Silica particles, their production method, and slurry composition
The VMC method produces silica particles with controlled size and low water absorption, addressing hollow particle and impurity issues, resulting in improved filling and electrical properties for encapsulants and electronic boards.
Patent Information
- Application Number
- JP2020067041
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-02
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-04-02
AI Technical Summary
Existing silica particles used in encapsulants and electronic boards have issues with high water absorption, presence of hollow particles, and impurities like alkali metals, which affect performance and surface smoothness, especially in miniaturized electronic devices and fine wiring.
A production method using the VMC method to produce silica particles with controlled particle size, low water absorption, and minimal hollow particles, involving surface treatment and a multi-step classification process to remove coarse and hollow particles, ensuring high purity and low impurity levels.
The produced silica particles exhibit excellent filling properties, stability, and electrical characteristics, enabling smoother surfaces and improved performance in sealing materials and resin compositions.
Abstract
Description
[Technical field]
[0001] The present invention relates to silica particles, a method for producing the same, and a slurry composition. [Background technology]
[0002] In recent years, the miniaturization of electronic devices (including electronic components) has shown no signs of stopping. Materials used in such electronic devices are required to have extremely high performance according to their size. For example, semiconductor devices, which are one type of electronic component, are generally manufactured by encapsulating semiconductor elements with an encapsulant. Encapsulating materials are required to have a wide range of performance capabilities, such as isolating semiconductor elements from the outside and ensuring heat dissipation, and extremely high performance is required as semiconductor devices become more miniaturized.
[0003] Similarly, electronic substrates are also required to have high performance due to the finer wiring. Electronic substrates are formed by disposing wiring made of a conductor on the surface or inside of an insulating layer, and the insulating layer is composed of a resin composition in which a filler is dispersed in a resin material. Therefore, by reducing the particle size of the filler, the thickness of the insulating layer can be reduced, and the entire electronic substrate can also be made thinner. In particular, electronic substrates include laminated substrates formed by stacking insulating layers and conductor layers in multiple layers, and by reducing the particle size of the filler, the thickness of the insulating layer can be reduced, and as a result, the entire laminated substrate can also be made thinner. Furthermore, by reducing the particle size of the filler, the particle size of the filler exposed on the surface of the substrate also becomes smaller, making it possible to reduce the roughness of the substrate surface and improve the surface smoothness.
[0004] As a sealant, silica is widely dispersed as a filler because it has high physical and chemical stability and reduces volume fluctuations due to thermal fluctuations. Since the sealant needs to fill fine gaps such as between a semiconductor element and a substrate, the dispersed filler must be fine. In addition, the particle size distribution of the filler must be considered in order to improve the gap filling ability. It has been found that preferable performance can be achieved by removing coarse particles larger than a certain particle size. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2008-247726 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention was completed in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a filler-containing composition that can be suitably employed in, for example, an encapsulating material for semiconductor devices, silica particles that are suitable for use as a filler in the composition, a method for producing the same, and a slurry composition containing the silica particles. [Means for solving the problem]
[0007] In order to solve the above problems, the present inventors conducted intensive research and found that silica particles used as fillers for packaging materials such as sealing materials and electronic substrates must have various properties. Specifically, (a) they must have a low content of alkali metals and alkaline earth metals such as sodium (high purity), and (b) they must have low water absorption. Water absorption can be evaluated by the water absorption rate. By reducing water absorption, electrical properties can be improved. The low water absorption is determined by the amount of silanol, and the lower the amount of silanol, the lower the water absorption. Silica produced by the VMC method has the characteristics of having a low amount of silanol and low water absorption.
[0008] The purity and water absorption of silica particles are affected by the manufacturing method. For example, the raw materials differ depending on the type of manufacturing method, and some raw materials are easier to improve the purity than others. In addition, the crystal structure and the bonding state between atoms differ depending on the manufacturing method, which affects the water absorption. Methods for manufacturing silica particles include the VMC method (Vaporized Metal Combustion Method), the water glass method, and the alkoxide method. The VMC method makes it possible to inexpensively manufacture silica particles that satisfy both of the above (a) and (b).
