
[0051] Heat seal paper The heat seal paper of the present invention is a heat seal paper in which the heat seal layer and the auxiliary coating layer are bonded to each other at 180° C., 0.2 MPa (20.0 N / cm 2 ), and peeled with a weight of 30 g, the hot tack peel distance is preferably less than 300 mm. The hot tack peel distance is the peel distance immediately after heat sealing (within 1 second), and the smaller the value, the stronger the adhesion even immediately after heat sealing. The hot tack peel distance of the heat seal paper of the present invention is more preferably 200 mm or less, even more preferably 100 mm or less, even more preferably 80 mm or less, even more preferably 60 mm or less, and even more preferably 40 mm or less.
[0052] The heat seal paper of the present invention is a heat seal paper in which the heat seal layer and the auxiliary coating layer are bonded to each other at 160° C., 0.2 MPa (20.0 N / cm 2 ), and then left to stand for 24 hours in an environment of 23°C and 50% humidity, and peeled at a peeling speed of 200 mm / min using a T-shaped strip, the peel strength is preferably 6.0 N / 15 mm or more. This peel strength is more preferably 6.4 N / 15 mm or more, even more preferably 6.8 N / 15 mm or more, even more preferably 7.2 N / 15 mm or more, even more preferably 7.6 N / 15 mm or more, even more preferably 8.0 N / 15 mm or more, even more preferably 8.4 N / 15 mm or more, even more preferably 8.8 N / 15 mm or more, and even more preferably 9.2 N / 15 mm or more.
[0053] The heat seal paper of the present invention preferably has a critical temperature for failure of 150° C. or less. The critical temperature for failure is the temperature at which the heat seal layer and the auxiliary coating layer are subjected to a pressure of 0.2 MPa (20.0 N / cm) at various temperatures. 2 ), and peeled off using a T-shaped strip at a peel speed of 200 mm / min. For example, if a material breaks after being heat-sealed at 150°C, the critical temperature for material breakage is 150°C or lower. The lower the critical temperature for material breakage, the more likely it is that heat sealing can be performed at a low temperature. The critical temperature for material breakage is more preferably 145°C or lower, and even more preferably 140°C or lower.
[0054] The heat seal paper of the present invention is easy to heat seal and can be suitably used for packaging applications. The heat seal paper of the present invention can be firmly attached to one side and the other side, so it is particularly suitable for packaging applications such as tubular or bag-shaped applications in which one side and multiple sides are attached to each other. Note that tubular shapes also include frustum shapes such as cup shapes. EXAMPLES
[0055] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, parts and % are by mass, respectively, unless otherwise specified.
[0056] (Evaluation method) Hot tack peeling distance The hot tack peel distance was measured using a heat seal tester (TP-701-B, manufactured by Tester Sangyo Co., Ltd.) and a hot tack property measuring tool (TP-704, manufactured by Tester Sangyo Co., Ltd.). Two pieces of heat seal paper cut to a length of 60 cm and a width of 4 cm were stacked so that the heat seal layer and the auxiliary coating layer faced each other, and then tested using a heat seal tester at 180°C and 0.2 MPa (20.0 N / cm) with a seal bar that was 30 cm long and 1 cm wide. 2 The moment the seal bar was released (within 1 second of heat sealing), a 30g weight was attached to each of the two sheets of heat seal paper in the direction that the sealed area peeled off. The distance that the sealed area peeled off was measured and recorded as the hot tack peel distance.
[0057] Peel strength The test was conducted in accordance with JIS Z1707:2019 7.4 "Heat seal strength test". Two square test pieces with sides of 100 mm were cut out from the obtained heat seal paper, and the heat seal layer and the auxiliary coating layer were brought into contact with each other and pressed at a pressure of 130°C to 160°C and a pressure of 0.2 MPa (20.0 N / cm). 2 ), heat-sealed with pressure for 1.0 second, and then left to stand for 24 hours in an environment of 23°C and 50% humidity. A measurement sample with a long side of 100 mm and a short side of 15 mm was then cut out from the heat-sealed 100 mm square test piece. The peeled long edge was then clamped between the upper and lower jigs of a vertical tensile testing machine (Tensilon, manufactured by A&D Corporation), and the peel strength, i.e., heat seal strength, was measured while peeling the measurement sample (T-type) from the long edge side at a speed of 200 mm / min. The peeled surface was visually observed and rated according to the following criteria: The rating of ⊚ indicates that material destruction has occurred. ◎: The paper base material is destroyed on 70% or more of the heat-sealed surface. ◯: The paper base material is destroyed on 30% to less than 70% of the heat-sealed surface. Δ: The paper base material is destroyed in less than 30% of the heat-sealed area. ×: Peeling occurs between the heat seal layer and the auxiliary coating layer.
