Polyesters with specific crystallization half-times
Semi-crystalline polyesters with controlled crystallization half-times and melting points address the moldability and weatherability issues of PET, enabling efficient processing and high-temperature applications.
Patent Information
- Application Number
- JP2021533472
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-13
- Filing Date
- 2019-12-12
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2039-12-12
AI Technical Summary
Existing polyesters, particularly polyethylene terephthalate (PET), face challenges in high-temperature applications due to high mold temperatures required for moldability and limited compatibility with current manufacturing processes, leading to poor processability and unsuitable melting points, which hinders their use in injection molded products and outdoor weatherability.
Development of semi-crystalline polyesters with specific repeating units, including aliphatic, aromatic, or heterocyclic groups, and diol residues, such as 1,4-butanediol and neopentanediol, with controlled crystallization half-times and melting points, achieved through a method involving transition metal catalysts and oxidizing agents, enabling improved processability and high-temperature performance.
The semi-crystalline polyesters exhibit enhanced crystallization half-times and melting points, allowing for efficient processing in existing equipment and improved weatherability, making them suitable for high-temperature applications and outdoor exposure.
Smart Images

Figure 0007594530000001 
Figure 0007594530000002 
Figure 0007594530000003
Abstract
Description
[Technical field]
[0001] This invention relates generally to improved polyesters, compositions containing such improved polyesters, and articles, such as films and injection molded articles, formed from such improved polyesters. [Background technology]
[0002]
[0002] Polyesters are often considered the world's most utilized class of polymers, with recently reported published world production (including recycling) well over 75 million tons. This level of commercial success is attributed in part to polyester's attractive combination of relative cost, manufacturability, and competitive performance attributes. The physical, chemical, and thermal properties of polyesters make them useful and desirable for a wide variety of end-use applications. Polyethylene terephthalate (PET) is perhaps one of the most common types of polyester for many end-use applications.
[0003]
[0003] Despite these commercial volumes, polyesters have generally not penetrated well into certain end-use markets, such as the manufacture of injection molded articles, particularly those used in higher temperature applications such as under-the-hood automotive parts. For example, U.S. Patent No. 4,486,561 states that PET "is not necessarily the most suitable material for use in injection molding because relatively high mold temperatures, e.g., 120°-140°C, must be used to ensure good moldability." Attempts to develop commercially cost-competitive, injection-moldable, and / or higher melting point polyesters have been less than successful.
[0004]
[0004] Similarly, as noted in U.S. Patent No. 4,355,080 issued to the assignee of the present invention, certain older generation polyesters are generally "unaccepted as sheet materials for signs, windows, and the like due to embrittlement and surface deterioration upon aging, particularly under outdoor exposure conditions." The invention in the '080 patent addresses this problem through the invention that "acrylic polymers can be compression laminated to the surface of a polyester substrate to produce a permanently bonded composite sheet that has excellent retention of surface and physical properties over extended outdoor exposure." While this solution is alleged to address weatherability, it requires additional materials and processing steps, significantly increasing manufacturing costs. Also notable with respect to the weatherability of polyesters is U.S. Patent No. 7,132,499, which describes polyester containers with improved weatherability, the containers being made from a polyester resin composition comprising (A) 100 parts by weight of a polyester resin and (B) 0.01 to 10 parts by weight of a specific triazine ultraviolet absorber. As with many common attempts to solve polymer deficiencies with additives, the additive materials increase cost, can affect the processability of the composition, have limited effectiveness, and may have undesirable side effects on other aspects of the composition's performance.
[0005]
[0005] Modifications within the conventional polyester polymer structure have been explored to improve various aspects of polyester performance in general. For example, U.S. Pat. No. 3,256,241 describes polyesters prepared by reacting 1,4-bicyclo[2.2.2]octanedicarboxylic acid or its ester-forming derivatives with dihydroxy compounds or their ester-forming derivatives. These polyester products are generally characterized by good light stability, both outdoors and indoors; however, their crystallization half-times and other properties make them less suitable, if not incompatible, for processing in the equipment and systems currently used to manufacture end products compared to more common polyesters such as polyethylene terephthalate (PET). Furthermore, none of the polyesters described in the '241 patent are expected to form well into injection molded articles or reach a melting point suitable for high temperature applications.
[0006]
[0006] Despite these techniques for improving polyesters and polyester compositions to meet the latest and greatest performance specifications, there remains a need for improved polyesters that cost-effectively meet and maintain performance specifications over time, while meeting the processability requirements of existing end-product manufacturing systems. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] U.S. Patent No. 4,486,561 [Patent Document 2] U.S. Patent No. 4,355,080 [Patent Document 3] U.S. Patent No. 7,132,499 [Patent Document 4] U.S. Patent No. 3,256,241 Summary of the Invention
[0008] In a first aspect, the present invention provides a compound of formula:
[0009] [ka]
[0010] wherein A is an aliphatic, aromatic, or heterocyclic group; R1 is selected from the group consisting of 1,4-butanediol and 1,4-cyclohexanedimethanol residues; R2 is a neopentanediol residue; m is 50 to 99, inclusive; n is 1 to 50, inclusive; and x is 1 to 200, inclusive; said semicrystalline polyesters exhibit a minimum crystallization half-time of about 0.3 minutes or greater, or about 0.5 minutes or greater, or about 0.6 minutes or greater, or about 0.7 minutes or greater.
