Surface-treated particles, their manufacturing method, and conductive composition containing surface-treated particles
Surface-treated copper particles with a silver layer and organic polysiloxane coating address the issue of copper ion elution, maintaining conductivity and improving storage stability in conductive compositions.
Patent Information
- Application Number
- JP2021024394
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-27
- Filing Date
- 2021-02-18
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-02-18
AI Technical Summary
Conductive compositions containing copper particles with silane coupling agent coatings suffer from increased viscosity due to copper ion elution, leading to poor storage stability.
Surface-treated copper particles with a silver layer and a coating layer of organic polysiloxane compound, where the siloxane bond groups are exclusively alkyl or alkoxy groups, are used to form a conductive composition with improved stability.
The surface-treated particles maintain conductivity while significantly reducing copper ion elution, thereby enhancing the storage stability of the conductive composition.
Smart Images

Figure 0007594460000001
Abstract
Description
[Technical field]
[0001] The present invention relates to surface-treated particles and a method for producing the same, and to a conductive composition containing the surface-treated particles. [Background technology]
[0002] As a material for forming a conductive circuit such as an electrode, various surface-treated particles in which the surface of copper particles is coated with a silicon-based compound are known. For example, Patent Documents 1 to 3 disclose copper particles whose surface is coated with a silane coupling agent or an organosilane compound for the purpose of improving the oxidation resistance and dispersibility of the particles.
[0003] Furthermore, Patent Document 4 discloses a surface-treated metal powder obtained by reacting a plasma-treated metal powder with a silane coupling agent for the purpose of producing molding materials with high moldability for use in automotive inductors, motor magnet fixing materials, and the like.
[0004] Furthermore, Patent Document 5 discloses a method for producing fine copper powder, in which the surface of copper oxide powder is coated with a silane coupling agent and the resulting copper oxide powder is reduced with hydrazine, with the aim of obtaining monodispersed spherical copper powder with a narrow particle size distribution in a short period of time. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 57-155386 [Patent Document 2] JP 2003-16832 A [Patent Document 3] International Publication No. 2013 / 125659 Brochure [Patent Document 4] JP 2018-135547 A [Patent Document 5] Japanese Patent Application Publication No. 02-34708 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the surface-treated copper particles of Patent Documents 1 to 5 are all formed by directly attaching a silane coupling agent to the surface of the copper particles, so when a conductive composition containing the copper particles is stored in the form of a paste or the like, the viscosity of the composition increases due to copper ions eluting from the copper particles, etc., and the composition has poor stability during storage. In addition to improving storage stability, a material that can further improve conductive properties is desired.
[0007] Therefore, an object of the present invention is to provide surface-treated particles that can provide a conductive composition having excellent storage stability. [Means for solving the problem]
[0008] The present invention relates to a coating layer comprising a core particle and an organic polysiloxane compound disposed on the surface of the core particle, the core particles are copper particles whose surfaces are coated with silver, In the organic polysiloxane compound, the groups bonded to silicon atoms, excluding the oxygen atoms constituting the siloxane bonds, are either only alkyl groups or only alkoxy groups and alkyl groups; The alkyl group is an alkyl group having 2 to 17 carbon atoms, or a methyl group and an alkyl group having 2 to 17 carbon atoms.
[0009] The present invention also provides a method for producing surface-treated particles, which comprises mixing core particles with an alkylalkoxysilane and polymerizing the alkylalkoxysilane to form an organic polysiloxane compound, which is a polymer of the alkylalkoxysilane, on the surface of the core particles, comprising: As the core particles, copper particles having a surface coated with silver are used, The present invention provides a method for producing surface-treated particles, in which the alkylalkoxysilane has a molecular weight of 150 or more and 390 or less and has, as an alkoxy group, at least one type of group selected from the group consisting of a methoxy group and an ethoxy group.
[0010] The present invention further provides a conductive composition comprising the above surface-treated particles, a binder resin and a solvent. Effect of the Invention
[0011] According to the present invention, there are provided surface-treated particles which can provide a conductive composition having excellent storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described below based on its preferred embodiments. The surface-treated particles of the present invention have a coating layer containing an organic polysiloxane compound arranged on the surface of a core particle. The core particle is a copper particle whose surface is coated with silver. That is, the surface-treated particles of the present invention include a core particle in which the surface of the copper particle is coated with silver, and a coating layer containing an organic polysiloxane compound arranged adjacent to the surface of the core particle.
[0013] The coating layer is the outermost layer of the surface-treated particle, and it is preferable that no other layer exists on the outer surface of the coating layer or between the core particle surface and the coating layer. That is, it is preferable that the silver layer is formed adjacent to the surface of the copper particle, and the coating layer is formed adjacent to the surface of the silver layer. However, it is not prevented from providing one or more other layers on the outer surface of the coating layer or between the core particle surface and the coating layer according to the specific use of the surface-treated particle.
[0014] As described above, the core particle is formed of copper particles and a silver layer covering the surface of the copper particles. The copper particles constituting the core particle are substantially formed only from copper and do not contain other elements except for inevitable impurities, or are composed of copper and elements other than copper. In the latter case, the elements other than copper include silver forming the silver layer and elements that can form an alloy or intermetallic compound with copper, and the ratio is preferably 35 mass% or less with respect to the total mass of the copper particles. By using such a content ratio, it is possible to achieve both improved storage stability when made into a conductive composition and improved conductivity due to the presence of copper.
[0015] From the viewpoint of improving storage stability and excellent electrical conductivity due to the presence of copper, the content of metal elements other than copper in the core particles is preferably 35% by mass or less based on the mass of the entire core particles. In this case, the core particles include both a case where a silver layer is formed to cover the surface of copper particles made of copper and inevitable impurities, and a case where a silver layer is formed to cover the surface of copper particles made of copper, elements other than copper, and inevitable impurities.