[0009] In the water glass method, the raw materials inevitably contain alkali metals, etc., so it is difficult to satisfy the requirement of (a). Furthermore, in terms of water absorption, while the water absorption is somewhat lower than that of silica particles produced by the alkoxide method, it is difficult to say that the water absorption is sufficiently small. Silica particles produced by the alkoxide method are produced from low molecular weight raw materials, so the raw materials can be easily purified, and in principle there is no need to contain alkali metals, etc., so it is possible to provide products that satisfy the requirement of (a), but the water absorption of (b) is high.
[0010] Although the VMC method can produce silica particles with such excellent properties, we discovered that the coarse particles, which are larger than the desired particle size, include solid particles and hollow particles. We also discovered that the inclusion of hollow particles can prevent the desired performance from being fully achieved when used as a filler, etc.
[0011] Conventionally, when performing precise classification, centrifugation has been widely used because of its high classification efficiency. However, since hollow particles have a low specific gravity, it has been difficult to sufficiently classify and remove them by centrifugation. Since the content of hollow particles is small and even if they remain, their presence has been left unattended, but it has been found that it is preferable for hollow particles to be absent, even if they are small, when applied to fine applications in recent years. For example, when silica particles are applied to fine applications as a filler to be contained in a resin composition, the surface of the resin composition may be scraped by polishing or etching, and in that case, if the hollow particles are scraped, the hollow parts are exposed as unevenness, making it difficult to achieve a smooth surface. Based on such knowledge, a method for removing hollow particles was investigated and the present invention was completed.
[0012] (1) The method for producing silica particles of the present invention, which solves the above-mentioned problems, comprises a raw silica particle production step of producing raw silica particles by dispersing a raw particle material made of metal silicon in a carrier and introducing it into a flame in an oxidizing atmosphere and combusting it to produce raw silica particles, a surface treatment step of surface-treating the raw silica particles with a silane compound to produce surface-treated raw silica particles, and a classification step of centrifuging a dispersion slurry in which the surface-treated raw silica particles are dispersed in a solvent to remove coarse particles, and then removing hollow particles with a filter to produce silica particles.
[0013] Although centrifugal separation, which is a precise and highly efficient method, is used as the classification step, the method is different from the conventional method in that classification using a filter is performed after centrifugation.
[0014] In particular, it is preferable that the (centrifugal field residence time: min) / (classified slurry viscosity: mPa s) in the centrifugation in the classification step is 0.9 or more, and the (centrifugal acceleration: G) / (classified slurry viscosity: mPa s) is 700 or more. The centrifugal field residence time is defined as the residence time (average value on a mass basis) in a centrifugal field having a centrifugal acceleration equal to or greater than the above-mentioned centrifugal acceleration.
[0015] (2) The silica particles of the present invention that solve the above problems have a D50 of 100 nm or more and 200 nm or less as measured by laser diffraction particle size distribution measurement, and a specific surface area of 30 m 2 / g or less, the number of hollow particles of 2 μm or more is 1000 pieces / 0.1 g or less, the water absorption rate is 1.0% or less based on the total mass, and the total amount of alkali metals and alkaline earth metals is 100 ppm or less. It is particularly preferable that the number of hollow particles of 0.8 μm or more is 1000 pieces / 0.1 g or less.
[0016] Specific surface area of 30m 2 By making the content of the polyaniline in the slurry composition or resin composition lower, it is possible to reduce the viscosity when the polyaniline is added to the slurry composition or resin composition. Since the water absorption is low, it is possible to improve the electrical properties.
[0017] Furthermore, it is preferable that the surface of the silica particles is treated with a silane compound as required, since the surface properties of the silica particles can be appropriately controlled by the type of silane compound.
[0018] In this specification, the particle size distribution by laser diffraction method is obtained using a SHIMADZU SALD-7500. The number of hollow particles can be measured using an image analyzer (JASCO International Co., Ltd.: IF3200). The judgment of whether or not a particle is hollow is based on the difference in appearance. Hollow particles are easily distinguishable because they look significantly different from solid particles.
