Iron ion-containing sol and ultraviolet absorber
A water-based iron ion-containing sol effectively absorbs UVA and visible light, addressing the limitations of existing absorbers by providing comprehensive protection and detection capabilities.
Patent Information
- Application Number
- JP2020053314
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-03-24
AI Technical Summary
Existing ultraviolet absorbers fail to effectively absorb 100% of UVA rays and are not stable under UV exposure, and they do not protect materials from visible light, especially those used in cosmetics and biochemistry applications.
A water-based iron ion-containing sol is developed by hydrolyzing and dialyzing an iron salt solution, which absorbs almost 100% of UVA rays and can extend absorption to visible light up to 600 nm, suitable for use in cosmetics, sunscreens, and protective coatings.
The iron ion-containing sol provides excellent UVA and visible light absorption, protecting materials from photobleaching and deterioration, and can be used in cosmetics, sunscreens, and coatings for structural detection.
Smart Images

Figure 0007588336000002 
Figure 0007588336000003 
Figure 0007588336000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an iron ion-containing sol having ultraviolet absorbing ability, an ultraviolet absorber containing the iron ion-containing sol or a dried product thereof, a cosmetic containing the ultraviolet absorber, an ultraviolet absorbing paint containing the iron ion-containing sol, an ultraviolet absorbing film containing a dried product of the iron ion-containing sol, coated particles having a coating layer made of the dried product of the iron ion-containing sol, and a method for producing the iron ion-containing sol. [Background technology]
[0002] Most of the ultraviolet rays that reach the earth are UVA waves (320-400 nm), which reach the dermis layer of the skin and are known to be the cause of photoaging, which causes wrinkles and sagging, so there is a demand for the development of effective ultraviolet absorbers. In addition, ultraviolet absorbers have been developed to protect various materials from deterioration due to ultraviolet rays. Organic ultraviolet absorbers have the problem of changing themselves due to ultraviolet rays and becoming discolored over time. Inorganic ultraviolet absorbers have higher chemical stability than organic substances, and metal oxide particles such as titanium oxide and zinc oxide are used, but there is a problem of compatibility with polymer materials. In addition, titanium oxide and zinc oxide cannot absorb 100% of near-ultraviolet rays around 400 nm, so the development of ultraviolet absorbers that absorb 100% of UVA waves is desired. Furthermore, in the fields of biochemistry and analytical chemistry, many studies using fluorescent dyes have been conducted, and the development of new dyes is also active. Many of the dyes used for fluorescent labeling are excited and emit light by visible light (especially the blue part). For example, the excitation wavelength of rhodamine B, a fluorescent analysis reagent, is 555 nm, and the excitation wavelength of BODIPY dyes used in various imaging applications is also 500 to 600 nm. In order to store these substances in a light-shielded state and prevent fading, it is necessary to develop a substance that can also block visible light. However, no ultraviolet absorber that meets these characteristics has been developed. For example, Patent Document 1 shows the spectral curves of various titanium oxides (Figure 1), but the absorption rate of each is reduced near 400 nm, and none of them exhibit absorption in the visible light region above 400 nm. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 9-221411 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide an ultraviolet absorbing material that can absorb ultraviolet light, particularly UVA light, and can be used for various purposes. [Means for solving the problem]
[0005] The present inventors have begun to develop a material with excellent UVA absorption. In the development, they worked on preparing a material based on inorganic materials and water from the viewpoint of safety, and found that a sol prepared by hydrolyzing an aqueous solution containing iron ions and then dialysis absorbed almost 100% of UVA. Moreover, the visible light region that this sol can absorb varies greatly depending on the concentration, and by changing the concentration, it was possible to absorb light up to 600 nm. Since this sol is based on highly safe iron-based materials and water, it can be used in cosmetics and sunscreens, and since it can absorb light up to 600 nm, it can protect many fluorescent dyes from excitation light and prevent photobleaching. Furthermore, since this sol can be uniformly mixed with a water-soluble binder, it can be coated on a luminescent material (especially a phosphorescent material) to prevent luminescence, but when it comes into contact with water, the sol dissolves and the luminescent material is exposed, allowing the luminescence to be visually confirmed, so it can be applied to detecting deterioration of structures and parts such as concrete and plastic materials due to water leakage.
