Method for forming lysine-like multilayer coating film and lysine-like multilayer coating film
The ricin-like laminated coating film method addresses the issues of followability, waterproofness, and weather resistance in ricin-based paints by using an undercoat and topcoat process with specific resin and pigment compositions, ensuring excellent substrate adhesion and durability without increasing costs or altering the matte finish.
Patent Information
- Application Number
- JP2020127137
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-28
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-07-28
AI Technical Summary
Conventional ricin-based paints suffer from poor followability to the substrate, low waterproofness, and low weather resistance, which are exacerbated by the need for additional clear coats that increase costs and alter the matte appearance.
A method involving an undercoat film formation process using a water-based emulsion resin with extender pigments and a topcoat film formation process using aggregate and colored gel particles, which includes mixing aggregates and aqueous dispersion medium at the application site, ensuring substrate followability, waterproofness, and high weather resistance.
The method produces a ricin-like laminated coating film with improved followability, waterproofness, and weather resistance while maintaining a matte appearance, reducing manufacturing and transportation costs, and avoiding the glossy finish of clear coats.
Smart Images

Figure 0007594251000001 
Figure 0007594251000002
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for forming a lysine-like multilayer coating film and a lysine-like multilayer coating film. More specifically, the present invention relates to a method for forming a lysine-like multilayer coating film using an undercoat paint and a topcoat paint, and a lysine-like multilayer coating film.
[0002] Various types of paint are applied to buildings and other structures. For example, various types of paint are frequently applied to the interior and exterior of buildings to form a coating film in order to protect the structure and improve the design.
[0003] Some surface coatings for such surfaces use lysine-based paints, which generally contain synthetic resin, granular materials (natural stone, ceramic, aggregate, etc.), and color pigments.
[0004] Using such lysine-based paints results in a subdued, calm appearance. Furthermore, lysine-based paints create a highly breathable coating, which helps prevent deterioration of the wood of the house. Furthermore, they are generally inexpensive, which helps keep painting costs down. Lysine-based paints, which have such excellent features, have been used for a long time.
[0005] For example, Patent Document 1 describes an exterior lysine paint that "consists of (a) 100 parts by weight (solids content) of a hydroxyl resin having an average particle size of 0.05 μm or less, (b) 10 to 200 parts by weight of a colorant, (c) 200 to 1,000 parts by weight of an aggregate, (d) 100 to 500 parts by weight of a filler, (e) 100 to 600 parts by weight of water, and (f) a titanium coupling agent, wherein the amount of component (f) is 0.1 to 10 parts by weight per 100 parts by weight of the total amount of components (b), (c), and (d)," and claims that this "has resulted in the completion of a water-based exterior lysine paint that adheres well to chalky substrates, presents an excellent appearance after coating formation, and has good weather resistance." [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 56-99266 A (Claim 1) Summary of the Invention [Problem to be solved by the invention]
[0007] However, conventional lysine-based paints, including the paint disclosed in Patent Document 1, have drawbacks such as poor conformability to the substrate, prone to cracking, poor waterproofing, and poor weather resistance.
[0008] In recent years, in particular, awareness of life cycle costs has grown, and there is an increasing need for highly weather-resistant paints that can extend the repair cycle and reduce the number of painting works, not just for the paint unit price. Among these, lysine-based paints have a distinctive appearance with a subdued luster that cannot be replaced by other paints, but they have drawbacks such as low weather resistance, so they have tended to be avoided, especially in recent years.
[0009] Therefore, in order to ensure the weather resistance of lysine-based paints, it has been considered to apply a clear coat as an additional process, but this not only increases costs but also makes the exterior glossy, losing the calm matte finish that is unique to lysine-based paints.
[0010] The present invention has been made with the above-mentioned matters in mind, and aims to provide a method for forming a lysine-style multilayer coating film that has excellent conformability to the substrate, waterproofness, and weather resistance, and a lysine-style multilayer coating film. [Means for solving the problem]
[0011] In order to solve the above problems, a method for forming a lysine-like multilayer coating film is provided, which includes a primer coating film formation process in which a primer coating is applied to the surface of a surface to be coated, such as an exterior wall, to form a film, and a topcoat coating film formation process in which a topcoat coating is applied to the surface of the primer coating film formed by the primer coating film formation process to form a film, wherein the primer coating contains 20 to 200 parts by weight of a color pigment and 50 to 800 parts by weight of an extender pigment having an average particle size of 1 to 100 μm per 100 parts by weight of solids of a first water-based emulsion resin, and the topcoat coating contains 200 to 1200 parts by weight of an aggregate and 50 to 800 parts by weight of colored gel particles per 100 parts by weight of solids of a second water-based emulsion resin.
[0012] In this method for forming a lysine-like multilayer coating film, the undercoat coating film ensures conformability to the substrate and waterproofness, while the topcoat coating film ensures a lysine-like matte appearance and high weather resistance. Specifically, the primer paint contains 50 to 800 parts by weight of an extender pigment with an average particle size of 1 to 100 μm per 100 parts by weight of the solid content of the water-based emulsion resin, which improves application suitability and ensures base conformability and waterproofness. Furthermore, when the primer contains 50 to 800 parts by weight of an extender pigment with an average particle size of 1 to 100 μm per 100 parts by weight of the solid content of the water-based emulsion resin, the topcoat, which contains a large amount of aggregate, is better suited to be applied to the primer film, resulting in better waterproofing. Furthermore, a lysine-like design can be achieved by adding 200 to 1,200 parts by weight of aggregate to 100 parts by weight of the solids content of the aqueous emulsion resin in the topcoat paint. While an aggregate-rich formulation can achieve a lysine-like design, this has traditionally come at the expense of weather resistance. However, the present inventors surprisingly discovered that even with an aggregate-rich formulation, weather resistance can be significantly improved by adding 50 to 800 parts by weight of colored gel particles to 100 parts by weight of the solids content of the aqueous emulsion resin. The present invention is based on this finding.
[0013] The method for forming a lysine-like multilayer coating film can include a topcoat paint aggregate blending step in which, before the topcoat coating film formation step, aggregate and an aqueous dispersion medium are mixed and stirred with a topcoat base paint, which is a paint that serves as the base for the topcoat paint and does not contain aggregate, to form the topcoat paint.
