Ethylene / α-olefin interpolymer composition having high glass adhesion

The ethylene/α-olefin/interpolymer composition with Si-containing compounds addresses adhesion and resistivity issues in photovoltaic encapsulant films, maintaining bond strength and resistivity under harsh conditions, enhancing solar cell module performance.

JP7594593B2Active Publication Date: 2024-12-04DOW GLOBAL TECHNOLOGIES LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022538690
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-12-26
Publication Date
2024-12-04
Estimated Expiration
2039-12-26

AI Technical Summary

Technical Problem

Current photovoltaic encapsulant films, primarily made from ethylene vinyl acetate (EVA), suffer from acid release that corrodes solar cells, low volume resistivity leading to potential induced degradation, and poor adhesion to glass, necessitating compositions with high volume resistivity and strong adhesion to glass.

Method used

A composition comprising ethylene/α-olefin/interpolymer, peroxide, and a Si-containing compound, such as vinyl oligomer siloxane, to enhance adhesion and resistivity, with specific ratios and additives to maintain bond strength and resistivity under high humidity and temperature conditions.

Benefits of technology

The composition provides high glass bonding strength, maintains adhesion after aging, and exhibits excellent volume resistivity, ensuring durability and efficiency of solar cell modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594593000069
    Figure 0007594593000069
  • Figure 0007594593000001
    Figure 0007594593000001
  • Figure 0007594593000002
    Figure 0007594593000002
Patent Text Reader

Abstract

A composition comprising: a) an ethylene / α-olefin / interpolymer; b) a peroxide; and c) a "Si-containing compound" selected from the following i) to v): (i) (wherein each R is independently selected from C1 to C3 alkyl and n is 1 to 16), (ii) (wherein each R is independently methyl or ethyl and n is 1 to 18), (iii) (wherein each R is independently methyl or ethyl), (iv) a vinyl oligomer siloxane, or (v) any combination of (i) to (iv). [Formula 1] JPEG2023514936000063.jpg18135
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] The demand for solar modules is increasing due to scarce and non-renewable fossil fuel resources and the need to reduce environmental pollution. Solar modules generally include a front protection material (usually a glass sheet), a front encapsulant, an array of solar cells, a back encapsulant, and a back protection material (which can be a backsheet or a glass sheet). Solar cells convert solar energy into electrical energy and are very fragile. If water penetrates the module, these cells will corrode. The encapsulant is designed to protect the array of cells from humidity, mechanical loads, and impacts. The encapsulant also provides electrical insulation to prevent loss of electrical current. The encapsulant must provide mechanical protection and some UV stability and have good adhesion to the glass and / or backsheet.

[0002] The requirements of the encapsulant necessitate that the polymer composition used to form the encapsulant film (photovoltaic, PV) has good lamination performance to provide sufficient adhesion to glass, solar cell arrays, and backsheets. The film must also have good electrical insulation, low water vapor permeability, and good light transmission. Current photovoltaic encapsulant films are primarily made from ethylene vinyl acetate (EVA)-based compositions. See, for example, U.S. Patent No. 2013 / 0324671 and China Patent No. 106189932(A). However, EVA releases acid during use, corroding solar cells and solder ribbons over time. Also, EVA has low volume resistivity (VR), increasing the possibility of potential induced degradation of the encapsulant. Thus, there is a need for polymer compositions that have and maintain strong adhesion, especially to glass, and have high volume resistivity.

[0003] CN106414592(A) discloses an encapsulation film for solar cells formed from a "metallocene-catalyzed" ethylene / α-olefin copolymer, an organic peroxide, a silane coupling agent, and magnesium hydroxide or magnesium oxide. The magnesium hydroxide or magnesium oxide prevents adhesion formation during storage by preventing bleeding, hydrolysis, and gelation of the peroxide and coupling agent. However, the magnesium hydroxide or magnesium oxide can potentially deteriorate the transparency of the encapsulation film. Additional polyolefin-based and other compositions for solar cell modules are described in CN105950039(A), CN106811150(A), and CN104263258(A).

[0004] However, as discussed, there remains a need for polymer compositions that, in their initial laminate form, have and maintain strong adhesion, especially to glass, after aging at high temperature and humidity, and also have high volume resistivity. These needs are met by the following inventions. Summary of the Invention

[0005] 1. A composition comprising: a) an ethylene / α-olefin / interpolymer; b) a peroxide; c) The following items i) through v): i) [ka] wherein each R is independently selected from C1-C3 alkyl and n is 1 to 16; ii) [ka] (wherein each R is independently methyl or ethyl, and n is 1 to 18); iii) [ka] wherein each R is independently methyl or ethyl; iv) vinyl oligomer siloxane, or v) "Si-containing compounds" selected from any combination of i) to iv). [Brief description of the drawings]

[0006] [Figure 1] Shown are a cross-section of a laminate (left), a test sample of said laminate for adhesion peel testing (center), and a schematic of the test sample geometry during adhesion peel testing (right). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] In laminated solar cell modules, it is necessary to have high adhesive strength between the encapsulant film and the front glass layer. Compositions have been discovered that provide and maintain high adhesive strength as required. In addition, these compositions have high volume resistivity and good curing properties.

[0008] As discussed above, a composition comprising: a) an ethylene / α-olefin / interpolymer; b) a peroxide; c) The following items i) through v): i) [ka] wherein each R is independently selected from C1-C3 alkyl, or C1-C2 alkyl, or C1 alkyl, and n is 1-16, or 1-14, or 1-12, or 1-10, or 1-8, or 1-6, or 1-4; ii) [ka] (wherein, each R is independently methyl or ethyl, or methyl; and n is 1 to 18, or 1 to 16, or 1 to 14, or 1 to 12, or 1 to 10, or 1 to 8, or 1 to 6, or 1 to 4, or 1 to 3); iii) [ka] wherein each R is independently methyl or ethyl, or ethyl; iv) vinyl oligomer siloxane, or and v) a "Si-containing compound" selected from any combination of i) to iv).

[0009] Vinyl oligomeric siloxanes include multiple (two or more) chemical molecules (or compounds) that differ only in molecular weight, each of which contains at least one vinyl group and at least one siloxane group. All of these similar molecules can be either linear, branched, or cyclic.

[0010] In one embodiment, or a combination of two or more embodiments, each described herein, the "Si-containing compound" (component c) is selected from the following i) to v): [ka] iv) vinyl oligomer siloxane, or v) any combination of i) to iv).

[0011] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” may be any of the following: iv) vinyl oligomer siloxanes.

[0012] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” has the following formula 4A: iv) R1 x R2 y R3 z S n O mA vinyl oligomer siloxane comprising at least two different compounds selected from (Formula 4A) (wherein R1 is vinyl, x is 1 or more, R2 is propyl, y is 0 or more and 1 or less, R3 is ethoxy or methoxy, z is 4n-xym, n is greater than 1 and less than 10, and m is n-1 or less).

[0013] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” may be any of the following: i) [ka] wherein each R is independently selected from C1-C3 alkyl, or C1-C2 alkyl, or C1 alkyl, and n is 1-16, or 1-14, or 1-12, or 1-10, or 1-8, or 1-6, or 1-4; ii) [ka] (wherein, each R is independently methyl or ethyl, or methyl; and n is 1 to 18, or 1 to 16, or 1 to 14, or 1 to 12, or 1 to 10, or 1 to 8, or 1 to 6, or 1 to 4, or 1 to 3); iii) [ka] wherein each R is independently methyl or ethyl, or ethyl; or v) Selected from any combination of i) to iii).

[0014] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” may be any of the following: ii) [ka] (wherein, each R is independently methyl or ethyl, or methyl; and n is 1 to 18, or 1 to 16, or 1 to 14, or 1 to 12, or 1 to 10, or 1 to 8, or 1 to 6, or 1 to 4, or 1 to 3); iii) [ka] wherein each R is independently methyl or ethyl, or ethyl; or v) A combination of ii) and iii).

[0015] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” may be any of the following: [ka] Or v) a combination of ii) and iii).

[0016] In one embodiment, or a combination of two or more embodiments, each described herein, the "Si-containing compound" is selected from a combination of ii) and iii).