[0016] Examples of elements other than copper that can form an alloy or intermetallic compound with copper include at least one metal element selected from Ni, Al, Sn, Cr, and Zr, in addition to Ag that forms the silver layer. When an element other than copper is further contained in the copper particles, from the viewpoint of further increasing the oxidation resistance and shrinkage resistance of the particles, it is preferable that at least one of Ni, Al, and Sn is contained as the element other than copper, and it is more preferable that Ni is contained. The presence or absence and content of copper and elements other than copper can be measured by, for example, ICP analysis or XRF analysis.
[0017] When Ni is contained as an element other than copper, the Ni element content in the core particle is preferably 1 mass% or more and 30 mass% or less, more preferably 5 mass% or more and 25 mass% or less, and even more preferably 10 mass% or more and 20 mass% or less. By having such a content ratio, the oxidation resistance and shrinkage resistance of the particle can be further improved.
[0018] When Al is contained as an element other than copper, the content of Al element in the core particle is preferably 0.1% by mass to 10% by mass, more preferably 1% by mass to 8% by mass, and even more preferably 3% by mass to 7% by mass. By using such a content ratio, the oxidation resistance and shrinkage resistance of the particle can be further improved.
[0019] When Sn is contained as an element other than copper, the Sn element content in the core particle is preferably 1 mass% or more and 30 mass% or less, more preferably 5 mass% or more and 25 mass% or less, and even more preferably 10 mass% or more and 20 mass% or less. By using such a content ratio, the oxidation resistance and shrinkage resistance of the particle can be further improved.
[0020] When Cr is contained as an element other than copper, the Cr element content in the core particle is preferably 0.1% by mass to 5% by mass, more preferably 0.5% by mass to 4% by mass, and even more preferably 1% by mass to 3% by mass. By using such a content ratio, the oxidation resistance and shrinkage resistance of the particle can be further improved.
[0021] When Cr and Zr are contained in combination as elements other than copper, the Cr element content in the core particle is preferably 0.5% by mass to 1.5% by mass, more preferably 0.6% by mass to 1.4% by mass, and even more preferably 0.7% by mass to 1.3% by mass. The Zr element content in the core particle is preferably 0.05% by mass to 0.25% by mass, more preferably 0.05% by mass to 0.20% by mass, and even more preferably 0.1% by mass to 0.20% by mass. By using such a content ratio, the oxidation resistance of the particle can be further improved.
[0022] The silver layer constituting the surface of the core particle is formed so as to cover at least a part of the surface of the copper particle. The silver covers the surface of the copper particle discontinuously, or covers the entire surface of the copper particle continuously and uniformly. In the former case, the surface of the core particle is composed of a part made of silver and a part made substantially of copper as an undercoat. In the latter case, the entire surface of the core particle is composed of only silver, and the copper as an undercoat is not exposed on the surface of the core particle.
[0023] From the viewpoint of obtaining particles having electrical conductivity equal to or higher than that of conventional particles and obtaining a conductive material containing the particles and having excellent storage stability, it is preferable that the core particles are in an embodiment in which silver is evenly and continuously coated over the entire surface of the copper particles. Whether or not the silver layer is evenly and continuously coated over the entire surface of the core particles can be determined by, for example, observation with an electron microscope, X-ray photoelectron spectroscopy, Auger electron spectroscopy, or the like.
[0024] The coating layer located on the surface of the core particle is composed of a single layer containing an organic polysiloxane compound. In the present invention, the organic polysiloxane compound refers to oligomers such as dimers, trimers, and tetramers, and polymers having one or more siloxane bonds, and does not include monomers. The coating layer may be composed of only an organic polysiloxane compound, or may contain a silane compound capable of generating a siloxane bond as a monomer in addition to the organic polysiloxane compound. Details of the silane compound will be described later.
[0025] The coating layer may be configured to cover the entire surface of the core particle continuously and uniformly, or to cover only a portion of the surface of the core particle. In the former case, the entire surface of the core particle is completely covered with the organic polysiloxane compound, and the surface of the core particle is not exposed. In the latter case, the surface of the surface-treated particle is composed of a portion of the core particle and a portion of the organic polysiloxane compound. When the organic polysiloxane compound covers only a portion of the surface of the core particle, the organic polysiloxane compound may form a continuous coating, a discontinuous coating in the form of islands in the sea, or a combination of these. From the viewpoint of further improving the storage stability of the surface-treated particles, the surface-treated particles are preferably in a form in which the coating layer uniformly and continuously covers the entire surface of the core particle. Whether or not the layer of the organic polysiloxane compound uniformly and continuously covers the entire surface of the core particle can be determined by, for example, X-ray photoelectron spectroscopy, Auger electron spectroscopy, infrared absorption spectroscopy, Raman spectroscopy, LC-MS measurement, or various chromatographic measurements.
[0026] Examples of the organic polysiloxane compound include polymers such as polysiloxane compounds made of dehydration condensates of silane compounds known as silane coupling agents.
[0027] One of the features of the organic polysiloxane compound constituting the coating layer is that a specific group is bonded to a silicon atom. In detail, the organic polysiloxane compound has only alkyl groups or only alkyl and alkoxy groups as groups directly bonded to silicon atoms, except for the oxygen atoms constituting the siloxane bond. In other words, the organic polysiloxane compound has a main chain made of siloxane bonds and a side chain made of only alkyl groups or only alkyl and alkoxy groups. By virtue of this constitution, it is possible to obtain surface-treated particles having electrical conductivity equal to or greater than that of conventional particles, and when the particles are used as a metal filler in a conductive composition, the storage stability is improved. The organic polysiloxane compound can be obtained by using an organic silane compound as a monomer and polymerizing the silane compound. In theory, the organic polysiloxane compound obtained by polymerizing an organic silane compound is formed from siloxane bonds and the above-mentioned side chains, but the unavoidable presence of a small amount of silanol groups derived from monomers or incomplete polymerization is permitted.