[0019] (3) The slurry composition of the present invention that solves the above-mentioned problems comprises the above-mentioned silica particles of the present invention and a dispersion medium that disperses the silica particles. Effect of the Invention
[0020] The silica particles produced by the production method of the present invention can be used as a filler dispersed in a slurry composition or a resin composition, and can be applied to sealing materials, etc., which have excellent filling properties and excellent stability. The production method of silica particles of the present invention can easily produce the silica particles of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The silica particles, the production method thereof, and the slurry composition of the present invention will be described in detail below with reference to the embodiments.
[0022] (Silica particles) The silica particles of the present embodiment have a D50 of 100 nm or more and 200 nm or less as measured by laser diffraction particle size distribution measurement, and a specific surface area of 30 m 2 / g or less, the number of hollow particles of 2 μm or more is 1000 / 0.1 g or less, the water absorption rate is 1.0% or less based on the total mass, and the total amount of alkali metals and alkaline earth metals is 100 ppm or less.
[0023] As the D50, the lower limit can be 110 nm, 120 nm, and 130 nm, and the upper limit can be 190 nm, 180 nm, and 170 nm. These upper and lower limits can be combined arbitrarily. D50 is a value measured by laser diffraction particle size distribution measurement, and is the particle size that is 50% by volume from the smallest particle size. Incidentally, D100 is the particle size that is 100% from the smallest particle size. Note that the values of D50 and D100 are values calculated as values within the measurement limit range by laser diffraction particle size distribution measurement, and in reality, there are coarse particles and fine particles that cannot be detected by laser diffraction particle size distribution measurement. Therefore, there is no contradiction in the existence of particles with a particle size larger than the value of D100.
[0024] The value of D50 can be adjusted by controlling the particle size distribution of the silica particles themselves produced by controlling the production conditions of the silica particles, and can also be adjusted by classification. As for classification, centrifugation, which will be described later in the production method, can be exemplified as a suitable example.
[0025] The specific surface area is 28m 2 / g or less, 26m 2 / g or less. The specific surface area is a value measured by the BET method using nitrogen. The smaller the specific surface area, the lower the viscosity when used in a slurry composition, etc., and therefore it is preferable. The method for controlling the specific surface area is not particularly limited, but the specific surface area can be reduced by performing a method in which the amount of fine powder is reduced when synthesizing silica, or by controlling the residence time in a classifier to be long when performing classification.
[0026] The number of hollow particles of 2 μm or more can be 800 / 0.1 g or less, 600 / 0.1 g or less, or 400 / 0.1 g or less. The number of hollow particles can be reduced by classification. As a classification operation, removal by a filter is preferable, but it is preferable to first reduce the number of solid particles above the classification point by centrifugation and then remove the hollow particles by a filter.
[0027] The water absorption rate is based on the mass of silica particles when dry. To measure the water absorption rate, a dry sample is left at 40°C and 80% RH for 1 hour, and the water generated by heating to 200°C is measured using a Karl Fischer moisture analyzer, and then the water absorption rate is calculated. To lower the water absorption rate, the VMC method can be used as a manufacturing method for the silica material, or the manufactured silica material can be heated to lower the water absorption rate. Heating temperatures of 200°C or higher, 300°C or higher, or 400°C or higher can be used.
[0028] The total amount of alkali metals and alkaline earth metals is preferably 80 ppm or less, 50 ppm or less, or 30 ppm or less. This can be achieved by purifying the materials used to manufacture silica particles. Since alkali metals and alkaline earth metals are oxidized and eluted or precipitated as ions, unexpected effects on semiconductor devices are expected when they are used as sealing materials for semiconductor devices. For example, assuming the electrical conductivity (EC) of the water extract, it is desirable that it is 10 μS / cm or less. In order to lower this value, it is desirable that the content of alkali metals and alkaline earth metals is low, so the above-mentioned content range is set. EC is measured as follows. Metal oxide particles are suspended in ion-exchanged water (electrical conductivity 1 μS / cm or less) to form a 10% slurry, which is then placed in a pressure-resistant container and shaken at room temperature for 30 minutes. The conductivity is measured by measuring the supernatant liquid, which has been centrifuged and then sedimented, using a conductivity meter (EC meter) ES-51 manufactured by Horiba, Ltd.