[0017] In one embodiment, or a combination of two or more embodiments, each described herein, the weight ratio of component iii) to component ii) is 2.0 or more, or 2.2 or more, or 2.4 or more, or 2.6 or more, or 2.8 or more, or 3.0 or more. In one embodiment, or a combination of two or more embodiments, each described herein, the weight ratio of component iii) to component ii) is 4.0 or less, or 3.8 or less, or 3.6 or less, or 3.4 or less, or 3.2 or less.

[0018] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” may be any of the following: i) [ka] (wherein each R is independently selected from C1-C3 alkyl, C1-C2 alkyl, or C1 alkyl; and n is 1 to 16, or 1 to 14, or 1 to 12, or 1 to 10, or 1 to 8, or 1 to 6, or 1 to 4).

[0019] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” may be any of the following: i) [ka] is selected from.

[0020] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” may be any of the following: ii) [ka] (wherein, each R is independently methyl or ethyl, or methyl; and n is 1 to 18, or 1 to 16, or 1 to 14, or 1 to 12, or 1 to 10, or 1 to 8, or 1 to 6, or 1 to 4, or 1 to 3).

[0021] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” may be any of the following: ii) [ka] is selected from.

[0022] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” may be any of the following: iii) [ka] wherein each R is independently methyl or ethyl, or ethyl.

[0023] In one embodiment, or a combination of two or more embodiments, each described herein, the “Si-containing compound” may be any of the following: iii) [ka] is selected from.

[0024] Crosslinking coagents promote the crosslinking reaction in the polymer composition and include, but are not limited to, triallyl isocyanurate, triallyl cyanurate, and trimethylolpropane trimethacrylate, divinylbenzene, polyol acrylates and methacrylates, allyl alcohol derivatives, and low molecular weight polybutadienes.

[0025] In one embodiment, or a combination of two or more embodiments, each described herein, the composition further comprises a coagent. In one embodiment, or a combination of two or more embodiments, each described herein, the weight ratio of peroxide to coagent is 0.5 or more, 0.8 or more, 1.0 or more, or 1.2 or more, or 1.4 or more, or 1.6 or more, or 1.8 or more, or 2.0 or more. In one embodiment, or a combination of two or more embodiments, each described herein, the weight ratio of peroxide to coagent is 3.0 or less, or 2.8 or less, or 2.6 or less, or 2.4 or less, or 2.2 or less.

[0026] The peroxide (containing at least one "-OO-" group) is preferably, for example, t-butylperoxy 2-ethylhexyl carbonate, di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di-(t-butylperoxy)hexane, di-(t-butylperoxy-isopropyl)benzene, t-butylperoxybenzoate, 1,1-di-(t-butylperoxy)-3,3,5-trimethyl-cyclohexane, 1,2-di-(t-butylperoxy)-2,3,5-trimethyl-cyclohexane, 1,3-di-(t-butylperoxy)-2 ... Organic peroxides such as hexane, 2,5-dimethyl-2,5-di(t-amylperoxy)-hexane, 2,5-dimethyl-2,5-di(t-butyl-peroxy)hexyne-3, 2,5-dimethyl-2,5-di(t-amylperoxy)hexyne-3, di-t-amyl peroxide, 1,3-dimethyl-3-(t-butyl-peroxy)butanol, 1,3-dimethyl-3-(t-amylperoxy)butanol, and mixtures of two or more of these initiators. See, for example, TRIGONOX peroxides from AkzoNobel, LUPEROX peroxides from ARKEMA.

[0027] In one embodiment, or a combination of two or more embodiments, each described herein, the weight ratio of peroxide to "Si-containing compound" is 1.0 or more, or 1.5 or more, or 2.0 or more, or 2.2 or more, or 2.4 or more, or 2.6 or more, or 2.8 or more, or 3.0 or more, or 3.2 or more, or 3.4 or more, or 3.6 or more, or 3.8 or more, or 4.0 or more. In one embodiment, or a combination of two or more embodiments, each described herein, the weight ratio of peroxide to "Si-containing compound" is 6.0 or less, or 5.8 or less, or 5.6 or less, or 5.4 or less, or 5.2 or less, or 5.0 or less, or 4.8 or less, or 4.6 or less, or 4.4 or less, or 4.2 or less.

[0028] Hindered amine light stabilizers (HALS) are chemical compounds that contain amine functional groups and are used as stabilizers in polymer compositions. The nitrogen atom of the amine is partially shielded by adjacent groups to reduce the possibility of side reactions with the nitrogen atom. Hindered amines include, but are not limited to, TINUVIN 770 (bis-(2,2,6,6-tetramethyl-4-piperidinyl) sebacate), CYASORB UV 3529, HOSTAVIN N30, UNIVIL 4050, UNIVIN 5050, CHIMASSORB UV 119, CHIMASSORB 944 LD, and TINUVIN 622 LD.

[0029] In one embodiment, or a combination of two or more embodiments, each of which is described herein, the composition further comprises a hindered amine light stabilizer. In one embodiment, or a combination of two or more embodiments, each of which is described herein, the weight ratio of "Si-containing compound" to hindered amine is 1.0 or more, 2.0 or more, 3.0 or more, or 3.1 or more, or 3.2 or more, or 3.3 or more, or 3.4 or more, or 3.5 or more. In one embodiment, or a combination of two or more embodiments, each of which is described herein, the weight ratio of "Si-containing compound" to hindered amine is 7.0 or less, or 6.8 or less, or 6.6 or less, or 6.4 or less, or 6.2 or less, or 6.0 or less.

[0030] In one embodiment, or a combination of two or more embodiments, each described herein, the composition comprises 50.0 wt% or more, 60.0 wt% or more, or 70.0 wt% or more, or 80.0 wt% or more, or 90.0 wt% or more of ethylene / α-olefin interpolymer (component a), based on the weight of the composition. In one embodiment, or a combination of two embodiments, each described herein, the composition comprises 95.0 wt% or more, or 95.5 wt% or more, or 96.0 wt% or more, or 96.5 wt% or more, or 97.0 wt% or more, or 97.5 wt% or more, or 98.0 wt% or more of ethylene / α-olefin interpolymer (component a), based on the weight of the composition.

[0031] In one embodiment, or a combination of two or more embodiments, each described herein, the composition comprises 99.8% by weight or less, or 99.6% by weight or less, or 99.4% by weight or less, or 99.2% by weight or less, or 99.0% by weight or less, or 98.8% by weight or less, or 98.6% by weight or less, or 98.4% by weight or less, or 98.2% by weight or less of ethylene / α-olefin interpolymer (component a), based on the weight of the composition.

[0032] In one embodiment, or a combination of two or more embodiments, each described herein, the composition comprises, by weight of the composition, 98.5% or more, or 99.0% or more, or 99.1% or more, or 99.2% or more, or 99.3% or more, or 99.4% or more of the sum of components a)-c), respectively. In one embodiment, or a combination of two or more embodiments, each described herein, the composition comprises, by weight of the composition, 100.0% or less, or 99.9% or less, or 99.8% or less, or 99.7% or less, or 99.6% or less, or 99.5% or less of the sum of components a)-c).

[0033] In one embodiment, or a combination of two or more embodiments, each described herein, for the ethylene / α-olefin interpolymer (component a), the α-olefin is a C3 to C20 α-olefin, further a C3 to C10 α-olefin. In one embodiment, or a combination of two or more embodiments, each described herein, the α-olefin is selected from propylene, 1-butene, 1-pentene, 1-hexene, or 1-octene, further propylene, 1-butene, or 1-octene, further 1-butene or 1-octene, further 1-octene.

[0034] In one embodiment, or a combination of two or more embodiments, each described herein, the ethylene / α-olefin interpolymer (component a) is an ethylene / α-olefin copolymer. In one embodiment, or a combination of two or more embodiments, each described herein, the ethylene / α-olefin interpolymer (component a) is selected from the following: ethylene / propylene copolymer, ethylene / butene copolymer, or ethylene / octene copolymer, or even ethylene / butene copolymer or ethylene / octene copolymer, or even ethylene / octene copolymer.