[0028] In the present invention, "only alkyl groups" includes an embodiment having only one alkyl group and an embodiment having two or more identical or different alkyl groups. Similarly, in the present invention, "only alkyl groups and alkoxy groups" includes an embodiment having only one alkyl group and only one alkoxy group, an embodiment having two or more identical or different alkyl groups and only one alkoxy group, an embodiment having one alkyl group and two or more identical or different alkoxy groups, and an embodiment having two or more identical or different alkyl groups and two or more identical or different alkoxy groups.
[0029] When the organopolysiloxane compound contains an alkyl group, the alkyl group is preferably exclusively linear or branched alkyl groups having from 2 to 17 carbon atoms, more preferably from 3 to 15 carbon atoms, and even more preferably linear alkyl groups having the above-mentioned number of carbon atoms. Alternatively, the alkyl group is exclusively a combination of a linear or branched alkyl group having from 2 to 17 carbon atoms, more preferably from 3 to 15 carbon atoms, and a methyl group. Furthermore, when the organic polysiloxane compound contains an alkoxy group, the alkoxy group preferably has a carbon atom number of 1 or 2. In other words, the alkoxy group is preferably a methoxy group, an ethoxy group, or a combination thereof.
[0030] The presence or absence of alkyl and alkoxy groups constituting the organic polysiloxane compound, and the number of carbon atoms of each group can be measured, for example, by TOF-SIMS or GC-MS (DI method). Alternatively, the powder of the particles to be measured can be eluted with an alkaline aqueous solution, and the eluate can be introduced into an LC-MS for measurement.
[0031] Examples of the silane compound capable of generating the organic polysiloxane compound that forms the coating layer include organic silane compounds. Specific examples of the organic silane compound include those represented by the general formula "(R A -) X Si(OR B ) 4-X Examples of the alkylalkoxysilanes include those represented by the formula R A and R B Each independently represents an alkyl group, and X is an integer of 1 to 3, preferably 1 or 2. A If there are multiple R A may be the same group or different groups. B If there are multiple R B may be the same group or different groups. These silane compounds may be used alone or in combination of two or more kinds.
[0032] In the above general formula, when X is 1, R A is preferably a straight-chain or branched-chain alkyl group having 1 to 18 carbon atoms, more preferably a straight-chain or branched-chain alkyl group having 2 to 17 carbon atoms, even more preferably a straight-chain or branched-chain alkyl group having 3 to 15 carbon atoms, and even more preferably a straight-chain alkyl group having the above-mentioned number of carbon atoms. A Specific examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, a hexadecyl group, and an octadecyl group.
[0033] In the above general formula, when X is 2 or 3, R A are each independently preferably a linear or branched alkyl group having from 1 to 18 carbon atoms, more preferably a linear or branched alkyl group having from 2 to 17 carbon atoms, even more preferably a linear or branched alkyl group having from 3 to 15 carbon atoms, and even more preferably a linear alkyl group having the above-mentioned number of carbon atoms. In particular, when X is 2 or 3, R A At least one of R is a linear or branched alkyl group having 2 to 17 carbon atoms, and R A At least one of R is preferably a methyl group. A Specific examples of the group include the groups mentioned above.
[0034] R B Each of R preferably independently has 1 to 2 carbon atoms. B is preferably a methyl group, an ethyl group, or a combination thereof.
[0035] The above mentioned R A and R B Examples of alkylalkoxysilanes having any of the above groups include alkyltrialkoxysilanes, dialkyldialkoxysilanes, and trialkylalkoxysilanes.
[0036] Examples of alkyltrialkoxysilanes include methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, isopropyltrimethoxysilane, n-butyltrimethoxysilane, isobutyltrimethoxysilane, tert-butyltrimethoxysilane, n-hexyltrimethoxysilane, isohexyltrimethoxysilane, n-octyltrimethoxysilane, isooctyltrimethoxysilane, n-nonyltrimethoxysilane, isononyltrimethoxysilane, and n-deoxytrimethoxysilane. alkyltrimethoxysilane, such as octyltrimethoxysilane, isodecyltrimethoxysilane, tert-decyltrimethoxysilane, n-dodecyltrimethoxysilane, isododecyltrimethoxysilane, tert-dodecyltrimethoxysilane, n-hexadecyltrimethoxysilane, isohexadecyltrimethoxysilane, tert-hexadecyldodecyltrimethoxysilane, n-octadecyltrimethoxysilane, isooctadecyltrimethoxysilane, and tert-octadecyldodecyltrimethoxysilane; Methoxysilane, methyltriethoxysilane, ethyltriethoxysilane, n-propyltriethoxysilane, isopropyltriethoxysilane, n-butyltriethoxysilane, isobutyltriethoxysilane, tert-butyltriethoxysilane, n-hexyltriethoxysilane, isohexyltriethoxysilane, n-octyltriethoxysilane, isooctyltriethoxysilane, n-nonyltriethoxysilane, isononyltriethoxysilane, n-decyltriethoxysilane, isodeoxytriethoxysilane, Examples of the alkyltriethoxysilane include alkyltriethoxysilanes such as siltriethoxysilane, tert-decyltriethoxysilane, n-dodecyltriethoxysilane, isododecyltriethoxysilane, tert-dodecyltriethoxysilane, n-hexadecyltriethoxysilane, isohexadecyltriethoxysilane, tert-hexadecyldodecyltriethoxysilane, n-octadecyltriethoxysilane, isooctadecyltriethoxysilane, and tert-octadecyldodecyltriethoxysilane.
[0037] An example of a dialkyldialkoxysilane is dimethoxy(methyl)-n-octylsilane.