[0029] The silica particles of the present embodiment are preferably surface-treated with a silane compound. The silane compound is not particularly limited, and a silane compound having an appropriate functional group can be selected as necessary for surface treatment. Surface treatment can also be performed with two or more types of silane compounds.
[0030] The silica particles of this embodiment can be surface-treated with a silane compound.The specific structure of the silane compound and the method of introducing it to the surface of the silica particles will be described in detail in the method of producing silica particles described later, so the description will be omitted here.In addition, the silica particles that are not surface-treated can also be obtained by removing the surface treatment agent after surface treatment with the surface treatment agent.
[0031] The silica particles of this embodiment have an alpha ray generation rate of 0.001 c / cm 2 In particular, it is desirable that the amount of uranium and thorium as alpha radiation sources be 3 ppb or less (even better, 1 ppb or less).
[0032] (Method of producing silica particles) The method for producing silica particles of the present embodiment includes a raw silica particle production step, a surface treatment step, a classification step, and other steps that are adopted as necessary. The method for producing silica particles of the present embodiment is a method that can suitably produce the silica particles of the present embodiment described above.
[0033] The raw silica particle manufacturing process is a process in which raw silica particles are manufactured by burning raw particle materials. This process is a method known as the VMC method, and the obtained raw silica particles tend to have high sphericity, are dense, and have excellent electrical properties.
[0034] The VMC method is a method in which a chemical flame is formed by burning a combustion enhancer (such as hydrocarbon gas) with a burner in an atmosphere containing oxygen, and raw material particles are introduced into this chemical flame in an amount sufficient to form a dust cloud, causing a deflagration to occur and obtaining raw silica particles.
[0035] The operation of the VMC method can be explained as follows. First, a container is filled with a gas containing oxygen, which is a reactive gas, and a chemical flame is formed in this reactive gas. Next, the raw material particles are put into this chemical flame to form a dust cloud. Then, the chemical flame gives thermal energy to the surface of the raw material particles, raising the surface temperature of the metallic silicon that constitutes the raw material particles, and metallic silicon vapor spreads from the surface of the raw material particles to the surroundings. This vapor reacts with oxygen gas, igniting and generating a flame. The heat generated by this flame further promotes the vaporization of the raw material particles, and the generated vapor and oxygen gas are mixed, causing a chain reaction of ignition and propagation. Therefore, the smaller the particle size of the raw material particles, the larger the specific surface area and the higher the reactivity, which allows less energy to be input.
[0036] As the ignition progresses in this way, the raw material particles themselves are destroyed and scattered, promoting flame propagation. After combustion, the generated gas is naturally cooled, forming a cloud of raw silica particles. The resulting raw silica particles are collected by a bag filter or an electrostatic precipitator.
[0037] The VMC method utilizes the principle of dust explosion. With the VMC method, a large amount of metal oxide particles can be obtained instantly. The obtained metal oxide particles have an almost perfectly spherical shape. It is possible to adjust the particle size distribution of the obtained metal oxide particles by adjusting the particle size, input amount, flame temperature, etc. of the metal particles to be input. In addition to metal particles (metallic silicon) alone, metal oxide particles (e.g., silica) can also be added as the raw material. By using metal oxide particles obtained by this method as the metal oxide particles to be input at the same time, the purity of the obtained metal oxide particles can be maintained.
[0038] The raw material particles may be surface-treated with a silane compound, etc. The type of silane compound that can be used is not particularly limited, and those used in the surface treatment step described below may be used.