[0006] That is, the present invention is specified by the following items. (1) An iron ion-containing sol having ultraviolet absorbing ability, comprising water as a solvent and an iron oxide precursor dispersed in the solvent. (2) The iron ion-containing sol according to (1) above, which is obtained by hydrolyzing the iron salt in an aqueous solution of the iron salt and dialyzing the solution after hydrolysis. (3) An ultraviolet absorber comprising the iron ion-containing sol according to (1) or (2) above, or a dried product of the iron ion-containing sol according to (1) or (2) above. (4) A cosmetic comprising the ultraviolet absorber described in (3) above. (5) An ultraviolet absorbing paint comprising the iron ion-containing sol according to (1) or (2) above and a binder. (6) An ultraviolet absorbing film comprising a dried product of the iron ion-containing sol according to (1) or (2) above and a binder. (7) Coated particles having a coating layer on the surface thereof, the coating layer comprising the dried product of the iron ion-containing sol according to (1) or (2) above. (8) The coated particles according to (7) above, characterized in that a coating layer containing a dried product of the iron ion-containing sol and a water-soluble binder is formed on the surface of the particles having a luminescent function. (9) A method for producing an iron ion-containing sol having ultraviolet absorbing ability, comprising the steps of hydrolyzing an iron salt in an aqueous solution and dialyzing the solution after the hydrolysis. Effect of the Invention
[0007] The iron ion-containing sol of the present invention has an excellent ultraviolet ray absorbing effect, particularly UVA, and can change the absorption wavelength range depending on the concentration, and can also absorb light in the visible light range. The ultraviolet ray absorbent, cosmetic, ultraviolet ray absorbing paint, and ultraviolet ray absorbing film using the iron ion-containing sol of the present invention have an excellent ultraviolet ray absorbing effect, particularly UVA. The coated particles using the iron ion-containing sol of the present invention can suppress deterioration caused by ultraviolet rays, and when light-emitting particles are coated with the sol, it is possible to emit light when light emission is required. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a diagram showing the absorption spectrum measured in Example 1. [Diagram 2] FIG. 2 is a diagram showing the absorption spectrum measured in Comparative Example 1. [Diagram 3]FIG. 3 is a TEM image of the particles in the sol obtained in Example 1. [Figure 4] FIG. 4 is a graph showing the particle size distribution of the particles in the sol obtained in Example 1. [Diagram 5] FIG. 5 is an X-ray diffraction pattern of the dried sol obtained in Example 2. [Figure 6] FIG. 6 shows the X-ray diffraction pattern of the sol obtained in Example 2 after drying and calcining. [Figure 7] Figure 7 shows photographs of the composite membrane produced in Example 3. Figure 7(a) is a photograph showing the state under room light irradiation, and Figure 7(b) is a photograph showing the state under ultraviolet light irradiation. [Figure 8] Figure 8 is a photograph of the composite membrane produced in Comparative Example 2. Figure 8(a) is a photograph showing the state under room light irradiation, and Figure 8(b) is a photograph showing the state under ultraviolet light irradiation. [Figure 9] Figure 9 shows optical microscope images of the α-Vega particles used in Example 4. Figure 9(a) shows an image under room light irradiation, and Figure 9(b) shows an image under ultraviolet light irradiation. [Figure 10] Figure 10 shows optical microscope images of the coated particles prepared in Example 4. Figure 10(a) shows an image under room light irradiation, and Figure 10(b) shows an image under ultraviolet light irradiation. [Figure 11] FIG. 11 is an optical microscope image of the coated particles prepared in Example 4. [Figure 12] 12(a) to (d) are optical microscope images showing the change over time when the coated particles prepared in Example 4 were brought into contact with water. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The iron ion-containing sol of the present invention is a sol having ultraviolet absorbing ability, in which the solvent is water and an iron oxide precursor is dispersed in the solvent. The iron ion-containing sol of the present invention can be obtained by hydrolyzing the iron salt in an aqueous solution of the iron salt and dialyzing the solution after hydrolysis. The iron salt in the present invention is not particularly limited as long as it is dissolved in water and hydrolyzed in the aqueous solution, and examples thereof include iron nitrate, chloride, and sulfate. Since divalent iron ions are converted to trivalent iron ions during the hydrolysis and dialysis in the aqueous solution except under certain conditions, the iron salt may be a divalent iron salt or a trivalent iron salt. In the iron ion-containing sol of the present invention, the sol is formed by trivalent iron, so it is preferable to use a trivalent iron salt as a raw material from the beginning. Specific examples of the compound include ferric nitrate, ferric chloride, ferric sulfate, and hydrates thereof. These iron salts are dissolved in water to prepare an aqueous solution of the iron salt. A base is added to the prepared aqueous solution to lower the hydrogen ion concentration in the aqueous solution and promote hydrolysis. The base to be added is not particularly limited, and examples thereof include sodium bicarbonate and sodium hydroxide. The base is preferably added in small amounts so that precipitation does not occur. The base is preferably added while stirring to suppress precipitation. In order to suppress a sudden change in pH, a salt of a strong base and a weak acid can be used rather than a strong base. Next, the solution after the addition is dialyzed. The dialysis