Polycrystalline aluminosilicate ceramic filament nonwoven mat and method for producing same

The production of polycrystalline aluminosilicate ceramic filaments with controlled diameter and mullite content addresses stability and flexibility issues, resulting in nonwoven mats with enhanced performance for high-temperature applications.

JP7592094B2Active Publication Date: 2024-11-293M INNOVATIVE PROPERTIES CO
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022540321
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-30
Filing Date
2020-12-18
Publication Date
2024-11-29
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Existing methods for producing nonwoven ceramic webs face challenges in achieving stable filament formation with diameters less than 2 microns, leading to unstable processes, reduced strength, flexibility, and handling issues due to variations in filament diameter and crystalline mullite content, which affects their performance at high temperatures and in filtration applications.

Method used

A method involving the production of polycrystalline aluminosilicate ceramic filaments with an average diameter of less than 2 microns and a high mullite content (15% to 80% by weight) using a meltblown fiber process, utilizing an aqueous ceramic precursor sol with silica particles and a hydrolyzable aluminum compound, followed by high-velocity air attenuation and controlled firing to form a cohesive nonwoven mat.

Benefits of technology

The resulting nonwoven mats exhibit excellent heat resistance, flexibility, and mechanical properties, suitable for filtration, thermal insulation, and structural reinforcement, with improved durability and thermomechanical properties, enabling applications in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592094000007
    Figure 0007592094000007
  • Figure 0007592094000008
    Figure 0007592094000008
  • Figure 0007592094000009
    Figure 0007592094000009
Patent Text Reader

Abstract

The nonwoven article comprises a plurality of polycrystalline aluminosilicate ceramic filaments entangled to form a cohesive nonwoven mat, each of the aluminosilicate ceramic filaments having an average diameter of less than about 2 microns (μm), and the aluminosilicate ceramic filaments comprising an average of about 15% to about 80% by weight of crystalline mullite.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] In a process for producing a nonwoven web using a sol-gel process, chemical precursors are spun and heat treated to produce ceramic filaments.

[0002] The fiber manufacturing process can produce either continuous filaments, typically in the form of multifilament rovings, or nonwoven webs. Continuous filaments can be converted into nonwoven mats by chopping them into shorter fiber strands that can be opened into individual fibers and then stacking them into a uniform mat (e.g., by wet laying or air laying). Nonwoven ceramic fiber mats or webs can also be directly produced using a fiber blowing process, also called the blown microfilament (BMF) process. In the fiber blowing process, an initial low viscosity ceramic precursor dispersion or sol is pumped through a nozzle and then stretched and fibrillated using a high velocity air stream to form separate fibers or filaments that are then collected to form a nonwoven green (unfired) fiber mat or web. The green fiber mat is then fired at high temperature to form a nonwoven ceramic filament mat. Summary of the Invention

[0003] In one aspect, the present disclosure is directed to a nonwoven article comprising a plurality of polycrystalline aluminosilicate ceramic filaments intertwined to form a cohesive nonwoven mat, each of the aluminosilicate ceramic filaments having an average diameter of less than about 2 microns (μm), and the aluminosilicate ceramic filaments comprising, on average, about 15% to about 80% crystalline mullite by weight.

[0004] In another aspect, the present disclosure is directed to a method of making a nonwoven web. The method includes flowing an aqueous ceramic precursor sol through at least one orifice to produce at least one substantially continuous filament. The aqueous ceramic precursor sol includes silica particles, water, and a hydrolyzable aluminum-containing compound. The filaments are attenuated with a high velocity air stream to elongate the filaments to an average diameter of 10 micrometers (μm) or greater, and at least a portion of the water is removed from the at least one substantially continuous filament to at least partially dry the at least one substantially continuous filament. The at least partially dried filaments are collected on a collector surface as a raw nonwoven web, and the raw nonwoven web is heated at a temperature and for a time sufficient to convert the raw nonwoven web into a cohesive mat. The cohesive mat includes at least one polycrystalline aluminosilicate ceramic filament comprising about 15% to about 80% by weight of crystalline mullite, and each of the aluminosilicate ceramic filaments in the cohesive mat has an average diameter of less than 2 microns (μm).

[0005] These and other unexpected results and advantages of the invention are within the scope of the following illustrative detailed description and examples. [Brief description of the drawings]

[0006] The present disclosure may be more fully understood from the following detailed description of various embodiments of the present disclosure when considered in conjunction with the accompanying drawings, in which:

[0007] [Figure 1] FIG. 2 is a cross-sectional view of a mounting mat reinforced according to one embodiment of the present disclosure.

[0008] [Diagram 2] FIG. 2 is a perspective view of an open pollution control device with a reinforced mounting mat, with a portion of the mat removed to more clearly show the aluminosilicate ceramic filaments, according to an embodiment of the present disclosure.

[0009] [Diagram 3] FIG. 1 is a schematic diagram of a meltblown fiber (BMF) apparatus used in the examples of this application.

[0010] [Figure 4] 1 is a scanning electron microscope (SEM) photograph of a filament of Sample 2 of Example 1 at 5000x magnification.

[0011] [Diagram 5] FIG. 13 is a plot of the green diameter of filament Samples 3-6 of Example 3A at 15 psi sol pressure with increasing die air flow from 15 cfm to 30 cfm.

[0012] [Figure 6] Photographs of a nonwoven mat made from filaments of Sample 7 of Example 3B in both flat (left) and folded (right) states.

[0013] [Figure 7] 13 is a plot showing the evolution of crystalline mullite as a function of heat treatment temperature for Sample 7 of Example 3B.

[0014] In the drawings, like reference numbers refer to like elements. The above-identified drawings may not be drawn to scale and illustrate various embodiments of the present disclosure, although other embodiments are also contemplated, as noted in the Detailed Description. In all cases, the disclosure describes the disclosure content disclosed herein by representing exemplary embodiments, and not by express limitation. It should be understood that numerous other modifications and embodiments may be devised by those skilled in the art that are within the scope and spirit of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] With regard to the following glossary of defined terms, these definitions shall apply throughout this application, unless a different definition is provided in the claims or elsewhere in this specification.

[0016] Glossary Certain terms are used throughout this specification and claims, most of which are well known, but may require some explanation. It should be understood that:

[0017] The term "adjacent" with respect to a particular layer means that the two layers are adjacent to (i.e., adjacent to) and in direct contact with one another, or are joined or attached to another layer in a position that is close to but not in direct contact with one another (i.e., with one or more additional layers interposed between the layers).

[0018] The locations of various elements in the disclosed coated articles refer to the relative position of the elements with respect to a horizontally positioned, upward-facing substrate by using orientation terms such as "atop," "on," "over," "covering," "uppermost," "underlying," etc. However, unless otherwise indicated, it is not intended that the substrate or the article should have any particular spatial orientation during or after manufacture.

[0019] The term "(co)polymer" or "singular" includes homopolymers and copolymers, as well as homopolymers or copolymers that may be formed in miscible blends, for example, by coextrusion or by reaction, including, for example, transesterification. The term "copolymer" includes random copolymers, block copolymers, and star (e.g., dendritic) copolymers.

[0020] By using the term "separated by" to describe the position of a layer relative to other layers, we are referring to the layer being located between two other layers, but not necessarily adjacent or contiguous to either layer.

[0021] The terms "about" or "approximately" with reference to a numerical value or shape mean ±5 percent of the numerical value or property or characteristic, but expressly include the exact numerical value. For example, a viscosity of "about" 1 Pa-sec refers to a viscosity between 0.95 and 1.05 Pa-sec, but also expressly includes a viscosity of exactly 1 Pa-sec. Similarly, a "substantially square" perimeter is intended to describe a geometry having four lateral edges, each lateral edge having a length that is between 95% and 105% of the length of any other lateral edge, but is also intended to include a geometry in which each lateral edge has the exact same length.