[0035] In one embodiment, or a combination of two or more embodiments, each described herein, the ethylene / α-olefin interpolymer (component a) has a viscosity of 0.860 g / cc or more, or 0.865 g / cc or more, or 0.868 g / cc or more, or 0.870 g / cc or more, or 0.872 g / cc or more, or 0.874 g / cc or more, or 0.876 g / cc or more, or 0.878 g / cc or more, or 0.880 g / cc or more (1 cc=1 cm 3 In one embodiment, or a combination of two or more embodiments, each described herein, the ethylene / α-olefin interpolymer has a density of 0.900 g / cc or less, or 0.898 g / cc or less, or 0.896 g / cc or less, or 0.894 g / cc or less, or 0.892 g / cc or less, or 0.890 g / cc or less, or 0.888 g / cc or less, or 0.886 g / cc or less, or 0.884 g / cc or less, or 0.882 g / cc or less.

[0036] In one embodiment, or a combination of two or more embodiments, each described herein, the ethylene / α-olefin interpolymer (component a) has a melt index (I2) of 8.0 g / 10 min or more, or 10 g / 10 min or more, or 12 g / 10 min or more, or 14 g / 10 min or more, or 16 g / 10 min or more, or 18 g / 10 min or more. In one embodiment, or a combination of two or more embodiments, each described herein, the ethylene / α-olefin interpolymer has a melt index (I2) of 35 g / 10 min or less, or 30 g / 10 min or less, or 28 g / 10 min or less, or 26 g / 10 min or less, or 24 g / 10 min or less, or 22 g / 10 min or less, or 20 g / 10 min or less.

[0037] The present invention also provides crosslinked compositions formed from the composition of any one embodiment, or a combination of two or more embodiments, each described herein.

[0038] In one embodiment, or a combination of two or more embodiments, each described herein, the composition has a glass bond strength of 90 N / cm or more, or 92 N / cm or more, or 94 N / cm or more, or 96 N / cm or more, or 100 N / cm or more, or 110 N / cm or more, or 120 N / cm or more, or 130 N / cm or more, or 140 N / cm or more. In one embodiment, or a combination of two or more embodiments, each described herein, the composition has a glass bond strength of 70 N / cm or more, or 75 N / cm or more, or 80 N / cm or more, or 85 N / cm or more, or 90 N / cm or more, or 95 N / cm or more, or 100 N / cm or more, or 105 N / cm or more after aging for 1000 hours at 85°C and 85% humidity.

[0039] In one embodiment, or a combination of two or more embodiments, each described herein, the composition comprises 1.0×10 14 ohm cm or more, or 5.0×10 15 ohm cm or more, or 1.0×10 16 ohm cm or more, or 2.0×10 16ohm cm or more, or 3.0×10 16 ohm cm or more, or 4.0×10 16 ohm cm or more, or 5.0×10 16 In one embodiment, or a combination of two or more embodiments, each described herein, the composition has a volume resistivity of 1.0×10 17 ohm cm or more, or 1.2×10 17 or more, or 1.4 x 10 17 or more, or 1.6 x 10 17 or more, or 1.8 x 10 17 or more, or 1.9 x 10 17 or more.

[0040] The present invention also provides an article comprising at least one component formed from the composition of any one embodiment or combination of two or more embodiments, each described herein. In one embodiment or combination of two or more embodiments, each described herein, the article is a film, even an extruded film. In one embodiment or combination of two or more embodiments, each described herein, the article is a solar cell module.

[0041] The present invention also provides a process for forming a solar cell module, comprising laminating an "array of solar cells" between two film layers, each of which is independently formed from the composition of any one embodiment, or a combination of two or more embodiments, each of which is described herein. In a further embodiment, each of the film layers is formed from the same composition.

[0042] In one embodiment, or a combination of two or more embodiments, each described herein, the composition of the present invention further comprises a thermoplastic polymer that differs from the interpolymer of component a) in one or more characteristics, such as the type and / or amount of monomer, Mn, Mw, Mz, MWD, Mooney viscosity, V0.1, V100, RR, or any combination thereof. The polymer includes, but is not limited to, ethylene-based polymers, propylene-based polymers, and olefin multi-block interpolymers. Suitable ethylene-based polymers include, but are not limited to, high density polyethylene (HDPE), linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), ultra-low density polyethylene (ULDPE), homogeneously branched linear ethylene-based polymers, and homogeneously branched substantially linear ethylene-based polymers (i.e., homogeneously branched long chain branched ethylene polymers). Suitable propylene-based polymers include, but are not limited to, polypropylene homopolymers and propylene / ethylene copolymers.

[0043] The composition of the present invention may comprise a combination of two or more embodiments as described herein. The ethylene / α-olefin interpolymer may comprise a combination of two or more embodiments as described herein. The peroxide may comprise a combination of two or more embodiments as described herein. The "Si-containing compound" may comprise a combination of two or more embodiments as described herein.

[0044] definition Unless otherwise stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are by weight and all testing methods are current as of the filing date of this disclosure.

[0045] As used herein, the term "composition" includes a mixture of materials that comprise the composition, as well as reaction products and decomposition products formed from the materials of the composition. Any reaction or decomposition products will typically be present in trace or residual amounts.

[0046] The term "polymer" as used herein refers to a polymeric compound prepared by polymerizing monomers, whether of the same or different kinds. Thus, the general term polymer includes the term homopolymer (used to refer to a polymer prepared from only one type of monomer, with the understanding that trace amounts of impurities may be incorporated into the polymer structure), and the term interpolymer, as defined herein below. Trace amounts of impurities, such as catalyst residues, may be incorporated into and / or within the polymer. Typically, polymers are stabilized with very small amounts ("ppm" amounts) of one or more stabilizers.

[0047] The term "interpolymer," as used herein, refers to a polymer prepared by the polymerization of at least two different types of monomers. Thus, the term interpolymer includes the term copolymer, which is used to refer to a polymer prepared from two different types of monomers, and polymers prepared from more than two different types of monomers.

[0048] As used herein, the term "propylene-based polymer" refers to a polymer that, in polymerized form, contains a majority weight percent propylene (based on the weight of the polymer) and may optionally contain one or more comonomers.

[0049] As used herein, the term "ethylene-based polymer" refers to a polymer that, in polymerized form, contains at least 50 weight percent or majority weight percent ethylene (based on the weight of the polymer), and may optionally contain one or more comonomers.

[0050] As used herein, the term "ethylene / α-olefin interpolymer" refers to an interpolymer that comprises, in polymerized form, 50 weight percent or majority weight percent ethylene (based on the weight of the interpolymer) and an α-olefin.

[0051] As used herein, the term "ethylene / α-olefin copolymer" refers to a copolymer that contains, in polymerized form, 50% by weight or a majority of ethylene monomer (based on the weight of the copolymer) and an α-olefin as the only two monomers.

[0052] As used herein, the term "Si-containing compound" refers to a compound that contains at least one "Si" atom and at least one "-CH2-" group and / or at least one "-CH3" group.

[0053] As used herein, the term "solar cell (or photovoltaic cell)" refers to a device that converts solar radiation into electricity. Solar cells are typically presented in an array pattern.

[0054] As used herein, the term "solar module (or solar panel or solar module)" refers to a photovoltaic panel comprising an assembly of solar cells.

[0055] As used herein, the terms "laminating, lamination, and like terms" refer to a process in which multiple layers of material are bonded together under heat and pressure, and optionally under vacuum.

[0056] The terms "comprising," "including," "having," and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether they are specifically disclosed or not. To avoid any doubt, all compositions claimed using the term "comprising" may include any additional additives, adjuvants, or compounds, whether polymeric or otherwise, unless stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any succeeding recitation any other component, step, or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not specifically delineated or listed.