[0011] In another aspect, the invention relates to a composition comprising the polyester of the first aspect of the invention. In yet another aspect, the present invention relates to a film, especially a monolayer film, comprising the semicrystalline polyester of the first aspect of the invention.
[0012] In yet another aspect, the present invention relates to an injection molded article comprising the semicrystalline polyester of the first aspect of the invention. In yet another aspect, the present invention provides a compound of formula:
[0013] [ka]
[0014] wherein A is an aliphatic, aromatic, or heterocyclic group; R1 is selected from the group consisting of 1,4-butanediol and 1,4-cyclohexanedimethanol residues; R2 is a neopentanediol residue; m is 50 to 99, inclusive; n is 1 to 50, inclusive; x is 1 to 200, inclusive, or 80 to 160, inclusive; said semicrystalline polyester exhibiting a minimum crystallization half-time of about 0.3 minutes or more, or about 0.5 minutes or more, or about 0.6 minutes or more, or about 0.7 minutes or more, The method comprises: Formula (A)
[0015] [ka]
[0016] (i) a transition metal catalyst comprising a palladium compound and (ii) an oxidizing agent, and optionally Formula (I)
[0017] [ka]
[0018] [Wherein, R represents hydrogen; and C1-C6 alkoxy, halo, nitro, and cyano, which may be substituted by one or more groups selected from the group consisting of C1-C6 alkoxy, halo, nitro, and cyano. 12 R is selected from alkyl; * is hydrogen; C1-C6 alkoxy, halo, nitro, and cyano, each of which may be substituted by one or more groups. 12 and an alkali metal cation; or Formula (II)
[0019] [ka]
[0020] C1-C12 Compounds having at least one alkanoyloxy moiety; and contacting in the presence of at least one of the formula
[0021] [ka]
[0022] wherein each R1 is independently hydrogen or a group of formula
[0023] [ka]
[0024]
[0043] wherein Formula (B)
[0025] [ka]
[0026] wherein each R1 is independently hydrogen or a group of formula
[0027] [ka]
[0028] with carbon monoxide in the presence of a strong acid, followed by quenching with at least one of (i) water or (ii) an alcohol of formula R-OH to produce a compound of formula
[0029] [ka]
[0030] resulting in a compound of formula (I); (C) optionally, a compound of the formula
[0031] [ka]
[0032] is treated with an oxidizing agent to obtain a compound of the formula
[0033] [ka]
[0034] resulting in a compound of formula (I); (D) Compound
[0035] [ka]
[0036] with a difunctional hydroxyl compound selected from the group consisting of 1,4-butanediol, neopentyl glycol, and 1,4-cyclohexanedimethanol; and (E) subjecting the resulting product to one or more polycondensation reaction steps to form a polyester; Includes.
[0037] Other aspects of the invention are disclosed and claimed herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] The term "residue" as used herein means any organic structure incorporated into a polymer from the corresponding monomer via polycondensation and / or esterification reactions. The term "repeating unit" as used herein means an organic structure having dicarboxylic acid and diol residues linked through carbonyloxy groups. The term "semicrystalline" as used herein indicates that the polyester has a substantially amorphous but partially crystalline morphology, meaning that the polyester contains substantially disordered polymeric regions along with some ordered regions. The crystallization half-times of the polyesters of the present invention are somewhat indicative of their character as semicrystalline.
[0039] In a first aspect, the present invention is directed to a semi-crystalline polyester comprising a repeat unit of formula (II)
[0040] [ka]
[0041] wherein A is an aliphatic, aromatic, or heterocyclic group; R1 is selected from the group consisting of 1,4-butanediol and 1,4-cyclohexanedimethanol residues; R2 is a neopentanediol residue; m is 50 to 99, inclusive; n is 1 to 50, inclusive; x is 1 to 200, inclusive, or 80 to 160, inclusive; said semicrystalline polyesters exhibit a minimum crystallization half-time of about 0.3 minutes or greater, or about 0.5 minutes or greater, or about 0.6 minutes or greater, or about 0.7 minutes or greater. The polyesters of this aspect of the invention, in various embodiments, exhibit one or more desirable performance characteristics and are therefore particularly useful in applications and utilities where a high level of performance in such characteristics is required.