[0014] In this method of forming a lysine-like multilayer coating, the topcoat base paint manufactured in a factory or other facility is transported to the application site, and before the topcoat film formation process (before the application work), aggregate and an aqueous dispersion medium are mixed and stirred into the topcoat base paint. Because the aggregate is not mixed and stirred during the topcoat base paint manufacturing process, manufacturing costs (such as labor hours) are reduced, and the cost of the topcoat paint itself is also reduced. While the aggregate is mixed and stirred with the topcoat base paint before application, it is common to mix and homogenize the paint before application, and mixing and stirring the aggregate as part of this process is thought to avoid significant workload during application. Furthermore, because the topcoat base paint does not contain aggregate, the amount of aqueous dispersion medium in the topcoat base paint can be significantly reduced, so the volume and weight of the topcoat base paint are smaller than those of the topcoat paint, and transportation costs can also be significantly reduced. Note that the aqueous dispersion medium added to the topcoat base paint together with the aggregate can be obtained from tap water or the like at the application site, for example.
[0015] The method for forming a lysine-like multilayer coating film may also be such that the colored gel particles contained in the topcoat paint contain a third water-based emulsion resin, a color pigment, and a hydrogel.
[0016] This method for forming a lysine-like multilayer coating film can form a lysine-like multilayer coating film with higher weather resistance.
[0017] The method for forming a lysine-like multilayer coating film can also be such that the colored gel particles contained in the topcoat paint are obtained by adding a colored gel raw material composition containing a third aqueous emulsion resin, a colored pigment, and a hydrogel component to an aqueous solution containing a hydrogel insolubilizer, and the content of the hydrogel component in the colored gel raw material composition is 5 to 90 parts by weight in solid content per 100 parts by weight of the solid content of the third aqueous emulsion resin.
[0018] This method for forming a lysine-like multilayer coating film results in colored gel particles with excellent flexibility, and by using these in a top coat paint, the colored gel particles are less likely to be crushed into small pieces when the aggregate is mixed and stirred in the top coat paint aggregate mixing process, etc.
[0019] Here, the method for forming a lysine-like multilayer coating film can be such that at least one of the first aqueous emulsion resin contained in the primer paint, the second aqueous emulsion resin contained in the top coat paint, and the third aqueous emulsion resin of the colored gel particles contained in the top coat paint is an acrylic silicone resin emulsion.
[0020] Acrylic silicone resin emulsions have excellent weather resistance and can form coating films with even better weather resistance.
[0021] The method for forming a lysine-style multilayer coating film can be one in which the colored gel particles contained in the top coat paint are of one color, or can be one in which the colored gel particles contained in the top coat paint are of two or more colors.
[0022] The topcoat paint may contain 10 to 80 parts by weight of acrylic beads per 100 parts by weight of the solid content of the second aqueous emulsion resin, thereby forming a lysine-like multilayer coating film.
[0023] This method of forming a lysine-like multilayer coating film results in a more subdued, lysine-like appearance due to the matte effect of the acrylic beads.
[0024] The above problems can also be solved by a lysine-style multilayer coating film comprising an undercoat film formed by applying an undercoat paint to the surface of a surface to be painted, such as an exterior wall, and a topcoat film formed by applying a topcoat paint to the surface of the undercoat film, wherein the undercoat film contains 20 to 200 parts by weight of a coloring pigment and 50 to 800 parts by weight of an extender pigment having an average particle size of 1 to 100 μm per 100 parts by weight of a first resin, and the topcoat film contains 200 to 1200 parts by weight of an aggregate and 30 to 500 parts by weight of dried coloring gel particles (solid content) per 100 parts by weight of a second resin. The first resin is the dried product (solid content) of the first aqueous emulsion resin contained in the primer paint, and the second resin is the dried product (solid content) of the second aqueous emulsion resin contained in the top coat paint.
[0025] Here, the dried colored gel particles contained in the topcoat coating film can be a lysine-like laminated coating film containing a third resin, a color pigment, and a dried hydrogel (solid content). The third resin is a dried product (solid content) of the third aqueous emulsion resin contained in the colored gel particles.
[0026] The dried colored gel particles contained in the top coat can also be a lysine-like laminated coat containing 5 to 90 parts by weight of dried hydrogel per 100 parts by weight of the third resin.
[0027] The present invention can also provide a lysine-like laminated coating film in which at least one of the first resin contained in the undercoat coating film, the second resin contained in the topcoat coating film, and the third resin contained in the dried product of the colored gel particles is an acrylic silicone resin.
[0028] The top coat film may be a lysine-style multilayer coating film in which the dried colored gel particles contained in the top coat film are one color, or the top coat film may be a lysine-style multilayer coating film in which the dried colored gel particles contained in the top coat film are two or more colors.
[0029] The topcoat film may also be a lysine-type laminated coating film containing 10 to 80 parts by weight of acrylic beads per 100 parts by weight of the solid content of the second resin. [Effects of the Invention]
[0030] According to the present invention, it is possible to provide a method for forming a lysine-like multilayer coating film that is excellent in conformity to the substrate, waterproofness, and weather resistance, and a lysine-like multilayer coating film. DETAILED DESCRIPTION OF THE INVENTION
[0031] Hereinafter, a method for forming a lysine-like multilayer coating film will be described by way of example. The method for forming a lysine-like multilayer coating film comprises a primer coating film forming step and a topcoat coating film forming step. Each step will be described in detail below, but the present invention is not limited to the following embodiments. In this specification, the "average particle size" refers to the 50% diameter of the weight cumulative particle size distribution, and the particle size distribution was measured using a laser diffraction particle size distribution measuring device (HRA Microtrack manufactured by Nikkiso Co., Ltd.).
[0032] [Undercoat coating process] The primer coating film forming process is a process of applying a primer paint to the surface of a surface to be painted, such as an exterior wall, to form a film. First, the primer paint used in this process will be described.
