Grain-oriented electrical steel sheet and its manufacturing method

The insulating film of pseudotetragonal aluminum borate and silica addresses the challenge of stable magnetic domain control and uniform groove widths in grain-oriented electrical steel sheets, achieving reduced iron loss and cost-effectiveness through stable electrolytic etching and precise groove formation.

JP7590674B2Active Publication Date: 2024-11-27NIPPON STEEL CORPORATION
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023505658
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-11
Filing Date
2022-03-11
Publication Date
2024-11-27
Estimated Expiration
2042-03-11

AI Technical Summary

Technical Problem

Existing grain-oriented electrical steel sheets face challenges in achieving stable magnetic domain control with uniform groove widths and reduced iron loss, while maintaining cost-effectiveness due to issues with insulating film resistance and peeling during electrolytic etching.

Method used

The use of an insulating film composed of pseudotetragonal aluminum borate and silica provides excellent chemical resistance to both acidity and alkalinity, allowing stable electrolytic etching and precise groove formation, which is then used as a resist film to refine magnetic domains.

Benefits of technology

This approach results in a grain-oriented electrical steel sheet with minimal groove width fluctuations, maintaining a stable magnetic domain refining effect and reduced iron loss, while also simplifying the manufacturing process and lowering costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590674000002
    Figure 0007590674000002
  • Figure 0007590674000003
    Figure 0007590674000003
  • Figure 0007590674000004
    Figure 0007590674000004
Patent Text Reader

Abstract

This grain-oriented electrical steel sheet has on the surface a finish-annealed coating predominantly composed of forsterite and an insulation coating containing pseudo-tetragonal crystalline aluminum borate and silica, and one or both surfaces of the steel sheet has linear grooves or rows of dot-shaped recesses having a depth of 5-40 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a grain-oriented electrical steel sheet, in particular a grain-oriented electrical steel sheet having low iron loss, and a manufacturing method thereof. This application claims priority based on Japanese Patent Application No. 2021-38990 filed on March 11, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] Grain-oriented electrical steel sheet has a crystal structure with the (110)

[0001] orientation as its main orientation, and usually contains 2% or more by mass of Si. Its main use is as an iron core material for transformers, etc., and there is a particular demand for materials with low energy loss during transformation, i.e., low iron loss.

[0003] The typical manufacturing process for grain-oriented electrical steel sheet is as follows. First, a slab containing 2% to 4% by mass of Si is hot rolled, and the hot-rolled sheet is annealed. Next, it is cold rolled once or at least twice with intermediate annealing to obtain the final sheet thickness, and then decarburization annealing is performed. After this, an annealing separator mainly made of MgO is applied, and finish annealing is performed. This develops a crystal structure with the (110)

[0001] orientation as the main orientation, and forsterite (Mg 2 SiO 4 Finally, a coating solution for forming an insulating film is applied and baked to form an insulating film, and the product is then shipped.

[0004] One method for reducing the iron loss of grain-oriented electrical steel sheets is magnetic domain control technology. When an AC magnetic field is applied to an electrical steel sheet, the direction of the magnetic field changes periodically, but eddy currents are generated within the electrical steel sheet to prevent the change in the direction of the magnetic field. Since these eddy currents increase with the magnetic domain width, they can be reduced by narrowing the magnetic domain width. Various methods have been developed as magnetic domain control technologies. For example, there is a method of subdividing magnetic domains by irradiating the steel sheet surface with a laser, a method of forming grooves in the steel sheet by mechanical loading (scribing, etc.) to subdivide the magnetic domains, and a method of forming exposed steel on the surface of a grain-oriented electrical steel sheet with an insulating coating, and then processing periodic grooves in the steel sheet by electrolytic etching to subdivide the magnetic domains.

[0005] Furthermore, grain-oriented electrical steel sheets have the property that the iron loss is improved by applying tension to the grain-oriented electrical steel sheets. Therefore, increasing the film tension applied to the grain-oriented electrical steel sheets is also effective in reducing iron loss. For example, Al sol obtained by baking a coating solution mainly composed of alumina sol and boric acid is 2 O 3 -B 2 O 3 It is known that the crystalline film of this system has a film tension that is about twice that of a normal film.

[0006] Combining these technologies makes it possible to produce grain-oriented electrical steel sheets with extremely low iron loss, but in actual production, it is also important to reduce costs as much as possible. In particular, when grooves are formed by etching, the application and removal of the resist film is one factor that increases costs. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 2001-316896 [Patent Document 2] Japanese Patent Application Publication No. 2003-301272 [Patent Document 3] Japanese Patent Application Publication No. 2004-269925 [Patent Document 4] International Publication No. 2020 / 085024 [Patent Document 5] Japanese Patent Application Publication No. 2004-099929 Summary of the Invention [Problem to be solved by the invention]

[0008] As described above, various developments have been carried out to reduce the core loss of grain-oriented electrical steel sheets.

[0009] Patent Document 1 discloses a method of using an insulating film formed on the surface of a grain-oriented electrical steel sheet as a resist when forming grooves by electrolytic etching. Specifically, Patent Document 1 proposes removing part of the insulating film of the grain-oriented electrical steel sheet by laser irradiation or the like, electrolytically etching the exposed base metal part, forming grooves, and then applying the insulating film again. The insulating film used as a resist does not need to be removed after the etching process, and can be used as an insulating film as it is. In other words, the manufacturing method of Patent Document 1 is said to improve the work efficiency and reduce costs when manufacturing low-iron-loss grain-oriented electrical steel sheets. However, the manufacturing method of Patent Document 1 does not disclose a specific example of an insulating film that can be used as a resist.

[0010] Patent Document 2 proposes using an insulating film containing colloidal silica and phosphate as main components as a resist film for electrolytic etching. However, as will be described in detail later, the resist film is required to have chemical resistance to both acid and alkali during electrolytic etching. The resist insulating film of Patent Document 2 may not have sufficient resistance to alkali, and peeling and deterioration often occurs during electrolytic etching. Peeling of the insulating film during electrolytic etching is most noticeable near the grooves. When peeling of the insulating film occurs near the grooves, the groove width expands in that area, causing variations in the groove width. Non-uniformity in the groove width results in insufficient magnetic domain refinement effect, as will be described later. Therefore, the resist film is also required to have further improved chemical resistance to acid and alkali.

