Curable composition, cured product, adhesive and sealant

JP7588753B1Active Publication Date: 2024-11-22SHIKOKU CHEM CORP

Patent Information

Application Number
JP2024126468
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-12-08
Filing Date
2024-08-02
Publication Date
2024-11-22
Estimated Expiration
2044-08-02

AI Technical Summary

Benefits of technology

【0018】 化学式(I)で示されるエポキシ·オキセタン化合物を含有する硬化性組成物は、硬化性に優れ、粘度が低く作業性に優れた硬化性組成物とすることができる。また、該硬化性組成物が硬化した硬化物は、高弾性で剛性に優れ、曲げ強度が大きく、硬化物中の構造欠陥が少なく均一な3次元ネットワークを形成していることにより優れた機械強度を有する硬化物とすることができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588753000027
    Figure 0007588753000027
  • Figure 0007588753000028
    Figure 0007588753000028
  • Figure 0007588753000029
    Figure 0007588753000029
Patent Text Reader

Abstract

The present invention provides a curable composition having high levels of curability, low viscosity, and mechanical strength, as well as a cured product thereof, an adhesive, and a sealant. The curable composition contains an epoxy-oxetane compound represented by chemical formula (I), in which R may be the same or different and represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. [Formula 1] JPEG0007588753000026.jpg3685
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition, a cured product, an adhesive, and a sealant. [Background technology]

[0002] Epoxy oxetane compounds have been attracting attention in recent years as photo- and heat-curable monomers. Curable compositions containing these compounds shrink little when cured, and the cured products (resins) have excellent toughness, mechanical properties (mechanical strength), heat resistance, electrical properties, water resistance (moisture resistance), weather resistance, transparency, and adhesion to other materials. Due to these excellent characteristics, curable compositions containing epoxy-oxetane compounds are increasingly being used as raw materials for coating materials, paints, inks, adhesive materials (glues), pressure-sensitive adhesive materials, films, pastes, optical materials, sealing materials (sealants), resist materials, etc.

[0003] The prior art related to the present invention will be described below with reference to the literature. The invention described in Patent Document 1 relates to an active energy ray-curable ink composition containing a polymerizable compound having a molecular weight of 600 or less and containing three or more cationically polymerizable groups in the molecule. In this document, as polymerizable compounds, an epoxy compound represented by the chemical formula (Ref-1) and an epoxy-oxetane compound represented by the chemical formula (Ref-2) are described.

[0004] [ka]

[0005] [ka]

[0006] The invention described in Patent Document 2 relates to a thin film adhesive composition containing a cyclic ether compound having an epoxy group and an oxetanyl group. This document describes an epoxy-oxetane compound represented by the chemical formula (Ref-3) as an example of a cyclic ether compound having an epoxy group and an oxetanyl group.

[0007] [ka]

[0008] Curable compositions containing epoxy-oxetane compounds used in various applications are required to have the following characteristics: a cured product can be obtained by curing; and a low viscosity is required from the viewpoint of workability during preparation and use of the curable composition. In addition, the cured product obtained by curing the curable composition is required to have the following characteristics: high elasticity and excellent rigidity, high bending strength, and excellent mechanical strength due to the formation of a uniform three-dimensional network with few structural defects in the cured product. Curable compositions containing epoxy-oxetane compounds represented by chemical formulas (Ref-1) to (Ref-3) and their cured products do not have these characteristics at a high level, and have problems with curability, viscosity, and / or mechanical strength. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2010-111713 A [Patent Document 2] JP 2019-189789 A Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a curable composition having high levels of curability, low viscosity, and mechanical strength, as well as a cured product thereof, an adhesive, and a sealant. [Means for solving the problem]

[0011] The present inventors have recognized that the desired object can be achieved by using a curable composition containing an epoxy-oxetane compound represented by chemical formula (I) as the curable composition, and have completed the present invention.

[0012] That is, the first invention is a curable composition containing an epoxy-oxetane compound represented by chemical formula (I).

[0013] [ka] (In the formula, R may be the same or different and represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.)

[0014] In addition, a cationic polymerization initiator may be contained.

[0015] A second invention relates to a cured product obtained by curing the curable composition of the first invention.

[0016] A third invention is an adhesive containing the curable composition of the first invention.

[0017] A fourth invention is a sealant containing the curable composition of the first invention. Effect of the Invention

[0018] The curable composition containing the epoxy-oxetane compound represented by chemical formula (I) can be a curable composition with excellent curability, low viscosity, and excellent workability. In addition, the cured product obtained by curing the curable composition has high elasticity, excellent rigidity, high bending strength, and excellent mechanical strength due to the formation of a uniform three-dimensional network with few structural defects in the cured product. [Brief description of the drawings]

[0019] [Figure 1] 1 is an IR spectrum chart of a pale yellow transparent liquid obtained in Synthesis Example 3. [Diagram 2] 1 is an IR spectrum chart of a colorless and transparent liquid obtained in Synthesis Example 4. [Diagram 3] 1 is an IR spectrum chart of the pale yellow transparent liquid obtained in Synthesis Example 7. [Figure 4] 1 is an IR spectrum chart of a colorless and transparent liquid obtained in Synthesis Example 10. [Diagram 5] 1 is an IR spectrum chart of a pale yellow transparent liquid obtained in Synthesis Example 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The curable compound of the present invention contains an epoxy-oxetane compound represented by chemical formula (I). The epoxy-oxetane compound represented by chemical formula (I) has a structure in which two epoxy groups are symmetrically arranged with respect to one oxetane ring having an ethyl group, and the oxetane ring and the two epoxy groups are bonded via a connector having one ether bond.

[0021] [ka]

[0022] In the above chemical formula (I), R is the same or different and represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. The alkyl group may be linear or branched. Specific examples include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. From the viewpoint of easy availability of raw materials and simplification of the synthesis process, it is preferable that R is the same and represents a hydrogen atom or a methyl group.

[0023] Examples of the epoxy-oxetane compound represented by chemical formula (I) include compounds represented by chemical formulas (I-1) to (I-6).

[0024] [ka]

[0025] From the viewpoints of easy availability of raw materials and simplification of the synthesis process, the epoxy oxetane compound represented by chemical formula (I) is preferably an epoxy oxetane compound represented by chemical formulas (I-1) to (I-6), and more preferably an epoxy oxetane compound represented by chemical formula (I-1). The epoxy oxetane compound represented by chemical formula (I) may be a single compound or a mixture of two or more kinds.

[0026] <Synthesis method of epoxy-oxetane compound represented by chemical formula (I)> A bifunctional olefin compound having a hydroxy group represented by chemical formula (II) is reacted with an oxetane compound having a leaving group represented by chemical formula (III) to produce an olefin-oxetane compound represented by chemical formula (Ia), and then the double bond of this compound is epoxidized to synthesize an epoxy-oxetane compound represented by chemical formula (I) (see reaction scheme (A)).

[0027] [ka]

[0028] In chemical formula (III), X is a leaving group and represents a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, a mesyloxy group (OMs), a tosyloxy group (OTs), or a trifluoromethanesulfonyloxy group (OTf). In chemical formulas (II) and (Ia), R has the same meaning as R in chemical formula (I), and the wavy line represents a trans form, a cis form, or a mixture thereof.

[0029] Examples of the oxetane compound having a leaving group represented by the above chemical formula (III) include 3-ethyl-3-methanesulfonyloxymethyloxetane, 3-bromomethyl-3-ethyloxetane, and the like.

[0030] Examples of the bifunctional olefin compound having a hydroxyl group represented by the above-mentioned chemical formula (II) include compounds represented by the chemical formulas (II-1) to (II-15). The bifunctional olefin compound may be used alone or in combination of two kinds.

[0031] [ka]

[0032] The bifunctional olefin compound having a hydroxyl group represented by the above chemical formula (II) can be synthesized, for example, by the method described in Chinese Patent Publication No. 102267878. The synthesis of the bifunctional olefin compound can also use a raw material derived from biomass, and from the viewpoint of reducing environmental load, it is preferable to use the bifunctional olefin compound synthesized from a raw material derived from biomass. Specifically, the bifunctional olefin compound derived from biomass can be synthesized by using 2-chloromethyloxirane (epichlorohydrin) derived from biomass and an olefin compound having a terminal hydroxyl group derived from biomass as raw materials.

[0033] The oxetane compound having a leaving group represented by the above chemical formula (III) can be synthesized, for example, by the method described in JP 2007-332294 A. A biomass-derived raw material can be used for the synthesis of the oxetane compound, and from the viewpoint of reducing the environmental load, it is preferable to use the oxetane compound synthesized from a biomass-derived raw material. By using a biomass-derived bifunctional olefin compound having a hydroxyl group represented by the chemical formula (II) and / or a biomass-derived oxetane compound having a leaving group represented by the chemical formula (III) as raw materials, a biomass-derived epoxy-oxetane compound represented by the chemical formula (I) can be synthesized.

[0034] The amount (charge amount) of the bifunctional olefin compound having a hydroxy group represented by the above chemical formula (II) is preferably an appropriate ratio in the range of 0.8 to 2 times the molar amount (charge amount) of the oxetane compound having a leaving group represented by the above chemical formula (III).

[0035] In addition, when the bifunctional olefin compound represented by the chemical formula (II-1) or the bifunctional olefin compound represented by the chemical formula (II-2) is used alone in the reaction, the epoxy-oxetane compound represented by the chemical formula (I-1) or the epoxy-oxetane compound represented by the chemical formula (I-2) can be obtained, respectively.