method is not particularly limited, and for example, a general dialysis method can be used. A method in which a semipermeable membrane bag containing the added solution is immersed in dialysis water is also possible. As the dialysis water, water is preferable, and examples thereof include pure water and ultrapure water. In addition, water in which an acid or the like is added to pure water or ultrapure water to adjust the pH may be used. The pH may be adjusted by adding an acid such as nitric acid to the dialysis water (for example, pH about 3.5, etc.) to reduce the difference between the pH of the dialysis water and the pH of the solution after the addition of the base, but the iron ion-containing sol of the present invention can also be obtained by using neutral water. The dialysis water in which the semipermeable membrane bag is immersed may be replaced during dialysis as necessary. Dialysis removes hydrogen ions and acid-derived anions contained in the solution after addition through a semipermeable membrane.The semipermeable membrane used for dialysis is not particularly limited, but for example, a semipermeable membrane with a molecular weight cutoff of about 3500 can be used to obtain the iron ion-containing sol of the present invention. When an aqueous solution of iron ions is hydrolyzed under strong acidity, it changes from a structure containing OH such as a hydroxy complex to a structure close to an oxide, and becomes nanoparticles. Under strong acidity, hydrogen ions are adsorbed on the particle surface, so that repulsion occurs between the surfaces of each particle, resulting in a highly dispersed state. If this is placed in a dialysis membrane, left alone, and dialyzed by changing the dialysis water from time to time, the hydrogen ions on the particle surface are released outside the dialysis membrane, and the nanoparticles are associated. In this way, the iron ion-containing sol of the present invention is obtained. The iron ions in the sol are [Fe(H2O)6]. 3+ , [Fe(OH)(HO)] 2+ , [Fe(OH)2(H2O)4] + The iron ion-containing sol thus obtained is considered to be present in the form of iron oxide when dried and heated. In the present invention, the iron oxide precursor dispersed in the solvent refers to dispersed particles that become iron oxide when heated. Here, iron oxides have different compositions and crystal structures, but the iron oxide precursor in the present invention is preferably one that becomes stable α-Fe2O3 by adjusting the heating conditions. The content of iron ions in the iron ion-containing sol of the present invention is not particularly limited as long as it can be appropriately selected according to the required light absorption wavelength range and can maintain the sol state, and can be, for example, 1 to 30 mass % with respect to the total amount of the sol including the solvent.
[0010] The iron ion-containing sol of the present invention has ultraviolet absorbing ability and can absorb ultraviolet rays (UVA) with a wavelength of 320 to 400 nm. Furthermore, the absorption wavelength region can be changed by changing the concentration of the iron oxide precursor in the sol, and light from the UVA wavelength region to a wavelength of 600 nm can be absorbed. Therefore, it can be suitably used for ultraviolet absorber applications. The ultraviolet absorber of the present invention includes the iron ion-containing sol of the present invention. Here, "including" means both the case where the ultraviolet absorber is composed of only the iron ion-containing sol and the case where the ultraviolet absorber contains other components in addition to the iron ion-containing sol. The iron ion-containing sol and ultraviolet absorber of the present invention have excellent UVA absorption effect, so they can be used for applications requiring UVA absorption or UVA shielding, such as sunscreens, cosmetics, and ultraviolet ray shielding packaging. The iron ion-containing sol of the present invention is a water-based solvent, so in the case of cosmetics, it can be easily mixed with, for example, lotion, and can also be used as an emulsion. In addition, the iron ion-containing sol of the present invention contains an iron oxide precursor, but iron oxide is a chemical substance permitted for use in cosmetics, and is water-based. In addition, the acid component is removed by dialysis, so that it is safe. The ultraviolet light-shielding packaging can be used for packaging when deterioration of the contents due to ultraviolet light, such as medicines, is a problem. Furthermore, since the iron ion-containing sol of the present invention can absorb not only ultraviolet light but also visible light up to a wavelength of about 600 nm, it can also be used for applications such as packaging and containers for storing substances that fade with visible light. For example, many fluorescent dyes used for fluorescent labeling are excited by visible light (especially the blue part) and emit light. The excitation wavelength of rhodamine B, which is a fluorescent analysis reagent, is 555 nm, and the excitation wavelength of BODIPY dyes used in various imaging is 500 to 600 nm. The ultraviolet light absorber containing the iron ion-containing sol of the present invention can be used to prevent the fading of such dyes. In addition, an ultraviolet light absorber containing a dried product obtained by drying the iron ion-containing sol of the present invention can also be used for similar applications. The dried product of the iron ion-containing sol in the present invention is obtained by removing the solvent from the iron ion-containing sol of the present invention and separating the iron oxide precursor, which is a solid content, and the separated solid content has an amorphous structure.The iron ion-containing sol and its dried product of the present invention can be used by coating or mixing it into ultraviolet light-shielding wrapping paper, containers, etc. or wrapping paper, containers, etc. for fluorescent dyes.