[0022] The term "web basis weight" is calculated from the weight of a 10 cm by 10 cm sample of the web.

[0023] The term "web thickness" is measured using a thickness test gauge having a 1 / 2 inch (12.7 mm) diameter tester foot available under the trade designation Model 49-70 from Testing Machines, Inc. (Amityville, NY).

[0024] The term "bulk density" is the mass per unit volume of the bulk ceramic material that makes up the web and is taken from the literature.

[0025] The term "substantially" with respect to a property or characteristic means that the property or characteristic is exhibited to a greater extent than the opposite of the property or characteristic is exhibited. For example, a "substantially" transparent substrate refers to a substrate that transmits more radiation (e.g., visible light) than it does not transmit (e.g., absorbs and reflects). In this case, a substrate that transmits more than 50% of the visible light incident on its surface is substantially transparent, while a substrate that transmits 50% or less of the visible light incident on its surface is not substantially transparent.

[0026] As used herein and in the accompanying embodiments, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to fine filaments containing "a compound" includes a mixture of two or more compounds. As used herein and in the accompanying embodiments, the term "or" is generally used in its sense including "and / or" unless the context clearly dictates otherwise.

[0027] As used herein, the recitation of numerical ranges by endpoints includes all numbers subsumed within that range (eg, 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.8, 4, and 5).

[0028] Unless otherwise indicated, all numbers expressing quantities or ingredients, measurements of properties, and the like used in the specification and embodiments are to be understood in all instances as being modified by the term "about". Accordingly, unless indicated to the contrary, the numerical parameters set forth in the foregoing specification and accompanying list of embodiments may vary depending upon the desired properties one of ordinary skill in the art would obtain utilizing the teachings of the present disclosure. At the very least, each numerical parameter should at least be construed in light of the number of reported significant digits and by applying ordinary rounding techniques, which is not intended to limit the application of the doctrine of equivalents to the scope of the claimed embodiments.

[0029] Various modifications and variations of the exemplary embodiments of the present disclosure may be made without departing from the spirit and scope of the present disclosure. It should be understood, therefore, that the embodiments of the present disclosure are not limited to the exemplary embodiments described below, but are instead governed by the limitations set forth in the claims and any equivalents thereof.

[0030] Various exemplary embodiments of the present disclosure will be described below with specific reference to the drawings. Various modifications and changes may be made to the exemplary embodiments of the present disclosure without departing from the spirit and scope of the present disclosure. Therefore, it should be understood that the embodiments of the present disclosure are not limited to the exemplary embodiments described below, but are governed by the limitations set forth in the claims and any equivalents thereof.

[0031] The sol-gel BMF process produces filaments with a limited range of diameters. Attempts to produce filaments with diameters that are too small can lead to an unstable process that breaks the filaments, producing short fibers, roughly spherical bodies called shots, and wide filament diameter variations. Attempts to produce filaments with diameters that are too large can also lead to unstable filament formation, which can reduce the strength, flexibility, and handleability of the nonwoven mat produced from the filaments.

[0032] Alumina-silica filaments are typically manufactured with low crystalline mullite (3Al2O3-2SiO2) content. If the filaments are heat treated at temperatures above 1200°C, where mullite crystallizes, the strength and flexibility of the nonwoven fabric can be significantly reduced. This lack of strength and flexibility can prevent the filaments from being used at high temperatures and also prevents the realization of mullite's advantageous properties, including thermal stability, creep resistance, and chemical stability.

[0033] Polycrystalline aluminosilicate ceramic filaments with increased crystalline mullite content, as well as nonwoven webs and mats incorporating the filaments, have excellent heat resistance up to 1300°C, excellent acid resistance, low pressure drop when used in filtration applications, and good flexibility. Smaller diameter filaments may also have greater softness and flexibility, lower thermal conductivity in mat form, and potentially improved mechanical properties when used as structural elements in fiber reinforced composites. When incorporated into nonwoven mats, polycrystalline aluminosilicate ceramic filaments with small diameter and higher mullite content may have a wide variety of potential applications including, for example, filtration, support media, backing media, thermal insulation, such as electrical vehicle battery insulation, and high temperature sound insulation.

[0034] In general, the present disclosure is directed to flexible polycrystalline aluminosilicate ceramic filaments having an average diameter of less than about 2 microns (μm) and an average crystalline mullite (3Al2O3-2SiO2) composition of about 15% to about 80% by weight, collected to form a coherent nonwoven web. These filaments may be more economically produced using a meltblown fiber (BMF) process compared to filaments produced using conventional electrospinning processes. The combination of a small diameter of less than about 2 μm and a high mullite content provides the ceramic filaments with excellent heat resistance, as well as softness, flexibility, durability, and resistance to breakage, which in some embodiments may also have improved thermomechanical properties (e.g., thermal creep resistance at high temperatures).

[0035] A plurality of small diameter high mullite content filaments can be collected and incorporated into a green nonwoven web, which can then be fired to produce an agglomerated ceramic mat. In some examples, but not intended to be limiting, the ceramic mat can be used for filtration, thermal insulation, sound insulation, fire protection, as a mounting mat, as a gasket, or as a catalyst support, can be incorporated as a structural element in a fiber reinforced composite, or can be incorporated into a pollution control device such as a vehicle catalytic converter.

[0036] In a further aspect, the present disclosure describes a method for producing a nonwoven web of small diameter, high mullite content filaments. The method includes flowing an aqueous ceramic precursor sol through at least one orifice to produce at least one substantially continuous filament. The aqueous ceramic precursor sol includes silica particles dispersed in water and a hydrolyzable aluminum-containing compound. The filaments are at least partially dried and collected on a collector surface to form a green nonwoven web on the collector surface. The green nonwoven web can then be fired to form a cohesive ceramic mat. Polycrystalline aluminosilicate ceramic nonwoven articles

[0037] In one aspect, the present disclosure is directed to a nonwoven article comprising a plurality of polycrystalline aluminosilicate ceramic filaments that can be collected and entangled to form a coherent nonwoven mat. The aluminosilicate ceramic filaments incorporated into the nonwoven article have an average diameter determined using electron microscopy of less than about 2 microns (μm) and an average crystalline mullite (3Al2O3-2SiO2) content of at least 15%, or at least 20%, or at least 30%, or at least 40%, or at least 50%, or at least 60%, or at least 70%, or at least 72%, or at least 75%, or at least 80% by weight.

[0038] In some exemplary embodiments, without intending to be limiting, the ceramic filaments include about 70% to about 90% alumina by weight, or about 73% to about 80% alumina by weight.

[0039] 1, a reinforced nonwoven web or mat 10 according to an embodiment of the present disclosure has a first major surface 12, a second major surface 14, and a thickness (i.e., the distance between surfaces 12 and 14). The nonwoven web or mat 10 has at least a first layer 16 and an optional second layer 18, and may include one or more additional layers (not shown in FIG. 1). At least one of the mat layer 16 and the optional mat layer 18 may include at least a portion of substantially continuous polycrystalline aluminosilicate ceramic filaments 20 having an average diameter of less than about 2 μm and an average mullite content of about 15% to about 80% by weight.

[0040] In some exemplary embodiments, the polycrystalline aluminosilicate ceramic filaments 20 may be incorporated into the nonwoven mat 10 along with other filaments or fibers. Thus, in certain exemplary embodiments, the reinforcement mat 10 may include other filaments or fibers selected from alumina fibers, silica fibers, silicon carbide fibers, silicon nitride fibers, carbon fibers, glass fibers, metal fibers, alumina-phosphorus pentoxide fibers, alumina-boria-silica fibers, zirconia fibers, zirconia-alumina fibers, zirconia-silica fibers, and mixtures or combinations thereof. In some embodiments, the nonwoven mat 10 may optionally include non-fibrous fillers, such as aerogel or glass / ceramic bubbles.