[0011] Patent Document 3 aims to provide an insulating film that does not deteriorate even when subjected to electrolytic etching and has the performance required for an insulating film of grain-oriented electrical steel sheet, such as insulation, ability to impart tension to the steel sheet, and corrosion resistance, and proposes baking a coating liquid containing phosphate and colloidal silica as a means of solving this problem. Specifically, it discloses that the performance of the insulating film can be improved by controlling the baking temperature, for example, that the film tension can be increased by setting the baking temperature to a relatively high temperature of 600 to 900°C, and that the film resistance (resist resistance) can be increased by setting the baking temperature to a relatively low temperature of 400 to 600°C. However, as will be described later, with an insulating coating whose main components are colloidal silica and phosphate, it is difficult to simultaneously increase both the film tension and the film resistance (resist resistance); rather, increasing one decreases the other, creating a so-called trade-off relationship.

[0012] Patent Document 4 does not mention or suggest electrolytic etching, but it does disclose an insulating film for grain-oriented electrical steel sheets that has high film tension and excellent corrosion resistance. Specifically, Patent Document 4 proposes coating an insulating film coating solution containing aluminum-containing hydrated silicate particles and boric acid on an electrical steel sheet, and baking the coating at 600 to 1000°C, and claims that film properties with high film tension and excellent corrosion resistance can be obtained without using a chromium compound. Note that the corrosion resistance here refers to the corrosion resistance of the baked insulating film against a neutral NaCl solution, and is not the resistance of the insulating film as a resist film in electrolytic etching. As described above, Patent Document 4 does not describe or suggest electrolytic etching of an insulating film, and the film resistance (resistance) when electrolytic etching is performed is unknown.

[0013] Patent Document 5 describes that after forming a forsterite finish annealing film and an insulating film containing aluminum borate, a low iron loss effect can be obtained by applying tension to a steel sheet by introducing a point-array of localized distortion or grooves by laser irradiation. However, the publication does not describe a specific method for forming the grooves, and it is unclear whether a groove formation method by electrolytic etching is possible.

[0014] In view of the above circumstances, an object of the present invention is to provide a grain-oriented electrical steel sheet which is low cost and has little variation in groove width, and as a result has a stable magnetic domain control effect, and a manufacturing method thereof. [Means for solving the problem]

[0015] The gist of the present invention is to form an insulating coating containing pseudo-tetragonal aluminum borate and silica as an insulating coating for grain-oriented electrical steel sheet, and to use this insulating coating also as a resist coating during electrolytic etching. The insulating film has excellent chemical resistance not only to acids but also to alkalis, and is unlikely to peel off during electrolytic etching. As a result, it is possible to form grooves with little variation in width and dot-like dents with little variation in hole diameter, achieving a magnetic domain refinement effect, i.e., low iron loss. Furthermore, these grooves and dot-like dents do not disappear even after subsequent stress relief annealing, so the magnetic domain refinement effect does not disappear either. Furthermore, the coating containing pseudotetragonal aluminum borate and silica can be used not only as a resist film but also as an insulating coating as it is, which simplifies the process, improves work efficiency, and ultimately reduces costs. In addition, the coating can impart high coating tension to the electrical steel sheet, thereby further promoting low iron loss.

[0016] The present invention provides the following aspects as means for solving the problems. (1) A grain-oriented electrical steel sheet having, on its surface, a finish annealing coating mainly composed of forsterite and an insulating coating containing pseudo-tetragonal aluminum borate and silica, characterized in that one or both surfaces of the steel sheet have linear grooves or dot-like depressions having a depth of 5 to 40 μm. (2) A method for producing grain-oriented electrical steel sheet, comprising the steps of: applying and baking a coating liquid containing aluminum-containing hydrous silicate particles and boric acid to a grain-oriented electrical steel sheet after finish annealing to form an insulating coating; removing a linear or dotted portion of the insulating coating on one or both sides to expose the base steel; and then forming linear grooves or dotted depressions having a depth of 5 to 40 μm by electrolytic etching. Effect of the Invention

[0017] The coating containing pseudotetragonal aluminum borate and silica provided on the grain-oriented electrical steel sheet according to one embodiment of the present invention is also used as a resist coating, and has excellent chemical resistance not only to acids but also to alkalis, so that the coating is less likely to peel off during electrolytic etching, allowing stable etching and a high product yield. In addition, such stable etching allows precise groove processing in the electromagnetic steel sheet, realizing the magnetic domain refinement effect, i.e., low iron loss. Furthermore, since the grooves do not disappear even after subsequent stress relief annealing, the magnetic domain refinement effect does not disappear either. Furthermore, the film can be used not only as a resist film but also as an insulating film as it is, which simplifies the manufacturing process, thereby improving work efficiency and achieving cost reduction. In addition, the coating, as an insulating coating, can impart high coating tension to the electrical steel sheet, thereby further promoting low iron loss. Therefore, according to the present invention, it is possible to provide a grain-oriented electrical steel sheet which is low in cost and has little variation in groove width, and as a result has a stable magnetic domain control effect, and a manufacturing method thereof. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic diagram illustrating direct and indirect current conduction in electrolytic etching. [Diagram 2] FIG. 2 is a graph showing the relationship between the baking temperature and the properties of the insulating coating (electrolysis current and coating tension) for grain-oriented electrical steel sheets provided with an insulating coating according to the prior art. [Diagram 3] FIG. 3 is a graph showing the relationship between the baking temperature and the film properties (electrolysis current and film tension) for a grain-oriented electrical steel sheet according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] A typical manufacturing process for grain-oriented electrical steel sheet is as follows, and unless there are any particular inconsistencies, the conventional manufacturing process can be applied to the grain-oriented electrical steel sheet according to this embodiment. First, a slab containing 2% to 4% by mass of Si is hot rolled, and the hot-rolled sheet is annealed. Next, the sheet is cold rolled once or at least twice with intermediate annealing to obtain the final sheet thickness, and then decarburization annealing is performed. After this, an annealing separator mainly composed of MgO is applied, and finish annealing is performed. This develops a crystal structure with the (110)

[0001] orientation as the main orientation, and forsterite (Mg 2 SiO 4 ) is formed on the surface of the finish annealed film. Next, a coating liquid for forming an insulating film (also referred to herein as a coating liquid for forming an insulating film or a coating liquid) is applied and baked to form an insulating film on the surface of the finish annealed film. Thereafter, the grain-oriented electrical steel sheet on which the insulating film has been formed is shipped.