[0039] The raw material particles are burned by being dispersed in a carrier and being fed into a flame. There is no particular limit to the speed at which the raw material particles are fed into the flame. As the carrier, a gas such as nitrogen, argon, or air, or a liquid such as water or alcohol can be selected. There is no particular limit to the manner in which the raw material particles are dispersed, but when dispersed in a liquid, it is preferable to spray the raw material particles into the flame in a mist form and feed the liquid. For example, it is preferable to include about 10% to 80% of the raw material particles by volume of the total volume.
[0040] The flame used is a flame in an oxidizing atmosphere. For example, a flame obtained by burning a flammable gas such as LPG in an atmosphere containing excess oxygen. Thermal plasma is also included in the flame category.
[0041] The raw material particles made of metal silicon are fed into the flame, vaporized by combustion, and rapidly cooled to become raw silica particles made of silica. The obtained raw silica particles are collected using a bag filter or the like. Classification can be performed before or after collection to obtain raw silica particles with the required particle size distribution. Classification can be performed using cyclone classification or the like.
[0042] The surface treatment step is a step in which raw silica particles are surface-treated with a silane compound to obtain surface-treated raw silica particles. The surface treatment is performed by directly contacting the surface with a silane compound (either in liquid or gas form) or by contacting the surface with a silane compound dissolved in a solvent. In the surface treatment, the raw silica particles can be heated after contacting the silane compound with the particles. The surface treatment step can also be performed in the form of a slurry after preparing a classification slurry to be used in the classification step described below.
[0043] The amount of the silane compound to be used for the surface treatment is not particularly limited, and can be selected from the amount of 100%, 75%, 50%, 25%, etc. based on the amount of OH groups present on the surface of the raw silica particles. An excessive amount exceeding 100% (120%, 150%, etc.) can also be selected.
[0044] The silane compound is not particularly limited, and examples thereof include those having a phenyl group, an alkyl group, a vinyl group, a methacryl group, an epoxy group, a phenylamino group, an amino group, and a styryl group.
[0045] The classification process is a process for removing particles (coarse particles) having a particle size equal to or larger than a predetermined size from the surface-treated raw silica particles. The coarse particles include solid coarse particles and hollow coarse particles. In the classification process, first, in order to separate the solid coarse particles, a dispersion slurry is prepared by dispersing the surface-treated raw silica particles in a solvent, and then centrifugation is performed. The classified slurry may be prepared after the surface-treated raw silica particles are prepared, or the surface treatment may be performed after the classified slurry is prepared.
[0046] The solvent used for the dispersion slurry in this process is desirably low in viscosity. Examples include methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), and toluene. Solid coarse particles can be separated with high accuracy by centrifuging the mixture dispersed in MEK at a concentration of about 10% by mass to 30% by mass (particularly 15% by mass to 25% by mass).
[0047] Centrifugation is carried out by decantation of the classified slurry in a centrifugal field. The relationship between the physical properties of the classified slurry and the classification conditions can be such that (residence time in centrifugal field: min) / (classified slurry viscosity: mPa·s) is 0.9 or more, preferably 1.4 or more, more preferably 1.8 or more, and (centrifugal acceleration: G) / (classified slurry viscosity: mPa·s) is 700 or more, preferably 900 or more, more preferably 1100 or more. The centrifugal field residence time is defined as the time spent in a centrifugal field with a centrifugal acceleration equal to or greater than the above-mentioned centrifugal acceleration.
[0048] After separating the coarse particles, the dispersed slurry is classified using a filter having a pore size required for separating the hollow coarse particles to remove the hollow coarse particles. The hollow coarse particles cannot be sufficiently separated by centrifugation, but can be sufficiently removed by classification using a filter. The classification using a filter is performed in the state of the dispersed slurry dispersed in a solvent. It is preferable to perform the classification using a filter multiple times. When performing the classification using a filter multiple times, it is preferable to perform the classification using a filter while changing from a filter with a large pore size to a filter with a small pore size.