[0041] In further exemplary embodiments, the polycrystalline aluminosilicate ceramic filaments 20 may be used with other optional performance enhancing materials (e.g., intumescent materials or inserts, non-intumescent inserts, support mesh, binders, etc.) As shown in the exemplary embodiment of a vehicular catalytic converter housing shown in Figure 2, an optional reinforcing mesh 22 is shown disposed between layer 16 and optional layer 18 so as to be generally coplanar with first major surface 12 and second major surface 14.

[0042] Suitable optional performance enhancing materials are described, for example, in U.S. Pat. Nos. 3,001,571 and 3,916,057 (Hatch et al.), 4,305,992, 4,385,135, 5,254,416 (Langer et al.), 5,242,871 (Hashimoto et al.), 5,380,580 (Rogers et al.), 7,261,864(B2) (Watanabe), 5,385,873 and 5,207,989 (MacNeil), and WO 97 / 48889 (Sanocki et al.).

[0043] In certain exemplary embodiments, the nonwoven web or mat 10 further comprises an optional binder for binding the plurality of polycrystalline aluminosilicate ceramic filaments together. A wide variety of suitable binders may be used, including inorganic binders, organic binders, and combinations thereof. For example, suitable organic binders are selected from (meth)acrylic (co)polymers, poly(vinyl)alcohols, poly(vinyl)pyrrolidones, poly(ethylene oxides), poly(vinyl)acetates, polyolefins, polyesters, and combinations thereof. In other embodiments, the inorganic binder may be selected from silica, alumina, zirconia, kaolin clays, bentonite clays, silicates, mica particles, and combinations thereof. In some embodiments, the optional binder is substantially free of silicone materials.

[0044] The polycrystalline aluminosilicate ceramic filaments described herein having a diameter of less than about 2 μm and a mullite content of about 15% to about 80% by weight provide excellent flexibility to the nonwoven mat. In one embodiment, discussed in detail in the Examples below, and not intended to be limiting, a circular nonwoven mat made from the filaments and having a diameter of about 1.5 inches to 2 inches (3.8 cm to 5 cm) was folded on itself along the diameter to form a semicircle having two overlapping layers. This semicircle was then folded again on itself along the radius of the semicircle to form a semicircle (sometimes called a quadrant) containing four overlapping layers. After multiple folding steps, the individual filaments forming the mat remained unbroken and the semicircle remained folded even after extended periods of time.

[0045] The ability of the mat to withstand repeated bending can also be determined using a flexural durability tester such as that described in ASTM D2176. As detailed in the examples below, mats made with small diameter filaments having greater than about 60% by weight crystalline mullite had flexural durability of 18 to 140 double cycles under a 100 g load and endured over 2000 cycles at zero tensile load without fracture.

[0046] Polycrystalline Aluminosilicate Ceramic Filament In some exemplary embodiments of the aforementioned nonwoven articles, each of the plurality of polycrystalline aluminosilicate ceramic filaments exhibits a green diameter of from about 1 μm to about 10 μm, or from about 2 μm to about 5 μm, and the as-fired filaments have an average diameter of from about 1 μm to about 5 μm, or from about 1 μm to about 2 μm, as determined using an electron microscopy filament diameter measurement procedure as further described below.

[0047] In further exemplary embodiments, the polycrystalline aluminosilicate ceramic filaments have a length of at least 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, or even 10 mm, or more. In some such exemplary embodiments, each of the polycrystalline aluminosilicate ceramic filaments is substantially continuous, which means in this application that the filaments have both ends or termination points, but behave as continuous filaments with respect to their processing characteristics and handling properties. Substantially continuous filaments typically have a length of more than 25 mm, more than 50 mm, more than 75 mm, more than 100 mm, more than 250 mm, more than 500 mm, more than 750 mm, or even longer, and have an infinite length, or a length of less than 10,000 mm, less than 7,500 mm, less than 5,000 mm, less than 2,500 mm, less than 1,000 mm, or even less than 900 mm. Thus, in certain exemplary embodiments, the plurality of polycrystalline aluminosilicate ceramic filaments can have a length of from 25 mm to infinity, or from about 50 mm to about 10,000 mm, or from about 100 mm to about 7500 mm, or from about 250 mm to about 5000 mm, or even from 500 mm to about 2500 mm.

[0048] In a further exemplary embodiment, the bulk density of the cohesive mat is between 0.05 and 0.3 g / cm 3 , 0.06~0.25g / cm 3 , or even 0.07 to 0.2 g / cm 3 The range may be:

[0049] In some exemplary embodiments, the nonwoven web and / or cohesive mat has a thickness of at least 0.5 mm, 1 mm, 2 mm, 2.5 mm, 5 mm, 7.5 mm, 10 mm, 20 mm, 30 mm, 40 mm, or even 50 mm or more. In some such exemplary embodiments, the nonwoven web and / or cohesive mat has a thickness of up to 100 mm, 90 mm, 80 mm, 70 mm, or even 60 mm or less.

[0050] In additional exemplary embodiments, the nonwoven web and / or cohesive mat has a basis weight of at least 50 g / m 2 (gsm), 60 gsm, 70 gsm, 80 gsm, 90 gsm, 100 gsm, or even higher. In some such exemplary embodiments, the basis weight is 4,000 gsm or less, 3,000 gsm or less, 2,000 gsm or less, 1,000 gsm or less, 750 gsm or less, 500 gsm or less, 250 gsm or less, or even lower. In some exemplary embodiments, the polycrystalline aluminosilicate ceramic filaments have an alumina to silica ratio ranging from 60:40 to 90:10 by weight, from 70:30 to 80:20 by weight, from 73:27 to 78:22 by weight, or even from 75:25 to 77:23 by weight.

[0051] Articles Comprising Polycrystalline Aluminosilicate Ceramic Nonwoven Mats In another aspect, the present disclosure describes an article comprising the aforementioned nonwoven aluminosilicate ceramic web having a plurality of polycrystalline aluminosilicate ceramic filaments having an average diameter of less than about 2 μm and an average mullite content of about 15% to about 80% by weight. In some such embodiments, the article may be selected from a filtration article, a thermal insulation article, a sound insulation article, a fire protection article, a mounting mat article, a gasket article, a catalyst support article, a component of a ceramic article, a thermal barrier in a battery, and combinations thereof.

[0052] Referring again to FIG. 2, a pollution control device 60 (e.g., catalytic converter and / or exhaust filter) according to the present disclosure may include a housing 50, a pollution control element 40 (e.g., catalytic element and / or filter) mounted inside the housing 50, and a mounting mat 10, such as those described herein, sandwiched therebetween to mount the element 40 within the housing 50. The housing 50 is typically made of a metal, such as stainless steel, and includes an inlet 52 and an outlet 54 for passing exhaust gases from an internal combustion engine through the device 60. The element 40 is typically a relatively fragile, thin-walled, monolithic structure. The mat 10 protects the element 40 from both thermal and mechanical (e.g., vibration) related damage.

[0053] It may be desirable for the optional mesh 22 to be located closer to the surface 12 of the mat 10 (i.e., layer 16 is relatively thinner than layer 18). For example, a mesh of about 1600 g / m 2 and a mat 10 having a total weight of about 80 to about 160 g / m 2 For a net product 22 having a weight in the range of about 40 to about 800 g / m 2 In other words, it may be desirable for layer 16 to comprise about 3% to 10% by weight of the total weight of mat 10.