[0042]
[0015] As used herein, "polyester" is generally intended to include, without limitation, homopolymers as well as copolymers, terpolymers, and the like, and is typically prepared by reacting a difunctional carboxylic acid or ester thereof, often a dicarboxylic acid, or a mixture of such acids or esters, with a difunctional hydroxyl compound, often a diol or glycol, or a mixture of such diols or glycols. Alternatively, the difunctional carboxylic acid can be a hydroxycarboxylic acid and the difunctional hydroxyl compound can be an aromatic nucleus bearing two hydroxyl substituents, such as hydroquinone. Polyesters and polyester manufacture are generally well known and are exemplified, for example, in U.S. Pat. No. 7,781,562, assigned to the assignee of the present invention, the contents and disclosure of which are incorporated herein by reference.
[0043] The substituent or group "A" in the above formula is selected from the group consisting of aliphatic groups, aromatic groups and heterocyclic groups. Suitable examples of group A include, but are not limited to, the residues of succinic acid, sebacic acid, azelaic acid, adipic acid, dimer acid such as that commercially available under the trade name Empol® 1010, glutaric acid, 1,4-cyclohexanedicarboxylic acid, isophthalic acid, carbonic acid, pimelic acid, dimethylmalonic acid, 2,6-naphthalenedicarboxylic acid, phthalic acid, suberic acid, 1,12-dodecanedicarboxylic acid, 4,4'-sulfonyldibenzoic acid, diglycolic acid, 1,3-phenylenedioxydiacetic acid, 5-(sodiosulfo)isophthalic acid and 4,4'-stilbenedicarboxylic acid.
[0044] In one or more embodiments, R1 and R2 are each independently selected from the group consisting of 1,2-ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, neopentyl glycol, neopentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, diethylene glycol, triethylene glycol, isosorbide, poly(oxytetramethylene glycol), bicyclo[2.2.2]octane-1,4-dimethanol and 1,4-benzenedimethanol residues, and mixtures thereof. In one or more embodiments, R1 is selected from the group consisting of 1,2-ethylene glycol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,4-cyclohexanedimethanol and bicyclo[2.2.2]octane-1,4-dimethanol residues, and R2 is selected from the group consisting of 1,2-ethylene glycol, 1,4-butanediol, neopentanediol, neopentyl glycol and 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues. In one or more embodiments, R1 is a 1,4-butanediol residue. In one or more embodiments, R1 is a 1,4-cyclohexanedimethanol residue. In one or more embodiments, R2 is a neopentanediol residue.
[0045] The value of "m" can be 50 to 99, inclusive, or 65 to 95, inclusive, or 80 to 90, inclusive. The value of n can be 1 to 50, inclusive, or 5 to 35, inclusive, or 10 to 20, inclusive. The value of x can be 1 to 200, inclusive. Thus, the semicrystalline polyester of the present invention may include other polyester repeat units. The semicrystalline polyester of the present invention preferably contains 1 to 100 mol % of the repeat unit of the above formula (II).
[0046]
[0019] Such other polyester repeat units are well known in the art and are exemplified in the above-referenced U.S. Patent No. 7,781,562. Briefly, such repeat units are prepared by the reaction of one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxyl compounds and / or polyfunctional hydroxyl compounds. Typically, the difunctional carboxylic acids can be dicarboxylic acids and the difunctional hydroxyl compounds can be dihydric alcohols such as, for example, glycols and diols. The term "glycols" as used in this application includes, but is not limited to, diols, glycols, and / or polyfunctional hydroxyl compounds, such as branching agents. Alternatively, the difunctional carboxylic acids can be hydroxycarboxylic acids, such as, for example, p-hydroxybenzoic acid, and the difunctional hydroxyl compounds can be aromatic nuclei bearing two hydroxyl substituents, such as, for example, hydroquinone. Thus, for example, the dicarboxylic acid residues can be derived from dicarboxylic acid monomers or their associated acid halides, esters, salts, anhydrides, or mixtures thereof. Thus, as used herein, the term dicarboxylic acid is intended to encompass dicarboxylic acids and any derivatives of dicarboxylic acids useful in the reaction process with diols to make polyesters, including their associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides, or mixtures thereof. Additionally, as used in this application, the term "diacid" includes polyfunctional acids, such as branching agents.
[0047] It should be noted that the designations used for the repeat units in the above formula do not in themselves designate or indicate any particular polymer morphology. Nonetheless, in one or more embodiments, the polyesters of the present invention are semicrystalline polyesters.
[0048] In one embodiment, the semicrystalline polyesters of the present invention have a minimum crystallization half-time of about 0.3 minutes or more, or about 0.5 minutes or more, or about 0.6 minutes or more, or about 0.7 minutes or more.
[0049] In one or more embodiments, the semicrystalline polyesters of the invention have melting points of 240° C. to 275° C., or 255° C. to 275° C., as measured using DSC techniques known in the art on standard commercially available equipment. Particularly suitable semicrystalline copolymers of the invention have melting points of 240° C. to 275° C. and contain 1,4-cyclohexanedimethanol residues as R1.