[0033] 1. Primer paint The primer paint contains a first water-based emulsion resin, a color pigment, and an extender pigment. Each material will be described in detail below. In addition, with regard to the content of each material contained in the primer paint, when it is based on 100 parts by weight of the solid content of the first aqueous emulsion resin, the same content applies to the primer paint film, and in this case, "100 parts by weight of the solid content of the first aqueous emulsion resin" is read as "100 parts by weight of the first resin."
[0034] a) First aqueous emulsion resin The resin component of the primer paint is a water-based emulsion resin (first water-based emulsion resin). The water-based emulsion resin is a fine particle resin that is hydrophilized with an emulsifier and exists in a dispersed state in water. The resin component of the first aqueous emulsion resin is not particularly limited. For example, known synthetic resins such as acrylic resin, ethylene-acrylic resin, vinyl acetate-acrylic resin, styrene-acrylic resin, urethane resin, silicone resin, urethane-acrylic resin, and silicone-acrylic resin can be used. Among them, from the viewpoint of weather resistance, it is preferable to use acrylic resin, particularly acrylic silicone resin. For example, acrylic silicone resin and ceramic-modified acrylic silicone resin are suitable.
[0035] An example of the acrylic silicone resin emulsion is "Polydurex G-624" manufactured by Asahi Kasei Corporation.
[0036] b) Color pigments The primer paint contains a color pigment. Examples of color pigments that can be used include, but are not limited to, titanium oxide, yellow iron oxide, red iron oxide (ferric oxide: red iron oxide), phthalocyanine blue, ochre, ultramarine blue, and carbon black. When a white primer paint is used, titanium oxide is often used as a white pigment.
[0037] The amount of the color pigment in the undercoat paint is 20 to 200 parts by weight per 100 parts by weight of the solid content of the first aqueous emulsion resin.
[0038] The amount of the color pigment to be blended is preferably 25 to 150 parts by weight, more preferably 30 to 120 parts by weight, even more preferably 35 to 90 parts by weight, and most preferably 40 to 80 parts by weight, per 100 parts by weight of the solid content of the first aqueous emulsion resin.
[0039] c) Extender pigment The primer paint contains an extender pigment having an average particle size of 1 to 100 μm, such as heavy calcium carbonate, light calcium carbonate, kaolin, clay, china clay, diatomaceous earth, hydrous fine silica powder, talc, barite powder, barium sulfate, precipitated barium sulfate, barium carbonate, magnesium carbonate, silica powder, or aluminum hydroxide.
[0040] The amount of the extender pigment in the undercoat paint is 50 to 800 parts by weight per 100 parts by weight of the solid content of the first aqueous emulsion resin.
[0041] The content of the extender pigment in the primer paint is preferably 200 to 700 parts by weight, more preferably 300 to 600 parts by weight, even more preferably 350 to 550 parts by weight, and most preferably 400 to 500 parts by weight per 100 parts by weight of the solids content of the first aqueous emulsion resin.
[0042] The average particle size of the extender pigment in the undercoat paint is preferably 1 to 60 μm, more preferably 5 to 50 μm, even more preferably 10 to 30 μm, and most preferably 15 to 25 μm.
[0043] The first aqueous emulsion resin, color pigment, and extender pigment are mixed and stirred to obtain a primer paint. At this time, aggregates and various additives (e.g., surfactants, preservatives, thickeners) can be added as needed.
[0044] 2. How to apply primer paint The surface to which the primer paint is applied is not particularly limited. For example, it can be applied to the exterior or interior walls of a building. The material of the surface to be painted is also not particularly limited. For example, porcelain, tile, concrete, ALC panel, mortar, siding board, extruded board, gypsum board, and plastic board can be used. Furthermore, it can be used not only on the surfaces of newly constructed buildings, but also when repainting the surfaces of existing buildings.
[0045] The method for applying the primer to the surface to be coated is not particularly limited. For example, it can be applied by spray coating or roller coating. After applying the primer, the surface can be smoothed using a trowel or the like before the paint dries. After applying the primer, it is dried to form a film. After forming the film, it is preferable to allow a curing period of about one day.
[0046] The formed primer coating film contains 20 to 200 parts by weight of a color pigment and 50 to 800 parts by weight of an extender pigment having an average particle size of 1 to 100 μm, relative to 100 parts by weight of the first resin, which is the dried product (solid content) of the first aqueous emulsion resin. The next step, the topcoat film forming step, will now be described.
[0047] [Topcoat coating process] The topcoat coating film forming step is a step of applying a topcoat paint to the surface of the undercoat coating film formed in the undercoat coating film forming step to form a film. First, the topcoat paint used in this step will be described.
[0048] 1. Topcoat paint The topcoat paint contains a second water-based emulsion resin, aggregate, and colored gel particles. Each of these materials will be described in detail below. In addition, with regard to the content of each material contained in the topcoat paint, if it is based on 100 parts by weight of the solid content of the second aqueous emulsion resin, the same content applies to the topcoat paint film, and in this case, "100 parts by weight of the solid content of the second aqueous emulsion resin" shall be read as "100 parts by weight of the second resin."
[0049] a) Second aqueous emulsion resin The resin component of the top coat paint is also a water-based emulsion resin, just like the primer paint. The resin component of the second aqueous emulsion resin is not particularly limited. Among them, as with the undercoat paint, it is preferable to use an acrylic resin, particularly an acrylic silicone resin, from the viewpoint of weather resistance. For example, an acrylic silicone resin or a ceramic-modified acrylic silicone resin is suitable.
[0050] The second aqueous emulsion resin, which is the resin component of the topcoat paint, can be the same resin as the first aqueous emulsion resin, which is the resin component of the undercoat paint.
[0051] b) Aggregate The topcoat paint also contains aggregates. Examples of aggregates include, but are not limited to, kansui stone, silica sand, and calcium carbonate. Among these, calcium carbonate is preferably used to form a lysine-like coating film.
[0052] The average particle size of the aggregate in the top coat paint is preferably 100 to 500 μm, more preferably 150 to 400 μm, even more preferably 200 to 350 μm, and most preferably 250 to 300 μm.
[0053] The amount of aggregate blended in the top coat paint is 200 to 1200 parts by weight per 100 parts by weight of the solid content of the second aqueous emulsion resin.