[0036] The olefin-oxetane compound represented by formula (Ia) can be synthesized in the presence of a base (i), a catalyst (ii) to promote the reaction, and a reaction solvent (iii) that does not inhibit the reaction. In addition, in the reaction for epoxidizing the double bond of the compound, a general epoxidation (oxidation) method can be adopted, for example, a method using a peracid, a method using hydrogen peroxide in the presence of sodium tungstate as a catalyst, a method using hydrogen peroxide together with a base in an acetonitrile-alcohol solvent, etc.

[0037] The base (i) may be a hydride, hydroxide, carbonate, hydrogencarbonate, alkoxide or organic amine compound of an alkali metal or alkaline earth metal. Examples include sodium hydride, potassium hydride, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium alkoxide, potassium alkoxide (eg, potassium t-butoxide, etc.), triethylamine, and the like. The amount of base used (charged amount) is preferably an appropriate ratio usually within a range of 1.1 to 20 times the amount of oxetane compound used (charged amount) having a leaving group.

[0038] The catalyst (ii) includes quaternary ammonium salts, quaternary phosphonium salts, and the like. Examples of quaternary ammonium salts include salts of tetrabutylammonium, tetramethylammonium, tetraethylammonium, tetrapropylammonium, tetrahexylammonium, tetraoctylammonium, tetradecylammonium, hexadecyltriethylammonium, dodecyltrimethylammonium, trioctylmethylammonium, octyltriethylammonium, benzyltrimethylammonium, benzyltriethylammonium, benzyltributylammonium, benzyldimethyloctadecylammonium, and phenyltrimethylammonium halides (fluorides, chlorides, bromides, iodides), and the like.

[0039] Examples of quaternary phosphonium salts include salts of tetrabutylphosphonium, tetramethylphosphonium, tetraethylphosphonium, tetrapropylphosphonium, tetrahexylphosphonium, tetradecylphosphonium, tetraoctylphosphonium, triethyloctadecylphosphonium, trioctylethylphosphonium, hexadecyltriethylphosphonium, tetraphenylphosphonium, and methyltriphenylphosphonium halides (fluorides, chlorides, bromides, iodides), and the like.

[0040] Combinations of these materials may also be used as catalyst (ii). The amount (charged amount) of the catalyst (ii) used is preferably an appropriate ratio within a range of 0.0001 to 1.0 times the amount (charged amount) of the oxetane compound having a leaving group used.

[0041] The reaction solvent (iii) is not particularly limited as long as it does not inhibit the reaction, and examples thereof include water, tetrahydrofuran, diethyl ether, dioxane, 4-methyltetrahydropyran, dimethoxyethane, ethyl acetate, propyl acetate, butyl acetate, propylene glycol monomethyl ether acetate (PGMEA), acetonitrile, benzene, toluene, xylene, dichloromethane, chloroform, carbon tetrachloride, N,N-dimethylformamide (DMF), dimethylacetamide (DMA), dimethylsulfoxide (DMSO), hexamethylphosphoric acid triamide (HMPA), and the like. One or more of these may be used in combination in an appropriate amount.

[0042] The reaction temperature in synthesizing the olefin-oxetane compound represented by the chemical formula (Ia) is preferably set in the range of 0 to 150° C., more preferably in the range of 20 to 120° C. The reaction time is appropriately set according to the set reaction temperature, but is preferably set in the range of 1 to 48 hours.

[0043] After the reaction is completed, the olefin-oxetane compound, which is the precursor of the target product, can be separated and extracted from the resulting reaction solution by, for example, solvent extraction. If necessary, the product can be further purified by washing with water or the like, treatment with activated carbon, silica gel chromatography, or the like.

[0044] In the reaction of epoxidizing an olefin-oxetane compound using the peracid, a peracid such as an oxone reagent, peracetic acid, metachloroperbenzoic acid (3-chloroperbenzoic acid) or the like can be used. The amount of peracid used (charged amount) is preferably an appropriate ratio within the range of 1.0 to 5.0 times the molar amount of the double bond of the olefin-oxetane compound.

[0045] In this epoxidation reaction, the reaction solvent is not particularly limited as long as it does not inhibit the reaction, but examples thereof include water, alcohols such as methanol, ethanol, and 2-propanol, aliphatic hydrocarbons such as hexane and heptane, ketones such as acetone and 2-butanone, esters such as ethyl acetate and butyl acetate, aromatic hydrocarbons such as benzene, toluene, and xylene, halogenated hydrocarbons such as methylene chloride (dichloromethane), chloroform, carbon tetrachloride, chlorotrifluoromethane, dichloroethane, chlorobenzene, and dichlorobenzene, ethers such as diethyl ether, diisopropyl ether, tetrahydrofuran, dioxane, dimethoxyethane, and diethylene glycol dimethyl ether, amides such as formamide, N,N-dimethylformamide (DMF), dimethylacetamide (DMA), N-methyl-2-pyrrolidone, N-methylpyrrolidinone, and hexamethylphosphorotriamide, and sulfoxides such as dimethyl sulfoxide (DMSO). These reaction solvents are used in appropriate amounts, either alone or in combination of two or more.

[0046] The reaction temperature in this epoxidation reaction is usually set in the range of −10 to 150° C., and preferably in the range of 0 to 100° C. The reaction time is appropriately set depending on the reaction temperature, and is usually set in the range of 1 to 48 hours, and preferably in the range of 1 to 24 hours.

[0047] After the reaction is completed, the target epoxy-oxetane compound represented by formula (I) can be separated and extracted from the resulting reaction solution by, for example, solvent extraction. If necessary, the product can be further purified by washing with water or the like, treatment with activated carbon, silica gel chromatography, or the like.

[0048] In the reaction of epoxidizing an olefin-oxetane compound with hydrogen peroxide using the sodium tungstate as a catalyst, hydrogen peroxide is used in a molar ratio of 1.0 to 5.0 times the double bond of the olefin-oxetane compound. The amount of sodium tungstate used (charged amount) is preferably an appropriate ratio within the range of 0.001 to 0.5 times the double bond of the olefin-oxetane compound.

[0049] The epoxidation reaction is not particularly limited as long as it does not inhibit the reaction, and for example, the same reaction solvents as those used in the above-mentioned epoxidation using a peracid can be used.

[0050] The reaction temperature in this epoxidation reaction is generally set in the range of −10 to 150° C., preferably 0 to 100° C., as in the case of the above-mentioned epoxidation using a peracid. The reaction time is appropriately set depending on the reaction temperature, but is generally set in the range of 1 to 48 hours, preferably 1 to 24 hours.

[0051] After the reaction is completed, the epoxy-oxetane compound represented by formula (I) can be separated and extracted from the reaction solution by, for example, solvent extraction, in the same manner as in the case of the epoxidation using peroxy acid. It may also be purified if necessary.

[0052] In the reaction of epoxidizing an olefin-oxetane compound using hydrogen peroxide together with a base in the above-mentioned acetonitrile-alcohol solvent, the amount of hydrogen peroxide used (charged amount) is preferably an appropriate ratio within the range of 1.0 to 5.0 times the molar amount of the double bond possessed by the olefin-oxetane compound. The amount of acetonitrile used (charged amount) is preferably an appropriate ratio within a range of 0.5 to 5.0 times by mole relative to the olefin / oxetane compound. The amount of alcohol used (charged amount) is preferably an appropriate ratio within the range of 10 to 80% by weight before the addition of hydrogen peroxide. In addition, it is preferable to set the pH within the range of 7 to 13 using a base.

[0053] The alcohol used in this epoxidation is preferably a saturated alcohol having 1 to 4 carbon atoms, such as methanol, ethanol, n-propanol, 2-propanol, n-butanol, sec-butanol (2-butanol), and isobutanol (2-methyl-1-propanol). These alcohols are used alone or in combination of two or more in appropriate amounts.

[0054] The base used in this epoxidation includes hydroxides, carbonates or hydrogencarbonates of alkali metals or alkaline earth metals, or organic amine compounds. It is preferable to use sodium hydroxide, potassium hydroxide, potassium carbonate, or potassium hydrogencarbonate, and an appropriate amount of one or a combination of two or more types is used.

[0055] The reaction temperature of this epoxidation is set, as in the case of the above-mentioned epoxidation using a peracid, usually in the range of −10 to 150° C., preferably in the range of 0 to 100° C. The reaction time is appropriately set depending on the reaction temperature, but is usually set in the range of 1 to 48 hours, preferably in the range of 1 to 24 hours.

[0056] After the reaction is completed, the epoxy-oxetane compound represented by formula (I) can be separated and extracted from the reaction solution by, for example, solvent extraction, in the same manner as in the case of the epoxidation using peroxy acid. It may also be purified if necessary.

[0057] <About the curable composition of the present invention> The epoxy-oxetane compound represented by formula (I) exhibits excellent curing performance. That is, by curing a curable composition containing an epoxy-oxetane compound represented by chemical formula (I) (hereinafter sometimes referred to as the "first curable compound"), a cured product (resin) that is expected to exhibit excellent properties can be obtained. In addition, in the curable composition of the present invention, it is also possible to use the first curable compound in combination with another curable compound (hereinafter, sometimes referred to as the "second curable compound").

[0058] During curing (polymerization) of the curable composition of the present invention, by allowing a second curable compound to coexist in addition to the first curable compound, a cured product in which the first curable compound and the second curable compound are copolymerized can be obtained. The second curable compound includes both a polymerizable monomer and a polymerizable oligomer (semi-cured product) having a structure in which a polymerizable monomer is polymerized.

[0059] Examples of such polymerizable monomers include known epoxy compounds (Note: sometimes called epoxy resins), oxetane compounds, epoxy-oxetane compounds (having an oxirane ring and an oxetane ring in the molecule), and acrylic compounds (Note: sometimes called acrylic resins).