[0054] Thus, in some exemplary embodiments, the pollution control device further comprises an intumescent layer, a reinforcing mesh, a non-intumescent insert, or a combination thereof. Suitable intumescent layers, reinforcing meshes, and non-intumescent inserts are described, for example, in U.S. Pat. Nos. 3,001,571 and 3,916,057 (Hatch et al.), 4,305,992, 4,385,135, 5,254,416 (Langer et al.), 5,242,871 (Hashimoto et al.), 5,380,580 (Rogers et al.), 7,261,864(B2) (Watanabe), 5,385,873, and 5,207,989 (MacNeil), and WO 97 / 48889 (Sanocki et al.), each of which has been previously incorporated by reference in its entirety.

[0055] In some such exemplary embodiments, the pollution control device may be installed in a motor vehicle exhaust system of a motor vehicle selected from an automobile, a motorcycle, a truck, a boat, a submarine, or an aircraft.

[0056] Method for producing polycrystalline ceramic filaments and nonwoven mats In another aspect, the present disclosure describes a method for making a nonwoven web comprising polycrystalline aluminosilicate ceramic filaments that can be sintered to form a cohesive mat having at least some filaments having an average diameter less than about 2 μm and an average crystalline mullite content greater than about 50 wt.%.

[0057] Generally, as shown diagrammatically in the blown melt fiber (BMF) apparatus 100 diagram in Figure 3, filaments are produced by flowing an aqueous ceramic precursor sol 102 stored in a sol reservoir 104 through at least one orifice 108 in a die 106 with the aid of surrounding high pressure attenuation air 109. This apparatus may also be called a meltblowing or blow spinning die. The apparatus may consist of a linear array of round holes in a V-shaped die where the air is injected at an angle to the sol extrusion direction, as in US Patent No. 3,825,380, or an array of nozzles surrounded by attenuation air, as in US Patent No. 5,476,616 and US Patent No. 5,286,182.

[0058] The aqueous ceramic precursor sol 102 comprises silica particles dispersed in water. Suitable alumina and silica sols are described, for example, in WO 2018 / 93624 A1 (DeRovere). The aqueous ceramic precursor sol further comprises a hydrolyzable aluminum-containing compound, which may have a stoichiometric amount of less than 3 moles of anion relative to Al, and has the nominal formula AlX n (OH) 3-n where X is a ligand such as Cl-, NO3-, or CH3COOH-, and can form clear aqueous solutions. These solutions can be formed using a number of methods, including dissolving aluminum metal in a salt solution, dissolving aluminum hydroxide in an acid, hydrolysis of an alkoxide, and neutralization of an acidic salt solution. In some embodiments, the soluble aluminum compound used to make the filaments contains about 0.5 to about 2 moles of anionic ligand per mole of aluminum. In certain embodiments, the aqueous ceramic precursor sol includes aluminum chlorohydrate and dispersed silica particles.

[0059] Optionally, the aqueous ceramic precursor sol further comprises at least one of a water-soluble (co)polymer and an antifoaming agent. Any suitable water-soluble (co)polymer may be used. However, poly(vinyl) alcohol (PVA), poly(vinyl) alcohol-co-poly(vinyl) acetate copolymers, poly(vinyl)pyrrolidone, poly(ethylene oxide), and poly(ethylene oxide)-co-(propylene oxide) copolymers have been found to be particularly suitable. Any suitable antifoaming agent may be used. In some embodiments, when a moderately hydrolyzed (e.g., 50-90% poly(vinyl) acetate) poly(vinyl) alcohol-co-poly(vinyl) acetate copolymer is used, the antifoaming agent is based on a long chain alcohol such as 1-octanol, and a polyol ester such as the FOAM-A-TAC series of antifoaming agents available from Enterprise Specialty Products Inc. (Laurens, SC), e.g., FOAM-A-TAC 402, 407, and 425.

[0060] In some embodiments, but not intended to be limiting, the aqueous ceramic precursor sol 102 has a viscosity of about 2000 centipoise (cP) to about 10,000 cP, (2 Pa-sec to 10 Pa-sec), or about 3000 cP to about 5000 cP (3 Pa-sec to 5 Pa-sec).

[0061] In some embodiments, but not intended to be limiting, the aqueous ceramic precursor sol 102 is delivered at a pressure of about 2 psi to about 20 psi, or about 3 psi to about 15 psi (14 Pa to 103 Pa), or about 5 psi to about 10 psi (34 Pa to 69 Pa). Higher pressures can increase the sol flow rate per orifice, and in some embodiments, higher pressures can also increase the filament diameter.

[0062] In some such exemplary methods, the at least one orifice 108 comprises a plurality of circular orifices positioned within a multi-orifice die 106 in flow communication with a source of the aqueous ceramic precursor sol 102. Optionally, each of the plurality of orifices has an inner diameter of 50-500 μm, 100-400 μm, 125-200 μm, or about 150 μm.

[0063] The method further includes directing a stream of high velocity gas proximate to the filaments to at least partially dry and attenuate the filaments. It is often desirable to humidify the attenuation air to prevent drying and allow for increased drawing and elongation of the extruded filaments. In some embodiments, the gas is at room temperature. In some embodiments, the gas is heated to a temperature of at least 50° C., 75° C., 100° C., 125° C., 150° C., or higher. In various embodiments, and not intended to be limiting, the attenuation air velocity can be very high, 10,000 feet per minute (fpm) (51 m / s), or even higher, such as 15,000 (76 m / s), 20,000 (102 m / s), or even 30,000 fpm (152 m / s), to draw the filaments. Higher air velocities can result in more drawing forces than lower air velocities, resulting in smaller filament diameters. However, if the drawing force is too high, the filaments break and do not form small diameter filaments. In some circumstances, the sol-gel liquid will bead up by surface tension and form short fibers, "shots", or roughly equiaxed particles, rather than filaments. High air flow rates can also cause turbulence, which, without being bound by theory, can cause variable air velocities, which in turn can cause variable drawing forces on the extruded filaments, which can cause large diameter variability, which may be undesirable. Turbulence can also break the filaments, which can lead to high diameter variability as well as shot particles.

[0064] The filaments 110 emerging from the orifices 108 are quenched with warm air in a quench box 116 to at least partially solidify the filaments. The warm air is heated to a temperature of at least 50° C., 75° C., 100° C., 125° C., 150° C., or higher to dry and solidify the filaments. The at least partially solidified filaments are then deposited on a surface 113 of the collection section 112 and entangled to form a raw nonwoven web 120 with the assistance of a vacuum 114. In some embodiments, the volume of air drawn into the collection section is much greater than the volume of the blowing air. This ensures capture of all the extruded filaments and may also entrain room air to further dry the nonwoven web 120.

[0065] Firing of green filaments can be thought of as involving two distinct steps. The first step is a lower temperature pre-firing (burnout) segment where organics are removed and inorganic phases begin to form. The second step is a high temperature crystallization and sintering segment where the filaments densify and the high temperature crystalline phase forms. The two segments may be performed separately (e.g., pre-firing followed by cooling to room temperature and then sintering) or sequentially in a continuous process (e.g., pre-firing followed by immediate sintering without allowing the material to cool).

[0066] Mullite (3Al2O3-2SiO2) is the only thermodynamically stable crystal in the alumina-silica phase diagram. Thus, mullite crystallizes in the sol-gel alumina-silica filaments during heat treatment at some elevated temperature and time. In some cases, mullite, where alumina and silica are mixed at a near atomic level, often referred to as single-phase gel, crystallizes at relatively low temperatures, 900°C to 1100°C, e.g., 980°C. In other cases, often referred to as dual-phase gel, consisting of separate particles or domains of alumina or silica, typically 10 nm to 1000 nm, has a higher crystallization temperature, e.g., 1200°C to 1400°C or even higher. During heat treatment of the dual-phase gel, other phases such as transition aluminas (e.g., gamma, eta, theta, delta alumina) may form at intermediate temperatures, typically 600°C to 1000°C, most commonly 800°C to 900°C.