[0020] According to one embodiment of the present invention, the grain-oriented electrical steel sheet has The steel has a finish annealing film mainly composed of forsterite on its surface, and an insulating film containing pseudotetragonal aluminum borate and silica; and The steel plate is characterized in that it has linear grooves with a depth of 5 to 40 μm and little variation in groove width, or dot-like depressions with little variation in diameter, on one or both surfaces.

[0021] The final annealed coating mainly composed of forsterite is obtained by applying an annealing separator containing MgO to the surface of a steel sheet (decarburized annealed sheet) and then performing final annealing. The MgO in the annealing separator and the Si in the steel sheet are oxidized during decarburization annealing to form SiO 2 The internal oxide layer reacts to form forsterite (Mg 2 SiO 4 If the amount of MgO in the annealing separator is insufficient, the forsterite (Mg 2 SiO 4 ) may not be generated sufficiently, so the MgO content of the annealing separator may be 50 mass % or more.

[0022] The insulating coating containing pseudo-tetragonal aluminum borate and silica is obtained by applying a coating liquid containing aluminum-containing hydrous silicate particles and boric acid to a steel sheet having the above-mentioned finish annealing coating, and baking the coating liquid. Therefore, this insulating coating is composed of pseudo-tetragonal aluminum borate xAl, which is generated by the reaction of the Al component in the hydrous silicate particles with boric acid. 2 0 3 ·yB 2 O 3 and amorphous components such as silica resulting from the remaining components other than Al in the hydrous silicate particles. An insulating coating containing pseudo-tetragonal aluminum borate and silica has excellent coating tension and excellent corrosion resistance. This is believed to be because the crystals of pseudo-tetragonal aluminum borate generate excellent coating tension, and the structure in which the amorphous layer of silica or the like surrounds the crystalline phase results in excellent corrosion resistance.

[0023] Here, excellent film tension and corrosion resistance may be equivalent to or greater than those of conventional insulating films, particularly insulating films using a coating solution containing a chromium compound that has been widely used in the past. For reference, an insulating film using a coating solution containing a chromium compound has a film tension of approximately 8 MPa and a corrosion resistance of 0%. In the insulating film according to the present embodiment, the film tension may be 5 MPa or more, preferably 8 MPa or more, and more preferably 10 MPa or more, taking into account an acceptable likelihood. The corrosion resistance may be 10% or less, preferably 5% or less, and more preferably 1% or less, or may be 0%. The method for evaluating the corrosion resistance will be described later. The detailed conditions for obtaining the insulating coating, such as the composition of the coating solution and the baking temperature, will be described later.

[0024] In addition, the insulating film according to this embodiment has excellent resist resistance in electrolytic etching, and therefore can be used as a resist film. Specifically, the insulating film has excellent chemical resistance not only to acids but also to alkalis, and is unlikely to dissolve or peel off during electrolytic etching. As a result, the variation in groove width and the variation in dent diameter after etching are small.

[0025] Here, the reason why electrolytic etching requires chemical resistance not only to acid but also to alkali will be explained with reference to FIG. 1. In electrolytic etching, the object to be etched (steel sheet) is immersed in an electrolyte and current is passed through the object to be etched (steel sheet) to electrically dissolve the object to be etched (steel sheet). Generally, in practical manufacturing scale, steel sheets are continuously processed in consideration of productivity. In continuous processing, if the steel sheet is not coated with an insulating film, direct current is possible, as shown on the left of FIG. 1, in which one electrode is brought into contact with the steel sheet S via a conductor roll 2 outside the electrolyte tank 1 and the other electrode 3 is placed in the electrolyte tank 1. However, in the case of a steel sheet coated with an insulating film, direct current cannot be passed through a conductor roll, so indirect current is adopted as shown on the right of FIG. 1. In indirect current, both electrodes 3A and 3B are placed in the electrolyte tank 1, and the surrounding liquid property changes depending on the electrodes 3A and 3B. Specifically, the anode 3A side becomes acidic, and the cathode 3B side becomes alkaline. Therefore, the object to be etched (steel sheet), and in particular the resist material, must have chemical resistance to both acids and alkalis.

[0026] Conventional insulating films (resist films) mainly composed of colloidal silica and phosphates, as seen in, for example, Patent Documents 2 and 3, do not have sufficient resistance to alkali and often dissolve and peel off during electrolytic etching. If the resist film is easily peeled off, the peeling of the resist film occurs more prominently near the grooves, resulting in significant variations in the groove width and the depression diameter. As a result, it becomes difficult to achieve the desired magnetic domain refining effect, i.e., low iron loss, and the product yield also decreases.

[0027] In contrast, the insulating coating according to the present embodiment has excellent chemical resistance not only to acids but also to alkalis, and is less likely to peel off during electrolytic etching. Therefore, electrolytic etching can be performed stably, and product yield can be increased. Furthermore, such stable electrolytic etching allows precise groove processing or dot-like dimple processing to be performed on the electromagnetic steel sheet, achieving a magnetic domain refinement effect, i.e., low iron loss. Note that these grooves and dot-like dimples do not disappear even after subsequent stress relief annealing, and therefore the magnetic domain refinement effect does not disappear either.

[0028] The following method may be used to quantitatively evaluate the chemical resistance of the insulating film as a resist film against acids and alkalis. That is, this method involves immersing a certain area of ​​the resist film, which is a portion where the base steel is not exposed, in an electrolyte, and observing the time-dependent change in current when electrolytic treatment is performed at a constant voltage. As an example, an electrical steel sheet on which an insulating film (resist film) is formed is cut to 55 mm x 150 mm, covered with vinyl adhesive tape so that a 20 mm x 20 mm resist film portion is exposed, and in a 10% NaCl solution, the exposed portion where the resist film portion is exposed is placed facing a platinum-plated Ti plate counter electrode, the distance between the electrodes is set to 40 mm, a voltage of 10 V is applied between the electrodes to perform electrolysis, and the time-dependent change in the current density flowing between the electrodes is measured. The less current flows when a voltage is applied to start electrolysis, the less likely it is to peel off, i.e., the higher the chemical resistance. The amount of insulating film formed after baking is about 4.5 g / m 2 When the current density is 0.5 A / cm 20 seconds after voltage application, 2 If the current density is less than 0.2 A / cm, the resist film portion can be evaluated as a stable region where the insulating film is not peeled off. The lower the current density, the higher the chemical resistance. Therefore, the current density is preferably 0.2 A / cm. 2 Less than 0.1 A / cm, more preferably 0.1 A / cm 2 It may be the following.

[0029] One or both surfaces of the grain-oriented electrical steel sheet according to this embodiment have linear grooves or dot-like depressions with a depth of 5 to 40 μm.