[0050] The semicrystalline polyesters of the present invention, in one or more embodiments, exhibit improved weatherability. Weatherability and the analytical methods for measuring it are well known in the art and are exemplified by ASTM methods D1435-12 and D4364-13 (accelerated).
[0051] In another aspect, the present invention is directed to a method for forming a polyester comprising repeat units of formula (I) above. The method of the present invention comprises: Formula (A)
[0052] [ka]
[0053] (i) a transition metal catalyst comprising a palladium compound and (ii) an oxidizing agent, and optionally Formula (I)
[0054] [ka]
[0055] [Wherein, R represents hydrogen; and C1-C6 alkoxy, halo, nitro, and cyano, which may be substituted by one or more groups selected from the group consisting of C1-C6 alkoxy, halo, nitro, and cyano. 12 R is selected from alkyl; *is hydrogen; C1-C6 alkoxy, halo, nitro, and cyano, each of which may be substituted by one or more groups. 12 and an alkali metal cation; or Formula (II)
[0056] [ka]
[0057] C1-C 12 Compounds having at least one alkanoyloxy moiety; and contacting in the presence of at least one of the formula
[0058] [ka]
[0059] wherein each R1 is independently hydrogen or a group of formula
[0060] [ka]
[0061]
[0043] Formula (B)
[0062] [ka]
[0063] wherein each R1 is independently hydrogen or a group of formula
[0064] [ka]
[0065] with carbon monoxide in the presence of a strong acid, followed by quenching with at least one of (i) water or (ii) an alcohol of formula R-OH to produce a compound of formula
[0066] [ka]
[0067] providing a compound of formula (I); (C) optionally, a compound of the formula
[0068] [ka]
[0069] is treated with an oxidizing agent to obtain a compound of the formula
[0070] [ka]
[0071] providing a compound of formula (I); (D) Compound
[0072] [ka]
[0073] with a difunctional hydroxyl compound selected from the group consisting of 1,4-butanediol, neopentyl glycol, and 1,4-cyclohexanedimethanol; and (E) subjecting the resulting product to one or more polycondensation reaction steps to form a polyester; Includes.
[0074]
[0025] Suitable compounds and their preparation methods are known in the art and are described, for example, in WO2018 / 075301 A1, which is assigned to the assignee of the present invention. The contents and disclosures of said patent are incorporated herein by reference. Particularly suitable compounds are bicyclo[2.2.2]octane compounds selected from the group consisting of 4-(methoxycarbonyl)bicyclo[2.2.2]octane-1-carboxylic acid and dimethylbicyclo[2.2.2]octane-1,4-dicarboxylate.
[0075] In another aspect, the present invention is directed to a composition comprising a semicrystalline polyester comprising a repeat unit of formula (II):
[0076] [ka]
[0077] wherein A is an aliphatic, aromatic, or heterocyclic group; R1 is selected from the group consisting of 1,4-butanediol and 1,4-cyclohexanedimethanol residues; R2 is a neopentanediol residue; m is 50 to 99, inclusive; n is 1 to 50, inclusive; x is 1 to 200, inclusive, or 80 to 160, inclusive; and the semi-crystalline polyester exhibits a minimum crystallization half-time of about 0.3 minutes or more, or about 0.5 minutes or more, or about 0.6 minutes or more, or about 0.7 minutes or more.
[0078]
[0027] The composition of the present invention may preferably contain at least 5 weight percent, or at least 10 weight percent, or at least 20 weight percent, or at least 30 weight percent, or at least 40 weight percent, or at least 50 weight percent of the semicrystalline polyester of the present invention.
[0079] The composition of the present invention may further include at least one other polymer. Polymers suitable for the composition of the present invention include, by way of non-limiting example, polycarbonates, acrylics, polystyrene, cellulose esters, polydimethylsiloxanes, and the like.
[0080] The compositions of the present invention may also contain one or more other conventional additives and ingredients. For example, additives such as reinforcement, mold release agents, fillers, surface friction modifiers, light and heat stabilizers, extrusion aids, antistatic agents, colorants, dyes, pigments, optical brighteners, antibacterial agents, anti-counterfeiting markers, hydrophobic and hydrophilic enhancers, viscosity modifiers, slip agents, tougheners, adhesion promoters, and the like may be used. Colorants, sometimes called toners, may be added to impart a desired neutral hue and / or brightness to the composition when applied in an end use that specifies such characteristics. Optional ingredients such as these, and their selected concentrations, are typically selected based on the specifications and suitability of the particular end use of the individual composition.
[0081] In another aspect, the present invention is directed to a film comprising the semicrystalline polyester of the present invention. In one aspect, the film is a monolayer film. The film of the present invention has a thickness of from 1 mil to about 14 mil in one aspect. The film of the present invention can be produced by methods known in the art, such as those exemplified in U.S. Pat. No. 5,958,581, the contents and disclosures of which are incorporated herein by reference. An important feature of the film of the present invention is that it can be uniaxially or biaxially stretched. Methods and apparatus for producing stretched polyester films, as well as the stretched polyester films themselves, are well known in the art and are described, for example, in U.S. Pat. Nos. 4,020,141 and 6,368,532, the contents and disclosures of which are incorporated herein by reference. Thus, in one or more aspects, the film of the present invention is a biaxially stretched film or a biaxially stretched monolayer film.