[0060] The epoxy compound can be used without any particular limitation as long as it has an oxirane ring (epoxy group / glycidyl group) in the molecule. For example, Polyglycidyl ethers obtained by reacting polyhydric phenols such as bisphenol A, bisphenol F, bisphenol AD, catechol, and resorcinol, or polyhydric alcohols such as glycerin and polyethylene glycol with epichlorohydrin; Glycidyl ether esters obtained by reacting hydroxycarboxylic acids such as p-hydroxybenzoic acid and β-hydroxynaphthoic acid with epichlorohydrin; Polyglycidyl esters obtained by reacting polycarboxylic acids such as phthalic acid and terephthalic acid with epichlorohydrin; Glycidyl glycoluril compounds having two or more epoxy groups in the molecule, such as 1,3,4,6-tetraglycidyl glycoluril; Alicyclic epoxy compounds such as 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate; Nitrogen-containing cyclic epoxy compounds such as triglycidyl isocyanurate and hydantoin-type epoxy compounds; Further examples include epoxidized phenol novolac resins, epoxidized cresol novolac resins, epoxidized polyolefins, cyclic aliphatic epoxy resins, urethane-modified epoxy resins, as well as epoxy-modified organopolysiloxane compounds obtained by a hydrosilylation addition reaction between an organic compound having a carbon-carbon double bond and a glycidyl group and a silicon compound having a SiH group (for example, the epoxy-modified organopolysiloxane compounds disclosed in JP-A-2004-99751 and JP-A-2006-282988), and these may be used in combination.

[0061] The oxetane compound can be used without any particular limitation as long as it has an oxetane ring (oxetanyl group / oxetane group) in the molecule. For example, 3-ethyl-3-hydroxymethyloxetane, 3-(meth)allyloxymethyl-3-ethyloxetane, (3-ethyl-3-oxetanylmethoxy)methylbenzene, 4-fluoro-[1-(3-ethyl-3-oxetanylmethoxy)methyl]benzene, 4-Methoxy-[1-(3-ethyl-3-oxetanylmethoxy)methyl]benzene, [1-(3-ethyl-3-oxetanylmethoxy)ethyl]phenyl ether, isobutoxymethyl(3-ethyl-3-oxetanylmethyl)ether, isobornyloxyethyl (3-ethyl-3-oxetanylmethyl) ether, isobornyl (3-ethyl-3-oxetanylmethyl) ether, 2-ethylhexyl (3-ethyl-3-oxetanylmethyl) ether, Ethyl diethylene glycol (3-ethyl-3-oxetanylmethyl) ether, Dicyclopentadiene (3-ethyl-3-oxetanylmethyl) ether, dicyclopentenyloxyethyl (3-ethyl-3-oxetanylmethyl) ether, dicyclopentenyl (3-ethyl-3-oxetanylmethyl) ether, tetrahydrofurfuryl (3-ethyl-3-oxetanylmethyl) ether, 2-hydroxyethyl (3-ethyl-3-oxetanylmethyl) ether, 2-hydroxypropyl (3-ethyl-3-oxetanylmethyl) ether, butoxyethyl (3-ethyl-3-oxetanylmethyl) ether, Bornyl (3-ethyl-3-oxetanylmethyl) ether, 3,7-bis(3-oxetanyl)-5-oxa-nonane, 3,3′-[1,3-(2-methylene)propanediylbis(oxymethylene)]bis-(3-ethyloxetane), 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, 1,2-bis[(3-ethyl-3-oxetanylmethoxy)methyl]ethane, 1,3-bis[(3-ethyl-3-oxetanylmethoxy)methyl]propane, Ethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, dicyclopentenyl bis(3-ethyl-3-oxetanylmethyl) ether, triethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, tetraethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, Tricyclodecanediyldimethylene (3-ethyl-3-oxetanylmethyl) ether, Trimethylolpropane tris(3-ethyl-3-oxetanylmethyl) ether, 1,4-bis(3-ethyl-3-oxetanylmethoxy)butane, 1,6-bis(3-ethyl-3-oxetanylmethoxy)hexane, Pentaerythritol tris(3-ethyl-3-oxetanylmethyl) ether, pentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl) ether, Polyethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, Dipentaerythritol hexakis(3-ethyl-3-oxetanylmethyl) ether, Dipentaerythritol pentakis(3-ethyl-3-oxetanylmethyl) ether, Dipentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl) ether, Caprolactone modified dipentaerythritol hexakis(3-ethyl-3-oxetanylmethyl) ether, Caprolactone modified dipentaerythritol pentakis(3-ethyl-3-oxetanylmethyl) ether, Ditrimethylolpropane tetrakis(3-ethyl-3-oxetanylmethyl) ether, EO modified bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, PO modified bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, EO modified hydrogenated bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, PO modified hydrogenated bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, Examples include EO modified bisphenol F (3-ethyl-3-oxetanylmethyl) ether.

[0062] The epoxy-oxetane compound may be any compound having an oxirane ring (ibid.) and an oxetane ring (ibid.) in the molecule, and examples of such compounds include those described in the above-mentioned Patent Documents 1 and 2. The epoxy-oxetane compounds described in these documents are incorporated by reference into the disclosure of this specification.

[0063] Examples of acrylic compounds include allyl (meth)acrylate, vinyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, (meth)acrylic acid modified allyl glycidyl ether (manufactured by Nagase ChemteX Corporation, "Denacol Acrylate DA111 (trade name)"), urethane (meth)acrylates, epoxy (meth)acrylates, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, butanediol di(meth)acrylate, nonanediol di(meth)acrylate, polypropylene glycol (meth)acrylate, bisphenol A di(meth)acrylate, tris(2-(meth)acryloyloxyethyl)isocyanurate, and (meth)acrylate group-containing polyorganosiloxane.

[0064] In the curable composition of the present invention, the second curable compound may be a combination of the above-mentioned polymerizable monomer and polymerizable oligomer, the polymerizable monomer may be a combination of the above-mentioned polymerizable monomers (different types of polymerizable monomers may be a combination), and the polymerizable oligomer may be a combination of different types.

[0065] Regarding the ratio of the content of the first curable compound to the content of the second curable compound in the curable composition of the present invention, the content of the second curable compound is preferably an appropriate ratio in the range of 0 to 1000 times (weight ratio) the content of the first curable compound, and more preferably an appropriate ratio in the range of 0.01 to 100 times (weight ratio).

[0066] Methods for curing (polymerizing) the curable composition of the present invention include photocuring and thermal curing. Examples of photocuring methods include a method of irradiating with active energy rays and a method of using a photopolymerization initiator in combination. The active energy rays include light, radiation, electromagnetic waves, electron beams, etc., but typically represent light, particularly ultraviolet rays. As the photopolymerization initiator, a photocationic polymerization initiator or a photoanionic polymerization initiator can be used, and if necessary, a photoradical polymerization initiator can be used in combination, and these may be contained in the curable composition. In addition, in order to improve production efficiency and properties of the cured product, a thermal curing method may be used in combination with the photocuring.

[0067] As the photocationic polymerization initiator, any commonly used one can be used without any particular limitation, and examples thereof include onium salts and organometallic complexes. Examples of the onium salts include diazonium salts, sulfonium salts and iodonium salts, and examples of the organometallic complexes include iron-arene complexes, titanocene complexes and arylsilanol-aluminum complexes. Examples of industrial chemicals commercially available as photocationic polymerization initiators include "OPTOMER SP-150 (product name)" and "OPTOMER SP-170 (product name)" manufactured by ADEKA Corporation, "CPI-100P (product name)" manufactured by San-Apro, "UVE-1014 (product name)" manufactured by General Electronics Corporation, and "CD-1012 (product name)" manufactured by Sartomer Corporation. The counter anion of the photocationic polymerization initiator is SbF6 - , AsF6 - , B(C6F5)4 -, PF6 - etc.

[0068] As the photoanionic polymerization initiator, any commonly used initiator may be used without any particular limitation, and examples of such initiators include onium salts and carbamates. Examples of the onium salts include 1,2-diisopropyl-3-(bis(dimethylamino)methylene)guanidium 2-(3-benzoylphenyl)propionate, 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanidium n-butyltriphenylborate, and the like. Examples of carbamates include 2-nitrophenylmethylpiperidine-1-carboxylate, 1-(anthraquinone-2-yl)ethylimidazole carboxylate, 1-(3-(2-hydroxyphenyl)-2-propenoyl)piperidine, and 9-anthranylmethyldiethylcarbamate.

[0069] The content of the photocationic polymerization initiator or photoanionic polymerization initiator in the curable composition of the present invention is preferably from 0.001 to 20% by weight, and more preferably from 0.01 to 10% by weight.

[0070] Examples of photoradical polymerization initiators include: Ketal compounds having 16 to 17 carbon atoms (e.g., acetophenone dimethyl ketal, benzyl dimethyl ketal, etc.), Acetophenone compounds having 8 to 18 carbon atoms (e.g., acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 2-hydroxy-2-methyl-phenylpropan-1-one, diethoxyacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, etc.), Benzophenone compounds having 13 to 21 carbon atoms (e.g., benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 4,4'-bismethylaminobenzophenone, etc.), benzoin compounds having 14 to 18 carbon atoms (e.g., benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isobutyl ether, etc.), Anthraquinone compounds having 14 to 19 carbon atoms (e.g., 2-ethylanthraquinone, 2-tert-butylanthraquinone, 2-chloroanthraquinone, 2-amylanthraquinone, etc.), Thioxanthone compounds having 13 to 17 carbon atoms (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone, etc.), Examples of the acylphosphine oxide compounds include those having 22 to 28 carbon atoms (for example, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, etc.).

[0071] The content of the photoradical polymerization initiator in the curable composition of the present invention is preferably from 0.001 to 20% by weight, and more preferably from 0.01 to 10% by weight.