[0038] An example of a trialkylalkoxysilane is methoxy(dimethyl)-n-octylsilane.
[0039] The molecular weight of the alkylalkoxysilane used to form the organic polysiloxane compound is preferably 150 to 390, more preferably 190 to 390, and even more preferably 230 to 390. In addition, it is preferable that the alkoxy group constituting the alkylalkoxysilane has only at least one group selected from a methoxy group and an ethoxy group. In particular, in the above-mentioned general formula of the alkylalkoxysilane, all R B is an alkylmethoxysilane in which all R B By using an alkylalkoxysilane that satisfies both the above-mentioned conditions of molecular weight and alkoxy group, the surface-treated particles of the present invention can suppress an increase in the viscosity of a conductive composition containing the particles even when the composition is stored for a long period of time, and the particles can have even better conductivity and storage stability.
[0040] The core particles constituting the surface-treated particles of the present invention preferably have a silver ratio of 1% by mass or more and 25% by mass or less, more preferably 3% by mass or more and 15% by mass or less. This configuration reduces the amount of silver used, which is more expensive than copper, and allows the surface-treated particles to be provided at low cost. When a conductive composition containing the surface-treated particles is stored for a long period of time, copper is prevented from eluting from the copper particles constituting the core particles, and the viscosity of the composition is prevented from increasing, resulting in further excellent storage stability. For example, the silver ratio of the surface-treated particles of the present invention can be quantitatively analyzed by potentiometric titration using a solution in which the particles are dissolved in acid.
[0041] From the viewpoint of improving the storage stability of the surface-treated particles and the conductive composition containing the particles, the content of the organic polysiloxane compound in the surface-treated particles is preferably 0.002% by mass or more and 0.3% by mass or less, more preferably 0.005% by mass or more and 0.1% by mass or less, in terms of silicon atoms. The above-mentioned silicon atom conversion means that the surface-treated particles to be measured are dissolved in an alkaline solution, and the mass of silicon atoms measured by ICP emission spectrometry of the solution is taken as the content of the organic polysiloxane compound in this specification. In addition, the solution can be subjected to LC-MS to identify the type of organic polysiloxane compound. In addition, the surface-treated particles to be measured themselves can be subjected to TOF-SIMS to identify the compounds present on the particle surface.
[0042] The surface-treated particles of the present invention may have a shape, for example, spherical, polyhedral, flake-like (flat shape having a pair of main surfaces and side surfaces intersecting both main surfaces), dendritic, amorphous, etc. Similarly, the core particles constituting the surface-treated particles may have a shape, for example, spherical, polyhedral, flake-like, dendritic, amorphous, etc. In particular, from the viewpoint of easily obtaining a dense sintered body, it is preferable that the surface-treated particles have a flake-like shape. In addition, from the viewpoint of easily obtaining surface-treated particles having a flake-like shape, it is preferable that the core particles have a flake-like shape. The shapes of the surface-treated particles and the core particles can be adjusted, for example, by pressing the copper particles constituting the core particles, as described later.
[0043] When the surface-treated particles are in the form of flakes, the aspect ratio, which is expressed as the ratio of the particle diameter of the major axis to the thickness of the surface-treated particles, is preferably 1.0 or more and less than 20, more preferably 3.0 or more and 15 or less. In measuring the aspect ratio, when the particle to be measured is observed under an electron microscope, the maximum diameter D of the main surface of the particle and the thickness T of the particle are measured from image data obtained by observation under the electron microscope, and the aspect ratio (D / T) is calculated by dividing D by T. This measurement and calculation is performed for 100 or more particles, and the arithmetic average value of the aspect ratios calculated for each particle is defined as the aspect ratio of the present invention.
[0044] The particle diameter of the surface-treated particles of the present invention is preferably 2 μm or more and 10 μm or less, more preferably 3 μm or more and 8 μm or less. By having such a particle diameter, when the surface-treated particles are contained in a conductive composition and used, the surface-treated particles have excellent filling properties, and when the conductive composition is used to manufacture, for example, electronic components, it is possible to obtain electronic components that have high conductivity and can be thin and compact. The particle diameter of the surface-treated particles is the volume cumulative particle diameter D at a cumulative volume of 50% by volume measured by a laser diffraction scattering particle size distribution measurement method using a laser diffraction scattering method. 50 By making the surface-treated particles satisfy the above-mentioned aspect ratio in addition to the above particle diameter, the storage stability of the conductive composition containing the surface-treated particles becomes excellent.
[0045] In addition, from the viewpoint of improving the storage stability of the conductive composition containing the surface-treated particles and obtaining surface-treated particles having conductivity equal to or higher than that of conventional ones, the thickness of the coating layer of the surface-treated particles is preferably 1 nm to 50 nm, more preferably 1 nm to 30 nm, and even more preferably 3 nm to 30 nm. The thickness of the coating layer can be measured, for example, by X-ray photoelectron spectroscopy. In detail, using an X-ray photoelectron spectroscopy measuring device (for example, PHI Quantes, manufactured by ULVAC-PHI, Inc.), sputtering is performed in the depth direction from the surface of the sample toward the inside at a sputtering rate of about 12 nm / min (SiO2 equivalent) with AlKα rays set at an output of 100 μmφ and 100 W. In the Si semi-quantitative profile in the depth direction, the position of the depth at which the intermediate value between the maximum value of the Si semi-quantitative value and the decrease saturation value of the Si semi-quantitative value inside the sample is the interface between the core particle and the coating layer, and the shortest distance from the sample surface to the interface is the thickness of the coating layer.