[0057] Listing some compositional features A] A composition comprising: a) an ethylene / α-olefin / interpolymer; b) a peroxide; c) The following items i) through v): i) [ka] wherein each R is independently selected from C1-C3 alkyl, or C1-C2 alkyl, or C1 alkyl, and n is 1-16, or 1-14, or 1-12, or 1-10, or 1-8, or 1-6, or 1-4; ii) [ka] (wherein, each R is independently methyl or ethyl, or methyl; and n is 1 to 18, or 1 to 16, or 1 to 14, or 1 to 12, or 1 to 10, or 1 to 8, or 1 to 6, or 1 to 4, or 1 to 3); iii) [ka] wherein each R is independently methyl or ethyl, or ethyl; iv) vinyl oligomer siloxane, or v) "Si-containing compounds" selected from any combination of i) to iv). B] "Si-containing compound" (component c) is one of the following i) to v): i) [ka] ii) [ka] iii) [ka] iv) a vinyl oligomer siloxane, or v) any combination of i) to iv), the composition described in A] above. C] "Si-containing compound" is any one of the following: iv) The composition described in A] above, wherein the siloxane is selected from vinyl oligomer siloxanes. D] The Si-containing compound has the following formula 4A: iv) R1 x R2 y R3 z SiO m The composition described in C] above, which is a vinyl oligomer siloxane containing at least two different compounds selected from (Formula 4A) (wherein R1 is vinyl, x is 1 or more, R2 is propyl, y is 0 or more and 1 or less, R3 is ethoxy or methoxy, z is 4n-xym, n is greater than 1 and less than 10, and m is n-1 or less). E] "Si-containing compound" is any one of the following: i) [ka] wherein each R is independently selected from C1-C3 alkyl, or C1-C2 alkyl, or C1 alkyl, and n is 1-16, or 1-14, or 1-12, or 1-10, or 1-8, or 1-6, or 1-4; ii) [ka] (wherein, each R is independently methyl or ethyl, or methyl; and n is 1 to 18, or 1 to 16, or 1 to 14, or 1 to 12, or 1 to 10, or 1 to 8, or 1 to 6, or 1 to 4, or 1 to 3); iii) [ka] wherein each R is independently methyl or ethyl, or ethyl; or v) The composition described in A] above, selected from any combination of i) to iii). F] "Si-containing compound" (component c) is one of the following i) to v): i) [ka] ii) [ka] iii) [ka] Or v) the composition described in E] above, selected from any combination of i) to iii). G] "Si-containing compound" is any of the following: ii) [ka] (wherein, each R is independently methyl or ethyl, or methyl; and n is 1 to 18, or 1 to 16, or 1 to 14, or 1 to 12, or 1 to 10, or 1 to 8, or 1 to 6, or 1 to 4, or 1 to 3); iii) [ka] wherein each R is independently methyl or ethyl, or ethyl; v) The composition described in A] above, selected from a combination of ii) and iii). H] "Si-containing compound" is the following: [ka] or v) a combination of ii) and iii). I] The composition described in G] or H] above, wherein the "Si-containing compound" is selected from a combination of ii) and iii). J] A composition described in any one of G] to I] (G to I), wherein the weight ratio of component iii) to component ii) is 2.0 or more, or 2.2 or more, or 2.4 or more, or 2.6 or more, or 2.8 or more, or 3.0 or more. K] A composition described in any one of G] to J] above, wherein the weight ratio of component iii) to component ii) is 4.0 or less, or 3.8 or less, or 3.6 or less, or 3.4 or less, or 3.2 or less. L] "Si-containing compound" is any of the following: i) [ka] (wherein each R is independently selected from C1 to C3 alkyl, C1 to C2 alkyl, or C1 alkyl, and n is 1 to 16, or 1 to 14, or 1 to 12, or 1 to 10, or 1 to 8, or 1 to 6, or 1 to 4). M] "Si-containing compound" is any one of the following: i) [ka] The composition according to L) above, selected from: N] "Si-containing compound" is any of the following: ii) [ka] (wherein each R is independently methyl or ethyl, or methyl, and n is 1 to 18, or 1 to 16, or 1 to 14, or 1 to 12, or 1 to 10, or 1 to 8, or 1 to 6, or 1 to 4, or 1 to 3). O] "Si-containing compound" is the following: ii) [ka] The composition according to N] above, selected from: P] "Si-containing compound" is any of the following: iii) [ka] (wherein each R is independently methyl or ethyl, or ethyl). Q] "Si-containing compounds" are as follows: [ka] The composition according to P] above, wherein the composition is selected from the following: R] The composition described in any one of A] to Q] (A-Q) above, wherein the composition further comprises a crosslinker. S] The composition described above in R], wherein the composition comprises 0.05 wt. % or more, or 0.10 wt. % or more, or 0.15 wt. % or more, or 0.20 wt. % or more of a crosslinking coagent, based on the weight of the composition. T] A composition described in R] or S] above, wherein the composition comprises 1.50 wt.% or less, or 1.40 wt.% or less, or 1.30 wt.% or less, or 1.20 wt.% or less, or 1.10 wt.% or less, or 1.00 wt.% or less of a crosslinking coagent, based on the weight of the composition. U] Auxiliary agents include the following: [ka] The composition according to any one of R] to T] above, V] The composition according to any one of the above R] to U], wherein the weight ratio of peroxide to coagent is 0.5 or more, or 0.8 or more, or 1.0 or more, or 1.2 or more, or 1.4 or more, or 1.6 or more, or 1.8 or more, or 2.0 or more. W] A composition according to any one of R] to V] above, wherein the weight ratio of peroxide to coagent is 3.0 or less, or 2.8 or less, or 2.6 or less, or 2.4 or less, or 2.2 or less. X] The composition according to any one of A] to W] above, comprising, based on the weight of the composition, 0.01 wt % or more, or 0.02 wt % or more, or 0.04 wt % or more, or 0.06 wt % or more, or 0.08 wt % or more, or 0.10 wt % or more of a "Si-containing compound." Y] A composition according to any one of A] to X] above, wherein the composition contains, based on the weight of the composition, 1.00 wt.% or less, or 0.80 wt.% or less, or 0.60 wt.% or less, or 0.40 wt.% or less of "Si-containing compounds." Z] The composition according to any one of A] to Y] above, wherein the weight ratio of the peroxide to the "Si-containing compound" is 1.0 or more, or 1.5 or more, 2.0 or more, or 2.2 or more, or 2.4 or more, or 2.6 or more, or 2.8 or more, or 3.0 or more, or 3.2 or more, or 3.4 or more, or 3.6 or more, or 3.8 or more, or 4.0 or more. AA] The composition according to any one of A] to Z] above, wherein the weight ratio of peroxide to "Si-containing compound" is 6.0 or less, or 5.8 or less, or 5.6 or less, or 5.4 or less, or 5.2 or less, or 5.0 or less, or 4.8 or less, or 4.6 or less, or 4.4 or less, or 4.2 or less. BB] A composition according to any one of A] to AA] above, wherein the composition comprises, based on the weight of the composition, 0.1% by weight or more, or 0.2% by weight or more, or 0.4% by weight or more, or 0.6% by weight or more, or 0.8% by weight or more, or 1.0% by weight or more of peroxide. CC] A composition described in any one of A] to BB] above, wherein the composition contains 3.0% by weight or less, or 2.8% by weight or less, or 2.6% by weight or less, or 2.4% by weight or less, or 2.2% by weight or less, or 2.0% by weight or less of peroxide, based on the weight of the composition. DD] peroxide, [ka] The composition according to any one of A] to CC] above, selected from the following: EE] The composition described in any one of A] to DD] above, wherein the composition further comprises a hindered amine. FF) hindered amine is selected from the group consisting of: [ka] The composition described in EE above, wherein GG] The composition described in EE] or FF] ​​above, wherein the weight ratio of "Si-containing compound" to hindered amine is 1.0 or more, or 2.0 or more, or 3.0 or more, or 3.1 or more, or 3.2 or more, or 3.3 or more, or 3.4 or more, or 3.5 or more. HH] The composition described in any one of EE] to GG] above, wherein the weight ratio of the "Si-containing compound" to the hindered amine is 7.0 or less, or 6.8 or less, or 6.6 or less, or 6.4 or less, or 6.2 or less, or 6.0 or less. II] A composition according to any one of A] to HH] above, wherein the composition comprises 50.0 wt.% or more, or 60.0 wt.% or more, or 70.0 wt.% or more, or 80.0 wt.% or more, or 90.0 wt.% or more of ethylene / α-olefin interpolymer (component a), based on the weight of the composition. JJ] A composition described in any one of A]-II] above, wherein the composition comprises 80.0 wt.% or more, or 82.0% or more, or 84.0% or more, or 86.0% or more, or 88.0% or more, or 90.0% or more, or 92.0% or more, or 94.0% or more of ethylene / α-olefin interpolymer (component a), based on the weight of the composition. KK] A composition described in any one of A] to JJ] above, wherein the composition comprises 95.0 wt.% or more, or 95.5 wt.% or more, or 96.0 wt.% or more, or 96.5 wt.% or more, or 97.0 wt.% or more, or 97.5 wt.% or more, or 98.0 wt.