[0054] The amount of aggregate in the top coat paint is preferably 400 to 1150 parts by weight, more preferably 500 to 1100 parts by weight, even more preferably 600 to 1050 parts by weight, and most preferably 700 to 1000 parts by weight per 100 parts by weight of the solids content of the second aqueous emulsion resin.
[0055] c) Colored gel particles The topcoat paint contains colored gel particles. Conventional lysine-based paints contain colored pigments, but the topcoat paint of the present invention contains colored gel particles instead of colored pigments, thereby ensuring weather resistance. The colored gel particles preferably include a third aqueous emulsion resin, a color pigment, and a hydrogel. The colored gel particles can be obtained, for example, by adding an emulsion composition (referred to as a colored gel raw material composition) containing a third aqueous emulsion resin, a color pigment, and a hydrogel component (a gel main raw material) to an aqueous solution containing a hydrogel insolubilizer (a gelling agent).
[0056] Here, the term "particles" in colored gel particles includes spherical, disc-shaped, and similar shapes. Disc-shaped includes not only plate-shaped objects having a perfect circle, ellipse, and the like, but also plate-shaped objects of similar shapes, such as irregular shapes that are close to a circle. For example, flake-shaped objects are also included in the term "disk-shaped particles." Disk-shaped particles include those of various thicknesses.
[0057] The amount of colored gel particles in the topcoat paint is preferably 75 to 600 parts by weight, more preferably 100 to 500 parts by weight, even more preferably 150 to 400 parts by weight, and most preferably 200 to 300 parts by weight, per 100 parts by weight of the solids content of the second aqueous emulsion resin. The content of the dry matter (solid content) of the colored gel particles in the topcoat coating film will be described later.
[0058] Hereinafter, examples of the materials constituting the colored gel particles will be described. In addition, with regard to the content of each material contained in the colored gel particles, when it is based on 100 parts by weight of the solid content of the third aqueous emulsion resin, the same content applies to the dried matter (solid content) of the colored gel particles, and in this case, "100 parts by weight of the solid content of the third aqueous emulsion resin" is read as "100 parts by weight of the third resin."
[0059] i. Third water-based emulsion resin The colored gel particles contain a water-based emulsion resin (third water-based emulsion resin).
[0060] The resin component of the third aqueous emulsion resin is not particularly limited. For example, known synthetic resins such as acrylic resin, ethylene-acrylic resin, vinyl acetate-acrylic resin, styrene-acrylic resin, urethane resin, silicone resin, urethane-acrylic resin, and silicone-acrylic resin can be used. Among them, from the viewpoint of weather resistance, it is preferable to use acrylic resin, particularly acrylic silicone resin. For example, acrylic silicone resin and ceramic-modified acrylic silicone resin are suitable.
[0061] An example of the acrylic silicone resin emulsion is "Polydurex G-625" manufactured by Asahi Kasei Corporation.
[0062] ii. Color pigments The colored gel particles contain a colored pigment, such as, but not limited to, titanium oxide, yellow iron oxide, red iron oxide (ferric oxide: red iron oxide), phthalocyanine blue, ochre, ultramarine, and carbon black.
[0063] The content of the color pigment in the color gel particles is preferably 50 to 250 parts by weight, more preferably 100 to 200 parts by weight, based on 100 parts by weight of the solid content of the third aqueous emulsion resin.
[0064] iii. Hydrogel Hydrogels have a structure in which water is held in a hydrogel-forming substance to form a gel. The hydrogel-forming substance is a compound that exhibits gelation by forming a network structure to hold water in the gel, and is formed by reaction or bonding between a hydrogel component (main gel ingredient), which is the main part of the network structure, and a hydrogel insolubilizer (gelling agent), which is the joint part of the network structure.
[0065] The hydrogel constituent material (main gel raw material) is not particularly limited as long as it can form a hydrogel, and may be an organic compound or an inorganic compound, or a mixture of both.
[0066] The organic compound is preferably a hydroxyl group-containing organic polymer. For example, polyvinyl alcohol, guar gum, carrageenan, xanthan gum, methyl cellulose, hydroxymethyl cellulose, and derivatives thereof can be used. Among them, polyvinyl alcohol, guar gum, and guar gum derivatives (modified by hydroxypropylation or the like) are preferred because they allow resins and the like to be well dispersed and provide a hydrogel with excellent stability.
[0067] The inorganic compound is preferably a water-swellable silicate compound. For example, water-swellable clay minerals such as hectorite, montmorillonite, bentonite, and attapulgite can be used. These water-swellable silicate compounds may be natural minerals or synthetic compounds.
[0068] Phosphates, borates, silicates, etc. can be used as hydrogel insolubilizers (gelling agents) that react or bond with the main gel ingredient to form the joints of the network structure. Phosphates and borates are preferred because they can form good hydrogels that are difficult to dissolve in water. Phosphates are particularly preferred when the main gel ingredient is a water-swellable silicate compound such as hectorite, and borates are particularly preferred when the main gel ingredient is a hydroxyl group-containing organic polymer such as polyvinyl alcohol or guar gum, as these can form stable hydrogels in water. Examples of phosphates that can be used include sodium phosphates such as sodium pyrophosphate, and potassium phosphates such as potassium pyrophosphate. Examples of borates that can be used include ammonium borates such as ammonium pentaborate, and borax.
[0069] When a hydrogel component (main gel ingredient) and a hydrogel insolubilizer (gelling agent) react or bond to form a network structure of the hydrogel-forming substance, the two may simply bond additively, such as by addition, or they may bond by condensation, such as by dehydration, in which some of their atoms are detached and then bonded. Although the hydrogel has been described as having a network structure formed by a gel main material and a gelling agent, the hydrogel may be formed by a different mechanism than the formation of the network structure.
[0070] III. Method for producing colored gel particles Next, a method for producing colored gel particles will be described by way of example. First, a colored gel raw material composition is prepared by adding a third aqueous emulsion resin, a color pigment, a hydrogel component (a gel main raw material), and optional components such as an extender pigment, if desired, and stirring the mixture until the components are uniformly dispersed.