[0049] (Slurry Composition) The slurry composition of the present embodiment is a mixture of the above-mentioned silica particles and a liquid dispersion medium (solvent, resin material precursor, etc.) The mixing ratio of the silica particles to the dispersion medium is not particularly limited. EXAMPLES
[0050] The silica particles and the method for producing the same of the present invention will be described with reference to examples. (Test Example 1) · Manufacturing raw silica particles Test Example 1: Raw silica particles were produced by the VMC method. The specific explanation is as follows. The reaction vessel has a reaction chamber, a combustor that is installed in the upper part of the reaction vessel and opens into the reaction chamber, a collector that is installed in the lower side wall of the reaction vessel and communicates with the reaction chamber, a hopper, and a powder supplying device that supplies the raw particle material in the hopper to the combustor.
[0051] The combustor is composed of a raw material particle supply passage that opens into the reaction chamber, a combustible gas supply passage that is arranged coaxially with the raw material particle supply passage and opens into the reaction chamber in a ring shape, and an oxygen supply passage that is arranged coaxially outside the combustible gas supply passage and opens into the reaction chamber in a ring shape.
[0052] The collector is composed of an exhaust pipe that opens into the reaction chamber, a bag filter connected to the other end of the exhaust pipe, and a blower, and is used to suck and exhaust the combustion exhaust gas in the reaction chamber by driving the blower, and to collect the raw silica particles that are generated. Note that the inside of the reaction chamber is kept at a negative pressure by the suction of the blower.
[0053] Using the above-mentioned manufacturing apparatus, spherical silica was manufactured by the manufacturing method described below. The raw material particles made of metal silicon were put into a hopper and fed into the reaction chamber together with air as a carrier from the powder feeder. The raw material particles were fed at a rate of 30 kg / hr, and the volume of the conveying air was 30 Nm 3 / hr. In addition, the ignition fuel, flammable gas (LPG), was 10 Nm 3 / hr, and oxygen gas, which is a combustion-supporting gas, is supplied from the oxygen supply line at a rate of 300 Nm 3 / hr.
[0054] The mixed powder fed from the powder feeder to the combustor was ignited by the ignition flame formed by the continuous combustion of combustible gas together with oxygen gas, and burned explosively to generate a flame. This flame extended from the combustor to the reaction chamber, and the generated raw silica particles (volume average particle size: 300 nm) were collected by a collector (raw silica particle production process). The specific surface area of the obtained raw silica particles was 17.8 m 2 / g.
[0055] The raw silica particles were surface-treated with N-phenyl-3-aminopropyltrimethoxysilane as a silane compound to prepare surface-treated raw silica particles (surface treatment step). The amount of the silane compound was 2% based on the weight of the raw silica particles.
[0056] The obtained surface-treated raw silica particles were dispersed in MEK to obtain a dispersion liquid (dispersed slurry) with a solid content concentration of 20 mass %. The viscosity of the dispersed slurry measured with a vibration viscometer was 2 mPa s.
[0057] Next, the coarse particles were precipitated and removed by decantation in a centrifugal field under conditions of a centrifugal acceleration of 1700G and a retention time of 2.8 minutes. (Residence time in centrifugal field: minutes) / (Classified slurry viscosity: mPa·s) was 1.4, and (Centrifugal acceleration: G) / (Classified slurry viscosity: mPa·s) was 850. After that, classification was performed once each using filters with pore sizes of 5μm, 3μm, and 1μm, and hollow coarse particles were removed. After classification, the classified slurry was left to dry for 30 minutes in a dryer at 160°C, and the dried silica particles were used as the test sample for this test example.
[0058] The obtained silica particles had a D50 of 150 nm, a D100 of 270 nm, and a specific surface area of 21.3 m2 as measured by laser diffraction particle size distribution. 2 / g, the number of hollow particles of 2 μm or larger was 104 / 0.1 g, the water absorption rate was 0.08%, and the total amount of alkali metals and alkaline earth metals was 30 ppm or less.