[0082]
[0031] The film of the present invention can generally be useful in end-use applications where the film is exposed to the elements, direct sunlight and / or UV light for extended periods of time. Thus, in one illustrative, non-limiting example, the film of the present invention is useful as a backsheet for a solar cell module. Solar cell modules and their manufacture as well as backsheets for modules are generally known in the art, as exemplified in U.S. Pat. No. 9,082,912 B2 and U.S. Published Patent Application No. 2008 / 0053512 A1, the contents and disclosures of which are incorporated herein by reference.
[0083] In another aspect, the present invention is directed to an injection molded article comprising the semicrystalline polyester of the present invention. An injection molded article is any article formed using known conventional injection molding techniques and equipment, for example, as described in U.S. Patent Nos. 5,707,667 and 3,533,594, the contents and disclosures of which are incorporated herein by reference.
[0084] The following examples are provided to illustrate the particularities and to detail the many aspects and advantages of the present invention, but are not to be construed as limiting the scope of the invention in any way. Those skilled in the art will readily recognize variations, modifications and adaptations that fall outside the scope of the invention. Throughout these examples, in measuring the indicated parameters, the following experimental and analytical techniques were employed when actually measuring these parameters: The inherent viscosity of the polyester was determined in 60 / 40 (w / w) phenol / tetrachloroethane at a concentration of 0.5 g / 100 mL at 25°C.
[0085]
[0035] Melting temperature (T m ) and glass transition temperature (T g) was determined using a TA Instruments Q2000 model Differential Scanning Calorimeter (DSC). Approximately 3 mg of sample was weighed and placed into an aluminum pan. A suitable lid was placed on top and crimped into place. The sample was then placed into the DSC cell along with an empty aluminum pan as a control. The lid was placed on the cell and the temperature scan was started. The instrument cooled the sample to 0°C to begin the first heating scan. During this heating scan, the sample was heated to the maximum temperature at a rate of 20°C / min and then held isothermally for 1 minute to ensure complete melting of the sample. The instrument then cooled the sample to 0°C at a rate of 20°C / min and held isothermally for 30 seconds to allow the instrument to equilibrate. The sample was then heated a second time to the maximum temperature at a rate of 20°C / min. Data was transferred to Universal Analysis software to measure the glass transition temperature (T g ), crystallization by heating (T ch ), T m , or crystallization by cooling (T cc ) and other transfers were integrated.
[0086] Crystallization half-time was measured on a Perkin Elmer 8500 DSC instrument. Measurements were made by measuring the heat flow of the sample versus temperature. Once the sample was prepared, the Pyrus operating software was opened and the appropriate identifying information was entered. The sample was placed in the DSC cell along with an empty pan as a control. The furnace lid was put in place and the test started. The instrument rotated the sample from 0° C. to T max Heat to T max The sample was then isothermally held at T for 2 minutes to ensure complete melting. The sample was then cooled at the maximum rate the instrument was designed to reach, up to 600°C / min, to the first designated crystallization temperature and held isothermally for a prescribed time, typically 30 minutes. If an additional crystallization temperature was present, the sample was cooled at a rate of 600°C / min to T maxThe crystallization temperature was then reheated to 0.5° C. and held isothermally for 2 minutes. It was then cooled to the next crystallization temperature as described above. This pattern of heating, cooling and isothermal holding would be continued until all crystallization temperatures had been tested. Once testing was completed, the data was analyzed by integrating the start of the isothermal hold and the maximum of the crystallization peak on a graph of heat flow versus time. The start time of the isothermal hold was subtracted from the time of the peak maximum, resulting in the crystallization half-time at the crystallization temperature. The "minimum crystallization half-time" (referred to herein as t 1 / 2 t (sometimes denoted as t ) is the minimum time required to achieve approximately half of the maximum achievable crystallinity at a given crystallization temperature. 1 / 2 is the crystallization temperature T c depends in part on t 1 / 2 is typically the glass transition temperature (T g ) and melting temperature (T m ) the minimum value, i.e., the maximum crystallization rate, is at a temperature approximately halfway between the temperatures. EXAMPLES