[0071] The content of the third aqueous emulsion resin in the colored gel raw material composition is preferably 3 to 45% by weight, more preferably 5 to 30% by weight, even more preferably 10 to 25% by weight, and most preferably 15 to 20% by weight, based on the resin solids content.
[0072] The content of the color pigment in the color gel raw material composition is preferably 5 to 50% by weight, more preferably 10 to 45% by weight, even more preferably 15 to 40% by weight, and most preferably 20 to 35% by weight.
[0073] The content of the hydrogel constituent material in the colored gel raw material composition is preferably 10 to 70 parts by weight, more preferably 15 to 50 parts by weight, and most preferably 20 to 30 parts by weight, based on 100 parts by weight of the solid content of the third aqueous emulsion resin. If the content is within this range, the colored gel particles will have excellent flexibility, and will not easily be crushed when the aggregate is mixed and stirred in the topcoat paint aggregate mixing step described below.
[0074] Next, the obtained colored gel raw material composition is added to an aqueous solution containing a hydrogel insolubilizer (gelling agent). At this time, it is preferable to gradually add the emulsion composition while stirring the aqueous solution containing the hydrogel insolubilizer (gelling agent), and then continue stirring for a while.
[0075] The concentration of the hydrogel insolubilizer (gelling agent) in the aqueous solution is preferably 0.05 to 0.5% by weight, more preferably 0.1 to 0.4% by weight, and even more preferably 0.2 to 0.3% by weight.
[0076] The stirring time is not particularly limited as long as a hydrogel is formed and colored gel particles with the color pigment uniformly dispersed in the hydrogel are obtained, and is usually from a few minutes to 2 hours. Furthermore, the size of the colored gel particles varies depending on the stirring time, and it is preferable to stir until the size of the colored gel particles becomes approximately 1 to 8 mm. The size of the colored gel particles is more preferably 2 to 6 mm, and even more preferably 3 to 5 mm.
[0077] After stirring, the mixture is left to stand at room temperature for at least 1 hour, preferably at least 5 hours, to form a stable gel. The upper limit of the standing time is usually about 24 hours, at which point the formed gel reaches an equilibrium state. By the above-mentioned production method, a gel-forming substance having a network structure or the like is formed, and the water in which the resin or the like is dispersed is held in the network structure or the like, thereby obtaining colored gel particles.
[0078] d) Acrylic beads The topcoat paint preferably contains acrylic beads, and the amount of the acrylic beads is preferably 10 to 80 parts by weight, more preferably 20 to 60 parts by weight, even more preferably 30 to 50 parts by weight, and most preferably 35 to 45 parts by weight, per 100 parts by weight of the solid content of the second aqueous emulsion resin.
[0079] The particle size of the acrylic beads is not particularly limited, but the average particle size is preferably 3 to 50 μm, more preferably 5 to 40 μm, even more preferably 10 to 30 μm, and most preferably 15 to 25 μm.
[0080] An example of the acrylic beads is "Techpolymer MBX-20" manufactured by Sekisui Plastics Co., Ltd.
[0081] The second aqueous emulsion resin, aggregate, and colored gel particles are mixed and stirred to obtain a topcoat paint. In this process, colored gel particles of one color or two or more colors can be used. The color of the colored gel particles is determined by the color of the color pigment contained therein. It is also preferable to mix and stir the acrylic beads. Furthermore, various additives (for example, surfactants, preservatives, thickeners) can be added as needed.
[0082] 2. How to apply topcoat paint The method for applying a topcoat paint to the surface of the undercoat paint film formed in the undercoat paint film forming step is not particularly limited. For example, it can be applied by spray coating or roller coating. After the topcoat paint is applied, it is dried to form a film.
[0083] The topcoat coating film obtained by forming the topcoat paint contains 200 to 1200 parts by weight of aggregate and 30 to 500 parts by weight of dried colored gel particles (solid content) per 100 parts by weight of the second resin, which is the dried product (solid content) of the second aqueous emulsion resin. By including 30 to 500 parts by weight of dried colored gel particles per 100 parts by weight of the second resin, weather resistance is significantly improved even in aggregate-rich formulations. The content of dried colored gel particles in the topcoat coating film is preferably 45 to 400 parts by weight, more preferably 60 to 310 parts by weight, even more preferably 90 to 250 parts by weight, and most preferably 120 to 190 parts by weight per 100 parts by weight of the second resin.
[0084] The dried colored gel particles contained in the topcoat coating film contain 5 to 90 parts by weight of the dried hydrogel relative to 100 parts by weight of the third resin, which is the dried (solid) content of the third aqueous emulsion resin. The dried colored gel particles preferably contain 10 to 70 parts by weight, more preferably 15 to 50 parts by weight, and most preferably 20 to 30 parts by weight of the dried hydrogel relative to 100 parts by weight of the third resin. Here, the content of the dried hydrogel per 100 parts by weight of the third resin in the topcoat coating film is approximately equal to the content of the hydrogel constituent material per 100 parts by weight of the solid content of the third aqueous emulsion resin in the colored gel raw material composition.
[0085] [Topcoat paint aggregate mixing process] Before the topcoat film forming step, a topcoat paint aggregate blending step may be carried out in which aggregate and an aqueous dispersion medium are mixed and stirred with the topcoat base paint to form a topcoat paint. The top coating paint aggregate blending step will be illustrated below.
[0086] The topcoat paint aggregate blending step is an optional step that occurs before the topcoat paint film forming step, in which aggregate and an aqueous dispersion medium are mixed and stirred with the topcoat base paint to form the topcoat paint. The topcoat paint aggregate blending step is usually carried out after the primer coating film forming step at the coating site, but can also be carried out before the primer coating film forming step.
[0087] The topcoat base paint used in the topcoat aggregate blending process is a paint that serves as the base for the topcoat paint and does not contain aggregate. Furthermore, since the topcoat base paint does not contain aggregate, the amount of aqueous dispersion medium is significantly less than that of the topcoat paint.