[0059] (Test Example 2) Silica particles were produced as in Test Example 1, except that the silane compound was changed to 3-glycidoxypropyltrimethoxysilane, and used as the test sample for this Test Example. The viscosity of the classified slurry was 1 mPa s. Therefore, (residence time in centrifugal field: min) / (classified slurry viscosity: mPa s) was 2.8, and (centrifugal acceleration: G) / (classified slurry viscosity: mPa s) was 1700.
[0060] The obtained silica particles had a D50 of 200 nm, a D100 of 370 nm, and a specific surface area of 20.3 m2 as measured by laser diffraction particle size distribution. 2 / g, hollow particles of 2 μm or larger were 429 / 0.1 g, the water absorption was 0.08%, and the total amount of alkali metals and alkaline earth metals was 30 ppm or less.
[0061] (Test Example 3) Silica particles were produced as a test sample for this test example in the same manner as in Test Example 1, except that hollow particles were not removed using a filter in the classification step.
[0062] The obtained silica particles had a D50 of 200 nm, a D100 of 370 nm, and a specific surface area of 21.3 m2 as measured by laser diffraction particle size distribution. 2 / g, hollow particles of 2 μm or larger were 9400 / 0.1 g, the water absorption rate was 0.08%, and the total amount of alkali metals and alkaline earth metals was 30 ppm or less.
[0063] (Test Example 4) Silica particles were produced in the same manner as in Test Example 1, except that the MEK used to prepare the classified slurry was changed to cyclohexanone, the centrifugal acceleration was set to 1900G, the centrifugal field residence time was set to 5.5 minutes, and hollow particles were not removed using a filter. The viscosity of the classified slurry was 7 mPa·s. Therefore, (centrifugal field residence time: minutes) / (classified slurry viscosity: mPa·s) was 0.786, and (centrifugal acceleration: G) / (classified slurry viscosity: mPa·s) was 271.4. The reason why hollow particles were not removed using a filter is that under these centrifugal classification conditions, the filter quickly became clogged, and hollow particles could not be sufficiently removed.
[0064] The obtained silica particles had a D50 of 330 nm, a D100 of 590 nm, and a specific surface area of 19.1 m2 as measured by laser diffraction particle size distribution. 2 / g, water absorption was 0.08%, and the total amount of alkali metals and alkaline earth metals was 30 ppm or less. Note that the number of hollow particles of 2 μm or more was not measured because it was too large.
[0065] (Test Example 5) Silica particles were produced in the same manner as in Test Example 1, except that the MEK used to prepare the classified slurry was changed to isopropyl alcohol, the centrifugal acceleration was set to 2500G, the centrifugal field residence time was set to 5.5 minutes, and the hollow particles were not removed using a filter. The viscosity of the classified slurry was 5 mPa·s. Therefore, (residence time in the centrifugal field: minutes) / (classified slurry viscosity: mPa·s) was 1.1, and (centrifugal acceleration: G) / (classified slurry viscosity: mPa·s) was 500. The reason why the hollow particles were not removed using a filter is that, as in Test Example 4, under these centrifugal classification conditions, the filter quickly became clogged, and the hollow particles could not be sufficiently removed.
[0066] The obtained silica particles had a D50 of 160 nm, a D100 of 740 nm, and a specific surface area of 19.8 m2 as measured by laser diffraction particle size distribution. 2 / g, the water absorption was 0.08%, and the total amount of alkali metals and alkaline earth metals was 30 ppm or less.
[0067] (Test Example 6) Colloidal silica (D50 100 nm, D100 210 nm: Cataloid SI-80P: manufactured by JGC Catalysts and Chemicals Co., Ltd., dispersed in water with a solid content of 40% by mass, surface-treated) was used as the raw silica particles, and the silica particles obtained by drying at 160°C for 30 minutes were used as the test sample for this test example.
[0068] The obtained silica particles had a D50 of 100 nm, a D100 of 210 nm, and a specific surface area of 35.6 m2 as measured by laser diffraction particle size distribution. 2 / g, hollow particles of 2 μm or larger were 0 / 0.1 g, water absorption was 1.2%, and the total amount of alkali metals and alkaline earth metals was 3000 ppm or less.