[0011] Since the iron ion-containing sol of the present invention uses water as a solvent, it can be mixed uniformly with any water-soluble polymer that serves as a binder. Therefore, the iron ion-containing sol of the present invention can be used as an ultraviolet absorbing paint by mixing it with a binder. The paint of the present invention may contain components other than the iron ion-containing sol of the present invention and the binder. The content of the iron ion-containing sol in the paint can be appropriately selected according to the intended absorption wavelength of light and is not particularly limited, but can be, for example, 0.1 to 3 mass% with respect to the total amount of the paint. In addition, a film can be formed by mixing the iron ion-containing sol of the present invention and the binder and drying it. That is, the ultraviolet absorbing film of the present invention contains a dried product of the iron ion-containing sol of the present invention and a binder. Here, the ultraviolet absorbing film includes a film that is applied to the surface of a substrate and formed in close contact with the substrate and handled together with the substrate, and a so-called film-like film that can be handled as a single film. The ultraviolet absorbing film of the present invention may contain components other than the iron ion-containing sol of the present invention and the binder. The binder is not particularly limited as long as it can be mixed with the iron ion-containing sol of the present invention, but from the viewpoint of uniform mixing, a water-soluble polymer is preferred, and examples of the water-soluble polymer include methyl cellulose, ethyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, polyethylene glycol, polyvinylpyrrolidone, and polyacrylamide. The drying temperature when preparing the ultraviolet absorbing film can be appropriately selected depending on the type of binder, and is not particularly limited as long as the film can be formed at the temperature, and examples thereof include 40 to 120°C. Water-soluble polymers dissolve in water, but some, such as methyl cellulose, require heating the water to dissolve. If such a water-soluble polymer is used as a binder, the composite film of the present invention can be used as an ultraviolet absorbing film without deterioration even in applications where it comes into contact with water at room temperature, and can be used as an ultraviolet shielding film from the viewpoint of protecting the target object. The mixing ratio of the iron ion-containing sol and the binder in the ultraviolet absorbing paint of the present invention is not particularly limited, and examples thereof include a mass ratio of iron ions in the sol:binder of 1:8 to 1:100.The mixing ratio of the dried iron ion-containing sol and the binder in the ultraviolet absorbing film of the present invention is not particularly limited, but for example, the mass ratio of the dried sol:binder can be 1:3 to 1:10. The ultraviolet absorbing paint and ultraviolet absorbing film of the present invention can be used for applications such as coating ultraviolet and / or visible light shielding containers, covering them with a film, etc. The ultraviolet absorbing film of the present invention can also be used in combination with other films. The ultraviolet absorbing film of the present invention may also contain other functional particles such as dyes and luminescent particles. A film containing functional particles may be formed on a film formed of an iron ion-containing sol and a binder, in which case the protective power of the composite film against the functional particles from the upper and lower surfaces is improved.