[0030] The presence of these linear grooves or depressions subdivides the magnetic domains of the magnetic steel sheet, realizing low iron loss. These linear grooves or depressions can be obtained by the following procedure. That is, the insulating film baked on one or both surfaces of the steel sheet is partially removed in a continuous line shape or a discontinuous dotted pattern. As a means for partially removing the insulating film, for example, laser irradiation described in Patent Documents 1 to 3 can be used, but other means that can achieve similar results may also be used. In the subsequent electrolytic etching process, the grooves or depressions are processed in the shape of the removed insulating film. This shape has a significant effect on the magnetic properties. The depth of the grooves or depressions, which are the removed parts of the insulating film, is 5 to 40 μm. If the depth of the grooves or depressions is less than 5 μm, the magnetic domain subdivision effect is insufficient, and if it exceeds 40 μm, the magnetic flux density drops significantly. Here, unless otherwise specified, the starting point of the depth is the base metal surface of the steel sheet, and the distance from the starting point toward the inside of the steel sheet (thickness direction) is referred to as the depth. For example, a depth of 5 μm refers to a distance of 5 μm from the base metal surface of the steel sheet toward the inside of the steel sheet (thickness direction). The depth of the groove or depression may be 22 mm or more, or may be 22 mm or less.

[0031] The shape of the grooves or depressions can be adjusted as appropriate depending on the desired effect of magnetic domain subdivision. In one embodiment, the width of the grooves may be 50 μm or more, or 150 μm or more. The width of the grooves may be 400 μm or less, or 150 μm or less. The spacing between the grooves may be, for example, 2 mm or more, or 3 mm or more. The spacing between the grooves may be, for example, 8 mm or less, or 3 mm or less. In the case of a dot sequence shape, the diameter of the dots may be, for example, 50 μm or more, or may be 150 μm or more. The diameter of the dots may be, for example, 400 μm or less, or may be 150 μm or less. The center-to-center distance between adjacent dots may be, for example, 50 μm or more, or may be 300 μm or more. The center-to-center distance between adjacent dots may be 1000 μm or less, or may be 300 μm or less. The row interval may be, for example, 2 mm or more, or may be 3 mm or more. The row interval may be, for example, 8 mm or less, or may be 3 mm or less. The direction of the line or dot sequence may be 45° to 90° from the rolling direction. The variations in groove width and dimple diameter are important, and in order to obtain an effective magnetic control effect, it is desirable to keep the standard deviation of the groove width and dimple diameter within ±20% in both the grooves and the point-array dimples, and more preferably within ±10%.

[0032] The depth of the grooves and depressions can be controlled by the current density and time during electrolytic etching. The etching speed can also be controlled by changing the current density. Therefore, even if the line speed changes due to the equipment conditions, it can be easily accommodated.

[0033] If the current density is too high, it will cause significant damage to the insulating film and the equipment will become large-scale, so a current density of 0.6 A / cm per steel sheet area is recommended. 2 (60A / dm 2 ) or less. If the current density is too small, the current efficiency will decrease, but as mentioned above, this is not a particular limitation from the viewpoint of responding to the conditions of the equipment. The electrolyte for electrolytic etching is preferably NaCl or NaNO because it is easy to process. 3 , Na 2 SO 4 As described above, since the steel sheet has an insulating film (resist film) applied thereto, the electric current is applied by the indirect electric current method.

[0034] On the surface of the steel sheet obtained by electrolytic etching, the base steel is exposed in grooves or depressions, so if necessary, an insulating film or anticorrosive film may be applied again to the entire surface of the steel sheet. At this time, SiO 2 Since the coating can be easily applied by precipitation of silicate, the steel sheet may be electrolytically treated in an aqueous silicate solution.

[0035] The manufacturing conditions of the insulating film (resist film) according to one embodiment will be described in detail. The insulating film is obtained by applying a coating liquid for forming an insulating film to a grain-oriented electrical steel sheet having a finish annealed film after finish annealing, and then performing a baking process.

[0036] <Coating solution for forming insulating film for grain-oriented electrical steel sheets> The coating liquid for forming the insulating film for grain-oriented electrical steel sheet according to this embodiment contains aluminum-containing hydrous silicate particles and boric acid, that is, the insulating film disclosed in Patent Document 4 is utilized.

[0037] Hereinafter, each material constituting the coating liquid according to this embodiment will be described.

[0038] (hydrated silicate particles) The coating liquid for forming an insulating film contains hydrous silicate particles. The hydrous silicate particles may be of one type or of two or more types. Hydrous silicates, also known as clay minerals, often have a layered structure. 2-3 S 2 O 5 (OH) 4 and the 1:1 silicate layer represented by the formula X 2-3 (Si,Al) 4 O 10 (OH) 2 (X is Al, Mg, Fe, etc.) and 2:1 silicate layers are laminated, either alone or in combination. At least one of water molecules and ions may be contained between the layers of the layered structure.

[0039] Representative examples of hydrous silicates include kaolin (or kaolinite) (Al 2 S 2 O 5 (OH) 4 ), Talc(Mg 3 S 4 O 10 (OH) 2 ), pyrophyllite (Al 2 S 4 O 10 (OH) 2 ) can be mentioned. Most of the hydrous silicate particles are made by purifying and pulverizing naturally occurring hydrous silicate. From the viewpoint of industrial availability, it is preferable to use at least one type of particle selected from the group consisting of kaolin, talc, and pyrophyllite as the hydrous silicate particles. Also, from the viewpoint of obtaining excellent film tension, excellent corrosion resistance, and excellent chemical resistance (chemical resistance to not only acid but also alkali as a resist film), hydrous silicate particles containing aluminum are used. Hydrous silicate particles containing aluminum have excellent reactivity with boric acid, generate pseudotetragonal aluminum borate and silica, and obtain excellent film tension, excellent corrosion resistance, and excellent chemical resistance. From that viewpoint, it is preferable to use at least one type of particle of kaolin and pyrophyllite as the hydrous silicate particles, and it is more preferable to use kaolin. Hydrous silicate particles may be used in combination.

[0040] The larger the specific surface area of ​​the hydrous silicate particles, the more easily the reaction between the hydrous silicate particles and boric acid is promoted. 2 / g or more, and 2 / g or more is more preferable, and 50m 2 It is more preferable that the molecular weight is 1 / g or more. On the other hand, the upper limit of the specific surface area is not particularly limited. For example, 2 / g or less, and 2 / g or less, and 2 / g or less. When the upper limit of the specific surface area is the above-mentioned or less, the dispersion stability (viscosity stability) of the coating liquid for forming the insulating coating film is easily maintained. The specific surface area of ​​the hydrous silicate particles is a specific surface area based on the BET method, and is measured by a method conforming to JIS Z 8830:2013.