[0046] The surface-treated particles having the above configuration are provided with a core particle in which the surface of the copper particle is coated with silver, and a coating layer containing an organic polysiloxane compound that coats the surface of the core particle, so that when the surface-treated particles or a composition containing the surface-treated particles are stored, the viscosity of the composition is suppressed from increasing due to the elution of metal ions, resulting in excellent storage stability. According to the study by the present inventor, it was presumed that gelation or hardening occurs due to the interaction between the copper ions eluted from the copper particles and the resin or solvent contained in the composition, resulting in an increase in the viscosity of the composition. In this regard, the surface-treated particles of the present invention can suppress the elution of copper ions that contribute to an increase in viscosity by both the silver layer and the coating layer containing an organic polysiloxane compound, so that the viscosity of the composition can be maintained at the same level as that at the time of manufacture, and it is believed that the storage stability is excellent. On the other hand, the surface-treated copper particles of the prior art have a layer derived from a silane compound directly formed on the surface of the copper particles, so that the elution of copper ions from the copper particles cannot be sufficiently suppressed, resulting in poor storage stability. In addition to the improved storage stability described above, the surface-treated particles of the present invention use copper, which has high conductivity and is cheaper than silver, thereby reducing manufacturing costs and providing conductive properties equal to or better than conventional particles.
[0047] Next, a preferred method for producing the surface-treated particles of the present invention will be described. The surface-treated particles are roughly divided into a process for producing core particles by coating the surface of copper particles with silver, and a process for forming a coating layer on the outer surface of the core particles. Each process will be described below.
[0048] First, the core particles are manufactured. The copper particles constituting the core particles can be manufactured by various methods. For example, the copper particles can be obtained by a wet reduction method in which a copper compound, such as a compound having divalent copper, such as copper acetate, copper sulfate, or copper oxide, or a compound having monovalent copper, such as cuprous oxide, is wet-reduced using various reducing agents such as hydrazine. Alternatively, the core particles can be obtained by an atomization method using molten copper. Furthermore, the copper particles can also be obtained by an electrolysis method in which an anode and a cathode are immersed in a sulfuric acid electrolyte containing copper ions, a direct current is passed through the electrolyte to perform electrolysis, and copper is precipitated in powder form on the surface of the cathode. Of these, it is preferable to obtain copper particles by a wet reduction method from the viewpoint of easily controlling the particle size and producing copper particles with few impurities.
[0049] The method for producing copper particles by the wet reduction method can be, for example, the method described in JP 2003-34802 A, JP 2015-168878 A, or JP 2017-179555 A. That is, a reaction solution containing a monovalent or divalent copper source such as copper chloride, copper acetate, copper hydroxide, copper sulfate, copper oxide, or cuprous oxide is prepared in a liquid medium containing water and a monohydric alcohol preferably having 1 to 5 carbon atoms. This reaction solution is mixed with hydrazine in a ratio of preferably 0.5 to 50 moles per mole of copper, and the copper source is reduced to obtain copper particles. The obtained copper particles may be washed by a washing method such as a decantation method or a rotary filter method as necessary. The copper particles obtained in this step do not have a silver layer or a coating layer formed on their surfaces, and preferably have a spherical shape.
[0050] Next, silver is arranged on the obtained copper particles to produce the core particles. The method of arranging silver can be, for example, the method described in JP-A-2013-1917 or JP-A-2017-179555. That is, a water-soluble silver compound such as silver nitrate is used as a silver source, and the silver ions generated from the silver source are brought into contact with copper particles in water to perform displacement plating, and silver is precipitated on the surface of the core particles to obtain precursor particles, and then the precursor particles, silver ions, and a reducing agent for silver ions are brought into contact with each other in water to further precipitate silver on the surface of the precursor particles. In this way, core particles can be obtained. The proportion of silver in the core particles can be controlled by appropriately adjusting the reaction time and the concentration of silver ions.
[0051] In order to make the core particles have a non-spherical shape such as a flake shape, for example, spherical copper particles are plastically deformed by compression or the like to make them have a non-spherical shape such as a flat shape, and then silver is arranged on the surface of the copper particles to make them non-spherical core particles, or silver is arranged on the surface of spherical copper particles, and then the particles are compressed to make them have a non-spherical shape. When making the core particles have a flake shape, it is preferable to adopt a step of arranging silver on the surface of flat copper particles from the viewpoint of uniformly and evenly forming a silver layer on the surface of the core particles.
[0052] The core particles obtained through the above steps are washed, if necessary, by solid-liquid separation or the like, and then the core particles are dispersed in water or an organic solvent such as an alcohol to form a slurry, or the core particles are dried to form a dry powder that is an aggregate of core particles, and then subjected to the next step.
[0053] Next, the core particles obtained through the above-mentioned process are mixed with the alkylalkoxysilane described above as a silane coupling agent, and the alkylalkoxysilane is polymerized to form a coating layer containing an organic polysiloxane compound, which is a polymer of alkylalkoxysilane, on the surface of the core particles.
[0054] The method of mixing the core particles with an alkylalkoxysilane using a dry powder that is an aggregate of the core particles, that is, a dry mixing method, will be described below as an example.
[0055] First, the alkylalkoxysilane is dissolved in a predetermined solvent to obtain a solution. At this time, as described above, the alkylalkoxysilane used has a molecular weight of preferably 150 to 390, and the alkoxy group preferably has at least one group selected from a methoxy group and an ethoxy group. As the solvent for dissolving the alkylalkoxysilane, for example, a lower monohydric alcohol such as methanol, ethanol, or 1-propanol, or a ketone such as acetone or methyl ethyl ketone can be used. The concentration of the alkylalkoxysilane in the alkylalkoxysilane solution is preferably 1 mol / L to 20 mol / L, more preferably 3 mol / L to 10 mol / L, in terms of silicon atoms.
[0056] Next, while stirring the dry powder that is an aggregate of core particles, add the alkylalkoxysilane solution to the dry powder, and mix the core particles and the alkylalkoxysilane.The method of adding the alkylalkoxysilane solution can be, for example, dripping or spraying.From the viewpoint of easily forming a uniform coating layer on the surface of the core particles, it is preferable to add the core particles in a stirred state, more preferably adopt a spraying method, and even more preferably spray the alkylalkoxysilane solution multiple times to mix the alkylalkoxysilane.