[0072] When the curable composition of the present invention is photocured, a sensitizer such as pyrene, perylene, acridine orange, thioxanthone, 2-chlorothioxanthone, or benzoflavin can be used.

[0073] On the other hand, when the curable composition of the present invention is thermally cured, a thermal polymerization initiator can be used. As the thermal polymerization initiator, a thermal cationic polymerization initiator, a thermal radical polymerization initiator, or a thermal anionic polymerization initiator can be adopted, and this may be contained in the curable composition.

[0074] As the thermal cationic polymerization initiator, any commonly used one can be used without any particular limitation, and examples thereof include various onium salts such as quaternary ammonium salts, phosphonium salts and sulfonium salts, and organometallic complexes. Examples of onium salts commercially available as industrial chemicals include "ADEKAOPTON CP-66 (product name)" and "ADEKAOPTON CP-77 (product name)" manufactured by ADEKA Corporation, "SAN-AID SI-60L (product name)," "SAN-AID SI-80L (product name)," and "SAN-AID SI-100L (product name)" manufactured by Sanshin Chemical Industry Co., Ltd., and "CI Series (product name)" manufactured by Nippon Soda Co., Ltd. Examples of organometallic complexes include alkoxysilane-aluminum complexes.

[0075] The thermal radical polymerization initiator may be any commonly used one without any particular limitation, and examples thereof include diisopropyl peroxydicarbonate, benzoyl peroxide, t-butyl peroxyisobutyrate, t-hexyl peroxyisopropyl monocarbonate, t-hexyl peroxy 2-ethylhexanoate, 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexanoate, t-butyl peroxypivalate, t-hexyl peroxypivalate, and t-butyl peroxyneodecanoate. peroxides such as benzoyl peroxide, t-hexylperoxyneodecanoate, 1,1,3,3-tetramethylbutylperoxyneodecanoate, 1,1-bis(t-hexylperoxy)cyclohexane, benzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, and lauroyl peroxide; and azo compounds such as azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), and dimethyl 2,2'-azobis(2-methylpropionate), which may be used in combination.

[0076] The thermal anionic polymerization initiator can be any commonly used one without any particular limitation. Examples of the thermal anionic polymerization initiator include amines and imidazoles, and these may be used in combination.

[0077] Regarding the heat curing conditions, the heating temperature / heating time can be appropriately set, but is preferably set within the range of 60 to 200° C. / 30 to 240 minutes, and more preferably within the range of 70 to 180° C. / 30 to 120 minutes.

[0078] The content of the thermal polymerization initiator in the curable composition of the present invention is preferably from 0.001 to 20% by weight, and more preferably from 0.01 to 10% by weight.

[0079] In the present invention, the cationic polymerization initiator refers to the above-mentioned photocationic polymerization initiator and / or thermal cationic polymerization initiator, the anionic polymerization initiator refers to the above-mentioned photoanionic polymerization initiator and / or thermal anionic polymerization initiator, and the radical polymerization initiator refers to the above-mentioned photoradical polymerization initiator and / or thermal radical polymerization initiator.

[0080] Another method for curing (polymerizing) the curable composition of the present invention includes a method of photocuring or heat curing using a curing agent. When heat curing is performed, a thermal polymerization initiator can be used in combination.

[0081] The curing agent includes an acid anhydride compound, a thiol compound, an amine compound, and the like.

[0082] Examples of the acid anhydride compound include Examples of the anhydride include methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, trimellitic anhydride, nadic anhydride, himic anhydride, methylnadic anhydride, methylbicyclo[2.2.1]heptane-2,3-dicarboxylic anhydride, bicyclo[2.2.1]heptane-2,3-dicarboxylic anhydride, and methylnorbornane-2,3-dicarboxylic acid.

[0083] Examples of the thiol compound include: Aliphatic thiol compounds such as ethanedithiol, propanedithiol, hexamethylenedithiol, decamethylenedithiol, tolylene-2,4-dithiol, 2,2-bis(mercaptomethyl)-1,3-propanedithiol, 2-(mercaptomethyl)-2-methyl-1,3-propanedithiol, and 2-ethyl-2-(mercaptomethyl)-1,3-propanedithiol; Cyclic sulfide compounds such as a 1,4-dithiane ring-containing polythiol compound represented by formula (XIV): mercaptoalkyl sulfide compounds such as 3-thiapentane-1,5-dithiol and 4-mercaptomethyl-3,6-dithia-1,8-octanedithiol; Mercaptopropionic acid esters such as pentaerythritol tetrakis(3-mercaptopropionate); Epoxy resin terminal mercapto compound; 3,6-dioxa-1,8-octanedithiol, a mercaptoalkyl ether disulfide compound represented by formula (XV), 2,2′-[[2,2-bis[(2-mercaptoethoxy)methyl]-1,3-propanediyl]bis(oxy)]bisethanethiol, 3,3′-[[2,2-bis[(3-mercaptopropoxy)methyl]-1,3-propanediyl]bis(oxy)]bis-1-propanethiol, 3-[2,2-bis[(3-mercaptopropoxy)methyl]butoxy]-1-propanethiol, 3-(3-mercaptopropoxy)-2,2-bis[(3-mercaptopropoxy)methyl]-1-propanol, mercaptoalkyl ether compounds such as 2,2-bis[(3-mercaptopropoxy)methyl]-1-butanol; 1,3,4,6-tetrakis(2-mercaptoethyl)glycoluril, Examples thereof include 1,3,4,6-tetrakis(3-mercaptopropyl)glycoluril, and 1,3,4,6-tetrakis(2-mercaptoethyl)glycoluril and 1,3,4,6-tetrakis(3-mercaptopropyl)glycoluril are preferred. These other thiol compounds may be used alone or in combination of two or more.

[0084] [ka] (In the formula, p represents an integer of 1 to 5.)

[0085] [ka] (In the formula, q represents an integer of 1 to 20.)

[0086] As is conventionally known, the amine compound may be any compound having at least one amino group selected from a primary amino group, a secondary amino group, and a tertiary amino group in the molecule.

[0087] Examples of such amine compounds include: Aliphatic amines such as diethylenetriamine, triethylenetetramine, isophoronediamine, xylylenediamine, diaminodiphenylmethane, 1,3,4,6-tetrakis(3-aminopropyl)glycoluril, n-propylamine, 2-hydroxyethylaminopropylamine, cyclohexylamine, 4,4′-diaminodicyclohexylmethane, and dimethylbenzylamine; Aromatic amines such as 4,4′-diaminodiphenylmethane and o-methylaniline; Examples of the heterocyclic compound include nitrogen-containing heterocyclic compounds such as 2-ethyl-4-methylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazoline, 2,4-dimethylimidazoline, piperidine, and piperazine.

[0088] The content of the curing agent in the curable composition of the present invention is preferably 0.1 to 50 parts by weight, and more preferably 1 to 40 parts by weight, based on 100 parts by weight of the epoxy-oxetane compound.

[0089] The reaction product of an epoxy compound with an amine compound or the reaction product of a compound having one or more isocyanate groups in the molecule with a compound having at least one of a primary amino group and a secondary amino group in the molecule is a solid that is poorly soluble in epoxy resins at room temperature, but is solubilized (made easily soluble) by heating and functions as a curing accelerator, and is therefore also called a latent curing accelerator (hereinafter, these reaction products may be referred to as "latent curing accelerators").

[0090] Examples of epoxy compounds used as a raw material for the latent curing accelerator consisting of a reaction product of an epoxy compound and an amine compound include, in addition to the above-mentioned epoxy compounds, glycidylamine compounds obtained by reacting 4,4'-diaminodiphenylmethane, m-aminophenol, or the like with epichlorohydrin; Examples of the epoxy compound include monofunctional epoxy compounds such as butyl glycidyl ether, phenyl glycidyl ether, and glycidyl methacrylate.

[0091] Examples of the amine compounds used as a raw material for the latent curing accelerator consisting of the reaction product of an epoxy compound and an amine compound include the above-mentioned amine compounds. Among these amine compounds, an amine compound having a tertiary amino group in the molecule is a raw material that gives a latent curing accelerator having excellent curing acceleration properties. Examples of such amine compounds include: amines such as dimethylaminopropylamine, diethylaminopropylamine, di-n-propylaminopropylamine, dibutylaminopropylamine, dimethylaminoethylamine, diethylaminoethylamine, and N-methylpiperazine; Amines having a tertiary amino group in the molecule, such as imidazole compounds such as 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, and 2-phenylimidazole; 2-Dimethylaminoethanol, 1-methyl-2-dimethylaminoethanol, 1-phenoxymethyl-2-dimethylaminoethanol, 2-diethylaminoethanol, 1-butoxymethyl-2-dimethylaminoethanol, 1-(2-hydroxy-3-phenoxypropyl)-2-methylimidazole, 1-(2-hydroxy-3-phenoxypropyl)-2-ethyl-4-methylimidazole, 1-(2-hydroxy-3-butoxypropyl)-2-methylimidazole, 1-(2-hydroxy-3-butoxypropyl)-2-ethyl-4-methylimidazole, 1-(2-hydroxy-3-phenoxypropyl)-2-phenylimidazoline, 1-(2-hydroxy-3-butoxypropyl)-2-methyl Examples of the tertiary amino group-containing alcohols, phenols, thiols, carboxylic acids, and hydrazides include alcohols, phenols, thiols, carboxylic acids, and hydrazides having a tertiary amino group in the molecule, such as thiolimidazoline, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, N-β-hydroxyethylmorpholine, 2-dimethylaminoethanethiol, 2-mercaptopyridine, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 4-mercaptopyridine, N,N-dimethylaminobenzoic acid, N,N-dimethylglycine, nicotinic acid, isonicotinic acid, picolinic acid, N,N-dimethylglycine hydrazide, N,N-dimethylpropionic acid hydrazide, nicotinic acid hydrazide, and isonicotinic acid hydrazide.