[0087] Example 1 (Control) A monomer composition of a mixture of 0.10 mol of 4-(methoxycarbonyl)bicyclo[2.2.2]octane-1-carboxylic acid, 0.15 mol of 1,4-butanediol, and 0.0029 g of titanium dioxide was placed in a 250 mL flask equipped with an inlet for nitrogen, a metal stirrer, and a short distillation column. The flask was placed in a metal bath at 200° C. The stirring speed was set at 200 RPM. The contents of the flask were heated at 200° C. for 5 minutes, after which the temperature was gradually increased to 255° C. over a period of 3 hours. The reaction mixture was held at 255° C. for 10 minutes, after which the pressure inside the flask was gradually reduced over a period of 10 minutes until the pressure inside the flask reached 100 mmHg. The pressure inside the flask was further reduced to 0.5 mmHg over a period of 5 minutes. The stirring speed was set at 100 RPM. A pressure of 0.5 mmHg was maintained for a total period of 3 hours to remove excess unreacted diol. IV of 0.872, T of 53.6°C g , and a T of 193.6 °C mA polyester (poly(1,4-butylene 1,4-bicyclo[2.2.2]octane dicarboxylate) having the formula (I) was obtained. Rapid crystallization was observed, and therefore the crystallization half-time was not measured. Example 2 The procedure used to form the polyester described in Example 1 was used in Example 2 with the following monomer composition: 0.10 mol dimethylbicyclo[2.2.2]octane-1,4-dicarboxylate, 0.135 mol 1,4-butanediol, and 0.015 mol neopentyl glycol. IV of 0.905, T of 47.0° C. g , and a T of 182.0 °C m A polyester (poly[(1,4-butylene 1,4-bicyclo[2.2.2]octane dicarboxylate)-co-(neopentylene 1,4-bicyclo[2.2.2]octane dicarboxylate)], 1,4-butylene:neopentylene=90:10) having the formula: ##STR1## was obtained. The crystallization half-time of this material was then measured at multiple temperatures, and the measured crystallization half-times were as follows: 2.1 min at 80°C, 1.0 min at 90°C, 0.7 min at 100°C, 0.6 min at 105°C, 0.6 min at 110°C, 0.7 min at 115°C, 0.8 min at 120°C, 1.3 min at 130°C, and 2.1 min at 140°C. Thus, the sample is characterized by a minimum crystallization half-time of 0.6 min.
[0088] Example 3 The procedure used to form the polyester described in Example 1 was used in Example 3 with the following monomer composition: 0.10 mol dimethylbicyclo[2.2.2]octane-1,4-dicarboxylate, 0.132 mol 1,4-butanediol, and 0.018 mol neopentyl glycol. IV of 0.998, T of 48.0° C. g , and a T of 165.0 °C mA polyester (poly[(1,4-butylene 1,4-bicyclo[2.2.2]octane dicarboxylate)-co-(neopentylene 1,4-bicyclo[2.2.2]octane dicarboxylate)], 1,4-butylene:neopentylene=88:12) having the above structure was obtained. The crystallization half-time of this material was then measured at several temperatures, and the measured crystallization half-times were as follows: 0.9 min at 80°C, 0.4 min at 90°C, 0.3 min at 100°C, 105°C, 110°C and 115°C, 0.4 min at 120°C, 0.9 min at 130°C, and 1.7 min at 140°C. Thus, the sample is characterized by a minimum crystallization half-time of 0.3 min. Example 4 The procedure used to form the polyester described in Example 1 was used in Example 4 with the following monomer composition: 0.10 mol dimethylbicyclo[2.2.2]octane-1,4-dicarboxylate, 0.128 mol 1,4-butanediol, and 0.023 mol neopentyl glycol. IV of 0.904, T of 42.0° C. g , and a T of 151.0 °C m A polyester (poly[(1,4-butylene 1,4-bicyclo[2.2.2]octane dicarboxylate)-co-(neopentylene 1,4-bicyclo[2.2.2]octane dicarboxylate)], 1,4-butylene:neopentylene=85:15) having the above structure was obtained. The crystallization half-time of this material was then measured at several temperatures, and the measured crystallization half-times were as follows: 10.8 min at 80°C, 5.8 min at 90°C, 4.6 min at 100°C, 4.5 min at 105°C, 4.9 min at 110°C, 5.6 min at 115°C, 7.2 min at 120°C, 14.2 min at 130°C, and 20.0 min at 140°C. Thus, the sample is characterized by a minimum crystallization half-time of 4.5 min.