[0058] (material) Paper base material: Nippon Paper Industries, basis weight 220g / m 2 Cup base paper, CUP-HD PHBH: Kaneka Corporation, mass average molecular weight 600,000 Inorganic pigment: Shiraishi Kogyosha, kaolin, KCS, average particle size 3.6 μm, aspect ratio 10 to 15 Adhesive: Kuraray, 28-98, fully saponified PVA, saponification degree 98 mol%, polymerization degree 1700
[0059] EVA1: Sumika Chemtex, S-408HQE, Tg-30℃, ethylene:vinyl acetate=40:60 EVA2: Sumika Chemtex, S-410HQ, Tg-18℃, ethylene:vinyl acetate=30:70 EVA3: Sumika Chemtex, S-401HQ, Tg-18℃, ethylene:vinyl acetate=30:70 EVA4: Sumika Chemtex, S-400HQ, Tg 0°C, ethylene:vinyl acetate = 20:80 EVA5: Sumika Chemtex, S-355HQ, Tg 10°C, ethylene:vinyl acetate = 10:90 Polyester: Polylactic acid A, Tg 56℃
[0060] Polyethyleneimine: Nippon Shokubai, Epomin P1000 Modified polyolefin: Unitika, Arrowbase SA-1010 Styrene acrylic: Daiichi Paint Co., Harvil HS-1 Ethylene (meth)acrylic: Mitsui Chemicals, Chemipearl S500
[0061] (Formation of heat seal layer (coating layer)) 30 parts by mass of PHBH, 70 parts by mass of inorganic pigment, 10 parts by mass of adhesive were added, and water was further added and stirred to obtain an undercoating liquid with a solids concentration of 40% by mass. 100 parts by mass of PHBH and 3 parts by mass of adhesive were added, and water was further added and stirred to obtain a top coating liquid with a solid content concentration of 40% by mass. On one side of the paper substrate, apply an undercoating liquid at a dry weight of 7 g / m 2 The undercoat layer was coated by a bar blade method so that the thickness of the undercoat layer was 23 g / m2 and then dried at 105°C for 1 minute. 2 The mixture was then dried at 105°C for 1 minute and then heat-treated at 160°C for 3 minutes to form a two-layer coating layer containing PHBH on the outermost surface of one of the paper substrates.
[0062] (Formation of auxiliary coating layer) An aqueous dispersion of each resin with a concentration of 22% by mass was prepared, coated by a bar blade method to the coating amount (dry mass) shown in Table 1, and dried at 105° C. for 1 minute to form an auxiliary coating layer.
[0063] [Table 1]
[0064] (Formation of heat seal layer (laminate layer)) A coating solution of PHBH and EVA4 mixed in a dry weight ratio of 50:50 was applied to the coating layer at a dry weight of 3g / m2. 2 Onto the anchor layer, PHBH was extruded to a thickness of 30 μm to form a laminate layer. (Formation of auxiliary coating layer) In Examples 13 to 17, auxiliary coating layers were formed in the same manner as in Examples 3, 4, 5, 7 and 9, respectively.