[0012] Since the iron ion-containing sol of the present invention is a sol in which fine nanoparticles are dispersed, it can be suitably used for coating fine materials such as particles. By immersing various particles to be coated in a mixed liquid (coating liquid) in which the iron ion-containing sol of the present invention and a binder are mixed and drying, a coating layer containing the dried product of the iron ion-containing sol can be formed on the surface of the particles. By forming the coating layer, it is possible to prevent deterioration of various particles due to ultraviolet light or visible light. As the binder used in the coating liquid, the same binder as in the case of the ultraviolet absorbing paint or ultraviolet absorbing film can be used. In order to precipitate the binder component, alcohol may be added, and examples of the alcohol include ethyl alcohol and isopropyl alcohol (IPA). Furthermore, a metal soap may be added as a release agent to prevent aggregation of particles in the sol, and examples of the metal soap include zinc stearate, aluminum stearate, magnesium stearate, and the like. The various particles to be coated are not particularly limited, and examples thereof include fluorescent dyes, phosphorescent pigments, inorganic oxides, and the like. An anionic surfactant may be added to the coating liquid in order to suppress aggregation of the iron ion-containing sol, and an example of the anionic surfactant is sodium dodecyl sulfate, etc. The mixing amounts (mixing ratios) of various components in the coating liquid can be 1 to 5 parts by mass of binder, 10 to 100 parts by mass of alcohol for precipitating the binder, 1 to 20 parts by mass of metal soap, and 1 to 5 parts by mass of anionic surfactant, relative to 100 parts by mass of the iron ion-containing sol.
[0013] A coating liquid is prepared using the iron ion-containing sol of the present invention and a water-soluble binder that is easily soluble in water at a temperature close to room temperature, and particles are coated with this coating liquid. Until the coated particles come into contact with water, however, ultraviolet light or visible light close to ultraviolet light does not reach the particles inside the coating. However, when the coated particles come into contact with water, the binder in the coating layer begins to dissolve in the water, and the dried iron ion-containing sol that is no longer fixed also disperses in the water. Therefore, ultraviolet light or visible light close to ultraviolet light can reach the particles inside the coating. By utilizing this property, the coated particles of the present invention can be used as a deterioration detection material for structures and parts such as concrete and plastic materials. Particles of luminous substances (particles having a luminous function) such as fluorescent substances and phosphorescent substances are coated with the coating liquid. The coated particles thus obtained are mixed in advance with concrete, plastic materials, etc. to prepare structures and parts. When cracks form in structures or parts due to deterioration over time or deterioration due to water erosion, the water that enters the cracks comes into contact with the coated particles inside the structure or part, causing the coating layer to peel off, causing the luminous particles to emit light. This allows the occurrence of cracks to be detected. That is, the coated particles of the present invention can be used as coated particles for detecting deterioration of structures. In addition, by applying the coated particles to the surface of a structure or part or embedding them near the surface, when water comes into contact with the surface of the structure or part, the coating layer of the coated particles peels off and the luminescent particles emit light. This allows water leakage to occur near the structure or part to which the coated particles are applied or embedded, and it is known that the water has dripped or flowed into the part where the coated particles are located, allowing the water leakage to be detected. That is, the coated particles of the present invention can be used as coated particles for detecting water leakage. The coated particles of the present invention can be suitably used in this way for detecting deterioration of structures and the like and detecting water leakage from aged structures and the like. The particles having a luminescent function are not particularly limited as long as they have excitation light within the absorption wavelength range of the dried product of the iron ion-containing sol in the present invention, and examples thereof include those having excitation wavelengths within the ultraviolet range, within the range of 450 nm from the ultraviolet range, within the range of 500 nm from the ultraviolet range, within the range of 550 nm from the ultraviolet range, and within the range of 600 nm from the ultraviolet range. Moreover, as the particles having a light-emitting function, particles having a light-storing function are preferable.If the particle has a phosphorescent function, the light emission can be continued even after the coating is peeled off and the particle is exposed to light and is no longer exposed to light. As the water-soluble binder used in the coated particle for detecting deterioration of a structure and the coated particle for detecting a water leak, not only a water-soluble binder that is easily soluble in water at a temperature close to room temperature, but also a binder that dissolves at the temperature of water that is expected to come into contact with the particle depending on the usage environment may be used. The coated particle for detecting deterioration of a structure and the coated particle for detecting a water leak can be prepared, for example, by immersing the luminescent particle in a mixed liquid (coating liquid) in which the iron ion-containing sol of the present invention and a binder are mixed. The above-mentioned alcohol, metal soap and / or anionic surfactant can be added to the mixed liquid as necessary. In addition, even if the luminescent particle is dispersed in a film formed by the iron ion-containing sol of the present invention and the water-soluble binder, the surface of the film is peeled off by contact with water, so that the particle can function in the same way as the coated particle.