% or more ethylene / α-olefin interpolymer (component a), based on the weight of the composition. LL] A composition described in any one of A] to KK] above, wherein the composition comprises 99.8 wt% or less, 99.6 wt% or less, or 99.4 wt% or less, or 99.2 wt% or less, or 99.0 wt% or less, or 98.8 wt% or less, or 98.6 wt% or less, or 98.4 wt% or less, or 98.2 wt% or less of ethylene / α-olefin interpolymer (component a), based on the weight of the composition. MM] A composition described in any one of A] to LL] above, wherein the composition comprises a sum of components a) to c) of 98.5% or more, 99.0% or more by weight, or 99.1% or more by weight, or 99.2% or more by weight, or 99.3% or more by weight, or 99.4% or more by weight, based on the weight of the composition. NN] A composition described in any one of A] to MM] above, wherein the composition comprises, based on the weight of the composition, 100.0% by weight or less, or 99.9% by weight or less, or 99.8% by weight or less, or 99.7% by weight or less, or 99.6% by weight or less, or 99.5% by weight or less of the sum of components a) to c). OO] For an ethylene / α-olefin interpolymer, the composition according to any one of A] to NN] above, wherein the α-olefin is a C3 to C20 α-olefin, further a C3 to C10 α-olefin. PP] For the ethylene / α-olefin interpolymer, the α-olefin is selected from propylene, 1-butene, 1-pentene, 1-hexene, or 1-octene, further propylene, 1-butene, or 1-octene, further 1-butene or 1-octene, further 1-octene. A composition according to any one of A] to OO] above. QQ]A composition described in any one of A] to PP] above, wherein the ethylene / α-olefin interpolymer (component a) is an ethylene / α-olefin copolymer. RR] The composition according to any one of A] to QQ] above, wherein the ethylene / α-olefin interpolymer (component a) is selected from the following: ethylene / propylene copolymer, ethylene / butene copolymer, or ethylene / octene copolymer, further ethylene / butene copolymer or ethylene / octene copolymer, further ethylene / octene copolymer. SS] Ethylene / α-olefin interpolymer (component a) is 0.860 g / cc or more, 0.865 g / cc or more, 0.870 g / cc or more, or 0.872 g / cc or more, or 0.874 g / cc or more, or 0.876 g / cc or more, or 0.878 g / cc or more, or 0.880 g / cc or more (1 cc = 1 cm 3 The composition according to any one of A] to RR] above, having a density of TT] The composition described in any one of A] to SS] above, wherein the ethylene / α-olefin interpolymer has a density of 0.900 g / cc or less, or 0.898 g / cc or less, or 0.896 g / cc or less, or 0.894 g / cc or less, or 0.892 g / cc or less, or 0.890 g / cc or less, or 0.888 g / cc or less, or 0.886 g / cc or less, or 0.884 g / cc or less, or 0.882 g / cc or less. UU] The composition described in any one of A] to TT] above, wherein the ethylene / α-olefin interpolymer (component a) has a melt index (I2) of 8.0 g / 10 min or more, or 10 g / 10 min or more, or 12 g / 10 min or more, or 14 g / 10 min or more, or 16 g / 10 min or more, or 18 g / 10 min or more. VV] The composition described in any one of A] to UU] above, wherein the ethylene / α-olefin interpolymer has a melt index (I2) of 35 g / 10 min or less, or 30 g / 10 min or less, or 28 g / 10 min or less, or 26 g / 10 min or less, or 24 g / 10 min or less, or 22 g / 10 min or less, or 20 g / 10 min or less. WW] The composition described in any one of A] to VV] above, wherein the ethylene / α-olefin interpolymer (component a) has a molecular weight distribution (MWD) (=Mw / Mn) of 1.70 or more, or 1.75 or more, or 1.80 or more, or 1.85 or more, or 1.90 or more, or 1.95 or more, or 2.00 or more. XX] The composition described in any one of A] to WW] above, wherein the ethylene / α-olefin interpolymer has a molecular weight distribution MWD of 2.70 or less, or 2.65 or less, or 2.60 or less, or 2.55 or less, or 2.50 or less, or 2.45 or less, or 2.40 or less, or 2.35 or less, or 2.30 or less, or 2.25 or less, or 2.20 or less. YY] The composition described in any one of A] to XX] above, wherein the ethylene / α-olefin interpolymer (component a) has a number average molecular weight (Mn) of 10,000 g / mol or more, or 12,000 g / mol or more, or 14,000 g / mol or more, or 16,000 g / mol or more, or 18,000 g / mol or more, or 20,000 g / mol or more. ZZ] The composition described in any one of A] to YY] above, wherein the ethylene / α-olefin interpolymer has a number average molecular weight Mn of 50,000 g / mol or less, or 45,000 g / mol or less, or 40,000 g / mol or less, or 35,000 g / mol or less, or 30,000 g / mol or less, or 25,000 g / mol or less. A3] The composition according to any one of A] to ZZ] above, wherein the ethylene / α-olefin interpolymer has a weight average molecular weight (Mw) of 30,000 g / mol or more, or 35,000 g / mol or more, or 40,000 g / mol or more, or 45,000 g / mol or more. B3] The composition according to any one of A] to A3] above, wherein the ethylene / α-olefin interpolymer has a weight average molecular weight Mw of 70,000 g / mol or less, or 65,000 g / mol or less, or 60,000 g / mol or less, or 55,000 g / mol or less. C3] The composition according to any one of A] to B3] above, wherein the ethylene / α-olefin interpolymer (component a) has a melting temperature (Tm, DSC) of 60°C or higher, or 65°C or higher, or 70°C or higher, or 72°C or higher, or 74°C or higher, or 76°C or higher, or 78°C or higher, or 80°C or higher. D3] The composition according to any one of A] to C3] above, wherein the ethylene / α-olefin interpolymer has a melting temperature (Tm, DSC) of 100°C or less, or 95°C or less, or 90°C or less, or 88°C or less, or 86°C or less, or 84°C or less, or 82°C or less. E3] The composition according to any one of A] to D3] above, wherein the ethylene / α-olefin interpolymer has a crystallization temperature (Tc, DSC) of 40°C or more, or 45°C or more, or 50°C or more, or 52°C or more, or 54°C or more, or 56°C or more. F3] The composition according to any one of A] to E3] above, wherein the ethylene / α-olefin interpolymer has a crystallization temperature (Tc, DSC) of 70°C or less, or 68°C or less, or 66°C or less, or 64°C or less, or 62°C or less, or 60°C or less. G3] The composition according to any one of A] to F3] above, wherein the ethylene / α-olefin interpolymer has a glass transition temperature (Tg, DSC) of -70°C or higher, or -65°C or higher, or -60°C or higher, or -58°C or higher, or -56°C or higher, or -54°C or higher, or -52°C or higher, or -50°C or higher. H3] The composition according to any one of A] to G3] above, wherein the ethylene / α-olefin interpolymer has a glass transition temperature (Tg, DSC) of -30°C or less, or -35°C or less, or -38°C or less, or -40°C or less, or -42°C or less, or -44°C or less, or -46°C or less. I3] A composition described in any one of A] to H3] above, wherein the composition contains less than 0.002 wt.%, or less than 0.001 wt.%, or less than 0.0005 wt.% titanium dioxide, based on the weight of the composition. J3] The composition according to any one of A] to I3] above, wherein the composition does not contain titanium dioxide. K3] A composition described in any one of A] to J3] above, wherein the composition contains less than 0.002 wt.%, or less than 0.001 wt.%, or less than 0.0005 wt.% magnesium hydroxide, based on the weight of the composition. L3] A composition described in any one of A] to K3] above, wherein the composition does not contain magnesium hydroxide. M3] A composition described in any one of A] to L3] above, wherein the composition contains less than 0.002 wt.%, or less than 0.001 wt.%, or less than 0.0005 wt.% magnesium oxide, based on the weight of the composition. N3] The composition described in any one of A] to M3] above, wherein the composition does not contain magnesium oxide. O3] A composition described in any one of A] to N3] above, wherein the composition comprises less than 0.002 wt. %, or less than 0.001 wt. %, or less than 0.0005 wt. % polymeric microspheres (such as crosslinked polymeric microspheres) based on the weight of the composition. P3] A composition described in any one of A] to O3] above, wherein the composition does not include polymeric microspheres (such as crosslinked polymeric microspheres). Q3] A crosslinked composition formed from the composition described in any one of A] to P3] above. R3] The composition according to any one of A] to Q3] above, wherein the composition has a glass adhesion strength of 90 N / cm or more, or 92 N / cm or more, or 94 N / cm or more, or 96 N / cm or more. S3] The composition according to any one of A] to R3] above, wherein the composition has a glass adhesion strength of 100 N / cm or more, or 110 N / cm or more, or 120 N / cm or more, or 130 N / cm or more, or 140 N / cm or more. T3] A composition according to any one of A] to S3] above, having a glass adhesion strength of 70 N / cm or more, or 75 N / cm or more, or 80 N / cm or more, or 85 N / cm or more, or 90 N / cm or more, or 95 N / cm or more, or 100 N / cm or more, or 105 N / cm or more after aging for 1000 hours at 85°C and 85% humidity. U3] A composition described in any one of A] to T3] above, wherein the composition has a maintained glass adhesion strength of 50% or more, or 55% or more, or 60% or more, or 65% or more, or 70% or more after aging for 1000 hours at 85°C and 85% humidity. V3] composition is 1.0 x 10 14 ohm cm or more, or 5.0×10 15 ohm cm or more, or 2.0×10 16 ohm cm or more, or 2.5×10 16 ohm cm or more, or 3.0×10 16 ohm cm or more, or 4.0×10 16 ohm cm or more, or 5.0×10 16 The composition according to any one of A] to U3] above, having a volume resistivity of ohm·cm or more. W3] composition is 1.0 × 10 17 ohm cm or more, or 1.2×10 17 ohm cm or more, or 1.4×10 17 ohm cm or more, or 1.6×10 17 ohm cm or more, or 1.8×10 17 ohm cm or more, or 1.9×10 17 The composition according to any one of A] to V3] above, having a volume resistivity of ohm·cm or more. X3] Composition is 1 x 10 19 The composition according to any one of A] to W3] above, having a volume resistivity of ohm·cm or less. Y3] An article comprising at least one component formed from a composition described in any one of A] to X3] above. Z3] The article according to Y3] above, wherein the article is a film, further an extruded film. A4] An article according to Y3] or Z3] above, wherein the article is a film comprising no more than two layers, even one layer. B4] The article described in Y3] above, wherein the article is a solar cell module. C4] A process for forming a solar cell module, comprising laminating an array of solar cells between two film layers, each of which is independently formed from a composition described in any one of A] to X3] above. D4] The process described in C4] above, wherein each of the film layers is formed from the same composition.