[0041] (Specific surface area 20m 2 / g or more of hydrous silicate particles) Hydrous silicate particles commercially available for industrial use have a specific surface area of ​​20 m 2 It is difficult to obtain a material with a specific surface area of ​​20 m2 or more. 2 / g or more.

[0042] As a means for pulverizing the hydrous silicate particles, a ball mill, a vibration mill, a bead mill, a jet mill, etc. are effective. The pulverization process may be a dry pulverization in which the hydrous silicate particles are pulverized as powder, or a wet pulverization in which the hydrous silicate particles are dispersed in a dispersion medium such as water or alcohol and pulverized in a slurry state. The pulverization process may be either a dry pulverization or a wet pulverization process. The specific surface area of ​​the hydrous silicate particles increases with the pulverization time, regardless of the pulverization method used. Therefore, by controlling the pulverization time, hydrous silicate particles and their dispersion liquid having a required specific surface area can be obtained.

[0043] The shape of the hydrous silicate particles is not particularly limited, but may be plate-like particles. This is because the hydrous silicate particles often have a layered structure, that is, a structure in which multiple layers are stacked. The crushing process causes peeling between the layers of the hydrous silicate particles. In other words, the crushing process reduces the thickness of the plate-like hydrous silicate particles. The thinner the thickness, the more easily the reaction with boric acid is promoted. Therefore, the thickness of the hydrous silicate particles (plate-like particles) is preferably 0.1 μm or less, more preferably 0.05 μm or less, and even more preferably 0.02 μm or less. On the other hand, the lower limit of the thickness of the hydrous silicate particles (plate-like particles) is not particularly limited, but if the thickness is too small, when suspended in water, the particle surface is activated and the viscosity of the suspension increases. Therefore, the thickness of the hydrous silicate particles may be 0.001 μm or more, preferably 0.002 μm or more, and more preferably 0.005 μm or more. The thickness of the hydrous silicate particles (plate-like particles) can be determined by analyzing images of the shape of the hydrous silicate particles obtained by a scanning electron microscope or a transmission electron microscope.

[0044] In the case of wet grinding, the viscosity of the dispersion increases as the specific surface area of ​​the hydrous silicate particles increases. 2 If the amount of the dispersion is increased to more than 1 / g, the viscosity of the dispersion increases and gelation may occur, which may cause problems in the grinding process. Therefore, a dispersant may be added to the dispersion as necessary.

[0045] The increase in viscosity during the grinding process can be suppressed by adding a dispersant. However, among dispersants, if an organic dispersant is added, it may decompose and carbonize during baking of the insulating film, causing carburization in the oriented electrical steel sheet, so when a dispersant is used, an inorganic dispersant is preferred. Examples of inorganic dispersants include polyphosphates and water glass. Specific examples of the former dispersants include sodium diphosphate and sodium hexametaphosphate. Specific examples of the latter dispersants include sodium silicate and potassium silicate. The amount of these dispersants added is preferably 20% by mass or less based on the total mass of the hydrous silicate particles. By keeping the amount of inorganic dispersants added at 20% by mass or less, changes in the composition of the insulating coating after baking are suppressed, making it easier to obtain higher coating tension, higher corrosion resistance, and higher chemical resistance. Since the dispersant is an optional component, the lower limit of the dispersant is not particularly limited and may be 0%. In other words, the coating liquid may not contain a dispersant such as polyphosphate or water glass. In the case of dry grinding, it is not necessary to add a dispersant during grinding.

[0046] (boric acid) The boric acid may be one obtained by a known method, and may be either orthoboric acid or metaboric acid. The boric acid is preferably orthoboric acid. The boric acid may be particulate boric acid or may be boric acid dissolved or dispersed in water.

[0047] (Ratio of hydrous silicate particles to boric acid) The content ratio of the hydrous silicate particles and boric acid contained in the coating solution for forming an insulating film is not particularly limited as a B (boron) / Al (aluminum) molar ratio. Incidentally, boric acid and boric acid salts have a relatively low solubility in water. Therefore, if the B / Al molar ratio is too large, the coating solution concentration must be reduced, making it difficult to obtain the desired amount of insulating film. Therefore, it is preferable to set the B / Al molar ratio to 1.5 or less, preferably 1.3 or less, and more preferably 1.0 or less. The lower limit of the B / Al molar ratio is not particularly limited, and the B / Al molar ratio may be 0.05 or more, or may be 0.1 or more. From the viewpoint of obtaining excellent coating tension, excellent corrosion resistance, and excellent chemical resistance, it is preferable that the B / Al molar ratio is 0.2 or more. Therefore, the content ratio of the hydrous silicate particles and boric acid is preferably 0.2 to 1.5 as a B (boron) / Al (aluminum) molar ratio.

[0048] (Dispersion medium (or solvent)) As the dispersion medium or solvent used in the coating solution for forming the insulating film, in addition to water, for example, alcohols such as ethyl alcohol, methyl alcohol, and propyl alcohol can be used. It is preferable to use water as the dispersion medium or solvent from the viewpoint of non-flammability.

[0049] The solid content concentration of the coating liquid for forming an insulating film is not particularly limited as long as it is within a range that allows application to a grain-oriented electrical steel sheet. The solid content concentration of the coating liquid for forming an insulating film may be, for example, 5% by mass or more, and preferably 10% by mass or more. The solid content concentration of the coating liquid for forming an insulating film may be, for example, 50% by mass or less, and preferably 30% by mass or less.

[0050] Furthermore, the coating liquid for forming an insulating film may contain a small amount of other additives, or may not contain other additives, as necessary, within a range that does not impair the film tension, corrosion resistance, and chemical resistance properties. In other words, the content of other additives may be 0 mass%. When a small amount of other additives is contained, it is preferable that the content is 3 mass% or less, and preferably 1 mass% or less, based on the total solid content of the coating liquid for forming an insulating film. An example of the other additives is a surfactant that prevents the coating liquid from being repelled on the steel sheet.

[0051] From the viewpoint of workability during application, the viscosity of the coating liquid for forming the insulating coating should be 1 mPa·s to 100 mPa·s. If the viscosity is too high, it becomes difficult to apply, and if the viscosity is too low, the coating liquid may flow, making it difficult to obtain the desired amount of insulating coating. Measurements are performed using a B-type viscometer (Brookfield viscometer). The measurement temperature is 25°C.