[0092] In order to further improve the storage stability of the curable composition of the present invention, an active hydrogen compound having two or more active hydrogens in the molecule may be used as a third component in addition to the above-mentioned epoxy compound and amine compound as a raw material for a latent curing accelerator consisting of a reaction product of an epoxy compound and an amine compound.

[0093] Examples of active hydrogen compounds include: Polyphenols such as bisphenol A, bisphenol F, bisphenol S, hydroquinone, catechol, resorcinol, pyrogallol, and phenol novolac resins; Polyhydric alcohols such as trimethylolpropane; Polycarboxylic acids such as adipic acid and phthalic acid; Examples of the mercaptoacid include 1,2-dimercaptoethane, 2-mercaptoethanol, 1-mercapto-3-phenoxy-2-propanol, mercaptoacetic acid, anthranilic acid, and lactic acid.

[0094] Furthermore, the latent curing accelerator consisting of the reaction product of an epoxy compound and an amine compound may be surface-treated with an isocyanate compound or an acidic compound. Examples of the isocyanate compound include Monofunctional isocyanate compounds such as n-butyl isocyanate, isopropyl isocyanate, phenyl isocyanate, and benzyl isocyanate; Examples of the polyfunctional isocyanate compounds include hexamethylene diisocyanate, toluylene diisocyanate, 1,5-naphthalene diisocyanate, diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, xylylene diisocyanate, paraphenylene diisocyanate, 1,3,6-hexamethylene triisocyanate, and bicycloheptane triisocyanate.

[0095] Instead of this polyfunctional isocyanate compound, a terminal isocyanate group-containing compound obtained by reacting a polyfunctional isocyanate compound with an active hydrogen compound can also be used in the same manner as the polyfunctional isocyanate compound. Examples of such terminal isocyanate group-containing compounds include an addition reaction product having a terminal isocyanate group obtained by reacting toluylene diisocyanate with trimethylolpropane, and an addition reaction product having a terminal isocyanate group obtained by reacting toluylene diisocyanate with pentaerythritol.

[0096] The acidic compound used for surface treatment of the latent curing accelerator consisting of the reaction product of the epoxy compound and the amine compound may be any of gas, liquid, or solid, and may be any of inorganic acid or organic acid. Examples of such acidic compounds include carbon dioxide gas, sulfurous acid gas, sulfuric acid, hydrochloric acid, oxalic acid, phosphoric acid, acetic acid, formic acid, propionic acid, adipic acid, caproic acid, lactic acid, succinic acid, tartaric acid, sebacic acid, p-toluenesulfonic acid, salicylic acid, boric acid, tannic acid, alginic acid, polyacrylic acid, polymethacrylic acid, phenol, pyrogallol, phenolic resin, and resorcinol resin.

[0097] A latent curing accelerator consisting of a reaction product of an epoxy compound and an amine compound can be easily obtained by mixing an epoxy compound, an amine compound, and, if necessary, an active hydrogen compound, reacting them at a temperature from room temperature to 200°C, solidifying and pulverizing the mixture, or by reacting them in a solvent such as methyl ethyl ketone, dioxane, or tetrahydrofuran, removing the solvent, and then pulverizing the solid content.

[0098] Alternatively, a commercially available latent curing accelerator consisting of a reaction product of an epoxy compound and an amine compound can be used. Examples of such products include "Amicure PN-23 (trade name)", "Amicure PN-H (trade name)", "Amicure PN-50 (trade name)", "Amicure PN-23J (trade name)", "Amicure PN-40J (trade name)", and "Amicure MY-24 (trade name)" manufactured by Ajinomoto Fine-Techno Co., Ltd.; "Novacure HX-3088 (trade name)", "Novacure HX-3721 (trade name)", "Novacure HX-3722 (trade name)", "Novacure HX-3742 (trade name)", "Novacure HX-3941HP (trade name)", and "Novacure HXA3922HP (trade name)" manufactured by Asahi Kasei Corporation; and "Fujicure FXR-1030 (trade name)", "Fujicure FXR-1081 (trade name)", and "Fujicure FXR-1121 (trade name)" manufactured by T&K TOKA Corporation.

[0099] The content of the latent curing accelerator consisting of a reaction product of an epoxy compound and an amine compound in the curable composition of the present invention is preferably 0.1 to 100 parts by weight, more preferably 1 to 90 parts by weight, and further preferably 1 to 80 parts by weight, based on 100 parts by weight of the epoxy-oxetane compound.

[0100] Examples of the isocyanate compound having one or more isocyanate groups in the molecule used as a raw material for the latent curing accelerator consisting of a reaction product between a compound having one or more isocyanate groups in the molecule and a compound having at least one of a primary amino group and a secondary amino group in the molecule include: n-Butyl isocyanate, isopropyl isocyanate, 2-chloroethyl isocyanate, phenyl isocyanate, p-bromophenyl isocyanate, m-chlorophenyl isocyanate, o-chlorophenyl isocyanate, p-chlorophenyl isocyanate, 2,5-dichlorophenyl isocyanate, 3,4-dichlorophenyl isocyanate, 2,6-dimethylphenyl isocyanate, o-fluorophenyl isocyanate, p-fluorophenyl isocyanate, m-tolyl isocyanate, p-tolyl isocyanate, o-trifluoromethylphenyl isocyanate, m-trifluoromethylphenyl isocyanate, benzyl isocyanate, hexamethylene Examples of the isocyanate include diphenylmethane-4,4'-diisocyanate, 2,4-toluylene diisocyanate, 2,6-toluylene diisocyanate, 1,5-naphthalene diisocyanate, diphenylmethane-4,4'-diisocyanate, 2,2-dimethyldiphenylmethane-4,4'-diisocyanate, tolidine diisocyanate, isophorone diisocyanate, xylylene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, p-phenylene diisocyanate, 1,3,6-hexamethylene triisocyanate, bicycloheptane triisocyanate, tris-(3-isocyanato-4-methylphenyl)isocyanurate, and tris-(6-isocyanatohexyl)isocyanurate.

[0101] Examples of compounds having at least one of a primary amino group and a secondary amino group in the molecule that are used as a raw material for the latent curing accelerator consisting of a reaction product between a compound having one or more isocyanate groups in the molecule and a compound having at least one of a primary amino group and a secondary amino group in the molecule include: Examples of the amines include dimethylamine, diethylamine, di-n-propylamine, di-n-butylamine, di-n-hexylamine, di-n-octylamine, di-n-ethanolamine, dimethylaminopropylamine, diethylaminopropylamine, morpholine, piperidine, 2,6-dimethylpiperidine, 2,2,6,6-tetramethylpiperidine, piperazine, pyrrolidine, benzylamine, N-methylbenzylamine, cyclohexylamine, metaxylylenediamine, 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, N-aminoethylpiperazine, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-phenylimidazole, and 1,1-dimethylhydrazine.

[0102] A reaction product of a compound having one or more isocyanate groups in the molecule and a compound having at least one of a primary amino group and a secondary amino group in the molecule can be obtained by reacting the two in an organic solvent such as dichloromethane.

[0103] In the curable composition of the present invention, the content of the latent curing accelerator consisting of a reaction product of a compound having one or more isocyanate groups in the molecule and a compound having at least one of a primary amino group and a secondary amino group in the molecule is preferably 1 to 10 parts by weight based on 100 parts by weight of the epoxy oxetane compound.

[0104] The curable composition of the present invention further includes, as long as the effects of the present invention are not impaired, Pigments (titanium white, cyanine blue, watching red, red iron oxide, carbon black, aniline black, manganese blue, iron black, ultramarine blue, Hansa red, chrome yellow, chrome green, etc.), Inorganic fillers (calcium carbonate, kaolin, clay, talc, mica, barium sulfate, lithopone, gypsum, zinc stearate, perlite, quartz, quartz glass, fused silica, silica powder such as spherical silica, spherical alumina, crushed alumina, oxides such as magnesium oxide, beryllium oxide, titanium oxide, nitrides such as boron nitride, silicon nitride, aluminum nitride, carbides such as silicon carbide, hydroxides such as aluminum hydroxide, magnesium hydroxide, metals and alloys such as copper, silver, iron, aluminum, nickel, titanium, carbon materials such as diamond, carbon, etc.), Thermoplastic resins and thermosetting resins (homopolymers such as various high-density, medium-density and low-density polyethylenes, polypropylene, polybutene, polypentene, etc., ethylene-propylene copolymers, polyamide resins such as nylon-6 and nylon-6,6, vinyl chloride resins, nitrocellulose resins, vinylidene chloride resins, acrylamide resins, styrene resins, vinyl ester resins, polyester resins, phenolic resins (phenolic compounds), silicone resins, fluorine-based resins, various elastomer resins such as acrylic rubber and urethane rubber, graft copolymers such as methyl methacrylate-butadiene-styrene graft copolymers and acrylonitrile-butadiene-styrene graft copolymers, etc.), Reinforcing agents (glass fiber, carbon fiber, etc.), Anti-sagging agents (hydrogenated castor oil, fine silica particles, etc.), Matting agents (fine silica, paraffin wax, etc.), Abrasives (zinc stearate, etc.), Internal release agents (fatty acids such as stearic acid, fatty acid metal salts such as calcium stearate, fatty acid amides such as stearic acid amide, fatty acid esters, polyolefin wax, paraffin wax, etc.), The composition may contain additives (modifiers) such as surfactants, leveling agents, antifoaming agents, viscosity adjusting diluents (organic solvents), coupling agents, fragrances, and flame retardants.