[0069] The results of Test Examples 1 and 3 show that hollow particles cannot be sufficiently removed by centrifugal separation alone. In addition, due to differences in the dispersion medium used when preparing the classified slurry, in Test Example 4 where the (centrifugal field residence time: min) / (classified slurry viscosity: mPa s) was 0.4 and less than 0.9, there was residual coarse particles that made classification using a filter impossible.
[0070] In addition, in Test Examples 4 and 5, in which the (centrifugal acceleration: G) / (classified slurry viscosity: mPa·s) was less than 900, residual coarse particles were observed that made classification using a filter impossible.
[0071] Furthermore, in Test Example 6, in which colloidal silica was used as the raw silica particles, the particle size distribution and the amount of coarse particles (including hollow particles) were completely satisfactory, but the water absorption rate was high at 1.2%, and the total amount of alkali metals and alkaline earth metals was large, so the performance was insufficient for practical use.
Claims
1. D50 measured by laser diffraction particle size distribution measurement is 100 nm or more and 200 nm or less, Specific surface area is 30m 2 / g or less, The number of hollow particles of 0.8 μm or more is 1,000 pieces / 0.1 g or less, Water absorption rate is 1.0% or less based on the total mass. The total amount of alkali metals and alkaline earth metals is 100 ppm or less. Silica particles (excluding surface-modified silica particles having D90 / D10 of 2 or more and D50 of 250 nm or less when integrating the volumes from the smallest particle size, water absorption of 1.0% or less based on the mass when dried, and a total amount of alkali metals and alkaline earth metals of 100 ppm or less, and having carbon-containing functional groups introduced onto the surface).
2. 2. The silica particles according to claim 1, which are surface-treated with a silane compound.
3. The silica particles according to claim 1 or 2, A dispersion medium for dispersing the silica particles; 1. A slurry composition comprising:
4. A method for producing silica particles, comprising the steps of: The silica particles are D50 measured by laser diffraction particle size distribution measurement is 100 nm or more and 200 nm or less, A specific surface area of 30 m 2 / g or less; The number of hollow particles of 2 μm or more is 1,000 pieces / 0.1 g or less, Water absorption rate is 1.0% or less based on the total mass. The total amount of alkali metals and alkaline earth metals is 100 ppm or less. Silica particles that have been surface-treated with a silane compound (excluding surface-modified silica particles having a D90 / D10 of 2 or more and a D50 of 250 nm or less when integrating the volumes from the smallest particle size, a water absorption of 1.0% or less based on the mass when dried, and a total amount of alkali metals and alkaline earth metals of 100 ppm or less, and having a carbon-containing functional group introduced onto the surface), a raw silica particle production step in which a raw particle material made of metal silicon is dispersed in a carrier and then charged into a flame in an oxidizing atmosphere to combust the material, thereby producing raw silica particles; a surface treatment step of surface-treating the raw silica particles with a silane compound to obtain surface-treated raw silica particles; a classification step in which the dispersion slurry in which the surface-treated raw silica particles are dispersed in a solvent is centrifuged to remove coarse particles, and then a classification operation is carried out multiple times using filters having pore sizes ranging from large to small, thereby removing hollow particles to obtain silica particles; having The method for producing silica particles, wherein in the centrifugation in the classification step, (residence time in centrifugal field: min) / (classified slurry viscosity: mPa·s) is 0.9 or more, and (centrifugal acceleration: G) / (classified slurry viscosity: mPa·s) is 700 or more.
Citation Information
Patent Citations
Production of synthetic quartz glass powder and quartz glass formed product
JP1998203821A
Metallic silicon powder and method for manufacturing the same, spherical silica powder, and resin composition
JP2008247726A
Process for producing surface treated silica particle, surface treated silica particle, epoxy resin composition and semiconductor device
JP2010275334A
Spherical silica particles material, silica particles material-containing composition, and method of producing silica particles
JP2014196226A
Method for producing surface-modified silica particle and method for producing filler-containing composition