[0088] In the topcoat paint aggregate blending step, aggregate and an aqueous dispersion medium are mixed and stirred with the topcoat base paint to prepare the topcoat paint. In other words, by mixing and stirring the topcoat base paint with aggregate and aqueous dispersion medium (water) at the application site, it is possible to reduce total costs.
[0089] In the topcoat paint aggregate mixing process, when the aggregate is mixed and stirred (strongly stirred) into the topcoat base paint, the colored gel particles contained in the topcoat base paint can be destroyed, resulting in a loss of design quality. However, as mentioned above, by setting the content of the hydrogel constituent material in the colored gel raw material composition used to produce the colored gel particles to preferably 10 to 70 parts by weight of solids, more preferably 15 to 50 parts by weight of solids, and most preferably 20 to 30 parts by weight of solids, per 100 parts by weight of solids of the third aqueous emulsion resin, the colored gel particles are less likely to be crushed excessively, and good design properties can be ensured.
[0090] As illustrated above, after going through the primer coating film forming process, top coating film forming process (and in some cases the top coating paint aggregate mixing process), a lysine-style laminated coating film is formed on the surface of the surface to be painted, such as an exterior wall. [Example]
[0091] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples, the ratios and the like are based on weight.
[0092] Example 1 i) Primer paint An undercoat paint was prepared based on the formulation in Table 1 below, using the acrylic resin emulsion "Polytron Z332" (manufactured by Asahi Kasei Corporation) as the first water-based emulsion resin, the white pigment JR-901 (manufactured by Teika Corporation) as the coloring pigment, and Whiten H (manufactured by Shiraishi Calcium Co., Ltd.), a calcium carbonate with an average particle size of 22 μm, as the extender pigment. In addition to the above materials, the primer paint contains additives such as water, surfactants, and preservatives, and the solid content of the first aqueous emulsion resin relative to the total primer paint is approximately 9 to 12% by weight.
[0093] ii) Topcoat paint The colored gel particles used in the topcoat were prepared by gradually adding a 0.0026% aqueous sodium tetraborate solution as a hydrogel insolubilizer (gelling agent) to a colored gel raw material composition prepared according to the recipe in Table 2 below, using the acrylic resin emulsion "Polytron Z332" (Asahi Kasei Corporation) as the third aqueous emulsion resin, the white pigment JR-603 (Teikai Corporation) as the color pigment, the calcium carbonate Whiten 305 (Shiraishi Calcium Co., Ltd.) as the extender pigment, and the PVA "Elvanol" (Kuraray Co., Ltd.) and the silicate compound "Laponite RD" (BYK Japan Co., Ltd.) as hydrogel components. The stirring time was adjusted to obtain colored gel particles approximately 4 mm in diameter. Then, using the obtained colored gel particles, the acrylic silicone resin emulsion "Polydurex G-625" (manufactured by Asahi Kasei Corporation) as the second aqueous emulsion resin, and K1 (manufactured by Sankyo Flour Milling Co., Ltd.), a calcium carbonate with an average particle diameter of 270 μm, as the aggregate, a topcoat paint was prepared based on the formulation in Table 1 below. In addition to the above materials, the topcoat paint contains 42 parts by weight of Techpolymer MBX-20 (Sekisui Chemical Co., Ltd.) acrylic beads for every 100 parts by weight of the solid content of the water-based emulsion resin, as well as additives such as water, antifoaming agent, thickener, and film-forming agent, so that the solid content of the second water-based emulsion resin relative to the total basecoat paint is approximately 4 to 7% by weight.
[0094] iii) Formation of lysine-like laminated coating film The ALC panel on the exterior wall of the building was used as the surface to be painted, and the primer was spray painted onto this surface. The amount of paint applied was approximately 1.0 kg / m 2 After painting, the surface was smoothed using a roller before the paint dried. It was then dried to form a film, and a curing period of about one day was provided to obtain a primer coating. The topcoat paint was spray-painted onto the surface of the obtained undercoat film. The amount of paint applied was approximately 0.5 kg / m. 2 The coating was then dried to form a film, yielding a lysine-like multilayer coating film consisting of an undercoat coating film and a topcoat coating film.
[0095] The lysine-like multilayer coating films of the above examples were evaluated for primer workability, topcoat workability, appearance, base conformability, waterproofness, and weather resistance. The evaluation methods are as follows.
[0096] 1) Primer workability The priming workability was evaluated by the degree to which pinholes were filled when the ALC was applied. Specifically, the priming work was checked and evaluated by several people, and a very good result was rated as ◎, a good result as ○, and a poor result as ×. 2) Topcoat workability The topcoat workability was evaluated by the degree of clogging of the spraying equipment during spray painting. Specifically, the topcoat work was checked and evaluated by several people using a universal gun Fukube (manufactured by Otsuka Brush Manufacturing Co., Ltd.: nozzle diameter 5.5 mm), and the results were rated as follows: ◎ if the spraying equipment hardly clogged, ○ if the spraying equipment hardly clogged, and × if the spraying equipment easily clogged. 3) Appearance The appearance of the finished product after ALC coating was evaluated by several people in comparison with a general lysine-like coating film, and was rated as ◎ if it was equal to or better than a general lysine-like coating film, ○ if it was almost equal to a general lysine-like coating film, and × if it was inferior to a general lysine-like coating film. 4) Substrate conformability The conformability to the substrate was evaluated by conducting an impact resistance test according to JIS A6909. The condition of the coating film after the impact resistance test was checked and evaluated by several people. 5) Waterproof The evaluation was carried out using the JIS A6909 water permeability test method B. A water permeability of 0.5 ml or less after 24 hours was considered to be acceptable. 6) Weather resistance The evaluation was carried out using JIS A6909 Weather Resistance Test Method B, Weather Resistance Type 1. All color tones were matched to the Japan Paint Color Table number "J19-60C."
[0097] [Table 1]
[0098] [Table 2]
[0099] Example 1 achieved very good results in all six evaluations of primer workability, topcoat workability, appearance, substrate conformability, waterproofness, and weather resistance.
[0100] In the topcoat paint of Example 1, the amount of colored gel particles was 250 parts by weight per 100 parts by weight of the solid content of the second acrylic resin emulsion, which in the state of the topcoat paint film corresponded to 155 parts by weight of the dried colored gel particles per 100 parts by weight of the second acrylic resin, which is the dried product of the second acrylic resin emulsion.