[0052] From the viewpoint of the working environment, it is preferable that the coating solution for forming the insulating film does not contain hexavalent chromium. In order to obtain an insulating film having high tension, high corrosion resistance, and excellent chemical resistance not only to acids but also to alkalis during etching, the coating liquid for forming the insulating film according to this embodiment is preferably baked at a high temperature, for example, 600°C or higher. If the coating liquid for forming the insulating film contains a resin, the resin will decompose during baking and carburize the steel sheet. As a result, the magnetic properties of the grain-oriented electrical steel sheet will deteriorate. From this perspective, it is preferable that the coating liquid for forming the insulating film does not contain organic components such as resin.

[0053] Here, the coating liquid for forming the insulating film described above can impart tension to the steel sheet by forming a film by baking. Therefore, the coating liquid for forming the insulating film described above is suitable as a coating liquid for forming an insulating film of a directional electrical steel sheet. The coating liquid for forming the insulating film described above can also be applied to a non-directional electrical steel sheet. However, even if the coating liquid for forming the insulating film described above is applied to a non-directional electrical steel sheet, the insulating film does not essentially contain an organic component, and there is no effect of improving the punchability of the steel sheet. Therefore, there is little benefit in applying it to a non-directional electrical steel sheet.

[0054] (Method of preparing coating solution) The coating solution for forming an insulating film may be prepared by mixing and stirring hydrous silicate particles and boric acid together with a dispersion medium (solvent). The order of adding the hydrous silicate particles and boric acid is not particularly limited. For example, a dispersion liquid may be prepared by dispersing a predetermined amount of hydrous silicate particles in water as a dispersion medium, and then a predetermined amount of boric acid may be added and mixed and stirred. Alternatively, a boric acid aqueous solution may be prepared by dissolving a predetermined amount of boric acid in water as a solvent, and then a predetermined amount of hydrous silicate particles may be added to the boric acid aqueous solution and mixed and stirred. If necessary, other additives may be added and mixed and stirred.The coating liquid for forming an insulating film may then be adjusted to a desired solid content concentration.The temperature of the coating liquid may be heated (e.g., 50°C) or may be at room temperature (e.g., 25°C).

[0055] (Analysis of coating solution components) In the coating solution for forming an insulating coating, the B / Al molar ratio can be measured as follows. A coating solution in which hydrous silicate particles and boric acid are mixed together hardly react with each other at temperatures below 100° C. Therefore, a coating solution at temperatures below 100° C. is in a slurry state in which, for example, hydrous silicate particles are dispersed in an aqueous solution of boric acid. Specifically, first, the coating solution for forming the insulating film is filtered. By filtering, the coating solution is separated into a filtrate containing an aqueous solution of boric acid derived from the boric acid before mixing, and a residue containing hydrous silicate derived from the hydrous silicate particles. Next, the amount of boric acid is determined by subjecting the filtrate to ICP-AES analysis (inductively coupled plasma-atomic emission spectroscopy). The amount of hydrous silicate is also determined from the weight of the residue, and the aluminum concentration in the hydrous silicate is determined by further subjecting the residue to X-ray fluorescence analysis. By summarizing the above results, the molar ratio of boron to aluminum (B / Al) in the coating solution is determined. Furthermore, the specific surface area of ​​the hydrous silicate particles is measured by dispersing the hydrous silicate particles separated above in a solvent in which the hydrous silicate particles are not dissolved. The specific surface area is then measured by the BET method described above. The thickness of the hydrous silicate particles (plate-like particles) is measured by observation using the electron microscope described above.

[0056] (Application and baking of coating solution for forming insulating film) A coating solution for forming an insulating film is applied to the grain-oriented electrical steel sheet after the final annealing, and then a baking process is performed. The amount of coating is not particularly limited. From the viewpoint of obtaining excellent film tension, excellent corrosion resistance, and excellent chemical resistance, it is preferable that the amount of the insulating film after the insulating film formation is 1 g / m 2 ~10g / m 2 It is preferable to apply the coating solution so that the amount of the insulating film after the insulating film formation is in the range of 2 g / m. 2 ~8g / m 2 The coating amount (amount of insulating film) after baking treatment can be determined from the difference in weight before and after peeling off the insulating film. Here, in the insulating coating according to this embodiment, taking into account the allowable likelihood, the coating tension may be 5 MPa or more, preferably 8 MPa or more, and more preferably 10 MPa or more. The corrosion resistance may be 10% or less, preferably 5% or less, and more preferably 1% or less, or may be 0%. An index of excellent chemical resistance is a current density of 0.5 A / cm2 20 seconds after voltage application under specified conditions. 2 Less than or equal to 0.2 A / cm 2 Less than 0.1 A / cm, more preferably 0.1 A / cm 2 The following may be used:

[0057] The method for applying the coating liquid for forming an insulating film to the grain-oriented electrical steel sheet after the finish annealing is not particularly limited, and examples thereof include coating methods using a roll coating method, a spray coating method, a dip coating method, and the like.

[0058] The coating liquid for forming the insulating film is applied to the surface of the steel sheet after the finish annealing, and then baking is performed. The reaction between the hydrous silicate particles and boric acid is promoted in order to form a dense insulating film and obtain excellent film tension, excellent corrosion resistance, and excellent chemical resistance. Many hydrous silicates release structural water at a heating temperature of about 550°C and react with boric acid in the process. If the baking temperature is less than 600°C, the reaction between the hydrous silicate particles and boric acid is not sufficient. Therefore, the insulating film is formed in which the hydrous silicate particles and boric acid are mixed. Therefore, the baking temperature may be 600°C or higher. The baking temperature is preferably 700°C or higher, and may be 800°C or higher. On the other hand, if a baking temperature of more than 1000°C is adopted, the grain-oriented electrical steel sheet softens and becomes more susceptible to distortion, so the baking temperature may be 1000°C or lower. The baking temperature is preferably 950° C. or less, more preferably 900° C. or less, and may be 850° C. or less, or may be 800° C. or less. The baking time may be, for example, 5 seconds or more, preferably 10 seconds or more. Also, the baking time may be 300 seconds or less, preferably 120 seconds or less.

[0059] The heating method for carrying out the baking treatment is not particularly limited, and examples thereof include a radiant oven, a hot air oven, and induction heating.