[0014] [Example 1] Fe(NO3)3·9H2O (4.04g) was dissolved in water and the volume was adjusted in a 50mL measuring flask to prepare a 0.2M Fe(NO3)3 aqueous solution. NaHCO3 (1.008g) was also dissolved in water and the volume was adjusted in a 50mL measuring flask to prepare a 0.24M NaHCO3 aqueous solution. The Fe(NO3)3 aqueous solution was transferred to an Erlenmeyer flask, and the NaHCO3 aqueous solution was dropped at a rate of 3mL / min while stirring with a stirrer at 500rpm. Four bags of semipermeable membrane (molecular weight cutoff 3500, width 45mm) cut to 12cm were prepared, and 25mL of the solution after dropping was placed in each bag, and the bags were dialyzed by immersing them in a beaker containing 1L of ultrapure water (manufactured by Merck Millipolya Milli-Q Integral MT) for 5 hours. The dialysis water (ultrapure water) was replaced every hour. In this way, the sol of the present invention was prepared. The prepared sol was diluted 100 times with water, and the concentration was measured using an ICP (inductively coupled plasma optical emission spectrometer: Agilent Technologies 5110 ICP-OES). 3+The ion concentration was 0.0731M, and the pH was 2.7. The absorption spectra of the prepared sol and the aqueous solutions obtained by diluting the prepared sol with water 2-fold, 4-fold, 8-fold, 16-fold, and 32-fold were measured (UV-1800, UV-Vis spectrophotometer, manufactured by Shimadzu Corporation). The measured absorption spectrum is shown in Figure 1. As shown in Figure 1, a shift in the absorption edge was observed due to dilution. The absorption spectra in Figure 1 are the prepared sol (before dilution), 2-fold diluted, 4-fold diluted, 8-fold diluted, 16-fold diluted, and 32-fold diluted in order of the highest absorbance at 600 nm. At 200 to 350 nm, the absorbance was 3 or higher at all concentrations. The pH of the sol when diluted 2-fold, 4-fold, and 32-fold was 2.9, 3.1, and 4.0, respectively.
[0015] [Comparative Example 1] A 0.0731 M aqueous solution of iron nitrate was prepared by dissolving Fe(NO3)3·9H2O (0.59 g) in 20 mL of water. The absorption spectra of the prepared aqueous solution and the aqueous solutions diluted 2-fold, 4-fold, 8-fold, 16-fold, and 32-fold with water in the same manner as in Example 1 were measured. The measured absorption spectra are shown in Figure 2. The absorption spectra in Figure 2 are, in order from highest absorbance at 450 nm, before dilution, 2-fold dilution, 4-fold dilution, 8-fold dilution, 16-fold dilution, and 32-fold dilution.
[0016] From a comparison between FIG. 1 and FIG. 2, it can be seen that the sol of the present invention obtained in Example 1 has an increased light absorption ability. That is, in the case of the sol obtained in Example 1, without dilution, the absorption starts at 750 nm, and at 575 nm, it shows an absorbance of 2 (99% light absorption, 1% transmitted light). [Table 1] shows the wavelengths at which the absorbance becomes 2 for each dilution ratio. In the case of the iron nitrate aqueous solution of Comparative Example 1, without dilution, it becomes an absorbance of 2 at 397 nm. This is almost the same absorption characteristic as when the sol obtained in Example 1 is diluted 32 times, and it can be seen from this that the sol obtained in Example 1 shows high absorption characteristics even at a lower concentration. Usually, light absorption by ion species is proportional to the concentration. Looking at FIG. 2, the absorbance of the shoulder peak near 450 nm changes approximately in proportion to the concentration. On the other hand, in FIG. 1, the position at which the absorption starts differs depending on the concentration, and the sol of the present invention can change the wavelength region of light that can be absorbed depending on the concentration. When the sol obtained in Example 1 is diluted with water, Fe 3+ A transmission electron microscope image (JEM-210, manufactured by JEOL Ltd.) after drying on a copper mesh with a carbon support film at an ion concentration of 2 mM is shown in Figure 3. Aggregates of fine particles with a size of several nanometers were observed. The particle size distribution of the sol obtained in Example 1 was measured using a laser diffraction particle size distribution measuring device (manufactured by Horiba, Ltd.) and the results are shown in Figure 4. The average particle size was calculated to be 20 nm.