[0101] (Example 2) to (Example 5) Examples 2 to 5 are examples in which the amounts of each compounded material (coloring raw material and extender pigment) in the primer paint were changed in Example 1. In these examples as well, very good or good results were obtained in all six evaluations.
[0102] (Example 6) to (Example 9) Examples 6 to 9 are examples in which the amounts of each compounding material (aggregate and colored gel particles) in the topcoat paint were changed in Example 1. In these examples as well, very good or good results were obtained in all six of the above evaluations.
[0103] In Example 1, the primer paint was evaluated in the six ways described above for two formulations containing 20 and 200 parts by weight of color pigment (60 parts by weight per 100 parts by weight of the first acrylic resin emulsion) and two formulations containing 50 and 800 parts by weight of extender pigment (440 parts by weight per 100 parts by weight of the first acrylic resin emulsion). All four formulations were found to be good. Similarly, the topcoat paint was evaluated in the six ways described above for two formulations containing 200 and 1200 parts by weight of aggregate (900 parts by weight per 100 parts by weight of the second acrylic resin emulsion) and two formulations containing 50 and 800 parts by weight of colored gel particles (250 parts by weight per 100 parts by weight of the second acrylic resin emulsion). All four formulations were found to be good. Furthermore, in Examples 1 and 6-9, a topcoat paint aggregate blending step was performed before the topcoat film formation step. This step involved mixing and stirring aggregate and an aqueous dispersion medium with a topcoat base paint, which is a base paint for the topcoat paint and does not contain aggregate, to form a topcoat paint. In all Examples, the colored gel particles were uniformly dispersed, ensuring excellent design (appearance). Similar results were also obtained when colored gels were prepared using a colored gel raw material composition in which the blending amounts of the hydrogel components in Table 2 were 80 parts by weight in solids to 100 parts by weight of the third acrylic emulsion resin. However, when colored gels were prepared using a colored gel raw material composition in which the blending amounts of the hydrogel components in Table 2 were 100 parts by weight in solids to 100 parts by weight of the third acrylic emulsion resin, and similar evaluations were performed using these colored gels, the colored gel particles hardened during the topcoat paint aggregate blending step, resulting in numerous gaps in the coating film, resulting in non-uniformity and a deterioration in design (appearance) and weather resistance.
[0104] In the topcoat paint of Example 8, the amount of colored gel particles was 75 parts by weight per 100 parts by weight of the solid content of the second acrylic resin emulsion, which in the state of the topcoat paint film corresponded to 47 parts by weight of the dried colored gel particles per 100 parts by weight of the second acrylic resin, which is the dried product of the second acrylic resin emulsion. In addition, in the topcoat paint of Example 9, the amount of colored gel particles was 600 parts by weight per 100 parts by weight of the solid content of the second acrylic resin emulsion, which in the state of the topcoat paint film corresponded to 373 parts by weight of dried colored gel particles per 100 parts by weight of the second acrylic resin, which is the dried product of the second acrylic resin emulsion.
[0105] (Comparative Example 1) Comparative Example 1 is an example in which the amount of color pigment in the primer paint in Example 1 was significantly reduced, resulting in a worsened appearance. Therefore, the conformability to the substrate, waterproofness, and weather resistance were not evaluated.
[0106] (Comparative Example 2) Comparative Example 2 is an example in which the amount of color pigment in the primer paint in Example 1 was significantly increased, resulting in poor weather resistance.
[0107] (Comparative Example 3) In Comparative Example 3, the amount of extender pigment in the primer paint was significantly reduced in Example 1, which resulted in poor primer workability. Therefore, the primer conformability, waterproofness, and weather resistance were not evaluated.
[0108] Comparative Example 4 Comparative Example 4 is an example in which the amount of extender pigment in the primer paint in Example 1 was significantly increased, resulting in poor conformability to the base and poor waterproofing, and therefore weather resistance was not evaluated.
[0109] (Comparative Example 5) Comparative Example 5 is an example in which the amount of aggregate in the top coat paint in Example 1 was significantly reduced, resulting in a worsened appearance. Therefore, the conformability to the substrate, waterproofness, and weather resistance were not evaluated.
[0110] (Comparative Example 6) Comparative Example 6 is an example in which the amount of aggregate in the topcoat paint in Example 1 was significantly increased, which resulted in a deterioration in topcoat workability. Therefore, the substrate conformability, waterproofness, and weather resistance were not evaluated.
[0111] (Comparative Example 7) Comparative Example 7 is an example in which the amount of colored gel particles in the top coat paint in Example 1 was significantly reduced, resulting in a worsened appearance. Therefore, the conformability to the substrate, waterproofness, and weather resistance were not evaluated. In the topcoat paint of Comparative Example 7, the amount of colored gel particles was 40 parts by weight per 100 parts by weight of the solid content of the second acrylic resin emulsion, which in the state of the topcoat paint film corresponded to 25 parts by weight of the dried colored gel particles per 100 parts by weight of the second acrylic resin, which is the dried product of the second acrylic resin emulsion.
[0112] (Comparative Example 8) Comparative Example 8 is an example in which the amount of colored gel particles in the top coat paint in Example 1 was significantly increased, resulting in poor conformability to the substrate and poor waterproofing, and therefore weather resistance was not evaluated. In the topcoat paint of Comparative Example 8, the amount of colored gel particles was 900 parts by weight per 100 parts by weight of the solid content of the second acrylic resin emulsion, which in the state of the topcoat paint film corresponded to 559 parts by weight of dried colored gel particles per 100 parts by weight of the second acrylic resin, which is the dried product of the second acrylic resin emulsion.
[0113] (Comparative Example 9) Comparative Example 9 is an example in which a colored pigment (approximately the same amount as the colored pigment contained in the colored gel particles) was blended in place of the colored gel particles in Example 1, and weather resistance was deteriorated. Comparing Example 1 with this comparative example, it can be seen that the weather resistance of an aggregate-rich topcoat paint is significantly improved by blending colored gel particles instead of colored pigment.