[0105] The curable composition of the present invention is prepared by any method, and is prepared by weighing out the above-mentioned components in a predetermined amount and mixing them by stirring. For example, after premixing, it can be prepared by mixing or melt-kneading using a roll mixer, kneader, extruder, etc. If necessary, an organic solvent (a diluent for adjusting viscosity) may be used.

[0106] The curable composition of the present invention polymerizes (cures) upon irradiation with ultraviolet light or heating to give a cured product. Examples of the ultraviolet ray irradiation means include a method using a light source such as a chemical lamp, a low pressure mercury lamp, a high pressure mercury lamp, an extra high pressure mercury lamp, a xenon lamp, or a metal halide lamp. The irradiation intensity and irradiation time of ultraviolet light are appropriately set taking into consideration the desired irradiation intensity or desired irradiation time, and also taking into consideration the composition and shape (thickness) of the curable composition to be irradiated. Examples of the heating means include hot air circulation, infrared heating, high frequency heating, etc. Also, as the curing device, a closed curing oven or a tunnel oven capable of continuous curing, etc. can be used. The heating (curing) temperature and heating (curing) time may be appropriately set in consideration of the composition and shape (thickness) of the curable composition to be irradiated, as in the case of ultraviolet irradiation.

[0107] The curable composition of the present invention has a low viscosity and can be used as a curable ink composition. Furthermore, the curable composition of the present invention has a low viscosity and is excellent in ejection properties. Therefore, it is also suitable as a curable ink composition for inkjet. By applying the curable ink composition for inkjet to a predetermined object using the inkjet method and curing it, it is used in the manufacture of various parts and members, etc., which will be described later. The inkjet method can form a resin film quickly, uniformly, and over a wide area, and therefore has advantages such as improved product accuracy of various parts and members, etc., which will be described later, as well as reduced manufacturing costs.

[0108] From the viewpoint of volatility, the curable ink composition and the curable ink composition for inkjet preferably have a 5% weight loss temperature (°C) of 185°C or higher, and more preferably 190°C or higher, as measured using a differential thermal thermogravimetry device under conditions of a sample weight of 10 mg, a heating condition of 10°C / min, and a nitrogen flow (200 mL / min).

[0109] The inkjet curable ink composition preferably has a viscosity of 5 mPa·s or more and 150 mPa·s or less, more preferably 10 mPa·s or more and 80 mPa·s or less, and even more preferably 10 mPa·s or more and 40 mPa·s or less, as measured at 25° C. using a dynamic viscoelasticity measuring device (manufactured by UBM, "Rheosol-G5000"). The inkjet curable ink composition may be heated during application by the inkjet method to reduce the viscosity before application.

[0110] Furthermore, the curable inkjet ink composition preferably has a surface tension of 15 mN / m or more and 35 mN / m or less, and more preferably 20 mN / m or more and 30 mN / m or less, as measured at 25° C. using a dynamic wettability tester.

[0111] Suitable examples of the inkjet curable ink composition include curable compositions for encapsulating optical elements, which are used as encapsulants for optical elements such as organic electroluminescence (hereinafter referred to as organic EL) elements and organic thin-film solar cell elements, as well as adhesives for optical components, which are used for bonding optical lenses, etc., curable compositions for stereolithography, which are used in the manufacture of various parts and members by 3D printers, and curable compositions for nanoimprinting, which are used in the formation of ultrafine circuit patterns for semiconductors.

[0112] As an example, a method for producing an optical element using the curable composition of the present invention as a curable composition for encapsulating an optical element includes a step of applying the curable composition for encapsulating an optical element to at least one of two substrates by an inkjet method, a step of curing the applied curable composition for encapsulating an optical element by light irradiation and / or heating, and a step of bonding the two substrates together.

[0113] In the step of applying the curable composition for encapsulating optical elements to at least one of the two substrates, the curable composition for encapsulating optical elements may be applied to the entire surface of the substrate, or may be applied to a part of the substrate. For example, when an organic EL element is produced as the optical element, the shape of the sealant portion formed by applying the curable composition for encapsulating optical elements is not particularly limited as long as it is a shape that can protect the laminate having the organic light-emitting material layer sandwiched between the two substrates from the outside air. That is, it may be a shape that completely covers the laminate, or a pattern shape that closes the periphery of the laminate.

[0114] The step of curing the curable composition for encapsulating optical elements by light irradiation and / or heating may be performed before or after the step of laminating the two substrates. When the step of curing the curable composition for encapsulating optical elements by light irradiation and / or heating is performed before the step of laminating the two substrates, the substrates may be laminated within a usable time (e.g., 1 minute) from the time of light irradiation and / or heating until the curing reaction progresses and adhesion becomes impossible.

[0115] In addition, the step of curing the applied curable composition for encapsulating optical elements by light irradiation and / or heating may be performed by the above-mentioned ultraviolet ray irradiation means and / or heating means.

[0116] The curable composition of the present invention is not particularly limited in its application, and can be applied to products (parts and components) in various fields where the material may be resin, and can be used as a raw material for materials in the fields of electricity / electronics, optics, architecture, civil engineering, automobiles / aircraft, and medicine, as well as for other daily necessities and miscellaneous goods.

[0117] For example, examples of parts, components and materials in the electrical and electronic fields include resin-coated copper foil, prepreg, copper-clad laminates, printed wiring boards, solder resist ink, anisotropic conductive film, anisotropic conductive paste, interlayer insulating materials, adhesives, pressure sensitive adhesives, sealing materials, sealants (sealants), sealing sheets, insulating materials, thermally conductive materials, hot melt materials, paints, potting agents, etc. More specifically, Sealing materials (sealants) for printed wiring boards and electronic components such as interlayer insulating films and wiring covering films, sealing materials (sealants) for image display devices, sealing sheets for image display devices, sealing materials (sealants) for organic electroluminescence display elements, sealing sheets for organic electroluminescence display elements, layer-forming materials; Materials for forming display devices such as color filters, polarizing plates, display materials, resist materials, and alignment films; Materials for forming semiconductor devices, such as resist materials and buffer coating films; Materials for forming optical components such as lenses, holograms, optical waveguides, optical circuits, optical circuit components, and anti-reflection films; Coating agents such as surface protective films, hard coat agents, antifouling films, and antireflection films for semiconductor elements and organic thin-film elements (for example, organic electroluminescence elements and organic thin-film solar cell elements); etc. Other examples include materials for organic electronics elements such as organic EL elements, organic transistors, and solar cells, materials for forming rigid wiring boards and flexible printed wiring boards for semiconductor mounting, mounting materials for semiconductor mounting, adhesives for flexible printed wiring boards, semiconductor encapsulants, solar cell encapsulants, insulating films for semiconductors, coverlay films for protecting flexible printed circuits, and coating agents for covering wiring.

[0118] Examples of materials in the optical field include lenses, prisms, films, core materials for optical fibers, cladding materials, wear-resistant coating agents for plastic lenses, materials for stereolithography, optical waveguides, filters, image display materials, lens arrays, sealing materials and reflector materials for optical semiconductor elements, light guide plates, light diffusion plates, diffraction elements, optical adhesives, etc. For example, lenses and prisms are not particularly limited as long as they utilize refraction on their surfaces. Also, Materials for camera modules, LiDAR modules, and still camera lenses; Adhesives for finder prisms, target prisms, finder covers, light receiving sensors, photographic lenses, projection lenses for projection televisions, etc.; Optical fiber materials around optical switches and optical connectors in optical communication systems; Sealing materials and adhesives for optical passive components, optical circuit components, and peripherals of optoelectronic integrated circuits; etc. Examples of bonding locations in a camera module include between an image sensor (imaging element) such as a CMOS or CCD and a substrate, between a cut filter and a substrate, between a substrate and a housing, between a housing and a cut filter, and between a housing and a lens unit.

[0119] As lenses and prisms, convex lenses such as biconvex lenses, plano-convex lenses, and convex meniscus lenses, and concave lenses such as biconcave lenses, plano-concave lenses, and concave meniscus lenses, etc., spherical lenses with spherical surfaces; Aspheric lenses, such as lenses having aspheric surfaces, such as symmetric paraboloids, ellipsoids, hyperboloids, and polymorphic surfaces (e.g. quartic surfaces), and lenses having freeform surfaces without an axis of symmetry; Cylindrical lenses are like semi-cylindrical lenses with a cylindrical surface; A toroidal lens, which has a toroidal surface with different radii of curvature in the longitudinal and transverse directions, like the surface of a doughnut; A thin Fresnel lens is a lens in which a number of concentric ring-shaped prisms, each of which has a reflective surface that changes the direction of light by inclining in the same way as the curve of a thick convex lens, and a refracting surface that transmits light, are arranged on a flat surface, and these multiple prisms become successively smaller or larger as they approach the center; A diffractive lens that has a minute relief with a depth of about the wavelength of light formed in a concentric pattern; Examples of such prisms include those having two or more optically flat surfaces, with at least one pair of surfaces being substantially non-parallel. Examples of films include reflective films that are made by treating inorganic compounds such as MgF2 and SiO2 using a vacuum deposition method, a sputtering method, or a CVD method, or by coexisting a light absorber, and that transmit light in a desired wavelength range while reflecting light in an undesired wavelength range.

[0120] Examples of materials in the construction field include sealants, coating materials, and primers for exterior materials such as various metal panels and siding boards; Sealing materials, adhesives, injection materials, vibration-damping materials, soundproofing materials, conductive materials for electromagnetic wave shielding, putty materials used between exterior materials, base materials, ceiling materials and interior materials; Adhesives for bonding tiles and stone to exterior walls and substrates; Adhesives and pressure sensitive adhesives for bonding wood flooring materials, polymeric floor sheets, and floor tiles to various floors; Examples include injection materials for repairing cracks in various exterior and interior materials.