[0067] The crystallization of sol-gel ceramic filaments into mullite often occurs over a wide range of temperatures, for example, 1200°C to 1400°C. In other words, the nucleation and growth rates of mullite crystals are kinetically slow. Furthermore, the volume nucleation rate of mullite is relatively slow, resulting in large grains of mullite in the filaments, for example, 0.2 μm to 0.5 μm or even larger. For filaments having diameters less than 10 μm, especially less than 2 μm, it is important to maintain a small grain size, preferably less than 0.25 μm, more preferably less than 0.2 μm, or even less than 0.1 μm. Filaments with larger grains have lower strength and flexibility, and in various embodiments, the filaments of the present disclosure may have a grain size less than 0.5 μm, or less than 0.3 μm, or even less than 0.1 μm.

[0068] XRD powder diffraction can be used to quantify the extent of conversion of the filament to mullite, and in some cases, determining the extent of conversion is not straightforward. Mullite crystallizes from a mixture of amorphous or partially amorphous alumina and silica phases that do not diffract X-rays. For this reason, comparing the ratio of mullite to other phases present in the filament is not a good measure of the volume fraction of mullite in the filament. Therefore, the amount of mullite in the filament is best determined by comparing the size of the mullite XRD peak, e.g., at 15° or 26° 2θ, of the test sample to one or more reference samples. As an example, a filament burned at 1500° C. for 1 hour can be considered to be 100% converted to mullite, and the size of the peak in the unknown sample can be compared to the size of the same XRD peak in the 1500° C. sample.

[0069] In one embodiment (not shown in FIG. 3), the raw nonwoven web 120 is heated (e.g., fired) at a temperature and for a time sufficient to convert the nonwoven web into a cohesive mat having polycrystalline aluminosilicate ceramic filaments incorporated therein having an average mullite percentage of about 15% to about 80% by weight. Generally, the raw nonwoven web 120 should be heated to a firing temperature of at least 1,000° C., 1,250° C., 1,500° C., or higher. Higher firing temperatures may result in shorter firing times, and conversely, longer firing times may allow for the use of lower firing temperatures. Generally, firing times should be at least 30 minutes, 1 hour, 2 hours, 4 hours, 5 hours, 7.5 hours, 10 hours, or even longer. Generally, firing times should be less than 24 hours, less than 20 hours, less than 15 hours, less than 12 hours, or even less than 10 hours. Suitable calciners (ie, kilns) are well known to those skilled in the art, such as, for example, continuous kilns manufactured by HED International, Inc. (Ringoes, NJ).

[0070] Optional processing steps Certain optional processing steps may be found to be advantageous in practicing various exemplary embodiments of the present disclosure, for example, the agglomerated ceramic mat may be subjected to at least one of needle punching, stitch bonding, hydroentangling, binder impregnation, and chopping the agglomerated mat into separate fibers.

[0071] Thus, in one exemplary embodiment contemplated by the present invention, the agglomerated mat may be chopped to produce a plurality of individual polycrystalline aluminosilicate ceramic fibers, each having an average diameter of less than about 2 microns and a mullite content of at least 15% and up to 80% by weight. The resulting chopped fibers may then be further processed, for example, using at least one of wet laying or air laying, to form a fibrous ceramic mat comprising the individual aluminosilicate ceramic fibers.

[0072] The fibrous nonwoven mounting mat embodiments described herein can be produced, for example, by feeding cut individual fibers (e.g., about 2.5 cm to about 5 cm long) into a licker-in roll equipped with pins, such as those available from Laroche (Cours la ville, France), and / or a conventional web former, such as that available from Rando Machine Corp. (Macedon, NY) under the trade designation "RANDO WEBBER", "DAN WEB" manufactured by ScanWeb Co. (Denmark), where the fibers are stretched onto a wire screen or mesh belt (e.g., a metal or nylon belt). When a "DAN WEB" type web former is used, the fibers are preferably individualized using a hammer mill followed by a blower. To facilitate ease of handling of the mat, the mat can be formed or placed on a scrim.

[0073] The fibrous nonwoven mounting mat embodiments described herein can also be manufactured using, for example, conventional wet forming or textile carding. For wet forming processes, the fibers are often from about 0.5 cm to about 6 cm in length.

[0074] In some exemplary embodiments, particularly for wet-formation processes, binders may be advantageously used to facilitate formation of the mat, and in some embodiments, the nonwoven mats described herein contain no more than 10% by weight (in some embodiments, no more than 4, 3, 2, 1, 0.75, 0.5, 0.25, or even 0.1% by weight) of binder based on the total weight of the mat.

[0075] Optionally, some embodiments of the fibrous nonwoven mounting mats described herein are needle punched (i.e., there is physical entanglement of the fibers, for example, caused by multiple full or partial (in some embodiments, full) penetration of the mat by barbed needles). The nonwoven mat may be needle punched using conventional needle punching equipment (e.g., a needle puncher commercially available from Dilo Gmbh (Germany) under the trade designation "DILO"), for example, with barbed needles commercially available from Foster Needle Company, Inc. (Manitowoc, WI) or Groz-Beckert Group (Germany) to obtain a needle punched nonwoven mat.

[0076] Needle punching, which results in fiber entanglement, typically involves compressing the mat and then punching and drawing barbed needles through the mat. When the aforementioned polymer and / or bicomponent organic fibers are included in the mat structure, the effectiveness of physical entanglement of fibers during needle punching is generally improved. Improved entanglement can further increase tensile strength and improve handling of the nonwoven mat. The optimal number of needle punches per area of ​​the mat varies depending on the particular application.

[0077] Typically, the nonwoven mat has about 5 to about 60 needle punches per cm 2 (In some embodiments, about 10 to about 20 needle punches / cm 2) is needle punched to obtain a nonwoven mat having a thickness of 10 mm. Optionally, some embodiments of the mounting mat described herein are stitch bonded using conventional techniques (see, for example, U.S. Pat. No. 4,181,514 (Lefkowitz et al.), the disclosure of which is incorporated herein by reference for teachings of stitch bonding of nonwoven mats). Typically, the mat is stitch bonded with organic yarns. A thin layer of organic or inorganic sheet material may be placed on one or both sides of the mat during stitch bonding to prevent or minimize the yarns cutting through the mat. If it is desired that the stitching yarns do not degrade during use, inorganic yarns (e.g., ceramic or metal, such as stainless steel) may be used. The spacing of the stitches is typically about 3 mm to about 30 mm, so that the fibers are uniformly compressed throughout the entire area of ​​the mat.

[0078] The operation of the present disclosure will be further described with reference to the following detailed examples. These examples are provided to further illustrate various specific preferred embodiments and techniques. However, it should be understood that many variations and modifications can be made while remaining within the scope of the present disclosure. EXAMPLES

[0079] These examples are merely illustrative and are not intended to unduly limit the scope of the appended claims. Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the present disclosure are approximations, the numerical values ​​set forth in the specific examples are reported as precisely as possible. However, any numerical value inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements. At the very least, each numerical parameter should be construed by at least applying ordinary rounding techniques in light of the number of reported significant digits, but this is not intended to limit the application of the doctrine of equivalents to the scope of the claims.

[0080] Material Overview All parts, percentages, ratios, etc. in the examples and elsewhere herein are by weight unless otherwise noted. Solvents and other reagents used are available from Sigma-Aldrich Chemical Company (Milwaukee, WI) unless otherwise noted. Additionally, Table 1 provides the abbreviations and sources for all materials used in the following examples. [Table 1]

[0081] Test Method The following test methods were used in evaluating some of the examples of the present disclosure.