[0017] [Table 1]
[0018] [Example 2] Fe(NO3)3·9H2O (7.57g) was dissolved in water to prepare 100mL of 0.0937M Fe(NO3)3 solution. NaHCO3 (2.016g) was dissolved in water to prepare 100mL of 0.24M NaHCO3 solution. HNO3 with pH 1 was also prepared by diluting 60% HNO3 (0.76mL) to 100mL with water. While stirring 100mL of 0.0937M Fe(NO3)3 solution at 250rpm with a stirrer, 100mL of 0.24M NaHCO3 solution was added dropwise from a dropping funnel at a rate of 3mL / min. The color changed from orange to reddish black upon addition. After addition, the mixture was stirred at the same stirring speed for 2 hours. Eight bags of semipermeable membrane similar to those in Example 1 were prepared, and 25 mL of the solution after dripping was placed in each bag. The bags were then dialyzed by immersing them in a beaker containing 1 L of dialysis water for 2 hours. The dialysis water used was HNO3 with a pH of 1, which was mixed with water to adjust the pH to 3.5, and the dialysis water was replaced every hour. In this way, the sol of the present invention was prepared. The Fe content of the obtained sol was 3+ The ion concentration was 0.069M by ICP measurement. The X-ray diffraction pattern (Rigaku MiniFlex 600) of the powder obtained by drying the obtained sol is shown in FIG. 5. There was no clear peak and it had an amorphous structure. 0.36 g of the powder obtained by drying was heated to 400°C over 24 minutes, held at 400°C for 11 hours and 36 minutes, then heated to 600°C over 1 hour, and held at 600°C for 12 hours to be fired. The X-ray diffraction pattern of the obtained powder is shown in FIG. 6. It was found that α-Fe2O3 was generated by firing. Therefore, the sol of the present invention is a precursor sol of α-Fe2O3.
[0019] [Example 3] (Preparation of UV-absorbing film) A 0.04M iron ion-containing sol was prepared in the same manner as in Example 1. 0.4 g (2% by mass relative to the iron ion-containing sol) of methylcellulose (MC400) was added to 20 mL of this sol, and the mixture was heated to 55°C in a hot water bath to disperse it, and then ultrasonically stirred in an ice bath to dissolve the methylcellulose. A uniform mixture of the sol and methylcellulose thus prepared was prepared. α-Vega (0.2 g) was added to this mixture, and the mixture was stirred to disperse it. The resulting dispersion was cast into a hydrophobized petri dish (diameter: about 9 cm) and dried at 40°C. The resulting film was cut into 1 cm x 3 cm pieces. The state is shown in Figure 7. Figure 7(a) shows the state under room light irradiation, and Figure 7(b) shows the state under ultraviolet light irradiation (pen-type UV light: Mos-Cure (registered trademark) mini 365). α-Vega (manufactured by LTI Corporation, product number GDK13100EP, water resistant, particle size: 100μm) is a commercially available phosphorescent pigment, a rare earth phosphorescent pigment consisting of strontium aluminate, europium and dysprosium. α-Vega is excited by light of 250 to 480nm and emits green light with a maximum emission wavelength of 530nm.
[0020] [Comparative Example 2] A composite film of methylcellulose and α-Vega was prepared in the same manner as in Example 3, except that water was used instead of the iron ion-containing sol. The result is shown in Figure 8. Figure 8(a) shows the state under indoor light irradiation, and Figure 8(b) shows the state under ultraviolet light irradiation as in Example 3.
[0021] As can be seen from FIG. 8(b), the composite film of methylcellulose and α-Vega emitted green light when irradiated with ultraviolet light. On the other hand, as shown in FIG. 7(b), the film prepared by adding the iron ion-containing sol of the present invention to methylcellulose and α-Vega did not emit light even when irradiated with ultraviolet light. This is thought to be because the dried iron ion-containing sol uniformly dispersed in the film absorbed light of 250 to 480 nm, and the excitation light did not reach α-Vega. It has been shown that the film formed by the iron ion-containing sol and methylcellulose of the present invention has excellent absorption and shielding properties as an ultraviolet absorbing film and, from the viewpoint of protecting the object, as an ultraviolet shielding film, and further, it has been shown to absorb light not only in the ultraviolet region but also in the visible light region.