[0065] [Table 2]
[0066] In Comparative Example 1, which did not have an auxiliary coating layer, no adhesion was observed even at 160°, but in the heat seal papers of Examples 1 to 12, which had EVA-based and polyester-based auxiliary coating layers, the heat seal layer containing PHBH was firmly fused to the auxiliary coating layer. A horizontal comparison of the peel strength at 160°C and the hot tack peel distance showed that the auxiliary coating layer containing EVA and polyester with a Tg range of -18°C to 10°C had excellent peel strength and initial adhesion. 2 From the results of the peel strength at 140°C on the test piece (Examples 4, 6, 8, 10, and 12), EVA had a better peel strength than polyester. 2 In the test pieces (Examples 3, 5, 7, 9, and 11), EVA was superior overall in terms of peel strength and material failure evaluation. These results show that EVA is the best auxiliary coating layer, and good peel strength is obtained even if the coating weight is slightly reduced. From this point of view, while a heat seal paper formulation with a more stable peel strength is desired from an industrial point of view, EVA is considered to be able to stably guarantee the target peel strength more than polyester even if the coating amount varies slightly during the manufacturing process of heat seal paper. The same is true during the processing process, where the specified peel strength can be stably guaranteed after processing. Furthermore, during the processing process, the processing temperature is sometimes lowered for reasons such as energy saving, but a stable peel strength can be achieved even at low temperatures. In contrast, the heat seal papers of Comparative Examples 2 to 9, which had an auxiliary coating layer using another resin, showed weak fusion between the heat seal layer containing PHBH and the auxiliary coating layer.
[0067] In Examples 13 to 17, in which the heat seal layer is a laminate layer, it was confirmed that the peel strength at 160°C was excellent, similar to Examples 3, 4, 5, 7, and 9. Even when the pressing temperature was lowered to 150°C, good peel strength and material fracture evaluation were obtained. It is obvious that Example 14 has better peel strength and material fracture evaluation than Example 13, which has a smaller coating amount. From the above results in Tables 1 and 2, it was confirmed that when a heat seal paper having a heat seal layer containing PHBH formed on one side by a water-based coating method or an extrusion lamination method is provided with an auxiliary coating layer containing EVA or polyester on the other side, good adhesion can be obtained when the one side and the other side are heat sealed.< / phbh>
Claims
1. A paper substrate and a heat seal layer containing PHBH on one outermost surface, A heat seal paper characterized in that it has an auxiliary coating layer containing an ethylene-vinyl acetate copolymer on the other outermost surface.
2. 2. The heat seal paper according to claim 1, wherein the glass transition temperature of the ethylene-vinyl acetate copolymer is from -25°C to 20°C.
3. The heat seal paper according to claim 1, characterized in that the molar ratio of ethylene to vinyl acetate in the ethylene-vinyl acetate copolymer (ethylene:vinyl acetate) is 30:70 to 1:
99.
4. The heat seal layer and the auxiliary coating layer are subjected to a heat treatment at 180°C and 0.2 MPa (20.0 N / cm 2 2. The heat seal paper according to claim 1, characterized in that when heat sealed under the conditions of 1) for 1 second and peeled with a weight of 30 g, the hot tack peel distance is less than 300 mm.
5. In accordance with JIS Z1707:2019 7.4 "Heat seal strength test", the heat seal layer and the auxiliary coating layer are subjected to a heat seal strength test at 160°C and 0.2 MPa (20.0 N / cm 2 2. The heat seal paper according to claim 1, characterized in that the peel strength when heat sealed under the conditions of 1) for 1 second, and then left to stand for 24 hours in an environment of 23°C and 50% humidity, and peeled off at a peel speed of 200 mm / min using a T-shaped peeler is 6.0 N / 15 mm or more.
6. In accordance with JIS Z1707:2019 7.4 "Heat seal strength test", the heat seal layer and the auxiliary coating layer are subjected to a heat seal strength test of 0.2 MPa (20.0 N / cm 2 2. The heat seal paper according to claim 1, characterized in that the critical temperature for material failure is 150°C or lower when the paper is heat sealed under the conditions of 1) for 1 second, and then left to stand for 24 hours in an environment of 23°C and 50% humidity, and peeled off at a peel speed of 200 mm / min using a T-shaped peeler.
7. A packaging material comprising the heat seal paper according to any one of claims 1 to 6.
Citation Information
Patent Citations
Biodegradable heat insulating container
JP2018162075A
Cellophane laminate
JP2024039713A
heat seal paper
JP7285387B1
JPP7285387B
Laminate and use thereof
WO2021100733A1