[0057] Furthermore, from the viewpoint of facilitating the formation of a uniform coating layer on the surface of the core particles, when a method is adopted in which an alkylalkoxysilane solution is added while the core particles are being stirred, a stirring method in which a rotor is rotated by a motor is desirable. The faster the stirring speed, the better. From the viewpoint of maintaining the shape of the core particles, for example, when a 90φ container is used to stir the core particles, the stirring speed can be preferably 10,000 rpm or more and 25,000 rpm or less, and more preferably 15,000 rpm or more and 20,000 rpm or less.
[0058] The mixing conditions of the core particles and the alkylalkoxysilane in this step, specifically, the conditions of contacting the surface of the core particles while polymerizing the alkylalkoxysilanes as monomers with each other, are preferably carried out so as to maintain a temperature of 5°C or more and 60°C or less from the start of the reaction to the end of the reaction, more preferably, so as to maintain a temperature of 10°C or more and 60°C or less, and even more preferably, so as to maintain a temperature of 50°C or less. The time from the start of the reaction to the end of the reaction in this step is preferably 10 minutes or more and 120 minutes or less. From the viewpoint of efficiently obtaining surface-treated particles in which a coating layer is uniformly formed on the entire surface of the core particles, it is also preferable to continue stirring the reaction system from the start of the reaction to the end of the reaction.
[0059] Subsequently, the polymer of alkylalkoxysilane is bonded to the surface of the core particle while undergoing dehydration condensation, and the particle is coated. The reaction conditions of the dehydration condensation are preferably such that the temperature is maintained at 70°C or more and 200°C or less from the start of the reaction to the end of the reaction, and more preferably such that the temperature is maintained at 100°C or more and 150°C or less from the viewpoint of obtaining suitable conditions for dehydration. The time from the start of the reaction to the end of this step is preferably 10 minutes or more and 120 minutes or less. This makes it easier to form the coating layer more uniformly over the entire surface of the core particle.
[0060] Instead of the above-mentioned mixing method, a wet mixing method may be adopted. For example, by using a dispersion method such as stirring or ultrasonic dispersion, the core particles are dispersed in a solvent such as water to form a slurry, and then an alkylalkoxysilane is added to the slurry to contact the core particles with the alkylalkoxysilane. The amount of alkylalkoxysilane added is preferably 1 mol / L or more and 20 mol / L or less, more preferably 3 mol / L or more and 10 mol / L or less, in terms of the concentration of silicon atoms in the slurry. In addition, in the wet mixing method, it is also preferable to carry out the reaction at the above-mentioned reaction temperature and reaction time.
[0061] Through the above steps, the desired surface-treated particles are obtained. The surface-treated particles are formed by forming a coating layer containing an organic polysiloxane compound made of a polymer of alkylalkoxysilane on the surface of a core particle having a silver layer on the surface of a copper particle. The surface-treated particles may be washed by solid-liquid separation or the like, and then dispersed in a predetermined dispersion medium to form a slurry, or the washed particles may be dried by a known method such as blowing hot air to form a dry powder that is an aggregate of the particles.
[0062] The surface-treated particles may be used as they are, or may be used in the form of a conductive composition containing the surface-treated particles, a binder resin, and a solvent. The conductive composition is preferably in a form having fluidity such as a conductive ink or a conductive paste.
[0063] The conductive composition containing the surface-treated particles of the present invention is composed of at least the surface-treated particles, a binder resin, and a solvent. As the binder resin, any binder resin that has been used in the technical field of conductive compositions containing metal powders can be used without any particular limitation. Examples of the binder resin include thermoplastic resins or thermosetting resins such as polyester resins, acrylic resins, bisphenol epoxy resins such as bisphenol A type epoxy resins and bisphenol F type epoxy resins, and epoxy resins such as novolac type epoxy resins, and resin components such as ethyl cellulose and carboxyethyl cellulose. Similarly, examples of the solvent include terpene-based solvents such as terpineol and dihydroterpineol, ether-based solvents such as ethyl carbitol, butyl carbitol, and diethylene glycol monobutyl ether. These binder resins and solvents can be used independently, alone or in combination of two or more.
[0064] It is also preferable to further add at least one of a binder resin curing agent, an organic solvent other than the above-mentioned solvent, a dispersing agent, and a glass frit to the conductive composition of the present invention as necessary. Examples of binder resin curing agents include phenol-based curing agents. Examples of organic solvents include monohydric alcohols, polyhydric alcohols, polyhydric alcohol alkyl ethers, polyhydric alcohol aryl ethers, polyethers, esters, nitrogen-containing heterocyclic compounds, amides, amines, and saturated hydrocarbons. Examples of dispersing agents include nonionic surfactants. Examples of glass frits include borosilicate glass, barium borosilicate glass, and zinc borosilicate glass.
[0065] The conductive composition containing the surface-treated particles has a viscosity increase rate of preferably 30% or less, more preferably 20% or less, even more preferably 10% or less, and even more preferably 0% after storage for one month under conditions of 25°C and 60% relative humidity, i.e., the viscosity is more preferably unchanged before and after storage. Such a viscosity increase rate allows the conductive composition containing the surface-treated particles to maintain the same viscosity as immediately after production even when stored for a long period of time, resulting in high storage stability and high convenience of the conductive composition. The viscosity of the conductive composition before and after storage can be measured, for example, at 25°C using a B-type viscometer.
[0066] The viscosity of the conductive composition at 25°C before storage is preferably 10 Pa·s or more and 20 Pa·s or less, more preferably 12 Pa·s or more and 18 Pa·s or less. Furthermore, the viscosity of the conductive composition at 25°C after storage under the above-mentioned conditions is preferably 10 Pa·s or more and 26 Pa·s or less, more preferably 12 Pa·s or more and 23 Pa·s or less.