[0022] [Example 4] (Coating of phosphorescent pigments with iron ion-containing sol) α-Vega (LTI Corporation, product number GDK13060WP, water resistant, particle size: 30 μm) (1 g) was added to an ethanol solution of sodium dodecyl sulfate (0.05 g / 10 ml) and stirred. The sol of the present invention prepared in Example 1 (2 mL) was added and stirred. The mixture was dried at 100° C. while stirring, then cooled to room temperature, 5% PVA solution (1 g) was added and stirred, IPA solution (10 mL) was added and stirred, and then lead stearate (0.2 g), a release agent, was added and stirred. The mixture was then heated to 100° C. while stirring and dried to obtain particles in which α-Vega was coated with the sol of the present invention. FIG. 9 shows an optical microscope image of the α-Vega used, and FIG. 10 shows an optical microscope image of the particles obtained by the treatment of Example 4. FIG. 9(a) and FIG. 10(a) show the state under room light irradiation, and FIG. 9(b) and FIG. 10(b) show the state under ultraviolet light irradiation. 11 and 12 are images observed by an optical microscope showing the change when the coated particles obtained by the treatment of Example 4 come into contact with water. FIG. 11 shows the state before coming into contact with water. FIG. 12(a)-(d) are images observed by an optical microscope showing the change over time when a water drop is placed on a slide glass and a coated particle is dropped on it. As can be seen from FIG. 9(b), α-Vega before the treatment emitted green light under ultraviolet irradiation. On the other hand, as can be seen from FIG. 10(b), the coated particles coated using the sol of the present invention did not emit light under ultraviolet irradiation. This is thought to be because the surface of the α-Vega particles was covered with the dried sol of the present invention, and this coating layer absorbed light of 250 to 480 nm, so that the excitation light did not reach the α-Vega particles. Thus, the coating layer using the sol of the present invention has excellent ultraviolet absorbing performance, and from the viewpoint of protecting the coated object (the object to be coated), it has excellent ultraviolet shielding performance. As can be seen from FIG. 12, the green emission becomes stronger as time passes from (a) to (d). This is believed to be because the PVA binder of the coating layer dissolves in water, and the dried sol also disperses in the water, causing the coating layer to peel off. In this way, if a binder that dissolves easily in water is used for the coated particles of the present invention, the coating can be protected from ultraviolet rays until it comes into contact with water, and the properties of the coating can be exhibited when it comes into contact with water. [Industrial Applicability]
[0023] The present invention can be suitably used in a variety of forms, such as a sol, a paint, a membrane on a substrate, a film, or a coating on particles, for applications requiring UVA absorption or UVA blocking. Furthermore, since the present invention is capable of absorbing not only UVA but also light of about 600 nm, it can be used in applications such as sunscreens, cosmetics, light-blocking packaging, deterioration detection materials, and water leak detection materials.
Claims
1. A method for producing an iron ion-containing sol having ultraviolet absorbing ability, comprising the steps of hydrolyzing an iron salt in an aqueous solution and dialyzing the solution after the hydrolysis.
2. A method for producing an iron ion-containing sol as described in claim 1, wherein the iron salt is iron nitrate, chloride or sulfate.
3. A method for producing an iron ion-containing sol as described in claim 1 or 2, in which sodium bicarbonate or sodium hydroxide is added to an aqueous solution to hydrolyze the iron salt.
4. A method for producing an iron ion-containing sol as described in any of claims 1 to 3, wherein the ultraviolet absorption ability is such that the absorbance of light at a wavelength of 546 nm or less is 2 or more when the Fe 3+ ion concentration is (0.0731 / 2) M, and the absorbance of light at a wavelength of more than 426 nm is less than 2 when the Fe 3+ ion concentration is (0.0731 / 16) M.
5. A method for producing an ultraviolet absorber, which comprises producing an iron ion-containing sol by the production method described in any one of claims 1 to 4, and drying the produced iron ion-containing sol.
6. Producing an iron ion-containing sol by the manufacturing method according to any one of claims 1 to 4, preparing a coating liquid containing the produced iron ion-containing sol and a water-soluble binder, and coating particles having a luminescent function with the coating liquid, or drying the produced iron ion-containing sol to obtain a dried product, preparing a coating liquid containing the dried product and a water-soluble binder, and coating particles having a luminescent function with the coating liquid. A method for producing coated particles.
7. A method for producing a cosmetic product, comprising producing an iron ion-containing sol by the production method described in any one of claims 1 to 4, and mixing the produced iron ion-containing sol with a lotion.
8. A method for producing an ultraviolet absorbing paint, comprising producing an iron ion-containing sol by the production method described in any one of claims 1 to 4, and mixing the produced iron ion-containing sol with a binder.
9. A method for producing an ultraviolet absorbing film, which comprises producing an ultraviolet absorbing paint by the manufacturing method described in claim 8 and drying the produced ultraviolet absorbing paint.
Citation Information
Patent Citations
cosmetic
JP1986289012A
Production of metal oxide or hydroxide sol
JP1997077503A
Titanium dioxide and composition containing the same
JP1997221411A