[0121] Examples of materials in the civil engineering field include joint sealants, coating materials, primers, paints, putty materials, injection materials, spraying materials, and formwork for various concrete products such as roads, bridges, tunnels, and breakwaters.

[0122] Examples of materials in the automotive and aerospace sectors include structural materials, fiber-reinforced composites, adhesives for bodies and parts, sealing materials, coating materials, cushioning materials, vibration-damping materials, sound-proofing materials, spraying materials; Adhesives, pressure sensitive adhesives, coatings and foams for automotive interiors; Examples include sealing materials for steel plate joints, adhesives, coating materials, etc. Furthermore, applications of substrates having a coating layer made of a cured product of the curable composition of the present invention formed on their surfaces include, for example, components of various industrial devices such as transport vehicles (automobiles, aircraft, etc.) and electronic and electrical devices (for example, sliding components such as cylinders, pistons, bearings, etc.).

[0123] Examples of materials in the medical field include artificial bones, dental impression materials, medical rubber materials, medical adhesives, and medical device sealing materials.

[0124] Other examples include paints that are applied to substrates such as metals, resin films, glass, paper, and wood. EXAMPLES

[0125] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited thereto. The main raw materials used are as follows: Allyl glycidyl ether (Tokyo Chemical Industry Co., Ltd.) Allyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Potassium tert-butoxide (Tokyo Chemical Industry Co., Ltd.) 3-Ethyl-3-methanesulfonyloxymethyloxetane (synthesized in accordance with the method described in JP 2007-332294 A) Sodium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Metachloroperbenzoic acid (Tokyo Chemical Industry Co., Ltd.) 1,2,3-Glycidyloxypropane (manufactured by Anhui Xinyuan Technology Co., Ltd, trade name "XY633", a compound represented by chemical formula (IV)) Glycerin (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 3-Ethyl-3-hydroxymethyloxetane (Ube Industries, Ltd.) Allyl chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 2-Chloromethyloxirane (Osaka Soda Co., Ltd.) Allyl chloride (Tokyo Chemical Industry Co., Ltd.) Sodium iodide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Potassium iodide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0126] [ka]

[0127] (C) Thermal cationic polymerization initiator Dibenzylmethyl-p-hydroxyphenylsulfonium hexafluoroantimonate (manufactured by Sanshin Chemical Industry Co., Ltd., "San-Aid SI-100L (trade name)")

[0128] The methods for measuring the viscosity, elastic modulus, loss tangent, flexural modulus, and flexural strength, which are evaluation tests employed in the examples and comparative examples, are as follows.

[0129] [Viscosity measurement] The viscosity at 25°C of the epoxy / oxetane compounds (including epoxy compounds and oxetane compounds) used in the examples and comparative examples described below was measured using a dynamic viscoelasticity measuring device (UBM, "Rheosol-G5000"). It is determined that the smaller the viscosity value (lower the viscosity), the better the workability during preparation of the curable composition and when using the curable composition as an adhesive.

[0130] [Measurement of elastic modulus and loss tangent] The curable compositions prepared in the examples and comparative examples described below were cured at 65° C. for 2 hours, and then heated and cured at 150° C. for 2 hours. The storage modulus G′ (MPa) and loss tangent tanδ at 25° C. were measured for the obtained cured products (test pieces: length 30 mm × width 10 mm × thickness 1 mm) using a dynamic viscoelasticity measuring device (UBM, “Rheosol-G5000”) (frequency: 1 Hz). The larger the storage modulus G' (high elasticity), the better the rigidity, and the smaller the loss tangent tan δ, the fewer structural defects there are in the cured product, forming a uniform three-dimensional network.

[0131] [Measurement of flexural modulus and flexural strength] The curable compositions prepared in the examples and comparative examples described below were cured at 65° C. for 2 hours, and then heated and cured at 150° C. for 2 hours. The flexural modulus (GPa) and flexural strength (MPa) of the obtained cured products (test pieces: length 80 mm × width 25 mm × thickness 1 mm) were measured in accordance with JIS K7203. The greater the flexural modulus (high elasticity), the more excellent the rigidity, and the greater the flexural strength, the more excellent the mechanical strength.

[0132] <Synthesis of epoxy-oxetane compound represented by chemical formula (I-1)> [Synthesis Example 1] In a 5L three-neck flask, 2178g (37500mmol) of allyl alcohol and 308.58g (2750mmol) of potassium tert-butoxide were charged, and the mixture was heated to 40°C. Then, 285.35g (2500mmol) of allyl glycidyl ether was added dropwise, and the mixture was stirred at 60°C for 14 hours. The reaction solution was then cooled to 25°C or below, filtered to remove solids, and the filtrate was distilled under reduced pressure. The resulting concentrated solution was purified by distillation to obtain 391.19g of a bifunctional olefin compound having a hydroxyl group represented by the chemical formula (II-1) as a colorless, transparent liquid (yield: 91%).

[0133] [ka]

[0134] [Synthesis Example 2] In a 5L 4-neck flask, 344.44g (2000mmol) of the colorless transparent liquid obtained in Synthesis Example 1, 1500g of dimethyl sulfoxide, and 114.96g (2874mmol) of sodium hydroxide were charged and heated to 60℃, after which 427.35g (2200mmol) of 3-ethyl-3-methanesulfonyloxymethyloxetane was added dropwise and stirred at 70℃ for 8 hours. The reaction solution was then cooled to 25℃ or below, the solid matter was removed, and the filtrate was extracted with 2000mL of ethyl acetate. The organic layer was then washed with 2000mL of water, and concentrated under reduced pressure. The resulting concentrated solution was purified by distillation to obtain 336.92g of an olefin-oxetane compound represented by the chemical formula (Ia-1) as a colorless transparent liquid (yield: 62%).

[0135] [ka]

[0136] [Synthesis Example 3] In a 1L three-neck flask, 54.07g (200.0mmol) of the colorless transparent liquid obtained in Synthesis Example 2, 86.29g (500.0mmol) of metachloroperbenzoic acid, and 500g of chloroform were charged and stirred at 30°C for 12 hours. The reaction liquid was filtered to remove solids, washed with 500mL of 10wt% potassium carbonate aqueous solution and 500mL of water, and then the organic layer was concentrated under reduced pressure. The resulting concentrate was purified by silica gel column chromatography (ethyl acetate / hexane = 1 / 3 (volume ratio)) to obtain 26.49g of a pale yellow transparent liquid (yield: 44%).

[0137] This pale yellow transparent liquid 1 The H-NMR spectrum data was as follows: · 1 H-NMR (CDCl3) δ: 4.46 (d, 2H), 4.37 (d, 2H), 3.79 (m, 2H), 3.74(t, 2H), 3.61 (m, 5H), 3.41 (m, 2H), 3.13 (quin., 2H), 2.79 (t, 2H), 2.60 (m, 2H), 1.74 (q, 2H), 0.88 (t, 3H). The IR spectrum data of this pale yellow transparent liquid was as shown in the chart in FIG. From these spectral data, the pale yellow transparent liquid obtained was identified as an epoxy-oxetane compound represented by the chemical formula (I-1).

[0138] [ka]

[0139] <Synthesis of oxetane compound represented by chemical formula (V)> [Synthesis Example 4] In a 500mL three-neck flask, 18.42g (200.0mmol) of glycerin, 180.0g of dimethyl sulfoxide, and 22.20g (555.0mmol) of sodium hydroxide were charged and heated to 60°C, after which 104.90g (540.0mmol) of 3-ethyl-3-methanesulfonyloxymethyloxetane was added dropwise and stirred at 70°C for 8 hours. Thereafter, the reaction solution was cooled to below 25°C, the solid matter was removed, and the filtrate was extracted with 200mL of ethyl acetate. Subsequently, the organic layer was washed with 60mL of water, and then concentrated under reduced pressure. The obtained concentrate was purified by silica gel column chromatography (ethyl acetate / hexane=2 / 3 (volume ratio)) to obtain 8.50 g of a colorless transparent liquid (yield: 11%).

[0140] This colorless and transparent liquid 1 The H-NMR spectrum data was as follows: · 1 H-NMR (CDCl3) δ: 4.44 (d, 6H), 4.35 (d, 6H), 3.72 (s, 2H), 3.66(quin., 1H), 3.57 (m, 6H), 3.55 (d, 2H), 1.74 (q, 6H), 0.88 (t, 9H). The IR spectrum data of this colorless, transparent liquid was as shown in the chart in FIG. From these spectral data, the obtained colorless transparent liquid was identified as an oxetane compound represented by chemical formula (V).

[0141] [ka]

[0142] <Synthesis of epoxy-oxetane compound represented by chemical formula (VIII)> [Synthesis Example 5] In a 1L three-neck flask, 174.24g (1500mmol) of 3-ethyl-3-hydroxymethyloxetane and 8.00g (200.0mmol) of sodium hydroxide were charged and heated to 45°C, after which 114.14g (1000mmol) of allyl glycidyl ether was added dropwise and stirred at 50°C for 12 hours. The reaction solution was then cooled to 25°C or below, extracted with 750mL of chloroform, washed with 500mL of water, and the organic layer was concentrated under reduced pressure to obtain 223.4g of the compound represented by the chemical formula (VI) as a pale yellow transparent liquid (yield: 97%).