[0060] The insulating film formed on the surface of the steel sheet after baking is preferably a dense insulating film from the viewpoint of obtaining excellent film tension, excellent corrosion resistance, and excellent chemical resistance. From this viewpoint, the thickness of the insulating film is preferably 0.5 μm or more, more preferably 1 μm or more. Moreover, the thickness of the insulating film is preferably 5 μm or less, more preferably 4 μm or less. The thickness of the insulating coating after baking can be determined by cross-sectional SEM observation.

[0061] The denseness can be evaluated by the porosity in the insulating coating. If a large amount of voids are present in the insulating coating, the insulating coating is considered to have low coating tension, inferior corrosion resistance, and low chemical resistance. In the insulating coating of the grain-oriented electrical steel sheet according to this embodiment, the porosity may be 10% or less, preferably 5% or less, further preferably 3% or less, more preferably 2% or less, and particularly preferably 1% or less.

[0062] Through the above steps, a grain-oriented electrical steel sheet having excellent properties such as film tension, corrosion resistance, and chemical resistance can be obtained by using the coating liquid for forming the insulating film described above. Furthermore, the grain-oriented electrical steel sheet provided with the insulating film using the coating liquid for forming the insulating film described above also has excellent magnetic properties and an excellent space factor.

[0063] When evaluating the coating characteristics, corrosion resistance, magnetic properties, and porosity of the insulating coating of grain-oriented electrical steel sheets, the evaluation methods for each evaluation are as follows.

[0064] (Corrosion resistance) While kept at 35°C, a 5 mass % NaCl aqueous solution is continuously sprayed onto a grain-oriented electrical steel sheet specimen of 60 mm x 100 mm, and the occurrence of rust is observed after 48 hours, and the area ratio is calculated.

[0065] (film tension) The film tension is calculated from the warping of the steel sheet that occurs when the insulating film is formed on only one side. The film tension is calculated from the warp of the grain-oriented electrical steel sheet using the following formula. Formula: Film tension = 190 x plate thickness (mm) x plate warp (mm) / {plate length (mm)} 2 [MPa]

[0066] (chemical resistance) In order to quantitatively evaluate the chemical resistance of the insulating film as a resist film against acids and alkalis, the current density may be measured by the following method. That is, a resist film portion of a certain area, which is a portion where the base steel is not exposed, is immersed in an electrolyte, and electrolytic treatment is performed at a constant voltage, and the change in current over time is observed. For example, when an insulating film (resist film) is formed with a film formation amount of about 4.5 g / m, the current density is measured by the following method. 2 The grain-oriented electrical steel sheet obtained by baking the coating solution so that it is as shown in the figure is cut into 55 mm x 150 mm, covered with vinyl adhesive tape so that the resist coating portion of 20 mm x 20 mm is exposed, and in a 10% NaCl solution, the exposed portion of the coating is placed opposite a platinum-plated Ti plate counter electrode, the distance between the electrodes is set to 40 mm, a voltage of 10 V is applied between the electrodes to perform electrolysis, and the change in the current density flowing between the electrodes over time is measured. The less current flows even when voltage is applied to start electrolysis, the less likely it is to peel off, i.e., the higher the chemical resistance. It is also possible to compare the current density of each sample 20 seconds after voltage application.

[0067] (occupancy factor) Measure in accordance with the method described in JIS C 2550-5:2011.

[0068] (Porosity of insulating film) An image of the cross section of the insulating film is obtained by backscattering electrons. This image is then binarized to obtain a binary image. The cross-sectional area A obtained by subtracting the area of ​​the voids (pores) from this binary image is C get. The cross-sectional area A, including the area of ​​the voids (pores), is obtained from the void-filled binary image. Then, the porosity F is calculated using the following formula (F). The insulating film is observed at a magnification of 5000 times to obtain five images, and the average value of the obtained porosity is calculated to be the porosity of the insulating film. Formula (F) F={1-(A C / A)}×100

[0069] (Iron loss and magnetic flux density) The iron loss and magnetic flux density are measured according to the method described in JIS C 2550-1:2011. Specifically, the iron loss per unit mass (W 17 / 50 ) and magnetic flux density (B 8 ) measures the value of magnetic flux density at a magnetizing force of 800 A / m.

[0070] Although one example of a preferred embodiment of the present invention has been described, the present invention is not limited to the above. The above is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. EXAMPLES

[0071] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. It is obvious that a person skilled in the art can come up with various modified or amended examples within the scope of the ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.

[0072] [Grain-oriented electrical steel sheets using conventional technology] In accordance with the disclosure of Patent Document 3, grain-oriented electrical steel sheets were produced with insulating films (resist films) baked at different baking temperatures, and their film tension and chemical resistance (current density 20 seconds after electrolytic etching as a resist film was started) were measured. Specifically, a coating liquid containing aluminum phosphate (50 mass% aqueous solution: 57 mass parts), chromic anhydride (6 mass parts), and colloidal silica (20 mass% aqueous dispersion: 100 mass parts) was used. The mass ratio Ws of colloidal silica to aluminum phosphate in the coating liquid was 0.70. This coating liquid was applied to finish-annealed grain-oriented electrical steel sheets (sheet thickness 0.23 mm, B 8 =1.93T), dried, and baked at 400°C, 500°C, 600°C, 700°C, 750°C, 800°C, 850°C, 900°C, and 950°C to form an insulating film. The amount of the insulating film formed was about 4.5 g / m 2 The aforementioned "film tension" and "chemical properties" were evaluated for each grain-oriented electrical steel sheet on which the insulating film was formed. The results are shown in Figure 2. The film tension was nearly 0 MPa when the baking temperature was 700°C or less, increased when the baking temperature exceeded 700°C, and reached approximately 8 MPa at 850°C and 900°C, but decreased at 950°C. On the other hand, regarding the chemical resistance (current density 20 seconds after the start of electrolytic etching as a resist film), as the baking temperature increases, the current density also increases, reaching approximately 0.6 A / cm at 700°C. 2 This is the stable region of 0.5A / cm where the insulation film does not peel off. 2 The values ​​were outside the range below. When the baking temperature was further increased, the current density also increased further, suggesting that the chemical resistance was not sufficient.