[0082] Mullite content determination procedure: Powder X-ray diffraction was used to measure the mullite content. Powders were analyzed on a Rigaku MiniFlex600 diffractometer (Tokyo, Japan) using CuKα radiation. The mullite content of the example materials was determined by measuring the relative peak height of the 26°2θ mullite and comparing it to the same peak after calcining the filaments to 1500°C for 1 hour. The filaments were considered to be 100% converted to mullite in the latter conditions.

[0083] Filament or fiber diameter measurement procedure: The diameter of the ceramic filaments was determined using an optical microscope (Kayence VHX Digital Microscope System) with analysis software. Samples were prepared by spreading a representative sampling of the ceramic filaments on double stick tape attached to a glass slide, and the diameter of at least 40 ceramic filaments was measured at 1000x magnification.

[0084] Images of the fiber mats were also taken using a Scanning Electron (Zeiss EVO MA, Carl Zeiss Microscopy USA, Thornwood, NY).

[0085] Sol-gel Precursor Aluminum chlorohydrate (ACH), colloidal silica, DI water, and polyvinyl alcohol (PVA) were mixed together and concentrated by evaporation under vacuum. As noted above in Table 1, ACH (DelPAC XG) was supplied by USALCO, LLC, the source of colloidal silica was Nalco 1034A, and PVA was supplied by Sekisui Selvol 523. The ceramic composition was 76% by weight alumina and 24% by weight silica, with 10% PVA (by weight of alumina).

[0086] Raw Filament Firing Method: Firing of green filaments can be considered to include two main segments. The first step is a lower temperature pre-firing (burnout) segment where organics are removed and inorganic phases begin to form. The second step is a high temperature crystallization and sintering segment where the filaments densify and the high temperature crystalline phase forms. The two segments may be performed separately (e.g., pre-firing followed by cooling to room temperature and then sintering) or sequentially in a continuous process (e.g., pre-firing followed by immediate sintering without allowing the material to cool).

[0087] The filament web was fired in a continuous roller kiln. The mat was transported through the kiln by a flat array of ceramic rollers. The web was laid on a section of woven Nextel ceramic fiber belt and transported through the kiln.

[0088] The roller kiln has a series of heating zones that gradually and steadily raise the temperature from room temperature to a temperature sufficient to partially or completely crystallize the filaments into mullite, generally from about 1200° C. to about 1350° C.

[0089] During this process, most of the organic components and chlorine (Cl) are volatilized from the filament at 250°C to 600°C. The rate of temperature increase is controlled to avoid decomposing the filament, for example, as the volatiles are removed and the filament is converted to ceramic, shrinks, and crystallizes. It may be desirable to control the volatilization process by introducing air, steam, nitrogen, or other gases into the kiln at 200°C to 700°C. It may also be desirable to vent the generated volatiles. In some embodiments, the kiln also includes an exhaust port for removing volatiles such as CO2 and HCl. The exhaust port also creates a negative pressure inside the kiln to prevent harmful or corrosive volatiles from escaping the kiln.

[0090] Example 1. 280 g of concentrated ACH-silica-PVA sol was diluted with 28 g of DI H2O and mixed to dissolve. The ACH-silica sol had a composition of 76% Al2O3-24% SiO2 and was made from aluminum chlorohydrate (Locron, Inc.), Nalco 1034 silica sol, and polyvinyl alcohol (a 9 wt% solution of Poval 22-88, a high molecular weight, intermediate hydrolysis level (88-89%) polyvinyl alcohol). The amount of PVA was 10 wt% relative to Al2O3. After dilution, the viscosity of the 76:24 sol was 5,000 cP (5 Pa-sec).

[0091] The filaments were blown using a 2 inch (5 cm) BMF die with 50 holes, each 6 mil (0.15 mm) in diameter. Silicone and fluorochemical release agents were used to avoid wetting with the aqueous sol. The blown air to the die was humidified to 90% RH using water spray injected into the chamber with heated air. The air was cooled in a water bath to return to room temperature. The filaments were blown at 15 cubic feet per minute (cfm) (0.007 m 3The die air was blown at 100 rpm (1.5 s / sec) into a space between two quench boxes measuring 12 in. (30 cm) high by 6 in. (15 cm) wide with 11 cfm of heated 85° C. air flow per quench box. The filaments were collected on a vacuum collection screen 30 in. (76 cm) below the blow die.

[0092] The diameter of the raw filaments as spun for each airflow setting is shown below in Table 2. The relative standard deviation of the diameter was 18% and 22% for Samples 1 and 2, respectively. [Table 2]

[0093] The filaments were fired in a continuous kiln at 1285°C for 54 minutes with flowing steam and air. The filaments remained flexible and felt soft to the touch. By SEM microscopy, the filaments were found to be 1.4 μm and 1.9 μm in diameter for samples 1 and 2, respectively, as shown in Table 2 above. As expected, the fired filament diameters shrunk to about 70% of the raw filament diameter, as shrinkage results from evaporation of volatiles and disappearance of porosity. The filaments were many centimeters long, perhaps tens or hundreds of centimeters long, with some filaments essentially continuous. The filament diameters were uniform over their lengths, with a relative standard deviation of diameter between filaments of 20%. There were no shots, and the filament surfaces were relatively smooth.

[0094] The mullite content of the filament of Sample 1 after firing at 1285° C. was 2% as measured by powder XRD. In this test, the mullite XRD peak height (26° 2θ) is compared to a reference sample heated to 1500° C. for 1 hour. After heating to 1330° C., the mullite content increased to 14%.

[0095] An SEM photograph at 5000x of a mat made using filaments of Sample 2 is shown in FIG.

[0096] Example 2.

[0097] An ACH-silica sol was prepared with a composition of 76% Al2O3-24% SiO2, and 10 wt% PVA relative to Al2O3. After dilution, the viscosity of the 76:24 sol was 9,800 cP (9.8 Pa-sec).

[0098] The sol was blown using a BMF die with 50 holes as in Example 1, except that the holes had a diameter of 15 mils (0.38 mm). The die gap was 30 mils (0.76 mm) and the standoff was +20 mils (0.50 mm). The sol was pressurized to 0.4 psi (3 Pa).

[0099] The filaments collected on the vacuum screen were uniform and dry. 3 With a die air of 9 cfm (0.004 m / sec), the green filament diameter was 5.3 μm. 3 / sec), the diameter decreased to 3.7 μm. The relative standard deviation of the diameter was 7% and 14% for the two samples, respectively. The fired diameter is expected to be 2.6 μm, which is 70% of the raw diameter. This example shows that BMF filaments can be produced using the large 15 mil holes, but larger diameters are not preferred.

[0100] The tensile strength of the nonwoven mat of Example 2 was measured using a tensile tester (Instron, Inc.). 2The webs were cut to 7 / 8 inch (22.2 mm) wide and 3 inch (76.2 mm) long and gripped using rubber faced grips with a 1 inch (25.4 mm) gauge length and 20 psi (146 Pa) grip pressure and loaded to failure at 0.5 inch (12.7 mm) / min. The mat thickness was measured with a TMI tester so that the strength could be calculated. Mats fired at 1285°C had tensile strengths in excess of 200 psi (1460 Pa). 65% mullite webs fired to 1330°C had tensile strengths up to 60 psi (410 Pa).

[0101] Detailed results are shown in Table 3 below. [Table 3]

[0102] The ability of the mat of Example 2 to withstand repeated bending was determined using a bending durability tester (Tinnius Olsen Testing Machine Co, Inc.). The test conforms to ASTM D2176 and consists of folding the mat over an arc of 270 degrees at 30-60 cycles per minute. One cycle is a double fold, bending the mat 135 degrees in one direction and then 135 degrees in the opposite direction. The machine also uses a pulley and dead load arrangement to apply a load of 100 grams to the sample. The gauge length of the mat in the tester was 1.5 inches. The mat was gripped in a steel fixture with a 70 mil wide gap with a 45 degree tapered sharp edge. This bending over a sharp edge provides a severe test for ceramic materials.