[0058] Test Method MDR Testing Cure properties were measured using an Alpha Technologies Moving Die Rheometer (MDR) 2000 E at 0.5 arc degrees according to ASTM D5289. The MDR was each filled with 5 g of uncured polymer composition (extruded film) and operated at a temperature of 145° C. for 30 minutes to generate a “time vs. torque” curve for the composition over a given interval. The following data from each MDR test were used: a) MH (dNm): the maximum torque applied by the MDR during the 30 minute test interval (usually corresponding to the torque applied at the 30 minute point), and b) t90 or the time to reach 90% of the MH value.

[0059] Glass Adhesion Test Each laminate sample was cut into three specimens each having a "1 inch" width (see Figure 1 (center)). The glass bond strength (average glass bond strength from 1 inch to 2 inches) was measured using a 180° peel test, as shown in Figure 1 (right). The test was performed on an INSTRON™ 5565 under controlled ambient conditions. Six specimens were tested and the average of the results was calculated. The initial strength and the strength after aging for 1000 hours at 85°C and 85% humidity (damp heat aging test) were recorded and the retention was calculated.

[0060] Volume Resistivity Test The volume resistivity test was based on ASTM D257. Measurements were performed using a KEITHLEY 6517 B electrometer in combination with a KEITHLEY 8009 test fixture. The leakage current was read directly from the instrument and used in the following equation to calculate the volume resistivity:

number

[0061] Melt Index The melt index (I2) of ethylene-based polymers is measured according to ASTM D-1238, condition 190°C / 2.16 kg (melt index at 190°C / 5.0 kg (I5), melt index at 190°C / 10.0 kg (I10), high load melt index at 190°C / 21.0 kg (I21)). The melt flow rate (MFR) of propylene-based polymers is measured according to ASTM D-1238, condition 230°C / 2.16 kg.

[0062] Polymer Density Polymer density is measured according to ASTM D-792.

[0063] Gel Permeation Chromatography The chromatography system consisted of a PolymerChar GPC-IR (Valencia, Spain) high temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5). The autosampler oven compartment was set at 160 °C and the column compartment was set at 150 °C. The columns were four AGILENT "Mixed A" 30 cm, 20 micron linear mixed bed columns. The chromatography solvent was 1,2,4-trichlorobenzene with 200 ppm butylated hydroxytoluene (BHT). The solvent source was sparged with nitrogen. The injection volume used was 200 microliters and the flow rate was 1.0 milliliters / min.

[0064] Calibration of the GPC column set was performed with 21 narrow molecular weight distribution polystyrene standards with molecular weights ranging from 580 to 8,400,000, arranged in six "cocktail" mixtures with at least 10 intervals between individual molecular weights. Standards were purchased from Agilent Technologies. Polystyrene standards were prepared at 0.025 grams in 50 milliliters of solvent for molecular weights of 1,000,000 or greater, and 0.05 grams in 50 milliliters of solvent for molecular weights less than 1,000,000. The polystyrene standards were dissolved at 80°C for 30 minutes with gentle agitation. The polystyrene standard peak molecular weights were converted to polyethylene molecular weights using Equation 1 (described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)): M ポリエチレン =A×(M ポリスチレン ) B (Equation 1) where M is the molecular weight, A has a value of 0.4315, and B is equal to 1.0.

[0065] A fifth order polynomial was used to fit each of the polyethylene equivalent calibration points, with a small adjustment to A (approximately 0.375 to 0.445) to correct for column resolution and band broadening effects for a linear homopolymer polyethylene standard obtained at 120,000 Mw.

[0066] Total plate counts of the GPC column set were performed using decane (prepared at 0.04 g in 50 milliliters of TCB and dissolved for 20 minutes with gentle agitation). Plate counts (Equation 2) and symmetry (Equation 3) were measured with a 200 microliter injection according to the following equations:

number

number

[0067] Samples were prepared semi-automatically using PolymerChar's "Instrument Control" software to target sample weights of 2 mg / mL and solvent (containing 200 ppm BHT) was added via the PolymerChar high temperature autosampler to septa-capped vials that had been pre-sparged with nitrogen. Samples were dissolved at 160° C. for 2 hours with "slow" shaking.

[0068] Mn (GPC) , Mw (GPC), and Mz (GPC) The calculation of was based on GPC results using the internal IR5 detector (measurement channel) of a PolymerChar GPC-IR chromatograph according to Equations 4-6 using PolymerChar GPCOne™ software, baseline-subtracted IR chromatograms at each equally spaced data collection point (i), and polyethylene equivalent molecular weights obtained from a narrow standard calibration curve at point (i) of Equation 1. Equations 4-6 are as follows:

number

[0069] To monitor deviations over time, a flow marker (decane) was introduced into each sample via a micropump controlled using a PolymerChar GPC-IR system. This flow marker (FM) was used to linearly correct the pump flow rate (Flow (Apparent)) of each sample by RV-aligning the respective decane peak in the sample (RV (FM Sample)) with that of the decane peak in the narrow standard calibration (RV (FM Calibrated)). Any time change in the decane marker peak was then assumed to be related to a linear shift in the flow rate (Flow (Effective)) throughout the run. To facilitate the highest accuracy of the RV measurement of the flow marker peaks, a least-squares fitting routine was used to fit the peaks of the flow marker concentration chromatogram to a quadratic equation. The first derivative of the quadratic equation was then used to determine the true peak position. After calibrating the system based on the flow marker peak, the effective flow rate (with respect to the narrow standard calibration) was calculated as Equation 7: Flow Rate (effective) = Flow Rate (apparent) x (RV (FM calibrated) / RV (FM sample)) (Equation 7).