[0073] [Grain-oriented electrical steel sheet according to the present invention] In accordance with the present disclosure, grain-oriented electrical steel sheets were produced with insulating coatings baked at different baking temperatures, and the coating tension and chemical resistance (current density 20 seconds after the start of electrolytic etching as a resist coating) were measured. Specifically, commercially available kaolin hydrous silicate particles were prepared and milled to a specific surface area of ​​50 m using a ball mill. 2A boric acid aqueous solution was added to prepare a coating solution so that the molar ratio of B / Al was 0.8 and the solid content concentration was 25%. This coating solution was applied to a finish-annealed grain-oriented electrical steel sheet (thickness 0.23 mm, B 8 =1.93T), dried, and baked at 400°C, 500°C, 600°C, 700°C, 750°C, 800°C, 850°C, 900°C, and 950°C to form an insulating film. The amount of the insulating film formed was about 4.5 g / m 2 The grain-oriented electrical steel sheets on which the insulating film was formed were evaluated for the aforementioned "film tension" and "chemical properties." The results are shown in Figure 3. Regarding the coating tension, when the baking temperature was 500°C or less, it was 2 MPa or less, and when the baking temperature exceeded 500°C, the coating tension increased, exceeding approximately 8 MPa at 600°C. The higher the temperature, the higher the coating tension became, and at 750°C or more, a high coating tension of more than 10 MPa was obtained. On the other hand, in terms of chemical resistance (current density 20 seconds after the start of electrolytic etching as a resist film), contrary to the example of the prior art, as the baking temperature increases, the current density decreases, reaching approximately 0.1 A / cm at 600°C. 2 This is well below the 0.5A / cm2 range that is considered to be stable and does not cause the insulation film to peel off. 2 The following is fully satisfied: If the baking temperature is further increased, the current density is further decreased, and it has been confirmed that the chemical resistance is sufficient.

[0074] [Improving iron loss value by groove machining or dot-array dimple machining] As shown in Table 1, the iron loss values ​​of a grain-oriented electrical steel sheet having an insulating coating (resist coating) according to the prior art and a grain-oriented electrical steel sheet having an insulating coating (resist coating) according to the present invention were measured before and after groove processing by electrolytic etching.

[0075] No. 1 in Table 1 is an example of a grain-oriented electrical steel sheet having an insulating coating formed using a coating liquid containing colloidal silica, phosphate, and chromic acid. No. 2 is an example of a grain-oriented electrical steel sheet having the same composition of the insulating coating as No. 1, but produced at a lower baking temperature than that of the No. 1 example. Nos. 3 and 4 are examples of grain-oriented electrical steel sheets provided with an insulating coating formed using a coating liquid containing alumina sol and boric acid. Nos. 5 to 11 are examples of grain-oriented electrical steel sheets provided with an insulating coating formed using a coating liquid containing kaolin and boric acid. No. 12 is an example of a grain-oriented electrical steel sheet having an insulating coating formed using a coating liquid containing pyrophyllite and boric acid. A finish annealed coating mainly composed of forsterite was formed on the surface of the base steel of Nos. 1 to 12. The insulating coating of Nos. 5 to 12 contained pseudotetragonal aluminum borate and silica.

[0076] The film tension was measured for each grain-oriented electrical steel sheet after the insulating film was formed. The film tension shown in Table 1 was measured after baking and before the YAG laser irradiation described below.

[0077] In this embodiment, in order to process grooves or dot-array depressions by electrolytic etching, the insulating film was locally peeled off by irradiating a YAG laser. In the cases of Nos. 1 to 3 and 5 to 10, the insulating film was removed linearly with a width of 0.15 mm and at 3 mm intervals perpendicular to the rolling direction on the surface of the grain-oriented electrical steel sheet. In the cases of No. 4, No. 11 and No. 12, the insulating film was removed from the surface of the grain-oriented electrical steel sheet in a dotted pattern with a diameter of 0.15 mm and a dot interval of 3 mm (dot interval 0.3 mm) perpendicular to the rolling direction.

[0078] The grain-oriented electrical steel sheets on which the insulating film had peeled off were then electrolytically etched in a 10% NaCl solution to form linear grooves or dot-like depressions. The depth of the grooves and depressions was adjusted by adjusting the current density and electrolysis time during electrolytic etching.

[0079] After processing, the surface was observed under a microscope, and the groove width or dent diameter was measured at 100 locations for each condition, and the standard deviation was calculated.

[0080] Before and after groove processing, the iron loss per unit mass (W) was measured under the conditions of a measured magnetic flux density amplitude of 1.7T and a frequency of 50Hz, in accordance with the method described in JIS C 2550-1:2011. 17 / 50 The results are shown in Table 1.

[0081] [Table 1]

[0082] From Table 1, it can be seen that in the examples of No. 1, 3, and 4, although the required film tension was obtained, the resistivity was poor, so the variation in groove width was large and it was difficult to reduce iron loss. In the case of No. 2, the resistivity is good, but the film tension is small, so it is found that the iron loss reduction effect is not obtained. In the case of No. 7, it was found that the groove depth was too small at 4 μm, and therefore sufficient iron loss reduction effect was not obtained. In the case of No. 10, the groove depth was too large at 50 μm, and it was found that a sufficient iron loss reduction effect was not obtained. In contrast, in the cases of Nos. 5, 6, 8, 9, 11, and 12, the resist properties were good, so the groove width and diameter variations were small, and the film tension was also large. Therefore, it was found that if the groove depth is set within the range of 5 to 40 μm, the magnetic domain refinement effect is exerted, resulting in a grain-oriented electrical steel sheet with low iron loss.

Claims

1. A grain-oriented electrical steel sheet having, on its surface, a finish annealing coating mainly composed of forsterite and an insulating coating containing pseudo-tetragonal aluminum borate and silica, characterized in that one or both surfaces of the steel sheet have linear grooves or dot-like depressions having a depth of 5 to 40 μm.

2. A method for producing grain-oriented electrical steel sheet, comprising: applying and baking a coating liquid containing aluminum-containing hydrous silicate particles and boric acid to a grain-oriented electrical steel sheet after finish annealing to form an insulating coating; removing a linear or dotted portion of the insulating coating on one or both sides to expose the base steel; and then forming linear grooves or dotted depressions having a depth of 5 to 40 μm by electrolytic etching.

Citation Information

Patent Citations

  • Sound recorder*reproducer

    JP1981003414A

  • Grain oriented silicon steel sheet with low core loss and its production

    JP1996325745A

  • Production method of low core loss directional electromagnetic steel sheet

    JP2001316896A

  • Method for forming insulative film superior in baking atmosphere resistance on grain-oriented electromagnetic steel sheet

    JP2003301271A

  • Method for manufacturing grain-oriented electromagnetic steel sheet with low core loss

    JP2003301272A