[0089] Example 5 (Control) A mixture of 0.10 mol of 4-(methoxycarbonyl)bicyclo[2.2.2]octane-1-carboxylic acid, 0.11 mol of 1,4-cyclohexanedimethanol (cis / trans=31 / 69), and 0.0029 g of titanium dioxide was placed in a 250 mL flask equipped with an inlet for nitrogen, a metal stirrer, and a short distillation column. The flask was placed in a metal bath at 200° C. The stirring speed was set at 200 RPM. The contents of the flask were heated at 200° C. for 5 minutes, after which the temperature was gradually increased to 255° C. over a period of 3 hours. The temperature was gradually increased to 280° C. over a period of another 10 minutes. The reaction mixture was held at 280° C. The pressure inside the flask was reduced to 400 mmHg over a period of 5 minutes. The pressure was further reduced to 100 mmHg, and the stirring speed was reduced to 100 RPM over a period of 5 minutes. The pressure was further reduced to 0.5 mmHg and the stirring speed was reduced to 50 RPM over 5 minutes. The 0.5 mmHg pressure was maintained for a total time of 3 hours to remove excess unreacted diol. IV of 0.629, T of 131° C. g , and a T of 299.0 °C m The crystallization half-times of this material were then measured at multiple temperatures, and the measured crystallization half-times were as follows: 0.1 min at 210° C., 0.2 min at 220° C., and 0.3 min at 230° C. The crystallization half-times of this material at 170° C., 180° C., 190° C., and 200° C. were too short (less than 0.1 min) to be accurately determined. Example 6 The procedure used to form the polyester described in Example 5 was used in Example 7 with the following monomer composition: 0.10 mol of 4-(methoxycarbonyl)bicyclo[2.2.2]octane-1-carboxylic acid, 0.097 mol of 1,4-cyclohexanedimethanol (cis / trans=31 / 69), and 0.018 mol of neopentyl glycol. IV of 0.689, T of 123° C. g , and a T of 274 °C mA polyester (poly[(1,4-cyclohexanedimethylene 1,4-bicyclo[2.2.2]octanedicarboxylate)-co-(neopentylene 1,4-bicyclo[2.2.2]octanedicarboxylate)], 1,4-cyclohexanedimethylene:neopentylene=88:12) having the formula: ##STR1## was then obtained. The crystallization half-time of this material was then measured at multiple temperatures, and the measured crystallization half-times were as follows: 2.4 min at 160°C, 1.4 min at 170°C, 0.5 min at 175°C, 0.4 min at 185°C, 0.4 min at 195°C, 0.5 min at 205°C, and 0.8 min at 215°C. Thus, the sample was characterized by a minimum crystallization half-time of 0.4 min.
[0090] Example 7 The procedure used to form the polyester described in Example 5 was used in Example 8 with the following monomer composition: 0.10 mol of 4-(methoxycarbonyl)bicyclo[2.2.2]octane-1-carboxylic acid, 0.096 mol of 1,4-cyclohexanedimethanol (cis / trans=31 / 69), and 0.023 mol of neopentyl glycol. IV of 0.610, T of 110° C. g , and a T of 255 °C m A polyester (poly[(1,4-cyclohexanedimethylene 1,4-bicyclo[2.2.2]octanedicarboxylate)-co-(neopentylene 1,4-bicyclo[2.2.2]octanedicarboxylate)], 1,4-cyclohexanedimethylene:neopentylene=85:15) having the formula: was obtained. The crystallization half-time of this material was then measured at multiple temperatures, and the measured crystallization half-times were as follows: 13.4 minutes at 160°C, 7.1 minutes at 170°C, 6.1 minutes at 180°C, 6.0 minutes at 190°C, and 7.8 minutes at 200°C. Thus, the sample was characterized by a minimum crystallization half-time of 6.0 minutes. Example 8 (Control) The procedure used to form the polyester described in Example 5 was used in Example 9 with the following monomer composition: 0.10 mol of 4-(methoxycarbonyl)bicyclo[2.2.2]octane-1-carboxylic acid, 0.088 mol of 1,4-cyclohexanedimethanol (cis / trans=31 / 69), and 0.030 mol of neopentyl glycol. IV of 0.765, T of 116° C. g , and a T of 244 °C m A polyester (poly[(1,4-cyclohexanedimethylene 1,4-bicyclo[2.2.2]octanedicarboxylate)-co-(neopentylene 1,4-bicyclo[2.2.2]octanedicarboxylate)], 1,4-cyclohexanedimethylene:neopentylene=80:20) was obtained with the formula: The crystallization half-time of this material at 110°C-200°C was significantly slow (>30 min) and therefore was not determined.