[0070] Processing of flow marker peaks was performed using PolymerChar GPCOne™ software. Acceptable flow corrections are such that the effective flow rate should be within ±0.7% of the apparent flow rate.

[0071] Differential Scanning Calorimetry (DSC) Differential scanning calorimetry (DSC) is used to measure the Tm, Tc, Tg, and crystallinity of ethylene-based (PE) and propylene-based (PP) samples. Samples (0.5 g) were each compression molded into films at 5000 psi for 2 min at 190°C. Approximately 5-8 mg of film sample was weighed and placed in the DSC pan. A lid was crimped onto the pan to ensure a closed atmosphere. The sample pan was placed in the DSC cell and then heated at a rate of approximately 10°C / min to a temperature of 180°C for PE (230°C for PP). The sample was held at this temperature for 3 min. The sample was then cooled at a rate of 10°C / min to -90°C for PE (-60°C for PP) and held isothermally at that temperature for 3 min. The sample was then heated at a rate of 10°C / min until completely melted (second heat). Unless otherwise stated, the melting point (Tm) and glass transition temperature (Tg) of each polymer were determined from the second heat curve, and the crystallization temperature (Tc) was determined from the first cooling curve. The peak temperatures of Tm and Tc were recorded. The percent crystallinity can be calculated by dividing the heat of fusion (Hf) determined from the second heat curve by the theoretical heat of fusion of 292 J / g for PE (165 J / g for PP) and multiplying this amount by 100 (e.g., % crystallinity = (Hf / 292 J / g) x 100 for PE).

[0072] Experimental Polymers and Additives Ethylene / 1-octene random copolymer: density 0.880 g / cc, I2 18.0 g / 10 min, Mn 22951 g / mol, MWD 2.16, Tm 81° C., Tc 57° C., Tg −47° C. (e.g., XUS 38661 from The Dow Chemical Company). This copolymer is listed as “POE” in the table below.

[0073] tert-Butylperoxy 2-ethylhexyl carbonate (listed as "TBEC" in the table below): an organic peroxide (e.g., from J&K Scientific Ltd.).

[0074] 5-Hexenyltrimethoxysilane (listed as "SC1" in the table below): a Si-containing compound (e.g., DOWSIL Z-6161 EX Silane from The Dow Chemical Company).

[0075] Trimethoxysilylpropanethiol (listed as "SC2" in the table below): a Si-containing compound (e.g., XIAMETER OFS-6062 from The Dow Chemical Company).

[0076] Tetraethyl orthosilicate (listed as "SC3" in the table below): a Si-containing compound (e.g., XIAMETER 6697 from The Dow Chemical Company).

[0077] Vinyl oligomer siloxane (listed as "SC4" in the table below): Si-containing compounds (e.g., DYNASYLAN 6598 from EVONIK).

[0078] 3-(Trimethoxysilyl)propyl-methacrylate (listed as "SCC" in the table below): a Si-containing compound (e.g., XIAMETER OFS-6030 from The Dow Chemical Company).

[0079] Triallyl isocyanurate (listed as "TAIC" in the table below): a crosslinking coagent (e.g., from Chemicals Co., Ltd).

[0080] Bis-(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (listed as "T770" in the table below): a hindered amine light stabilizer (e.g., TINUVIN 770 from BASF).

[0081] Backsheet: ZTT-KPE (PVDF / PET / PEVA) available from Zhongtian Photovoltaic Materials Co., Ltd.

[0082] Polymer Composition The inventive and comparative compositions were prepared according to the formulations listed in Table 1. The comparative compositions represent current compositions used in photovoltaic encapsulant films.

[0083] [Table 1] Table 1: Polymer composition

[0084] For each polymer composition, the organic peroxide, Si-containing compound, crosslinking coagent, and POE resin (pellets) were weighed out in the desired percentages and premixed in a sealable bottle. The bottle and its contents were shaken for 1 minute and then placed in an oven equilibrated at 40°C to allow the additives to soak into the POE resin. For the first 60 minutes in the oven, the bottle was shaken every 10 minutes to maintain uniform distribution of the cure package. After 60 minutes, the bottle was stored in the 40°C oven for 15-20 hours (overnight).

[0085] Film Extrusion After soaking, the pellets were fed into a BRABENDER single screw extruder equipped with three barrels. The temperature of each barrel and the die temperature were set at 100° C., and the screw speed was 40 rpm. Approximately “0.5 mm thick POE extrusion films” were prepared and then stored in aluminum foil bags for testing.

[0086] Compression Molding The extruded film (POE film) was cured during the compression molding process. The extruded film was preheated at 120°C for 5 minutes, then degassed, and then pressed at 150°C for 15 minutes at 10 MPa to ensure complete curing of the sample. The temperature was then lowered to room temperature. The compression molded film was used for volume resistivity testing.

[0087] Lamination For each sample, a glass substrate (4" x 6" x 0.12" (thickness)) was used. The substrate was washed using water and then dried before use. The backsheet with a thickness of 0.35 mm was cut into "4 x 6" square pieces. The extruded film (POE film) was cut to fit the size of the glass and the size of the backsheet, respectively. Before lamination, the backsheet, extruded film, and glass were layered together (from top to bottom: backsheet, POE film, and glass). The lamination process was carried out on a PENERGY L036 laminator at 150°C for 20 minutes (4 minutes of vacuum process (vacuum pressure -0.095MPa) and 16 minutes of pressing (press pressure 0.075MPa)) to form a "glass-film-backsheet" laminate. The thickness of the laminate ranged from 3.9mm to 4.0mm. The laminated samples were used for glass adhesion testing.

[0088] Test results The cure, volume resistivity, and adhesion properties are shown in Table 2.

[0089] [Table 2] Table 2: Characteristics of Comparative Examples and Inventive Examples

[0090] It was found that the compositions of the present invention provide acceptable glass bond strength before and after aging. The crosslinking coagent also accelerated the cure of these compositions. Inventive Example 1 having SC1 as the Si-containing compound maintained higher glass bond strength after aging for 1000 hours at 85°C and 85% humidity (humid heat aging test) compared to the comparative example having SCC as the Si-containing compound. This inventive example had good volume resistivity (VR). The t90 of this inventive sample was slightly shorter than the comparative sample, indicating that "SC1" provides a slight increase in cure speed at the expense of a little torque after cure.

[0091] Inventive Example 2, which has SC2 as the Si-containing compound, also maintained higher glass adhesion after the moist heat aging test compared to the comparative example. This inventive example had excellent initial glass adhesion and good volume resistivity. However, the t90 of Inventive Example 2 was longer than that of the comparative sample, and the MH was lower than that of the comparative example. It is speculated that the thiol group of SC2 reacts with peroxide, resulting in a lower degree of crosslinking, i.e., a lower MH. By reducing the dosage of SC2 and adding some SC3 to the formulation, the glass adhesion properties and curing behavior can be balanced, as seen in Inventive Example 3. Inventive Example 3 had excellent initial glass adhesion, maintained glass adhesion after the aging test, and maintained excellent volume resistivity. Inventive Example 4, which has SC4 as the Si-containing compound, also had excellent initial glass adhesion, maintained glass adhesion after the aging test. This inventive example had excellent volume resistivity.