[0067] The conductive composition of the present invention can be used for various purposes by applying it to a substrate or the like to form a coating film, and then heating and curing the coating film. The cured coating film is preferably used, for example, to form a circuit on a printed wiring board, to ensure electrical continuity of an external electrode of a ceramic capacitor, or to join two objects to be joined. Depending on the type of electronic circuit, examples of the substrate include a printed circuit board made of a glass epoxy resin or a flexible printed circuit board made of a polyimide. By curing the conductive composition of the present invention, a product having high conductivity and less susceptible to defects such as cracks can be obtained.
[0068] The temperature at which the conductive composition is cured varies depending on the materials of the substrate and the objects to be joined, but is preferably 80°C or higher and 300°C or lower, more preferably 100°C or higher and 290°C or lower, and even more preferably 120°C or higher and 280°C or lower. EXAMPLES
[0069] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. In the following tables, the column marked with "-" indicates that the component is not contained.
[0070] Example 1 (1) Core particles Spherical copper particles produced by the method described in JP 2002-115001 A were plastically deformed in a dispersion mill to form flakes. Next, silver was precipitated on the surfaces of the flake-shaped copper particles by the method described in JP 2004-52044 A so that the ratio of silver in the core particles was the value shown in Table 1 below. After that, the particles were washed and dried to obtain dry, flake-shaped core particles. The particle diameter D of these core particles was 50 The particle diameter was 5.7 μm, the particle length was 4.95 μm, the average particle thickness was 1.5 μm, and the particle aspect ratio was 3.3.
[0071] (2) Formation of the coating layer 50 g of the above-mentioned dry core particles were put into a force mill (manufactured by Osaka Chemical Co., Ltd.), and while stirring at 22000 rpm, a 50% by mass solution of alkylalkoxysilane in acetone was sprayed onto the core particles multiple times, and the mixture was mixed at 50°C for 30 minutes to bring the polymer of alkylalkoxysilane into contact with the particle surface. After that, the mixture was heated at 120°C for 30 minutes to carry out dehydration condensation to coat the particles. As a result, a dry powder was obtained consisting of an aggregate of surface-treated particles in which an organic polysiloxane compound, which is a polymer of alkylalkoxysilane, was formed as a coating layer. The surface-treated particles were flake-shaped, with a particle length D of 4.95 μm, a particle thickness T of 1.5 μm, and an aspect ratio (D / T) of 3.3. The thickness of the coating layer of the surface-treated particles was 3 nm. The content of the organic polysiloxane compound in the surface-treated particles, as well as the alkylalkoxysilane and its molecular weight used, are shown in Table 1 below.
[0072] [Examples 2 to 6 and Comparative Examples 1 to 2] Surface-treated particles were obtained in the same manner as in Example 1, except that core particles were produced so that the silver content was the value shown in Table 1 below, and the alkylalkoxysilane used was changed to that shown in Table 1 below. All of these surface-treated particles were flake-shaped, with a particle length D of 4.95 μm, a particle thickness T of 1.5 μm, and a particle aspect ratio (D / T) of 3.3. The thickness of the coating layer of each surface-treated particle was in the range of 1 to 10 nm. The content of the organic polysiloxane compound in the surface-treated particles is shown in Table 1 below.
[0073] Example 7 Silver was precipitated on the surface of spherical copper particles produced by the method described in JP 2002-115001 A to produce spherical core particles, and surface-treated particles were obtained in the same manner as in Example 1, except that the alkylalkoxysilane used was changed to that shown in Table 1 below. The surface-treated particles were spherical, with a particle length D of 3.1 μm, a particle thickness T of 3.1 μm, and a particle aspect ratio (D / T) of 1.0. The thickness of the coating layer of the surface-treated particles was 6 nm. The content of the organic polysiloxane compound in the surface-treated particles is shown in Table 1 below.
[0074] [Examples 8 and 9] 90 kg of electrolytic copper (copper purity: Cu 99.95% by mass) and 10 kg of nickel plate (nickel purity: 99.99% by mass) were heated to 1400°C to form a molten metal. Next, 100 kg of the molten metal was dropped into a tundish in a water atomizer while being water atomized to obtain nickel-containing copper particles. The particles were spherical particles (average particle size 3.3 μm) containing nickel in the ratio shown in Table 1 below. Next, the nickel-containing copper particles were classified, and then silver was precipitated on the surface of the particles by the method described in JP-A-2002-115001 to produce spherical core particles. Finally, surface-treated particles were obtained in the same manner as in Example 1, except that the alkylalkoxysilanes used were those shown in Table 1 below. All of these surface-treated particles were spherical, with a particle length D of 3.3 μm, a particle thickness T of 3.3 μm, and a particle aspect ratio (D / T) of 1.0. The thickness of the coating layer of the surface-treated particles was 6 nm. The content of the organic polysiloxane compound (silicon atom content) in the surface-treated particles of each Example is shown in Table 1 below.
[0075] [Examples 10 and 11] The nickel-containing copper particles obtained in Examples 8 and 9 were plastically deformed in a dispersion mill to obtain particles, and silver was precipitated on the surfaces of the particles in the same manner as in Examples 8 and 9 to produce flaky core particles. Surface-treated particles were obtained in the same manner as in Example 1, except that the alkylalkoxysilane used was changed to that shown in Table 1 below. The surface-treated particles of Example 10 were flake-shaped, had a particle length D of 5.4 μm, a particle thickness T of 1.2 μm, and a particle aspect ratio (D / T) of 4.5. The thickness of the coating layer of the surface-treated particles was 3 nm. The surface-treated particles of Example 11 were flake-shaped, had a particle length D of 7.8 μm, a particle thickness T of 0.5 μm, and a particle aspect ratio (D / T) of 15.2. The thickness of the coating layer of the surface-treated particles was 3 nm. The content of the organic polysiloxane compound (silicon atom content) in the surface-treated particles of each Example is shown in Table 1 below.