[0114] (Comparative Example 10) Comparative Example 10 is a general lysine paint, which has problems with its surface conformability, waterproofing, and weather resistance.
[0115] The present invention has been described above with reference to specific embodiments and examples, but the present invention is not limited to the above embodiments, and various changes and modifications can be made by those skilled in the art without departing from the scope of the claims attached to the application of this application.
Claims
1. The method includes a basecoat coating film forming process for applying a basecoat paint to the surface of a surface to be painted, such as an exterior wall, to form a film, and a topcoat coating film forming process for applying a topcoat paint to the surface of the basecoat coating film formed by the basecoat coating film forming process to form a film, The undercoat paint is Relative to 100 parts by weight of the solid content of the first aqueous emulsion resin, Contains 50 to 800 parts by weight of an extender pigment having an average particle size of 1 to 100 μm, The topcoat paint is Relative to 100 parts by weight of the solid content of the second aqueous emulsion resin, 200 to 1200 parts by weight of aggregate, Contains 50 to 800 parts by weight of colored gel particles; A method for forming a lysine-like multilayer coating film, comprising the steps of: The colored gel particles include a third aqueous emulsion resin, a color pigment, and a hydrogel. A method for forming a lysine-like multilayer coating film.
2. The method includes a basecoat coating film forming process for applying a basecoat paint to the surface of a surface to be painted, such as an exterior wall, to form a film, and a topcoat coating film forming process for applying a topcoat paint to the surface of the basecoat coating film formed by the basecoat coating film forming process to form a film, The undercoat paint is Relative to 100 parts by weight of the solid content of the first aqueous emulsion resin, Contains 50 to 800 parts by weight of an extender pigment having an average particle size of 1 to 100 μm, The topcoat paint is Relative to 100 parts by weight of the solid content of the second aqueous emulsion resin, 200 to 1200 parts by weight of aggregate, 50 to 800 parts by weight of colored gel particles, 10 to 80 parts by weight of acrylic beads, A method for forming a lysine-like multilayer coating film.
3. Before the topcoat coating process, The method includes a topcoat paint aggregate blending step of mixing and stirring an aggregate and an aqueous dispersion medium with a topcoat base paint, which is a base paint for a topcoat paint and does not contain an aggregate, to form a topcoat paint. A method for forming the lysine-like multilayer coating film according to claim 1 or 2.
4. The colored gel particles contained in the topcoat paint The colored gel raw material composition containing a third aqueous emulsion resin, a color pigment, and a hydrogel component is added to an aqueous solution containing a hydrogel insolubilizer, The content of the hydrogel constituent material in the colored gel raw material composition is 5 to 90 parts by weight in terms of solid content per 100 parts by weight of the solid content of the third aqueous emulsion resin. A method for forming the lysine-like multilayer coating film according to any one of claims 1 to 3.
5. At least one of the first aqueous emulsion resin contained in the undercoat paint, the second aqueous emulsion resin contained in the topcoat paint, and the third aqueous emulsion resin of the colored gel particles contained in the topcoat paint is an acrylic silicone resin emulsion. A method for forming the lysine-like multilayer coating film according to any one of claims 1 to 4.
6. The topcoat paint is Relative to 100 parts by weight of the solid content of the second aqueous emulsion resin, Contains 10 to 80 parts by weight of acrylic beads; A method for forming a lysine-like multilayer coating film according to any one of claims 1 and 3 to 5.
7. The undercoat paint comprises: Relative to 100 parts by weight of the solid content of the first aqueous emulsion resin, Contains 20 to 200 parts by weight of a color pigment; A method for forming the lysine-like multilayer coating film according to any one of claims 1 to 6.
8. It is composed of an undercoat coating film formed by applying an undercoat paint to the surface of a surface to be painted such as an exterior wall, and a topcoat coating film formed by applying a topcoat paint to the surface of the undercoat coating film, The undercoat coating film is Relative to 100 parts by weight of the first resin, Contains 50 to 800 parts by weight of an extender pigment having an average particle size of 1 to 100 μm, The topcoat coating film is For 100 parts by weight of the second resin, 200 to 1200 parts by weight of aggregate, Contains 30 to 500 parts by weight of dried colored gel particles; A lysine-like laminated coating film, The dried product of the colored gel particles includes a third resin, a color pigment, and a dried product of a hydrogel. Lysine-like multilayer coating.
9. It is composed of an undercoat coating film formed by applying an undercoat paint to the surface of a surface to be painted such as an exterior wall, and a topcoat coating film formed by applying a topcoat paint to the surface of the undercoat coating film, The undercoat coating film is Relative to 100 parts by weight of the first resin, Contains 50 to 800 parts by weight of an extender pigment having an average particle size of 1 to 100 μm, The topcoat coating film is For 100 parts by weight of the second resin, 200 to 1200 parts by weight of aggregate, 30 to 500 parts by weight of dried colored gel particles, 10 to 80 parts by weight of acrylic beads, Lysine-like multilayer coating.
10. The dried colored gel particles contained in the topcoat are The composition contains 5 to 90 parts by weight of a dried hydrogel relative to 100 parts by weight of the third resin. The lysine-like multilayer coating film according to claim 8 or claim 9.
11. At least one of the first resin contained in the undercoat coating film, the second resin contained in the topcoat coating film, and the third resin contained in the dried product of the colored gel particles is an acrylic silicone resin. The lysine-like multilayer coating film according to any one of claims 8 to 10.
12. The topcoat coating is Relative to 100 parts by weight of the solid content of the second resin, Contains 10 to 80 parts by weight of acrylic beads; The lysine-like multilayer coating film according to any one of claims 8, 10 and 11.
13. The undercoat coating film comprises: Relative to 100 parts by weight of the first resin, Contains 20 to 200 parts by weight of a color pigment; The lysine-like multilayer coating film according to any one of claims 8 to 12.
Citation Information
Patent Citations
Cladding lysine paint
JP1981099266A
Method for forming patterned surface
JP2005246370A
Coating method
JP2008142691A
Coating film structure
JP2012143685A
Coated film formation method
JP2019063779A