[0092] Polymer compositions have been discovered that provide one of the most important property features required for a photovoltaic encapsulant film: good adhesion to glass and excellent maintenance of this glass adhesion. These compositions also have a high degree of crosslinking and high volume resistivity. The present invention includes the following aspects. Section 1. 1. A composition comprising: a) an ethylene / α-olefin / interpolymer; b) a peroxide; c) The following items i) through v): i) [ka] wherein each R is independently selected from C1-C3 alkyl and n is 1 to 16; ii) [ka] (wherein each R is independently methyl or ethyl, and n is 1 to 18); iii) [ka] wherein each R is independently methyl or ethyl; iv) vinyl oligomer siloxane, or v) "Si-containing compounds" selected from any combination of i) to iv). Section 2. The "Si-containing compound" (component c) is one of the following i) to v): [ka] Item 1. The composition according to item 1, wherein the vinyl oligomer siloxane is selected from the group consisting of vinyl oligomer siloxane, vinyl oligomer siloxane, and any combination of i) to iv). Section 3. The "Si-containing compound" is any one of the following: iv) vinyl oligomer siloxane. Section 4. The "Si-containing compound" is represented by the following formula 4A: iv) R1 x R2 y R3 z S n O m (Formula 4A) (Wherein, R1 is vinyl, x is 1 or more, R2 is propyl, y is 0 or more and 1 or less, R3 is ethoxy or methoxy, z is 4n-xym, n is greater than 1 and less than 10, and m is n-1 or less. The composition according to item 3, which is a vinyl oligomer siloxane containing at least two different compounds selected from the group consisting of: Section 5. The "Si-containing compound" is any one of the following: i) [ka] wherein each R is independently selected from C1-C3 alkyl and n is 1 to 16; ii) [ka] (wherein each R is independently methyl or ethyl, and n is 1 to 18); iii) [ka] wherein each R is independently methyl or ethyl; or v) The composition according to item 1, selected from any combination of i) to iii). Section 6. The "Si-containing compound" is any one of the following: ii) [ka] (wherein each R is independently methyl or ethyl, and n is 1 to 18); iii) [ka] wherein each R is independently methyl or ethyl; or v) The composition according to item 1, selected from a combination of ii) and iii). Section 7. The "Si-containing compound" is any one of the following: [ka] Item 7. The composition according to item 6, wherein the compound is selected from the combination of items ii) and iii). Section 8. Item 6. The composition according to item 6 or 7, wherein the "Si-containing compound" is selected from a combination of ii) and iii). Section 9. Item 9. The composition according to item 8, wherein the weight ratio of component iii) to component ii) is 2.0 or more. Section 10. Item 10. The composition according to item 8 or 9, wherein the weight ratio of component iii) to component ii) is 4.0 or less. Section 11. The "Si-containing compound" is any one of the following: i) [ka] (wherein each R is independently selected from C1 to C3 alkyl, and n is 1 to 16). Section 12. The "Si-containing compound" is any one of the following: i) [ka] Item 12. The composition according to item 11, selected from: Section 13. Item 13. The composition according to any one of items 1 to 12, wherein the composition further comprises an auxiliary agent. Section 14. Item 14. The composition according to any one of items 1 to 13, wherein a weight ratio of the peroxide to the "Si-containing compound" is 1.0 or more. Section 15. Item 15. The composition according to any one of items 1 to 14, wherein a weight ratio of the peroxide to the "Si-containing compound" is 6.0 or less. Section 16. Item 16. The composition according to any one of items 1 to 15, wherein the composition further comprises a hindered amine. Section 17. Item 17. The composition according to any one of items 1 to 16, wherein the composition comprises 50.0 wt.% or more of the ethylene / α-olefin / interpolymer (component a) based on the weight of the composition. Section 18. Item 18. The composition according to any one of items 1 to 17, wherein the composition comprises a total of 98.5% by weight or more of components a) to c), based on the weight of the composition. Section 19. Item 19. The composition according to any one of items 1 to 18, wherein for the ethylene / α-olefin / interpolymer, the α-olefin is a C3 to C20 α-olefin. Section 20. 20. The composition according to any one of items 1 to 19, wherein the ethylene / α-olefin / interpolymer (component a) is an ethylene / α-olefin copolymer. Section 21. The ethylene / α-olefin / interpolymer (component a) has a viscosity of 0.860 g / cc or more (1 cc=1 cm3 21. The composition according to any one of items 1 to 20, having a density of 0.1 g / mol / g or less. Section 22. 22. The composition according to any one of items 1 to 21, wherein the ethylene / α-olefin / interpolymer has a density of 0.900 g / cc or less. Section 23. 23. The composition according to any one of items 1 to 22, wherein the ethylene / α-olefin / interpolymer (component a) has a melt index (I2) of 8.0 g / 10 min or more. Section 24. 24. The composition according to any one of items 1 to 23, wherein the ethylene / α-olefin / interpolymer has a melt index (I2) of 35 g / 10 min or less. Section 25. 25. A crosslinked composition formed from the composition according to any one of items 1 to 24. Section 26. Item 26. The composition according to any one of items 1 to 25, wherein the composition has a glass adhesion strength of 90 N / cm or more. Section 27. 27. The composition according to any one of items 1 to 26, wherein the composition has a glass adhesion strength of 70 N / cm or more after aging at 85° C. and 85% humidity for 1000 hours. Section 28. The composition is 1.0×10 14 Item 28. The composition according to any one of items 1 to 27, having a volume resistivity of ohm·cm or more. Section 29. The composition is 1.0×10 17 Item 29. The composition according to any one of items 1 to 28, having a volume resistivity of ohm·cm or more. Section 30. 30. An article comprising at least one component formed from the composition according to any one of claims 1 to 29. Section 31. 31. The article of claim 30, wherein the article is a film. Section 32. Item 31. The article of item 30, wherein the article is a solar cell module. Section 33. 30. A process for forming a solar cell module, comprising laminating an "array of solar cells" between two film layers, each of the film layers being independently formed from the composition of any one of claims 1 to 29.

Claims

1. 1. A composition comprising: a) an ethylene / α-olefin / interpolymer; b) a peroxide; and c) a "Si-containing compound" selected from any combination of the following i) to iv); i) 【Chemistry 1】 wherein each R is independently selected from C1-C3 alkyl and n is 1 to 16; ii) 【Chemistry 2】 wherein each R is independently methyl or ethyl, and n is 1 to 18; iii) 【Chemistry 3】 wherein each R is independently methyl or ethyl; or iv) Vinyl oligomer siloxane A composition comprising:

2. The vinyl oligomeric siloxane has the following formula 4A: iv) R1 x R2 y R3 z Si n O m (Formula 4A) 2. The composition of claim 1, which is a vinyl oligomer siloxane comprising at least two different compounds selected from: wherein R1 is vinyl, x is 1 or more, R2 is propyl, y is 0 or more and 1 or less, R3 is ethoxy or methoxy, z is 4n-x-y-m, n is greater than 1 and less than 10, and m is n-1 or less.

3. The composition according to claim 1, wherein the "Si-containing compound" is selected from the combination of the following ii) and iii): ii) 【Chemistry 2】 wherein each R is independently methyl or ethyl, and n is 1 to 18; iii) 【Chemistry 3】 wherein each R is independently methyl or ethyl.

4. The composition according to claim 1, wherein the "Si-containing compound" is selected from any combination of the following i) to iv): 【Chemistry 4】 iv) Vinyl oligomer siloxane

5. The composition according to claim 1, wherein the "Si-containing compound" is selected from the combination of the following ii) and iii): 【Chemistry 5B】

6. A crosslinked composition formed from the composition of any one of claims 1 to 5.

7. The crosslinked composition according to claim 6, having a volume resistivity of 1.0×10 14 ohm·cm or more.

8. The crosslinked composition according to claim 6, having a volume resistivity of 1.0×10 17 ohm·cm or more.

9. An article comprising at least one component formed from the composition of any one of claims 1-8.

10. 9. A process for forming a solar cell module, comprising laminating an "array of solar cells" between two film layers, each of said film layers independently formed from the composition of any one of claims 1 to 8.

Citation Information

Patent Citations

  • Sealing material for solar cell

    JP1996148708A

  • Heat-crosslinkable resin composition for laser engraving, relief printing plate original plate for laser engraving and method for manufacturing the same, relief printing plate and method for making the same

    JP2011136431A

  • Solar cell sealing film and solar cell using the same

    JP2012174881A

  • Sealing film for solar cell and solar cell using the same

    JP2012174952A

  • Solar cell sealing film and solar cell using same

    WO2015111702A1