[0103] Mats with greater than 60% mullite had flexural endurance of 18 to 140 double cycles under a 100 g load and endured greater than 2000 cycles at zero tensile load without fracture. The results are shown in Table 4 below. [Table 4]

[0104] Example 3A. The filaments were spun through a 6 mil (0.15 mm) die as in Example 1, with die air flow ranging from 15 cfm (7 liters / min) to 30 cfm (14 liters / min). As the air flow increased, the diameter decreased from 4.1 μm to 3.1 μm, consistent with an increase in drawing force from the die air.

[0105] When the sol pressure was reduced to 7 psi (48 Pa), the filament diameter decreased to 2.1 μm (equivalent to 1.4 μm after firing). Based on the collected weight, the flow rate of collected filaments decreased from 0.19 g / hole / min to 0.05 g / hole / min. This demonstrates that the filament diameter can be reduced by reducing the sol pressure and the flow per hole. The relative standard deviation was less than 30% for all conditions.

[0106] The results are shown in Table 5 below and plotted in Figure 5 for Samples 3-6 where the die air flow rate was increased from 15 cfm to 30 cfm (7 liters / min to 14 liters / min) at a sol pressure of 15 psi (103 Pa). [Table 5]

[0107] Example 3B. Approximately 200 g / m produced from filaments of samples 3 and 7 2 The filament mats having a web basis weight of 1.001 mm were fired to 1300° C. as in Example 1. The filament diameters after firing were 63% and 71% of the green (unfired) diameter for the two filaments, respectively. The results are shown in Table 6 below. Increasing the air flow rate and speed results in smaller filament diameters. [Table 6]

[0108] The mullite content of sample 7 after firing to 1300°C was 3% and after firing to 1330°C it was 72%. A photograph of the 1330°C fired mat is shown in Figure 6. The mat or web on the right side of Figure 6 has been folded twice. The mat can be folded and unfolded without visible damage, indicating the flexibility and soft feel of this small diameter mat.

[0109] The graph in FIG. 7 shows the evolution of crystalline mullite as a function of heat treatment temperature for Sample 7. The mullite content increases from about 2% to more than about 50% above 1315°C. At the same time, the γ-Al2O3 content decreases to 25% relative to the height of the peak at 2θ=67° at 1285°C. A third phase, θ-Al2O3, appears above 1360°C. The presence of transition aluminas γ-Al2O3 and θ-Al2O3 indicates that a metastable alumina phase occurs at very high temperatures where one would expect α-Al2O3 to be found, with a composition of 76% Al2O3, higher than the 72% Al2O3 in 3Al2O3-2SiO2 mullite.

[0110] Example 4. ACH-silica sol with the composition 76% Al2O3-24% SiO2, and 10 wt% PVA relative to Al2O3 was prepared at 2,000 cP (2 Pa-sec). The sol was blown using a BMF die with 80 6 mil (0.15 mm) holes as in Example 1. The die tip setback was -0.02 in. (0.50 mm) and the die gap was 0.03 in. (0.76 mm). The sol was pressurized to 6 psi (41 Pa). At less than 10 cfm (5 liters / min) of die air, fiberization was poor and the sol dripped from many of the holes in the die. When the die was at 13 cfm (6 liters / min), the filaments were uniform and dry.

[0111] At a sol pressure of 6 psi (41 Pa), the green filament diameter was 3.1 μm and the collection rate was 1.3 g / min. When the sol pressure was reduced to 3 psi (21 Pa), the green filament diameter decreased to 2.9 μm (equivalent to 2.0 μm after firing). The RSDs were 19% and 32%, respectively.

[0112] Example 5. An ACH-silica sol with the composition 76% Al2O3-24% SiO2, and 10 wt% PVA relative to Al2O3 was prepared at 4,000 cP (4 Pa-sec). The sol was blown using a BMF die with 80 6 mil (0.15 mm) holes as in Example 1. The die tip setback was -0.02 in. (0.50 mm) and the die gap was 0.03 in. (0.76 mm). The sol was pressurized to 12.5 psi (86 Pa). The filaments were blown with 25 cfm (12 liters / min) of die air.

[0113] The resulting filaments were uniform and dry. The raw filament diameter was 3.8 μm with an RSD of 17% and after firing the diameter was 3.3 μm with a measured RSD of 28%. The filaments were collected at 2.35 g / min or 0.29 g / hole / min. The web basis weight was 250 g / m 2 A flexible and soft nonwoven mat was produced.

[0114] After firing at 1285° C. and 1330° C., the mullite content was 2 wt % and 58 wt %, respectively. The matte was flexible after both firing conditions.

[0115] Throughout this specification, references to "one embodiment," "a particular embodiment," "one or more embodiments," or "an embodiment" mean that the particular feature, structure, material, or characteristic described in connection with that embodiment is included in at least one of the particular exemplary embodiments of the disclosure, regardless of whether the term "embodiment" is preceded by the term "embodiment." Thus, the appearances of phrases such as "in one or more embodiments," "in a particular embodiment," "in one embodiment," or "in an embodiment" in various places throughout this specification do not necessarily refer to the same particular exemplary embodiments of the disclosure. Furthermore, particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.

[0116] Although some exemplary embodiments have been described in detail herein, it is understood that those skilled in the art can easily imagine modifications, variations, and equivalents of these embodiments after understanding the above content. Therefore, it should be understood that the present disclosure is not unduly limited to the exemplary embodiments described so far. In particular, as used herein, the recitation of numerical ranges by end values ​​is intended to include all numerical values ​​subsumed within the range (e.g., 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.80, 4, and 5). In addition, all numerical values ​​used herein are intended to be modified by the term "about".