[0076] [Evaluation of Conductivity] The electrical conductivity of the surface-treated particles in the examples and comparative examples was evaluated using a powder resistance measurement system (PD-51, manufactured by Mitsubishi Chemical Analytech Co., Ltd.) and a resistivity meter (MCP-T600, manufactured by Mitsubishi Chemical Analytech Co., Ltd.). In detail, 10 g of the surface-treated particles to be measured were placed in a probe cylinder, and the probe unit was set on the PD-51. The resistance value when a load of 1000 kg was applied by a hydraulic jack was measured using the resistivity meter. The volume resistivity (powder resistance: Ω·cm) was calculated from the measured resistance value and the thickness of the sample. The lower the volume resistivity, the higher the electrical conductivity. The results are shown in Table 1 below.
[0077] [Evaluation of storage stability] The storage stability of the conductive compositions containing the surface-treated particles in the examples and comparative examples was evaluated by the following method. Specifically, 70 mass% of the surface-treated particles to be evaluated, 10 mass% of bisphenol A type epoxy resin (manufactured by Japan Epoxylen Co., Ltd.), 2 mass% of a phenol-based hardener (novolac type phenol resin, manufactured by DIC Corporation), and the remainder of the mixture was mixed with butyl carbitol as a solvent to obtain a conductive composition A. Separately from this, 70 mass% of the surface-treated particles to be evaluated, 10 mass% of bisphenol A type epoxy resin (manufactured by Japan Epoxy Resin Co., Ltd.), 2 mass% of a phenol-based curing agent (resol type phenolic resin, manufactured by Showa Polymer Co., Ltd.), and the remainder being diethylene glycol monobutyl ether as a solvent were mixed to obtain a conductive composition B. Conductive compositions A and B were each stored independently for one month at 25°C and a relative humidity of 60%. The viscosity (Pa s) of each conductive composition at 25°C before and after storage was measured using a B-type viscometer (Brookfield, HBDV-1, No. 14), and the percentage of the viscosity (Pa s) after storage relative to the viscosity (Pa s) before storage was defined as the viscosity increase rate (%). The lower the viscosity increase rate, the higher the storage stability. The results are shown in Table 1.
[0078] [Table 1]
[0079] As shown in Table 1, it is found that the surface-treated particles of each Example have electrical conductivity equal to or greater than that of conventional ones. In addition, it is found that the conductive composition containing the surface-treated particles of each Example has little change in viscosity even after long-term storage, and has high storage stability. In particular, it is found that the surface-treated particles of Examples 4 to 9, which use alkylalkoxysilanes having a molecular weight in a suitable range, can provide a conductive composition with even more excellent storage stability.
Claims
1. The present invention has a core particle and a coating layer including an organic polysiloxane compound disposed on the surface of the core particle, the core particles are copper particles whose surfaces are coated with silver, In the organic polysiloxane compound, the groups bonded to silicon atoms, excluding the oxygen atoms constituting the siloxane bonds, are either only alkyl groups or only alkoxy groups and alkyl groups; the alkyl group is an alkyl group having from 2 to 17 carbon atoms, or a methyl group and an alkyl group having from 2 to 17 carbon atoms; The surface-treated particles have a silver content of 1% by mass or more and 25% by mass or less in the core particle.
2. The surface-treated particles according to claim 1 , which are in a flake shape.
3. 3. The surface-treated particle according to claim 1, wherein the alkyl group comprises a linear alkyl group having from 2 to 17 carbon atoms.
4. 4. The surface-treated particles according to claim 1, comprising the organopolysiloxane compound in an amount of 0.002% by mass or more and 0.3% by mass or less in terms of silicon atoms.
5. The surface-treated particle according to any one of claims 1 to 4, wherein the copper particle is substantially formed only from copper and does not contain other elements except for unavoidable impurities, or is composed of copper and a metal element other than copper.
6. A method for producing surface-treated particles, comprising mixing core particles with an alkylalkoxysilane and polymerizing the alkylalkoxysilane to form an organic polysiloxane compound, which is a polymer of the alkylalkoxysilane, on the surface of the core particles, the method comprising the steps of: As the core particles, copper particles having a surface coated with silver are used, The method for producing surface-treated particles uses, as the alkylalkoxysilane, one having a molecular weight of 150 or more and 390 or less and having, as an alkoxy group, at least one type of group selected from the group consisting of a methoxy group and an ethoxy group.
7. A conductive composition comprising the surface-treated particles according to claim 1 , a binder resin, and a solvent.
8. 8. The conductive composition according to claim 7, wherein the increase in viscosity (25°C) after storage in an environment at 25°C for one month is 30% or less.
9. A method for producing an electrochemical particle comprising the steps of: (a) providing a core particle having a coating layer disposed on a surface of the core particle and comprising: the core particles are copper particles whose surfaces are coated with silver, In the organic polysiloxane compound, the groups bonded to silicon atoms, excluding the oxygen atoms constituting the siloxane bonds, are either only alkyl groups or only alkoxy groups and alkyl groups; the alkyl group is an alkyl group having from 2 to 17 carbon atoms, or a methyl group and an alkyl group having from 2 to 17 carbon atoms; Surface treatment particles in the form of flakes.
Citation Information
Patent Citations
Preventing method for oxidation of copper powder
JP1982155386A
Manufacture of copper fine powder
JP1990034708A
Copper powder for conductive paste with superior oxidation resistance, and manufacturing method therefor
JP2003016832A
Conductive paste and prepreg using the same, metal foiled laminated plate, and printed wiring board