[0143] [ka]

[0144] [Synthesis Example 6] In a 2L three-neck flask, 184.73g (750.0mmol) of the pale yellow transparent liquid obtained in Synthesis Example 5, 750.00g of dimethyl sulfoxide, 45.00g (1125.0mmol) of sodium hydroxide, and 5.62g (37.5mmol) of sodium iodide were charged, and the mixture was heated to 50°C, after which 86.10g (1125.0mmol) of allyl chloride was added dropwise and stirred at 50°C for 8 hours. Thereafter, the reaction solution was cooled to below 25°C, the solid matter was removed, and the filtrate was extracted with 1500mL of ethyl acetate. Subsequently, the mixture was washed with 1500mL of water, and the organic layer was concentrated under reduced pressure. The obtained concentrated liquid was purified by distillation to obtain 121.67g of the compound represented by the chemical formula (VII) as a colorless transparent liquid (yield: 60%).

[0145] [ka]

[0146] [Synthesis Example 7] In a 500mL three-neck flask, 27.03g (100.0mmol) of the colorless transparent liquid obtained in Synthesis Example 6, 43.14g (250.0mmol) of metachloroperbenzoic acid, and 250g of chloroform were charged and stirred at 30°C for 12 hours. The reaction liquid was filtered to remove solids, washed with 250mL of 10wt% potassium carbonate aqueous solution and 250mL of water, and then the organic layer was concentrated under reduced pressure. The resulting concentrate was purified by silica gel column chromatography (ethyl acetate / hexane = 1 / 3 (volume ratio)) to obtain 12.02g of a pale yellow transparent liquid (yield: 40%).

[0147] This pale yellow transparent liquid 1 The H-NMR spectrum data was as follows: · 1 H-NMR (CDCl3) δ: 4.46 (d, 2H), 4.36 (d, 2H), 3.91 (m, 1H), 3.76(m, 2H), 3.60 (m, 7H), 3.41 (m, 1H), 3.15 (m, 2H), 2.78 (m, 2H), 2.61 (m, 2H), 1.74 (q, 2H), 0.89 (t, 3H). The IR spectrum data of this pale yellow transparent liquid was as shown in the chart in FIG. From these spectral data, the pale yellow transparent liquid obtained was identified as an epoxy-oxetane compound represented by chemical formula (VIII).

[0148] [ka]

[0149] <Synthesis of epoxy-oxetane compound represented by chemical formula (XI)> [Synthesis Example 8] In a 1L three-neck flask, 278.78g (2400.0mmol) of 3-ethyl-3-hydroxymethyloxetane and 38.40g (960.0mmol) of sodium hydroxide were charged and heated to 47°C, after which 74.02g (800.0mmol) of 2-chloromethyloxirane was added dropwise and stirred at 60°C for 4 hours. The reaction solution was then cooled to 25°C or below, extracted with 900mL of chloroform, washed with 500mL of water, and the organic layer was concentrated under reduced pressure. The concentrated solution was purified by distillation to obtain 87.51g of the compound represented by chemical formula (IX) as a colorless, transparent liquid (yield: 38%).

[0150] [ka]

[0151] [Synthesis Example 9] In a 300mL three-neck flask, 40.37g (140.0mmol) of the colorless transparent liquid obtained in Synthesis Example 8, 8.12g (203.0mmol) of sodium hydroxide, and 1.16g (7.0mmol) of potassium iodide were charged, and the mixture was heated to 67°C, after which 13.93g (182.0mmol) of allyl chloride was added dropwise and stirred at 70°C for 2 hours. The reaction solution was then cooled to below 25°C, the solid matter was removed, and the filtrate was extracted with 80mL of ethyl acetate. The organic layer was then washed with 40mL of water, and the organic layer was concentrated under reduced pressure to obtain 44.79g of the compound represented by the chemical formula (X) as a colorless transparent liquid (yield: 97%).

[0152] [ka]

[0153] [Synthesis Example 10] In a 500 mL three-neck flask, 42.70 g (130.0 mmol) of the colorless transparent liquid obtained in Synthesis Example 9, 22.43 g (130.0 mmol) of metachloroperbenzoic acid, and 300 g of chloroform were charged and stirred at 30° C. for 12 hours. The reaction liquid was then filtered to remove solid matter, and washed with 150 mL of a 10 wt % aqueous potassium carbonate solution and 150 mL of water. The organic layer was concentrated under reduced pressure to obtain 38.44 g of a colorless transparent liquid (yield: 86%).

[0154] This colorless and transparent liquid 1 The H-NMR spectrum data was as follows: · 1 H-NMR (CDCl3) δ: 4.44 (d, 4H), 4.35 (d, 4H), 3.89 (dd, 1H), 3.72 (quin., 1H), 3.56 (m, 9H), 3.12(quin, 1H), 2.77 (t, 1H), 2.60 (dd, 1H), 1.72 (q, 4H), 0.87 (t, 6H). The IR spectrum data of this colorless, transparent liquid was as shown in the chart in FIG. From these spectral data, the obtained colorless transparent liquid was identified as an epoxy-oxetane compound represented by chemical formula (XI).

[0155] [ka]

[0156] [Synthesis Example 11] In a 1L three-necked eggplant flask, 49.26g (200.0mmol) of the pale yellow transparent liquid obtained in Synthesis Example 5, 200.00g of dimethyl sulfoxide, 10.40g (260.0mmol) of sodium hydroxide, and 1.50g (10.0mmol) of sodium iodide were charged and heated to 50°C, after which 50.51g (260.0mmol) of 3-ethyl-3-methanesulfonyloxymethyloxetane was added dropwise and stirred at 50°C for 8 hours. Thereafter, the reaction solution was cooled to below 25°C, the solid matter was removed, and the filtrate was extracted with 400mL of ethyl acetate. Subsequently, after washing with 400mL of water, the organic layer was concentrated under reduced pressure. The obtained concentrated solution was purified by distillation to obtain 26.32g of the compound represented by the chemical formula (XII) as a colorless transparent liquid (yield: 40%).

[0157] [ka]

[0158] [Synthesis Example 12] In a 1L three-necked eggplant flask, 26.28g (80.0mmol) of the colorless transparent liquid obtained in Synthesis Example 11, 16.57g (96.0mmol) of metachloroperbenzoic acid, and 500g of chloroform were charged and stirred at 30°C for 12 hours. The reaction liquid was filtered to remove solids, washed with 100mL of 10wt% potassium carbonate aqueous solution and 100mL of water, and then the organic layer was concentrated under reduced pressure. The resulting concentrate was purified by silica gel column chromatography (ethyl acetate / hexane = 2 / 3 (volume ratio)) to obtain 17.05g of a pale yellow transparent liquid (yield: 62%).

[0159] This pale yellow transparent liquid 1 The H-NMR spectrum data was as follows: · 1H-NMR (CDCl3) δ: 4.43 (d, 4H), 4.32 (d, 4H), 3.77 (dd, 1H), 3.72 (d, 2H), 3.56 (m, 7H), 3.39 (m, 1H), 3.12(quin., 1H), 2.78 (t, 1H), 2.59 (dd, 1H), 1.72 (q, 4H), 0.87 (t, 6H). The IR spectrum data of this pale yellow transparent liquid was as shown in the chart in FIG. From these spectral data, the pale yellow transparent liquid obtained was identified as an epoxy-oxetane compound represented by chemical formula (XIII).

[0160] [ka]

[0161] <Evaluation of the cured product> Example 1 A curable composition was prepared by uniformly mixing 100 parts by weight of the epoxy-oxetane compound represented by the chemical formula (I-1) synthesized in Synthesis Example 3 and 0.2 parts by weight of a thermal cationic polymerization initiator. The above-mentioned evaluation tests were carried out on this curable composition and a cured product obtained by curing the curable composition, and the test results obtained are shown in Table 1.

[0162] [Comparative Examples 1 to 5] In the same manner as in Example 1, curable compositions having the formulations shown in Table 1 were prepared, and the above-mentioned evaluation tests were carried out on those curable compositions and cured products obtained by curing the curable compositions. The test results obtained are as shown in Table 1.

[0163] [Table 1]

[0164] From Table 1, it was confirmed that the epoxy-oxetane compound contained in the curable composition of the present invention has an extremely low viscosity, and therefore has excellent workability during preparation and use as a curable adhesive. In addition, the curable composition of the present invention exerts a crosslinking function, and a cured product is obtained by curing. Despite the low viscosity, the cured product has high values ​​of storage modulus G' and flexural modulus, and a high flexural strength, confirming that the cured product has excellent mechanical strength. Since the loss tangent tanδ of the cured product obtained by curing the curable composition of the present invention is small, it is presumed that a uniform three-dimensional network with few structural defects is formed in the cured product. [Industrial Applicability]

[0165] According to the curable composition of the present invention, it is possible to provide a curable composition and a cured product thereof which have, compared with conventional curable compositions, excellent curability, low viscosity, and mechanical strength, and the industrial applicability of the present invention is great.

Claims

1. A curable composition comprising an epoxy oxetane compound represented by formula (I). 【Chemistry 1】 (In the formula, R may be the same or different and represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.)

2. The curable composition according to claim 1, which contains a cationic polymerization initiator.

3. A cured product obtained by curing the curable composition according to any one of claims 1 to 2.

4. An adhesive comprising the curable composition according to any one of claims 1 to 2.

5. A sealant comprising the curable composition according to any one of claims 1 to 2.

Citation Information

Patent Citations

  • Actinic energy ray-curing inkjet ink and printed matter

    JP2005002191A

  • Ink composition, ink composition for inkjet recording, method for inkjet recording, and recorded matter

    JP2010111713A

  • Epoxy oxetane compound, synthetic method thereof, and application of the compound

    JP2019077674A

  • Curable composition for encapsulation of optical element and sheet for encapsulation of optical element, and optical element device

    JP2019189769A

  • Adhesive composition for thin film, laminate using the same, and manufacturing method of laminate

    JP2019189789A

Cited By

  • Curable composition, cured product, adhesive, and sealant

    WO2025121227A1