[0117] Furthermore, all publications and patents referenced herein are incorporated by reference in their entirety to the same extent as if each individual publication or patent was specifically and individually indicated to be incorporated by reference. Various exemplary embodiments have been described. These and other embodiments are within the scope of the following claims. Below are exemplary embodiments. [Item 1] 1. A nonwoven article comprising a plurality of polycrystalline aluminosilicate ceramic filaments intertwined to form a cohesive nonwoven mat, wherein each of the aluminosilicate ceramic filaments in the mat has an average diameter of less than about 2 microns (μm), and the aluminosilicate ceramic filaments comprise, on average, about 15% to about 80% crystalline mullite by weight. [Item 2] Item 2. The nonwoven article of item 1, wherein the aluminosilicate ceramic filaments comprise about 50% to about 80% by weight crystalline mullite. [Item 3] 3. The nonwoven article of claim 1 or 2, wherein the nonwoven mat further comprises fibers selected from the group consisting of alumina fibers, silica fibers, silicon carbide fibers, silicon nitride fibers, carbon fibers, glass fibers, metal fibers, alumina-phosphorus pentoxide fibers, alumina-boria-silica fibers, zirconia fibers, zirconia-alumina fibers, zirconia-silica fibers, non-fibrous materials selected from the group consisting of aerogels and glass bubbles, and mixtures or combinations thereof. [Item 4] 4. The nonwoven article of any one of the preceding claims, wherein the plurality of polycrystalline aluminosilicate ceramic filaments have an alumina to silica ratio in the range of 60:40 to 90:10 by weight. [Item 5] 5. The nonwoven article of any one of the preceding claims, wherein the plurality of polycrystalline aluminosilicate ceramic filaments have an alumina to silica ratio of about 76:24 by weight. [Item 6] 6. The nonwoven article of any one of the preceding claims, wherein the plurality of polycrystalline aluminosilicate ceramic filaments comprises about 73% to about 80% alumina. [Item 7] 7. The nonwoven article of any one of the preceding claims, wherein the nonwoven mat further comprises a binder for binding the plurality of polycrystalline aluminosilicate ceramic filaments together. [Item 8] 8. The nonwoven article of claim 7, wherein the binder is selected from (meth)acrylic (co)polymers, poly(vinyl) alcohols, poly(vinyl)pyrrolidones, poly(ethylene oxides), poly(vinyl) acetates, polyolefins, polyesters, and combinations thereof. [Item 9] 8. The nonwoven article of claim 7, wherein the binder is selected from silica, alumina, zirconia, kaolin clay, bentonite clay, silicates, mica particles, and combinations thereof. [Item 10] Item 10. The nonwoven article of any one of the preceding items, wherein the article is selected from the group consisting of a filtration article, a thermal insulation article, a sound insulation article, a fire protection article, a mounting mat for a vehicle component, a gasket, a catalyst support, and combinations thereof. [Item 11] 1. A method for producing a nonwoven web, comprising: flowing an aqueous ceramic precursor sol including silica particles, water, and a hydrolyzable aluminum-containing compound through at least one orifice to produce at least one substantially continuous filament; attenuating the filaments with a high velocity air stream to draw the filaments to an average diameter of 10 micrometers (μm) or greater; removing at least a portion of the water from the at least one substantially continuous filament to at least partially dry the at least one substantially continuous filament; collecting the at least partially dried filaments as a raw nonwoven web on a collecting surface; and heating the green nonwoven web at a temperature and for a time sufficient to convert the green nonwoven web into a coherent mat comprising at least one polycrystalline aluminosilicate ceramic filament comprising about 15% to about 80% by weight crystalline mullite, wherein each of the aluminosilicate ceramic filaments in the coherent mat has an average diameter of less than 2 microns (μm). [Item 12] Item 12. The method of claim 11, further comprising directing a flow of gas proximate to the at least one substantially continuous filament to at least partially dry the at least one substantially continuous filament, and optionally, the flow of gas is heated. [Item 13] 13. The method according to claim 11 or 12, wherein the aqueous ceramic precursor sol comprises aluminum chlorohydrate, silica, and polyvinyl alcohol (PVA). [Item 14] Item 14. The method according to item 13, wherein the aqueous ceramic precursor sol further comprises an antifoaming agent. [Item 15] 15. The method according to any one of items 11 to 14, wherein the plurality of polycrystalline aluminosilicate ceramic filaments have an alumina to silica ratio in the range of 60:40 to 90:10 by weight. [Item 16] Item 16. The method of claim 15, wherein the plurality of polycrystalline aluminosilicate ceramic filaments have an alumina to silica ratio of about 76:24 by weight. [Item 17] Item 16. The method of claim 15, wherein the plurality of polycrystalline aluminosilicate ceramic filaments comprises about 73% to about 80% alumina. [Item 18] 18. The method according to any one of items 11 to 17, wherein the aqueous ceramic precursor sol contains about 10% by weight of PVA relative to the weight of alumina. [Item 19] 19. The method according to any one of items 11 to 18, wherein the at least one polycrystalline aluminosilicate ceramic filament comprises at least 50 wt.% crystalline mullite. [Item 20] 20. The method of claim 19, wherein the at least one polycrystalline aluminosilicate ceramic filament comprises at least 70% by weight of crystalline mullite. [Item 21] 21. The method of any one of items 11 to 20, further comprising at least one of needle punching, stitch bonding, hydroentangling, binder impregnation, and cutting of the cohesive mat.

Claims

1. 1. A nonwoven article comprising a plurality of polycrystalline aluminosilicate ceramic filaments intertwined to form a cohesive nonwoven mat, wherein each of the aluminosilicate ceramic filaments in the mat has an average diameter of less than about 2 microns (μm), and the aluminosilicate ceramic filaments comprise, on average, about 15% to about 80% by weight crystalline mullite.

2. 10. The nonwoven article of claim 1, wherein the aluminosilicate ceramic filaments comprise from about 50% to about 80% by weight crystalline mullite.

3. 3. The nonwoven article of claim 1 or 2, wherein the nonwoven mat further comprises fibers selected from the group consisting of alumina fibers, silica fibers, silicon carbide fibers, silicon nitride fibers, carbon fibers, glass fibers, metal fibers, alumina-phosphorus pentoxide fibers, alumina-boria-silica fibers, zirconia fibers, zirconia-alumina fibers, zirconia-silica fibers, non-fibrous materials selected from the group consisting of aerogels and glass bubbles, and mixtures or combinations thereof.

4. The nonwoven article of any one of claims 1 to 3, wherein the plurality of polycrystalline aluminosilicate ceramic filaments have an alumina to silica ratio in the range of 60:40 to 90:10 by weight.

5. The nonwoven article of any one of claims 1-4, wherein the plurality of polycrystalline aluminosilicate ceramic filaments comprises about 73% to about 80% alumina.

6. The nonwoven article of any one of claims 1 to 5, wherein the nonwoven mat further comprises a binder for binding the plurality of polycrystalline aluminosilicate ceramic filaments together.

7. 7. The nonwoven article of any one of claims 1-6, wherein the article is selected from the group consisting of a filtration article, a thermal insulation article, a sound insulation article, a fire protection article, a mounting mat for a vehicle component, a gasket, a catalyst support, and combinations thereof.

8. 1. A method for producing a nonwoven web, comprising: flowing an aqueous ceramic precursor sol comprising silica particles, water, and a hydrolyzable aluminum-containing compound through at least one orifice to produce at least one substantially continuous filament; attenuating the filaments with a high velocity air stream to draw the filaments to an average diameter of 10 micrometers (μm) or greater; removing at least a portion of the water from the at least one substantially continuous filament to at least partially dry the at least one substantially continuous filament; collecting the at least partially dried filaments as a raw nonwoven web on a collecting surface; heating the green nonwoven web at a temperature and for a time sufficient to convert the green nonwoven web into a coherent mat comprising at least one polycrystalline aluminosilicate ceramic filament comprising from about 15% to about 80% by weight crystalline mullite, wherein each of the aluminosilicate ceramic filaments in the coherent mat has an average diameter of less than 2 microns (μm).

9. 10. The method of claim 8, further comprising directing a flow of gas proximate to the at least one substantially continuous filament to at least partially dry the at least one substantially continuous filament, and optionally, the flow of gas is heated.

10. 10. The method according to claim 8 or 9, wherein the aqueous ceramic precursor sol comprises aluminum chlorohydrate, silica, and polyvinyl alcohol (PVA).

11. The method of claim 10 , wherein the aqueous ceramic precursor sol further comprises an antifoaming agent.

12. The method of any one of claims 8 to 11, wherein the plurality of polycrystalline aluminosilicate ceramic filaments have an alumina to silica ratio in the range of 60:40 to 90:10 by weight.

13. The method of claim 12, wherein the plurality of polycrystalline aluminosilicate ceramic filaments comprises about 73% to about 80% alumina.

14. The method according to any one of claims 8 to 13, wherein the aqueous ceramic precursor sol comprises about 10 wt% PVA relative to the weight of alumina.

15. The method according to any one of claims 8 to 14, wherein the at least one polycrystalline aluminosilicate ceramic filament comprises at least 50% by weight of crystalline mullite.

Citation Information

Patent Citations

  • Acid resistant ceramic paper

    JP1986239100A

  • Catalyst carrier holding material and catalytic converter

    JP2003020938A

  • Light-weight inorganic fiber molded body and method for producing the same

    JP2011208344A

  • Compositions incorporating silica fibers

    JP2021518493A

  • Polycrystalline aluminosilicate ceramic filament nonwoven mat and method for producing same

    JP2023508111A