[0091]
[0045] The foregoing description of various embodiments of the present invention has been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise embodiments disclosed. Many modifications or variations are possible in light of the above teachings. The embodiments discussed have been chosen and described to provide the best illustration of the principles of the present invention and its application, and to enable those skilled in the art to utilize the invention in its various embodiments, and with various modifications to suit the particular uses contemplated. All such modifications and variations are within the scope of the present invention, as determined by the appended claims, when interpreted in accordance with the full breadth to which they are fairly, legally and equitably entitled. This specification includes the disclosure of the following inventions. [Item 1] Formula: [ka] Semicrystalline polyesters containing repeat units of [wherein A is an aliphatic, aromatic or heterocyclic group; R 1 is selected from the group consisting of 1,4-butanediol residues and 1,4-cyclohexanedimethanol residues; R 2 is the residue of neopentanediol; m is 50 to 99, inclusive; n is 1 to 50, inclusive; x is 1 to 200, inclusive; and said semi-crystalline polyester exhibits a minimum crystallization half-time of about 0.3 minutes or greater. [Item 2] The semi-crystalline polyester according to item 1, wherein the minimum crystallization half-time is 0.5 minutes or more. [Item 3] The semi-crystalline polyester according to item 2, wherein the minimum crystallization half-time is 0.6 minutes or more. [Item 4] The semi-crystalline polyester according to item 1, wherein the semi-crystalline polyester has a melting point of 240°C to 275°C. [Item 5]R 1 2. The semicrystalline polyester according to claim 1, wherein is the residue of 1,4-butanediol. [Item 6]R 1 2. The semicrystalline polyester according to claim 1, wherein is a 1,4-cyclohexanedimethyl residue. [Item 7] The semicrystalline polyester according to item 1, wherein m is 65 to 95 inclusive. [Item 8] The semicrystalline polyester according to item 1, wherein n is 5 to 35, inclusive. [Item 9] The semicrystalline polyester according to item 1, wherein n is 10 to 20, inclusive. [Item 10] A composition comprising the semi-crystalline polyester according to item 1. [Item 11] The composition according to item 10, further comprising at least one component selected from the group consisting of reinforcing agents, release agents, fillers, surface friction modifiers, light and heat stabilizers, extrusion aids, antistatic agents, colorants, dyes, pigments, optical brighteners, antibacterial agents, anti-counterfeiting markers, hydrophobic and hydrophilic enhancers, viscosity modifiers, slip agents, reinforcing agents, adhesion promoters, toners, and colorants. [Item 12] A film comprising the semi-crystalline polyester according to item 1. [Item 13] The film according to item 12, wherein the film is a monolayer film. [Item 14] The film according to item 13, wherein the monolayer film is biaxially stretched. [Item 15] The film of item 12, wherein the film is a backsheet of a solar cell module. [Item 16] The film of item 12, wherein the monolayer film is a backsheet of a solar cell module. [Item 17] A solar cell module comprising the film according to item 12. [Item 18] An injection molded article comprising the semi-crystalline polyester according to item 1.
Claims
1. formula: 【Chemistry 1】 Semicrystalline polyesters containing repeat units of [wherein A is an aliphatic, aromatic or heterocyclic group; R 1 is selected from the group consisting of 1,4-butanediol residues and 1,4-cyclohexanedimethanol residues; R 2 is the residue of neopentanediol; m is 50 to 99, inclusive; n is 1 to 50, inclusive; x is 1 to 200, inclusive; and said semi-crystalline polyester exhibits a minimum crystallization half-time of 0.3 minutes or greater, where the minimum crystallization half-time is the minimum time required for the semi-crystalline polyester to achieve half of the maximum achievable crystallinity at a temperature intermediate its glass transition temperature (Tg) and melting temperature (Tm).
2. 2. The semi-crystalline polyester of claim 1, wherein said minimum crystallization half-time is 0.5 minutes or greater.
3. 3. The semi-crystalline polyester of claim 2, wherein said minimum crystallization half-time is 0.6 minutes or greater.
4. 2. The semicrystalline polyester of claim 1, wherein the semicrystalline polyester has a melting point of from 240°C to 275°C.
5. R 1 2. The semicrystalline polyester of claim 1, wherein is the residue of 1,4-butanediol.
6. R 1 The semicrystalline polyester of claim 1, wherein is the residue of 1,4-cyclohexanedimethyl.
7. 2. The semicrystalline polyester of claim 1, wherein m is from 65 to 95, inclusive.
8. 2. The semicrystalline polyester of claim 1, wherein n is from 5 to 35, inclusive.
9. 2. The semicrystalline polyester of claim 1, wherein n is from 10 to 20, inclusive.
10. A composition comprising the semicrystalline polyester of claim 1.
11. 11. The composition of claim 10 further comprising at least one component selected from the group consisting of reinforcing agents, mold release agents, fillers, surface friction modifiers, light and heat stabilizers, extrusion aids, antistatic agents, colorants, dyes, pigments, optical brighteners, antimicrobial agents, anti-counterfeiting markers, hydrophobic and hydrophilic enhancers, viscosity modifiers, slip agents, toughening agents, adhesion promoters, toners, and colorants.
12. A film comprising the semicrystalline polyester of claim 1.
13. The film of claim 12 , wherein the film is a monolayer film.
14. 14. The film of claim 13, wherein the monolayer film is biaxially oriented.
15. 13. The film of claim 12, wherein the film is a backsheet for a solar cell module.
16. 13. The film of claim 12, wherein the monolayer film is a backsheet for a solar cell module.
17. A solar cell module comprising the film of claim 12.
18. 10. An injection molded article comprising the semicrystalline polyester of claim 1.
Citation Information
Patent Citations
Modified copolyester and optical film containing modified copolyester
JP2008517139A
Composition and method for enhancement of acid value of polyesters
US20080125567A1
Glycol 1, 4-bicyclo [2. 2. 2] octanedicarboxylate polyesters
US3256241A
Polyester-acrylic composite sheet having improved weatherability
US4355080A
Injection-moldable thermoplastic polyester composition
US4486561A